Thermoplastic polyurethane elastomer foamed yarn as well as preparation method and application thereof
Through the one-step impregnation and foaming method of high-pressure fluid impregnation, a double-layer structure thermoplastic polyurethane elastomeric foaming yarn is formed, which solves the problems of hard touch, poor weight and mechanical properties of the existing thermoplastic polyurethane elastomeric yarn, and achieves high Strength, lightweight and convenient weaving effect.
Patent Information
- Application Number
- CN202411233896.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-09-04
AI Technical Summary
The existing thermoplastic polyurethane elastomer foamed yarns have problems such as hard touch, heavy weight and reduced mechanical properties, which limit their application in uppers, seat fabrics, cushions, etc.
The one-step impregnation and foaming method of high-pressure fluid impregnation is adopted to form a double-layer thermoplastic polyurethane elastomeric foaming yarn through the impregnation and foaming of thermoplastic polyurethane hot melt adhesive in high-pressure fluid. Combined with the low-temperature thermoforming process, the feel and and reduce production costs and energy consumption.
The high strength, good hand feel, light weight and easy weaving performance of thermoplastic polyurethane elastomer foamed yarns is achieved, which reduces surface roughness, improves weaving continuity and yield, and avoids problems of air-running and pore collapse.
Smart Images

Figure CN118910774A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermoplastic polyurethane elastomer foaming materials, and in particular to a thermoplastic polyurethane elastomer foaming yarn and a preparation method and application thereof. Background Art
[0002] Thermoplastic polyurethane elastomer (TPU) is a semi-crystalline block polymer material prepared by a reaction extruder by combining diisocyanate, long-chain diol and short-chain diol in a certain proportion. It has excellent mechanical properties, heat resistance, chemical resistance and wear resistance. Due to its special block structure, by adjusting the proportion of each component, a product with a very wide hardness range can be obtained.
[0003] TPU yarn is a new type of textile environmentally friendly material. Compared with traditional textile fibers, it has excellent wear resistance and bending resistance, high tear strength, easy shaping, environmental protection and recyclability. At the same time, TPU yarn can also improve the strength of the upper, provide strong support for the upper, make the upper more stylish, wear-resistant, fold-resistant and burst-resistant, and facilitate lightweight design.
[0004] However, TPU yarns currently have the problem of being hard to the touch and heavy, which limits the application of TPU yarns in the fields of shoe uppers, seat fabrics, cushions, etc. At present, patents CN116770454A and CN116770455A both describe the use of thermoplastic polyurethane as the main body to prepare thermoplastic polyurethane elastomer foam yarns. Compared with traditional TPU yarns, thermoplastic polyurethane elastomer foam yarns have greatly reduced density, are lighter, and feel softer. However, the mechanical properties have declined. In addition, the surface has increased roughness due to the presence of micropores, which is not conducive to the weaving of foam yarns, resulting in certain application limitations. Summary of the invention
[0005] In view of the above technical problems and the shortcomings in the art, the present invention provides a thermoplastic polyurethane elastomer foamed yarn and a preparation method and application thereof. The thermoplastic polyurethane elastomer foamed yarn of the present invention has the excellent properties of high strength, good hand feel, light weight, high strength and convenient weaving. The preparation method of the present invention has simple process operation, safety and environmental protection, and can be produced continuously.
[0006] The specific technical solutions are as follows:
[0007] In a first aspect, the present invention provides a thermoplastic polyurethane elastomer foam yarn, comprising a thermoplastic polyurethane elastomer foam core yarn and a thermoplastic polyurethane adhesive layer covering the thermoplastic polyurethane elastomer foam core yarn.
[0008] The diameter of the thermoplastic polyurethane elastomer foamed yarn may be 0.4 to 1.5 mm.
[0009] The thermoplastic polyurethane elastomer foamed yarn can be obtained by one-step dipping and foaming, shaping, and cooling the thermoplastic polyurethane elastomer yarn impregnated with high-pressure fluid.
[0010] The one-step dipping and foaming process described in the present invention means that the foaming process and the dipping process are carried out simultaneously.
[0011] The dipping adhesive may be thermoplastic polyurethane hot melt adhesive.
[0012] In some embodiments, the high pressure fluid is a supercritical fluid.
[0013] The high-pressure fluid may include at least one of nitrogen and carbon dioxide.
[0014] The pressure of the high-pressure fluid may be 5 to 30 MPa.
[0015] The thermoplastic polyurethane elastomer yarn impregnated with high-pressure fluid contains 0.5 to 8.0 wt. % of high-pressure fluid dissolved therein.
[0016] The diameter of the thermoplastic polyurethane elastomer yarn may be 0.05-0.3 mm, such as 0.1 mm.
[0017] The thermoplastic polyurethane elastomer yarn can be obtained by extruding, drawing and shaping the thermoplastic polyurethane elastomer.
[0018] The Shore hardness of the thermoplastic polyurethane elastomer may be 70-90A, such as 80A, 85A, etc.
[0019] The extrusion temperature may be 150-220°C.
[0020] The thermoplastic polyurethane elastomer yarn impregnated with high-pressure fluid can be stored at -20 to 10°C (eg 0°C) before use, and the weight loss rate of the high-pressure fluid is preferably not higher than 25% (preferably not higher than 20%).
[0021] The high-pressure fluid-impregnated thermoplastic polyurethane elastomer yarn can be obtained by immersing the thermoplastic polyurethane elastomer yarn in a high-pressure fluid. The immersion temperature can be -10 to 50° C. The immersion time can be 1 to 10 hours.
[0022] In some embodiments, the initial flow temperature of the thermoplastic polyurethane hot melt adhesive is not higher than 120°C, and may further be 90-120°C.
[0023] In some embodiments, the temperature of the one-step dipping and foaming is 130-180°C.
[0024] In some embodiments, the residence time of the one-step dipping and foaming is 10 to 20 seconds.
[0025] The setting temperature can be 40-60° C., and the setting time can be 10-20 seconds.
[0026] The shaping may be hot air shaping.
[0027] The cooling may be spray cooling. The cooling may be cooling with cooling water. Further, the temperature of the cooling water may be 5 to 10° C. The cooling time may be 5 to 10 seconds.
[0028] A constant speed drawing operation may be added between the shaping and the cooling, and the speed of the constant speed drawing may be 3-5 m / min.
[0029] The thermoplastic polyurethane elastomer foaming core wire may be composed of one or more thermoplastic polyurethanes. The thermoplastic polyurethane adhesive layer may also be composed of one or more thermoplastic polyurethanes. The thermoplastic polyurethane constituting the thermoplastic polyurethane elastomer foaming core wire and the thermoplastic polyurethane constituting the thermoplastic polyurethane adhesive layer may be completely identical, partially identical or completely different. The present invention does not specifically limit the raw material composition of these thermoplastic polyurethanes, and common materials in the art may be used, for example, they may all include polyols, isocyanates and chain extenders. The polyol may include at least one of polyester diols, polyether diols, and polycarbonate diols. The isocyanate may include at least one of diphenylmethane-4,4' diisocyanate, toluene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, xylene diisocyanate, and hydrogenated phenylmethane diisocyanate. The chain extender may include at least one of aliphatic, aromatic or alicyclic diol compounds.
[0030] In a second aspect, the present invention provides a method for preparing the thermoplastic polyurethane elastomer foamed yarn according to the first aspect, comprising:
[0031] The thermoplastic polyurethane elastomer yarn impregnated with high-pressure fluid is subjected to one-step dipping, foaming, shaping, and cooling to obtain the thermoplastic polyurethane elastomer foamed yarn;
[0032] The dipping adhesive is made of thermoplastic polyurethane hot melt adhesive.
[0033] In the preparation method described in the second aspect, the specific selection and optimization of the technical solution can be carried out with reference to the content of the first aspect of the present invention.
[0034] In the preparation method described in the second aspect, the wire feeding speed of the thermoplastic polyurethane elastomer yarn impregnated with high-pressure fluid can be 30 to 70 mm / s.
[0035] The one-step dipping and foaming can adopt a one-step dipping and foaming device.
[0036] In some embodiments, the one-step dipping and foaming device is filled with a thermoplastic polyurethane hot melt adhesive melt, and a wire feed guide wheel, a wire guide wheel, a wire withdrawal guide wheel and a diameter limiter are sequentially arranged in the one-step dipping and foaming device along the wire feeding direction, and the position of the diameter limiter is higher than the liquid level of the thermoplastic polyurethane hot melt adhesive melt.
[0037] The number of godet wheels can be zero, one or more.
[0038] The thermoplastic polyurethane elastomer yarn impregnated with the high-pressure fluid simultaneously completes the process of dipping and foaming in the thermoplastic polyurethane hot melt adhesive melt.
[0039] The diameter of the diameter limiter may be 0.5 to 1.5 mm.
[0040] In a third aspect, the present invention provides the use of the thermoplastic polyurethane elastomer foamed yarn described in the first aspect in shoe uppers, seat fabrics, cushions, watch straps, thermal insulation shells, shock-absorbing coating shells, and bags.
[0041] Compared with the prior art, the present invention has the following beneficial effects:
[0042] The thermoplastic polyurethane elastomer foamed yarn of the present invention has the characteristics of a double-layer structure, with foamed yarn filaments inside and a thermoplastic polyurethane adhesive layer outside, wherein the internal foaming layer can provide the thermoplastic polyurethane elastomer foamed yarn with a good hand feel, and the plastic feel is significantly reduced; the external adhesive layer, on the one hand, ensures the strength of the thermoplastic polyurethane elastomer foamed yarn, and on the other hand, the external thermoplastic polyurethane adhesive layer can be thermoformed at low temperature, and the products woven from the thermoplastic polyurethane elastomer foamed yarn can be prepared into products of required shapes by adopting a low-temperature heat setting process, and the internal foamed yarn filaments will not cause the problem of gas leakage; secondly, the two steps of rubber coating and TPU yarn foaming in the preparation process of the thermoplastic polyurethane elastomer foamed yarn are combined into one step, so that the production efficiency is improved and the energy consumption is reduced. In addition, the external thermoplastic polyurethane adhesive layer can reduce the roughness of the foamed yarn surface, reduce the friction between the yarns during its weaving process, and improve the continuity and yield rate of the foamed yarn cloth weaving.
[0043] The present invention does not require the two-step operation of foaming first and then dipping in glue, and does not require secondary heating of the foamed fibers, thereby avoiding problems such as air leakage or pore collapse of the foamed fibers during the dipping process. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 The present invention is a schematic structural diagram of a one-step dipping and foaming device used in the present invention. DETAILED DESCRIPTION
[0045] The present invention will be further described below in conjunction with the accompanying drawings and specific examples. It should be understood that these examples are only intended to illustrate the present invention and are not intended to limit the scope of the present invention. The operating methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturer.
[0046] See also Figure 1 , a one-step dipping and foaming device 9, a glue inlet 6 is arranged on the bottom side, and a heating module 8 is arranged on the bottom surface. The thermoplastic polyurethane hot melt adhesive melt can enter the one-step dipping and foaming device 9 through the glue inlet 6, and the temperature is controlled by the heating module 8. A temperature controller 3 is arranged in the one-step dipping and foaming device 9 for monitoring the temperature of the thermoplastic polyurethane hot melt adhesive melt, and the number of the temperature controllers 3 can be one or more, and in this case, two. When there are multiple temperature controllers 3, they can be arranged at different heights and different positions to fully reflect the overall temperature distribution of the thermoplastic polyurethane hot melt adhesive melt in the one-step dipping and foaming device 9. The temperature controller 3 can form an interlocking control with the heating module 8, and the heating module 8 can adjust the heating work (including opening and closing, heating power, etc.) according to the comparison between the temperature of the thermoplastic polyurethane hot melt adhesive melt fed back by the temperature controller 3 and the set temperature. In the one-step dipping and foaming device 9, a wire feed guide wheel 1, a wire guide wheel 7, a wire withdrawal guide wheel 4 and a diameter limiter 5 are sequentially arranged along the wire feeding direction, and the position of the diameter limiter 5 is higher than the liquid level of the thermoplastic polyurethane hot melt adhesive melt in the one-step dipping and foaming device 9. The number of wire guide wheels 7 can be zero, one or more, and in this example, there are 6 in total. One or more of the wire feed guide wheel 1, the wire guide wheel 7, and the wire withdrawal guide wheel 4 can be partially or completely immersed in the thermoplastic polyurethane hot melt adhesive melt. The thermoplastic polyurethane elastomer yarn 10 impregnated with high-pressure fluid advances under the action of the wire feed guide wheel 1, the wire guide wheel 7, and the wire withdrawal guide wheel 4, contacts with the thermoplastic polyurethane hot melt adhesive melt, and completes the process of dipping and foaming in the thermoplastic polyurethane hot melt adhesive melt in one step, and finally passes through the diameter limiter 5. A liquid level limiter 2 is also provided in the one-step dipping and foaming device 9, and the number can be one or more, and in this example, there are 2. The liquid level limiter 2 can provide feedback when the liquid level of the thermoplastic polyurethane hot melt adhesive reaches a preset height, so as to control the liquid level of the thermoplastic polyurethane hot melt adhesive to be below the diameter limiter 5 .
[0047] The one-step dipping and foaming devices used below are all as follows Figure 1 The above structure shown.
[0048] Example 1
[0049] The preparation of thermoplastic polyurethane elastomer foamed yarn comprises the following steps:
[0050] a. Prepare the thermoplastic polyurethane elastomer yarn primary product of thermoplastic polyurethane A-1.
[0051] b. Place the thermoplastic polyurethane elastomer yarn product in a high pressure device and immerse it in a supercritical fluid (supercritical CO 2 fluid), forming an equilibrium state, after the impregnation is completed, taking out the thermoplastic polyurethane filament and subjecting it to low-temperature gas locking treatment to obtain an impregnated thermoplastic elastomer filament; wherein the amount of the supercritical fluid dissolved in the thermoplastic elastomer filament is 5.0wt.%, the temperature of the low-temperature gas locking is -20°C, and during the low-temperature gas locking treatment, the weight loss rate of the supercritical fluid is not higher than 20%.
[0052] c. The thermoplastic polyurethane elastomer yarn impregnated with high-pressure fluid prepared in step b is loaded on the unwinding wheel, passed through a one-step dipping and foaming device, a hot air channel constant speed drawing unit and a spray cooling unit and rewound at the other end to obtain a high-strength thermoplastic polyurethane elastomer foamed yarn; during this period, the selection of thermoplastic polyurethane B is listed in Table 1, thermoplastic polyurethane B-1 is added to the one-step dipping and foaming device, the temperature of the one-step dipping and foaming is 130°C, the residence time in the one-step dipping and foaming device is 20s, the temperature of the channel setting is 60°C, the residence time in the channel is 20s, the speed of the constant speed drawing is 3m / min, the cooling water temperature used in the spray cooling unit is 10°C, and the cooling time is 10s. The size of the limiter is 0.5mm. The performance evaluation of the thermoplastic polyurethane elastomer foamed yarn is listed in Table 3.
[0053] Table 1
[0054]
[0055] The specific preparation process of step a includes:
[0056] A thermoplastic polyurethane elastomer yarn preliminary product containing thermoplastic polyurethane A is prepared. According to the components and their molar ratios shown in Table 2, all components of thermoplastic polyurethane A are dried, added into a twin-screw extruder, melt-extruded and cooled to obtain thermoplastic polyurethane fiber filaments, and wound to obtain a thermoplastic polyurethane elastomer yarn preliminary product; wherein, the drying is hot air drying, the moisture content after drying is less than 0.07wt.%, the winding speed is 2m / s, and the diameter of the thermoplastic polyurethane elastomer yarn preliminary product is 0.10mm; the molar ratios and characteristics of the components of thermoplastic polyurethane A are listed in Table 2.
[0057] Table 2
[0058]
[0059] Example 2
[0060] The preparation of thermoplastic polyurethane elastomer foamed yarn comprises the following steps:
[0061] a. Prepare the thermoplastic polyurethane elastomer yarn primary product of thermoplastic polyurethane A-1; the specific process is the same as Example 1.
[0062] b. Place the thermoplastic polyurethane elastomer yarn product in a high pressure device and immerse it in a supercritical fluid (supercritical CO 2 fluid), forming an equilibrium state, after the impregnation is completed, taking out the thermoplastic polyurethane filament and subjecting it to low-temperature gas locking treatment to obtain an impregnated thermoplastic elastomer filament; wherein the amount of the supercritical fluid dissolved in the thermoplastic elastomer filament is 5.0wt.%, the temperature of the low-temperature gas locking is -20°C, and during the low-temperature gas locking treatment, the weight loss rate of the supercritical fluid is not higher than 20%.
[0063] c. The thermoplastic polyurethane elastomer yarn impregnated with high-pressure fluid prepared in step b is loaded on the unwinding wheel, passed through a one-step dipping and foaming device, a hot air channel constant speed drawing unit and a spray cooling unit and rewound at the other end to obtain a high-strength thermoplastic polyurethane elastomer foamed yarn; during this period, thermoplastic polyurethane B-1 is added to the one-step dipping and foaming device, the temperature of the one-step dipping and foaming is 150°C, the residence time in the one-step dipping and foaming device is 20s, the temperature of the channel setting is 60°C, the residence time in the channel is 20s, the speed of the constant speed drawing is 3m / min, the cooling water temperature used in the spray cooling unit is 5°C, and the cooling time is 10s. The size of the limiter is 1mm. The performance evaluation of the thermoplastic polyurethane elastomer foamed yarn is listed in Table 3.
[0064] Example 3
[0065] The preparation of thermoplastic polyurethane elastomer foamed yarn comprises the following steps:
[0066] a. Prepare the initial product of thermoplastic polyurethane elastomer yarn of thermoplastic polyurethane A-2; the specific process is referred to Example 1, the main difference is that the components of thermoplastic polyurethane A-1 in Example 1 are replaced by the components of thermoplastic polyurethane elastomer A-2.
[0067] b. Place the thermoplastic polyurethane elastomer yarn product in a high pressure device and immerse it in a supercritical fluid (supercritical CO 2 fluid), forming an equilibrium state, after the impregnation is completed, taking out the thermoplastic polyurethane filament and subjecting it to low-temperature gas locking treatment to obtain an impregnated thermoplastic elastomer filament; wherein the amount of the supercritical fluid dissolved in the thermoplastic elastomer filament is 5.0wt.%, the temperature of the low-temperature gas locking is -20°C, and during the low-temperature gas locking treatment, the weight loss rate of the supercritical fluid is not higher than 20%.
[0068] c. The thermoplastic polyurethane elastomer yarn impregnated with high-pressure fluid prepared in step b is loaded on the unwinding wheel, passed through a one-step dipping and foaming device, a hot air channel constant speed drawing unit and a spray cooling unit and rewound at the other end to obtain a high-strength thermoplastic polyurethane elastomer foamed yarn; during this period, thermoplastic polyurethane B-2 is added to the one-step dipping and foaming device, the temperature of the one-step dipping and foaming is 160°C, the residence time in the one-step dipping and foaming device is 10s, the temperature of the channel setting is 40°C, the residence time in the channel is 10s, the speed of the constant speed drawing is 5m / min, the cooling water temperature used in the spray cooling unit is 5°C, and the cooling time is 5s. The size of the limiter is 1mm. The performance evaluation of the thermoplastic polyurethane elastomer foamed yarn is listed in Table 3.
[0069] Example 4
[0070] The preparation of thermoplastic polyurethane elastomer foamed yarn comprises the following steps:
[0071] a. Prepare the thermoplastic polyurethane elastomer yarn primary product of thermoplastic polyurethane A-1; the specific process is the same as Example 1.
[0072] b. Place the thermoplastic polyurethane elastomer yarn product in a high pressure device and immerse it in a supercritical fluid (supercritical CO 2 fluid), forming an equilibrium state, after the impregnation is completed, taking out the thermoplastic polyurethane filament and subjecting it to low-temperature gas locking treatment to obtain an impregnated thermoplastic elastomer filament; wherein the amount of the supercritical fluid dissolved in the thermoplastic elastomer filament is 5.0wt.%, the temperature of the low-temperature gas locking is -20°C, and during the low-temperature gas locking treatment, the weight loss rate of the supercritical fluid is not higher than 20%.
[0073] c. The thermoplastic polyurethane elastomer yarn impregnated with high-pressure fluid prepared in step b is loaded on the unwinding wheel, passed through a one-step dipping and foaming device, a hot air channel constant speed drawing unit and a spray cooling unit and rewound at the other end to obtain a high-strength thermoplastic polyurethane elastomer foamed yarn; during this period, thermoplastic polyurethane B-2 is added to the one-step dipping and foaming device, the temperature of the one-step dipping and foaming is 180°C, the residence time in the one-step dipping and foaming device is 10s, the temperature of the channel setting is 40°C, the residence time in the channel is 10s, the speed of the constant speed drawing is 5m / min, the cooling water temperature used in the spray cooling unit is 5°C, and the cooling time is 5s. The size of the limiter is 1.5mm. The performance evaluation of the thermoplastic polyurethane elastomer foamed yarn is listed in Table 3.
[0074] Comparative Example 1
[0075] The difference between Comparative Example 1 and Example 1 is that in step c, thermoplastic polyurethane B-1 is not added to the one-step dipping and foaming device. Instead, saturated water vapor at 130°C is used instead and enters the one-step dipping and foaming device from the glue inlet. The other parameters remain unchanged to obtain thermoplastic polyurethane foamed fiber. The performance evaluation is listed in Table 3.
[0076] Comparative Example 2
[0077] The difference between Comparative Example 2 and Comparative Example 1 is that the thermoplastic polyurethane foam fiber obtained in Comparative Example 1 is loaded on the unwinding wheel, passed through a one-step dipping and foaming device, a hot air channel constant speed drawing unit and a spray cooling unit and rewound at the other end to obtain a thermoplastic polyurethane elastomer foam yarn with secondary dipping; during this period, thermoplastic polyurethane B-1 is added to the one-step dipping and foaming device, the temperature of the one-step dipping and foaming is 130°C, the residence time in the one-step dipping and foaming device is 20s, the temperature of the channel setting is 60°C, the residence time in the channel is 20s, the speed of the constant speed drawing is 3m / min, the cooling water temperature used in the spray cooling unit is 10°C, and the cooling time is 10s. The size of the limiter is 0.5mm. The performance evaluation of the thermoplastic polyurethane elastomer foam yarn is listed in Table 3.
[0078] Comparative Example 3
[0079] The difference between Comparative Example 3 and Comparative Example 1 is that the thermoplastic polyurethane foam fiber obtained in Comparative Example 1 is loaded on the unwinding wheel, passed through a one-step dipping and foaming device, a hot air channel constant speed drawing unit and a spray cooling unit and rewound at the other end to obtain a thermoplastic polyurethane elastomer foam yarn simulating secondary dipping and heating; during this period, 130°C saturated water vapor enters the one-step dipping and foaming device from the glue inlet, and stays in the one-step dipping and foaming device for 20s, the channel shaping temperature is 60°C, the residence time in the channel is 20s, the constant speed drawing speed is 3m / min, the cooling water temperature used in the spray cooling unit is 10°C, and the cooling time is 10s. The size of the limiter is 0.5mm. The performance evaluation of the thermoplastic polyurethane elastomer foam yarn is listed in Table 3.
[0080] Table 3
[0081]
[0082] From the comparative data in Table 3, we can see that:
[0083] The thermoplastic polyurethane elastomer foamed yarn of the present invention has better tensile strength, elongation at break and tear strength than that of Comparative Example 1, and the surface smoothness of the product is better, indicating that the thermoplastic polyurethane elastomer foamed yarn of the present invention has better mechanical properties than the unimpregnated thermoplastic polyurethane elastomer foamed yarn.
[0084] Compared with the comparative example 2 of the two-step dipping and foaming, the thermoplastic polyurethane elastomer foamed yarn of the present invention can achieve a lower foaming density, higher tensile strength, elongation at break and tear strength at the same foaming temperature, and the surface smoothness of the product is better, indicating that the thermoplastic polyurethane elastomer foamed yarn of the present invention through one-step dipping and foaming has better film coating and more efficient foaming efficiency than the thermoplastic polyurethane elastomer foamed yarn through two-step dipping and foaming.
[0085] Comparative Example 1 Compared with the polyurethane elastomer foamed yarn prepared in Comparative Example 3 simulating the secondary dipping heating process, the density of the foamed yarn increased significantly after being heated again after foaming, which shows that the original gas in the pores of the two-step dipping foaming process is heated and expanded, and the pores cannot wrap the gas with increased pressure therein, resulting in gas leakage. The shrinkage of the pores will lead to an increase in the density of the foamed fibers. By comparing the fiber diameters of Comparative Examples 1, 2 and 3, it can be seen that the foamed fibers are heated again during the two-step dipping process. Because of heat exchange, the hot melt adhesive will form a plastic shell that covers the fibers when it first contacts the foamed fibers. As the residence time increases, the gas in the pores escapes and the fibers shrink, resulting in a tendency for the fibers to separate from the hot melt adhesive that has been coated, which leads to poor coating of the two-step hot melt adhesive and the foamed fibers, and thus poor mechanical properties of the thermoplastic polyurethane elastomer foamed yarn foamed by the two-step dipping process.
[0086] In the description of this specification, the description of the terms "one embodiment", "some embodiments", "specific embodiments", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0087] In addition, it should be understood that after reading the above description of the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.
Claims
1. A thermoplastic polyurethane elastomer foamed yarn, characterized in that: The invention comprises a thermoplastic polyurethane elastomer foaming core wire and a thermoplastic polyurethane adhesive layer covering the thermoplastic polyurethane elastomer foaming core wire.
2. The thermoplastic polyurethane elastomer foamed yarn according to claim 1, characterized in that: The thermoplastic polyurethane elastomer foamed yarn is obtained by one-step dipping, foaming, shaping and cooling of the thermoplastic polyurethane elastomer yarn impregnated with high-pressure fluid; The dipping adhesive is made of thermoplastic polyurethane hot melt adhesive.
3. The thermoplastic polyurethane elastomer foamed yarn according to claim 2, characterized in that: The high-pressure fluid includes at least one of nitrogen and carbon dioxide; The pressure of the high-pressure fluid is 5 to 30 MPa; The thermoplastic polyurethane elastomer yarn impregnated with high-pressure fluid contains 0.5 to 8.0 wt. % of high-pressure fluid dissolved therein.
4. The thermoplastic polyurethane elastomer foamed yarn according to claim 2, characterized in that: The diameter of the thermoplastic polyurethane elastomer yarn is 0.05 to 0.3 mm; The diameter of the thermoplastic polyurethane elastomer foamed yarn is 0.4-1.5 mm.
5. The thermoplastic polyurethane elastomer foamed yarn according to claim 2 or 4, characterized in that: The thermoplastic polyurethane elastomer yarn is obtained by extruding, stretching and shaping the thermoplastic polyurethane elastomer; The Shore hardness of the thermoplastic polyurethane elastomer is 70-90A.
6. The thermoplastic polyurethane elastomer foamed yarn according to claim 2, characterized in that: The thermoplastic polyurethane elastomer yarn impregnated with high-pressure fluid is stored at -20 to 10° C. before use, and the weight loss rate of the high-pressure fluid is not higher than 25%.
7. The thermoplastic polyurethane elastomer foamed yarn according to claim 2, characterized in that: The high-pressure fluid-impregnated thermoplastic polyurethane elastomer yarn is obtained by immersing the thermoplastic polyurethane elastomer yarn in a high-pressure fluid; The immersion temperature is -10 to 50°C; The immersion time is 1 to 10 hours.
8. The thermoplastic polyurethane elastomer foamed yarn according to claim 2, characterized in that: The initial flow temperature of the thermoplastic polyurethane hot melt adhesive is not higher than 120°C, and can further be 90-120°C.
9. The thermoplastic polyurethane elastomer foamed yarn according to claim 2 or 8, characterized in that: The temperature of the one-step dipping and foaming is 130-180°C; The residence time of the one-step dipping and foaming is 10 to 20 seconds.
10. The thermoplastic polyurethane elastomer foamed yarn according to claim 2, characterized in that: The setting temperature is 40-60° C. and the time is 10-20 seconds.
11. The method for preparing thermoplastic polyurethane elastomer foamed yarn according to any one of claims 1 to 10, characterized in that: include: The thermoplastic polyurethane elastomer yarn impregnated with high-pressure fluid is subjected to one-step dipping, foaming, shaping, and cooling to obtain the thermoplastic polyurethane elastomer foamed yarn; The dipping adhesive is made of thermoplastic polyurethane hot melt adhesive.
12. The preparation method according to claim 11, characterized in that: The one-step dipping and foaming adopts a one-step dipping and foaming device; The one-step dipping and foaming device contains a thermoplastic polyurethane hot melt adhesive melt, and a wire feed guide wheel (1), a wire guide wheel (7), a wire withdrawal guide wheel (4) and a diameter limiter (5) are sequentially arranged in the one-step dipping and foaming device along the wire feeding direction, and the position of the diameter limiter (5) is higher than the liquid level of the thermoplastic polyurethane hot melt adhesive melt; The number of the godet wheels (7) is zero, one or more; The thermoplastic polyurethane elastomer yarn impregnated with the high-pressure fluid simultaneously completes the process of dipping and foaming in the thermoplastic polyurethane hot melt adhesive melt.
13. Use of the thermoplastic polyurethane elastomer foamed yarn according to any one of claims 1 to 10 in shoe uppers, seat fabrics, cushions, watch straps, thermal insulation shells, shock-absorbing coating shells, and bags.
Citation Information
Patent Citations
Breathable and moisture-absorbing automotive interior material and production process thereof
CN110144736A
Thermoplastic elastomer foaming fiber as well as preparation method and application thereof
CN116770455A
A kind of thermoplastic elastomer hollow porous fiber and its preparation method and application
CN116770456B
A core-sheath foaming line
TW202206657A
Composite filament with elastomeric core and closed-cell foam sheath
US3507741A
Cited By
Lightweight high-strength foamed TPU wrap yarn as well as preparation method and application thereof
CN120486008A