Full-scale column for compression creep test and test method

By dividing the foot ruler into a creep test section and a contraction control section, and setting up loading parts at both ends of the test section, using the load holding assembly and threaded loading component to apply pressure, the compression creep test of the large-size foot ruler is solved. The problem of the test improves the accuracy and reliability of the test and realizes an effective evaluation of the creep characteristics of the foot ruler.

CN118913907APending Publication Date: 2024-11-08HEBEI UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411159843.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art is difficult to effectively carry out compression creep tests for large-size concrete foot-size columns, and there is a lack of test devices and processes suitable for most test environments and conditions.

Method used

A foot ruler for compression creep test was designed. By dividing the foot ruler into a creep test section and a contraction control section, and loading parts are set at both ends of the test section, and loading is applied using multiple sets of load holding components and threads. The component applies axial pressure, combined with the pressure sensor and the pad, to realize the compression test of the creep test section, and at the same time, the shrinkage control section is used as a control to eliminate the influence of dry humidity and temperature.

Benefits of technology

The compression creep test of large-sized foot-sized columns is realized, which improves the accuracy and reliability of the test, avoids the equipment volume limitation, can effectively calculate the creep characteristics of the entire foot-sized column, and performs compression failure after testing. test.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118913907A_ABST
    Figure CN118913907A_ABST
Patent Text Reader

Abstract

The invention provides a full-scale column for a compression creep test and a test method, the full-scale column for the compression creep test comprises a full-scale column, a creep test section and a shrinkage contrast section are distributed on the full-scale column along the axis direction, and the two ends of the creep test section are respectively provided with a loading part extending along the radial direction of the full-scale column; and the multiple sets of load holding assemblies are arranged in the circumferential direction of the full-scale column, the load holding assemblies are connected with the two loading parts, and the load holding assemblies are used for tensioning the two loading parts to enable the two loading parts to generate a movement trend approaching each other so as to apply axial pressure to the creep test section. The full-scale column for the compression creep test has the advantages that the compression creep test can be conveniently carried out, and the test result is more accurate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure generally relates to the technical field of concrete creep testing, and in particular to a full-scale column for compression creep testing and a testing method. Background Art

[0002] Creep is an inherent time-varying property of concrete materials. Correctly estimating and predicting the impact of creep on the long-term deformation of large concrete structures is an urgent problem to be studied and solved in the current design and construction of building projects in my country. At present, most of the research on compression creep is limited to the creep of small-scale structures, while there is an extreme lack of research on the creep of full-scale concrete columns. The fundamental reason behind this is that the size of full-scale column concrete is relatively large, and there are high requirements for test conditions such as materials, space and loading equipment. At present, there is a lack of a full-scale column creep test device and test process that is suitable for most test environments and conditions. Summary of the invention

[0003] In view of the above defects or deficiencies in the prior art, it is desirable to provide a full-scale column for compression creep testing and a test method to solve the above problems.

[0004] The first aspect of the present application provides a full-scale column for compression creep testing, comprising:

[0005] A full-size column, wherein the full-size column is provided with a creep test section and a shrinkage control section along the axial direction, and both ends of the creep test section are provided with a loading portion extending radially along the full-size column;

[0006] A plurality of groups of load-holding components are arranged circumferentially around the full-size column, the load-holding components are connected to the two loading parts, and the load-holding components are used to tighten the two loading parts so that the two loading parts tend to move closer to each other, so as to apply axial pressure to the creep test section.

[0007] According to the technical solution provided in the embodiment of the present application, the load holding component includes:

[0008] A connecting member, the connecting member extending in a direction parallel to the axis of the full-length column, and having two ends respectively passing through the two loading portions;

[0009] A threaded load-applying member is disposed on a side of the load-applying portion away from the creep test section and sleeved on an end portion of the connector. The threaded load-applying member is threadedly connected to the connector so as to apply axial pressure to the load-applying portion by tightening the threaded load-applying member.

[0010] According to the technical solution provided in the embodiment of the present application, a pressure sensor and a pad are also provided on the connecting member, the pad is provided between the threaded loading member and the loading portion, one side of the pad is in contact with the loading portion, and the pressure sensor is provided at at least one end of the connecting member; and is provided between the threaded loading member and the pad.

[0011] According to the technical solution provided in the embodiment of the present application, a support section is also distributed on the full-size column on the side of the creep test section away from the shrinkage control section; a plurality of stirrups are arranged along the axial direction in the full-size column, and the stirrup density of the shrinkage control section and the support section is greater than the stirrup density of the creep test section.

[0012] According to the technical solution provided in the embodiment of the present application, carbon fiber cloth is pasted on the outer surfaces of the shrinkage control section and the support section.

[0013] According to the technical solution provided in the embodiment of the present application, a plurality of pairs of first strain terminals are arranged on the circumferential side walls of the creep test section along the axial direction of the full-size column, and each pair of the first strain terminals is arranged in a direction parallel to the axial direction of the full-size column; a plurality of pairs of second strain terminals are arranged on the circumferential side walls of the shrinkage control section around the axial direction of the full-size column, and each pair of the second strain terminals is arranged in a direction parallel to the axial direction of the full-size column.

[0014] According to the technical solution provided in the embodiment of the present application, each of the connecting members is provided with a pair of third strain terminals, and the pair of third strain terminals are arranged in an axial direction parallel to the full-size column.

[0015] According to the technical solution provided in the embodiment of the present application, a plurality of pairs of displacement meters are provided between the two loading parts, and the displacement meters are used to measure the displacement between the two loading parts.

[0016] A second aspect of the present application provides a test method, based on the full-scale column for compression creep test as described above, comprising:

[0017] Casting full-scale columns for the compression creep test of corresponding sizes according to test requirements;

[0018] Recording a first distance between each pair of the first strain terminals and a second distance between each pair of the second strain terminals;

[0019] Apply loads to the two loading parts respectively through a loading device, and tighten the threaded loading member when the reading of the pressure sensor meets the required load, so that the reading of the pressure sensor remains at the required load after the loading device is removed;

[0020] Standing for a set time to start a compression creep test, and after the compression creep test is completed, recording a third distance between each pair of the first strain terminals and a fourth distance between each pair of the second strain terminals;

[0021] The creep amount of the creep test area is calculated according to the difference between the first distance and the third distance and the difference between the second distance and the fourth distance.

[0022] According to the technical solution provided in the embodiment of the present application, after the compression creep test result, the method further includes:

[0023] recording a fifth distance between each pair of the third strain terminals and recording a sixth distance of the displacement meter;

[0024] Transferring the full-scale column after the compression creep test to a multifunctional testing machine for a compressive failure test until the creep test section is destroyed;

[0025] Record the seventh distance between each pair of the third strain terminals and the eighth distance of the displacement meter; calculate the creep amount of the connecting member according to the seventh distance and the fifth distance, and calculate the displacement difference between the two loading parts before and after the compression creep full-size column failure according to the eighth distance and the sixth distance;

[0026] The residual load of the connecting member after the compression creep test is calculated according to the creep amount of the connecting member and the elastic modulus of the connecting member.

[0027] Compared with the prior art, the beneficial effects of the present application are as follows: for a full-size column that is inconveniently large in size, the full-size column is divided into a creep test section and a shrinkage control section, and loading parts integrally formed in the creep test section are arranged at both ends of the creep test section. Loads are applied to the two loading parts through multiple groups of load-holding components so that the two loading parts have a movement tendency to approach each other, thereby achieving a compressive load on the creep test section. Since the structures of the various parts of the full-size column are exactly the same when the full-size column is cast, the creep characteristics of the entire full-size column in the compression creep test can be inferred by detecting the strain of the creep test section during the compression creep test, and the entire test process does not require the entire full-size column to be placed in a loading device for load application; by dividing the full-size column into a shrinkage control section, since the structural components of the shrinkage control section and the creep test section are the same, the shrinkage control section can be used as a control under the influence of dryness, humidity and temperature, thereby improving the accuracy of the test. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Other features, objects and advantages of the present application will become more apparent by reading the detailed description of non-limiting embodiments made with reference to the following drawings:

[0029] Figure 1A schematic diagram of the structure of a full-scale column for compression creep testing provided in Example 1 of the present application;

[0030] Figure 2 for Figure 1 Front view of a full-scale column for compression creep testing shown;

[0031] Figure 3 for Figure 1 A top view of a full-scale column used for compression creep testing is shown;

[0032] Figure 4 for Figure 2 Schematic diagram of stirrup distribution of full-scale column section for compression creep test;

[0033] Figure 5 Schematic diagram of the full-scale column dimensions for the compression creep test provided in Example 1.

[0034] Figure numbers: 1. creep test section; 2. shrinkage control section; 3. support section; 4. loading part; 5. connecting part; 6. threaded load-applying part; 7. pressure sensor; 8. pad; 9. stirrups; 10. first strain terminal; 11. second strain terminal; 12. third strain terminal. DETAILED DESCRIPTION

[0035] The present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It is to be understood that the specific embodiments described herein are only used to explain the relevant invention, rather than to limit the invention. It is also necessary to explain that, for ease of description, only the parts related to the invention are shown in the accompanying drawings.

[0036] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0037] Due to the limitation of the volume of the loading equipment in the prior art, the compression creep test is usually carried out by scaling down the actual concrete structure in proportion, which makes the test unable to fully reflect the actual performance of the concrete structure. Therefore, how to carry out the compression creep test on a large-volume full-scale column based on the limited volume of the loading equipment has become an urgent problem to be solved. Therefore, the present application proposes a full-scale column and test method for compression creep test to solve the above problem.

[0038] Example 1

[0039] Please refer to Figure 1-Figure 5 This embodiment provides a full-scale column for compression creep testing, comprising:

[0040] A full-size column, wherein a creep test section 1 and a shrinkage control section 2 are distributed along the axial direction of the full-size column, and two ends of the creep test section 1 are respectively provided with a loading portion 4 extending along the radial direction of the full-size column;

[0041] A plurality of groups of load-holding components are arranged around the circumference of the full-size column, and the load-holding components are connected to the two loading parts 4. The load-holding components are used to tighten the two loading parts 4 so that the two loading parts 4 tend to move closer to each other, so as to apply axial pressure to the creep test section 1.

[0042] Specifically, the full-scale column is cast in a one-to-one ratio according to the concrete structure to be tested according to actual needs. The cast full-scale column is at least divided into the creep test section 1 and the shrinkage control section 2 along the axis extension direction of the full-scale column. A pair of loading parts 4 are provided on the full-scale column. The loading parts 4 are integrally formed on the side wall of the full-scale column. The loading parts 4 are made of the same concrete material as the full-scale column. The pair of loading parts 4 are respectively provided at both ends of the creep test section 1. In this embodiment, the full-scale column is a four-cornered column structure of 400mm×400mm×3200mm, and the cross-sectional dimension of the full-scale column at the loading part 4 position is greater than the cross-sectional dimension at the creep test section 1 position. During the compression creep test, the creep test section 1 is used as the test section, and the shrinkage control section 2 is used as the control section. The composition and structure of the creep test section 1 are exactly the same as the actual concrete structure, but the test only intercepts a part of the full-scale column. By recording and calculating the strain of the creep test section 1, the compression creep characteristics of the creep test section 1 can be obtained, and then by calculating the ratio of the creep test section 1 to the full-scale column, the creep characteristics of the entire full-scale column in the compression creep test can be obtained. By dividing the large-sized full-scale column into different sections, the compression creep test of the large-sized full-scale column can be performed through the existing loading equipment, without being limited by the equipment volume. During the test, no load is applied to the shrinkage control section 2 to ensure that the shrinkage control section 2 creeps naturally under the current environment. Since the shrinkage control section 2 and the creep test section 1 belong to the same full-scale column, the shrinkage control section 2 and the creep test section 1 have the same creep amount under the natural state. By setting the shrinkage control section 2, interference with the test results due to factors such as humidity and temperature can be eliminated. In this embodiment, the size of the full-scale column is referenced to Figure 5 .

[0043] In this embodiment, four load-holding assemblies are provided, and the four load-holding assemblies are respectively arranged corresponding to the four sides of the full-size column. The load-holding assemblies are connected to a pair of the loading parts 4. The load-holding assemblies are used to continue to apply load to the loading parts 4 after the loading equipment is removed. The load-holding assemblies respectively apply a force to the pair of loading parts 4 to move them closer to each other, thereby compressing the creep test section 1, thereby achieving the purpose of continuously applying load to the creep test section 1.

[0044] Furthermore, the load holding component comprises:

[0045] A connecting member 5, the connecting member 5 extends in a direction parallel to the axis of the full-length column, and two ends of the connecting member 5 respectively penetrate the two loading parts 4;

[0046] The threaded load-applying member 6 is arranged on a side of the loading portion 4 away from the creep test section 1 and is sleeved on the end of the connecting member 5. The threaded load-applying member 6 is threadedly connected to the connecting member 5 so as to apply axial pressure to the loading portion 4 by tightening the threaded load-applying member 6.

[0047] Specifically, the load-holding assembly includes a connector 5 and a threaded load-applying member 6. The connector 5 is a cylindrical structure. The connector 5 is arranged between a pair of the loading parts 4. The two ends of the connector 5 respectively penetrate the pair of the loading parts 4. Optionally, the connector 5 is a precision-rolled threaded steel bar. The threaded load-applying member 6 is arranged on the side of the loading part away from the creep test section 1. The threaded load-applying member 6 is threadedly connected to the end of the connector 5. Optionally, the threaded load-applying member 6 is a bolt. During the compression creep test, the load is first applied to the loading part 4 by a loading device. When the load reaches a set value, the threaded load-applying member 6 is tightened. The load is maintained at the set value by the cooperation between the threaded load-applying member 6 and the connector 5. Then, the loading device is removed. The threaded load-applying member 6 is fixed to the connector 5 to continuously apply pressure to the loading part 4, and then the creep test section 1 is continuously pressurized to perform the compression creep test.

[0048] Furthermore, the connecting member 5 is also provided with a pressure sensor 7 and a pad 8, the pad 8 is arranged between the threaded loading member 6 and the loading portion 4, and one side of the pad 8 is in contact with the loading portion 4; the pressure sensor 7 is arranged at at least one end of the connecting member (5) and between the threaded loading member 6 and the pad 8.

[0049] Specifically, the pad 8 is sleeved on the connector 5 and cushioned between the threaded load-applying member 6 and the load-applying portion 4. The pad 8 is used to increase the effective area of ​​the threaded load-applying member 6 on the load-applying portion 4 to prevent the threaded load-applying member 6 from being over-tightened and damaging the load-applying portion 4. The pressure sensor 7 is arranged between the threaded load-applying member 6 and the pad 8 so as to detect the load applied by the threaded load-applying member 6 on the load-applying portion 4. The pressure sensor 7 only needs to be arranged at one end of the connector 5.

[0050] Furthermore, a support section 3 is distributed on the full-size column on the side of the creep test section 1 away from the shrinkage control section 2; a plurality of stirrups 9 are arranged along the axial direction in the full-size column, and the density of the stirrups 9 in the shrinkage control section 2 and the support section 3 is greater than the density of the stirrups 9 in the creep test section 1.

[0051] Specifically, after completing the compression creep test on the full-size column, it is also necessary to perform a compressive failure test on the full-size column. The compressive failure test is performed by applying pressure to both ends of the full-size column until it is destroyed. In this embodiment, the creep test section 1 needs to be subjected to compressive failure. Since the compressive failure test can apply pressure loads to both ends of the entire full-size column, the shrinkage control section 2 serves as one end to which the load is applied in the compressive failure test. The full-size column also has a support section 3 at one end of the creep test section 1 away from the shrinkage control section 2, and the support section 3 serves as the other end to which the load is applied in the compressive failure test. During the casting process of the full-scale column, a plurality of stirrups 9 are arranged along the axis direction of the full-scale column to improve the structural strength, thereby simulating the strength of the actual concrete structure; unlike the actual concrete structure, the stirrups 9 in the creep test section 1 are arranged at the same density as the actual concrete structure, and the stirrups 9 in the shrinkage control section 2 and the support section 3 are arranged at a density greater than that in the creep test section 1, so that the structural strength of the shrinkage control section 2 and the support section 3 is higher than that of the creep test section 1, thereby preventing the shrinkage control section 2 and the support section 3 from being damaged before the creep test section 1 in the compression damage test. It should be noted that the stirrups 9 are arranged perpendicular to the axis direction of the full-scale column, so increasing the stirrups 9 in the shrinkage control section 2 does not affect the creep generated by the shrinkage control section 2 under natural conditions such as dryness, humidity and temperature.

[0052] Furthermore, carbon fiber cloth is pasted on the outer surfaces of the shrinkage control section 2 and the support section 3 .

[0053] Specifically, in order to further improve the structural strength of the shrinkage control section 2 and the support section 3, three layers of CFS-I-300 carbon fiber cloth are pasted on the outer surfaces of the shrinkage control section 2 and the support section 3. The thickness of the carbon fiber cloth is set to 0.167 mm, the tensile strength is 3400 MPa, and the elastic modulus is 240 GPa.

[0054] Furthermore, a plurality of pairs of first strain terminals 10 are arranged on the circumferential side walls of the creep test section 1 along the axial direction of the full-size column, and each pair of the first strain terminals 10 is arranged in a direction parallel to the axial direction of the full-size column; a plurality of pairs of second strain terminals 11 are arranged on the circumferential side walls of the shrinkage control section 2 around the axial direction of the full-size column, and each pair of the second strain terminals 11 is arranged in a direction parallel to the axial direction of the full-size column.

[0055] Specifically, when performing the compression creep test, since the creep amount of the full-scale column is small and not easy to observe, strain terminals are provided on the creep test section 1 and the shrinkage control section 2 to facilitate the detection of the deformation amount. The deformation amount of the creep test section 1 is detected by the first strain terminal 10. At least one pair of the first strain terminals 10 is provided on each of the four side walls of the creep test section 1. The pair of the first strain terminals 10 is arranged along the axial direction of the full-scale column. Each pair of the first strain terminals 10 is used to detect the deformation amount of one side of the creep test section 1. Specifically, the deformation amount of the creep test section 1 is obtained by detecting the distance between the pair of the first strain terminals 10 before and after the test. The deformation amount of the contraction control section 2 is detected by the second strain terminal 11. At least one pair of the second strain terminals 11 is arranged on each of the four side walls of the contraction control section 2. A pair of the second strain terminals 11 is arranged along the axial direction of the full-scale column. Each pair of the second strain terminals 11 is used to detect the deformation amount of one side of the contraction control section 2. Specifically, the deformation amount of the contraction control section 2 is obtained by detecting the distance between a pair of the second strain terminals 11 before and after the test.

[0056] Furthermore, each of the connecting members 5 is provided with a pair of third strain terminals 12 , and the pair of third strain terminals 12 are arranged in an axial direction parallel to the full-length column.

[0057] Specifically, the third strain terminal 12 is used to detect the deformation of the connector 5. In the compression failure test, the deformation of the connector 5 before and after the creep test section 1 is destroyed can be detected by a pair of the third strain terminals 12. Before the connector 5 yields, the stress on the connector 5 can be calculated by multiplying the deformation of the connector 5 obtained by detection and the elastic modulus of the connector 5.

[0058] Furthermore, a plurality of pairs of displacement meters are provided between the two loading parts 4 , and the displacement meters are used to measure the displacement between the two loading parts 4 .

[0059] Specifically, the displacement meter is disposed between a pair of the loading parts 4, and is used to detect the distance between the pair of loading parts 4; one end of the displacement meter is fixed to one of the loading parts 4 through a steel bar, and the other end of the displacement meter is connected to the other loading part 4. After the creep test section 1 is destroyed, the deformation generated when the creep test section 1 is destroyed cannot be detected by the first strain terminal 10, and thus, the distance between the pair of loading parts 4 is detected by the displacement meter to obtain only the deformation of the creep test section 1.

[0060] Example 2

[0061] This embodiment provides a test method, based on the full-scale column for compression creep test as described in Embodiment 1, comprising:

[0062] S1. Casting full-scale columns of corresponding sizes for the compression creep test according to test requirements;

[0063] S2, recording a first distance between each pair of the first strain terminals 10 and a second distance between each pair of the second strain terminals 11;

[0064] S3, applying loads to the two loading parts 4 respectively through a loading device, and tightening the threaded loading member 6 when the reading of the pressure sensor 7 meets the required load, so that the reading of the pressure sensor 7 remains at the required load after the loading device is removed;

[0065] S4, standing for a set time to start a compression creep test, and after the compression creep test is completed, recording a third distance between each pair of the first strain terminals 10 and a fourth distance between each pair of the second strain terminals 11;

[0066] S5. Calculate the creep amount of the creep test area according to the difference between the first distance and the third distance and the difference between the second distance and the fourth distance.

[0067] Specifically, the test method includes a compression creep test method and a compressive failure test method, wherein the compression creep test method includes steps S1-S5:

[0068] In step S1, first, the full-scale column is cast according to the concrete structure actually to be tested. Before casting, stirrups 9 with different densities are pre-embedded in the creep test section 1, the shrinkage control section 2 and the support section 3, respectively, so that the creep test section 1, the shrinkage control section 2 and the support section 3 have different structural strengths, wherein the structural strength of the creep test section 1 is the same as the concrete structure actually to be tested, and the structural strengths of the shrinkage control section 2 and the support section 3 are higher than the structural strength of the creep test section 1.

[0069] In step S2, the first strain terminals 10 are respectively placed on the four side walls of the creep test section 1, and the second strain terminals 11 are respectively placed on the four side walls of the shrinkage control section 2. The distance between each pair of the first strain terminals 10 and the distance between each pair of the second strain terminals 11 are measured by a handheld strain gauge to obtain four first distances and four second distances, respectively, and the four first distances and the four second distances correspond to each other one by one.

[0070] In step S3, the load required for the test is first applied to the loading part 4 through the loading device, and then the threaded loading member 6 is tightened. During the tightening process, the indication of the pressure sensor 7 is observed until the pressure sensor 7 shows that the applied load is the load required for the test. The loading device is then removed. At this time, the threaded loading member 6 and the connecting member 5 cooperate to apply continuous pressure to the creep test section 1.

[0071] In step S4, after the threaded load-applying member 6 and the connecting member 5 begin to apply pressure to the creep test section 1, the compression creep process of the creep test section 1 begins, and the full-scale column is left to stand for a set time, which is set by the test personnel according to the test requirements. After the set time is over, the distance between each pair of the first strain terminals 10 is measured by a handheld strain gauge to obtain four third distances, and the distance between each pair of the second strain terminals 11 is measured by a handheld strain gauge to obtain four fourth distances.

[0072] In step S5, the compressive creep amount of the creep test section 1 on the surface can be calculated by subtracting the first distance and the third distance corresponding to each pair of the first strain terminals 10; the natural creep amount of the shrinkage control section 2 on the surface can be calculated by subtracting the second distance and the fourth distance corresponding to each pair of the second strain terminals 11. The actual creep amount of the creep test section 1 during the compressive creep process can be obtained by subtracting the compressive creep amount and the natural creep amount.

[0073] The test method provided in this embodiment can be used to perform a compressive creep test on a large-sized full-scale column, and by providing the shrinkage control section 2 on the same full-scale column, the influence of natural factors such as humidity and temperature can be eliminated, thereby ensuring more accurate test results.

[0074] Furthermore, after the compression creep test results are obtained, the following is also included:

[0075] S6, recording the fifth distance between each pair of the third strain terminals 12, and recording the sixth distance of the displacement meter;

[0076] S7, transferring the full-scale column after the compression creep test to a multifunctional testing machine for a compressive failure test until the creep test section 1 is destroyed;

[0077] S8, recording the seventh distance between each pair of the third strain terminals, and recording the eighth distance of the displacement meter; calculating the creep amount of the connecting member 5 according to the seventh distance and the fifth distance, and calculating the displacement difference between the two loading parts 4 before and after the compression creep full-size column failure according to the eighth distance and the sixth distance;

[0078] S9. Calculate the stress of the connecting member 5 in the compression failure test according to the creep amount of the connecting member 5 and the elastic modulus of the connecting member 5.

[0079] Usually, after the compression creep test of the full-scale column, it is also necessary to perform a compressive failure test on the full-scale column. The compressive failure test needs to be performed under the 30000kN multifunctional testing machine of Harbin Institute of Technology.

[0080] Specifically, the pressure failure test includes steps S6-S9:

[0081] In step S6, after completing the compression creep test, the distance between each pair of the third strain terminals 12 is measured by a handheld strain gauge, which is the fifth distance; and the reading of each displacement meter is recorded at the same time, which is the sixth distance.

[0082] In step S7, the full-size column is transferred to a multifunctional testing machine for a compressive failure test. During the compressive failure test, the full-size column is vertically placed under the pressure head of the multifunctional testing machine, with the support section 3 at the bottom and the shrinkage control section 2 at the top. The pressure of the pressure head is adjusted to control the pressure head to press down the shrinkage control section 2 until the creep test section 1 is destroyed.

[0083] In step S8, after the creep test section 1 is destroyed, the distance between each pair of the third strain terminals 12 is detected by a handheld strain gauge, which is the seventh distance; at the same time, the distance displayed by each displacement meter is recorded, which is the eighth distance; based on the difference between the fifth distance and the seventh distance corresponding to each pair of the third strain terminals 12, the creep amount of the corresponding connector 5 can be calculated; based on the difference between the sixth distance and the eighth distance corresponding to each displacement meter, the displacement difference of the corresponding surface of the creep test section 1 before and after destruction can be calculated, and then the displacement of the creep test section 1 when destroyed can be obtained.

[0084] In step S9, before the connector 5 yields, the stress of the connector 5 can be calculated based on the creep amount of the connector 5 obtained in step S8 and the elastic modulus corresponding to the connector 5. The elastic modulus of the connector 5 is related to the material of the connector 5. Taking the connector 5 in this embodiment as a high-quality rolled threaded steel bar as an example, its corresponding elastic modulus is between 200 GPa and 220 GPa.

[0085] The full-scale column provided in the present application is not only convenient for compression creep testing, but also can be used for compression failure testing after the compression creep testing. Since the structural strength of the shrinkage control section 2 and the support section 3 is relatively high, it can be avoided that the shrinkage control section 2 and the support section 3 are destroyed before the creep test section 1 during the compression failure test, resulting in the inability to conduct the test normally.

[0086] The above description is only a preferred embodiment of the present application and an explanation of the technical principles used. Those skilled in the art should understand that the scope of the invention involved in the present application is not limited to the technical solution formed by a specific combination of the above technical features, but should also cover other technical solutions formed by any combination of the above technical features or their equivalent features without departing from the inventive concept. For example, the above features are replaced with (but not limited to) technical features with similar functions disclosed in the present application.

Claims

1. A full-scale column for compression creep testing, characterized in that: include: A full-size column, wherein the full-size column is provided with a creep test section (1) and a shrinkage control section (2) distributed along the axial direction, and both ends of the creep test section (1) are respectively provided with a loading portion (4) extending along the radial direction of the full-size column; A plurality of groups of load-holding components are arranged around the circumference of the full-size column, the load-holding components are connected to the two loading parts (4), and the load-holding components are used to tighten the two loading parts (4) so ​​that the two loading parts (4) have a tendency to move toward each other, so as to apply axial pressure to the creep test section (1).

2. The full-scale column for compression creep testing according to claim 1, characterized in that: The load holding component comprises: A connecting member (5), the connecting member (5) extending in a direction parallel to the axis of the full-length column, and having two ends respectively passing through the two loading portions (4); A threaded load-applying member (6), wherein the threaded load-applying member (6) is disposed on a side of the load-applying portion (4) away from the creep test section (1), and is sleeved on an end portion of the connecting member (5), and the threaded load-applying member (6) is threadedly connected to the connecting member (5) so as to apply axial pressure to the load-applying portion (4) by tightening the threaded load-applying member (6).

3. The full-scale column for compression creep testing according to claim 2, characterized in that: The connecting member (5) is also provided with a pressure sensor (7) and a pad (8); the pad (8) is provided between the threaded load-applying member (6) and the load-applying portion (4), and one side of the pad (8) is in contact with the load-applying portion (4); the pressure sensor (7) is provided at at least one end of the connecting member (5) and between the threaded load-applying member (6) and the pad (8).

4. The full-scale column for compression creep testing according to claim 3, characterized in that: A support section (3) is also provided on the full-size column at a side of the creep test section (1) away from the shrinkage control section (2); a plurality of stirrups (9) are arranged along the axial direction in the full-size column, and the density of the stirrups (9) in the shrinkage control section (2) and the support section (3) is greater than the density of the stirrups (9) in the creep test section (1).

5. The full-scale column for compression creep testing according to claim 4, characterized in that: Carbon fiber cloth is pasted on the outer surfaces of the shrinkage control section (2) and the support section (3).

6. The full-scale column for compression creep testing according to claim 5, characterized in that: A plurality of pairs of first strain terminals (10) are arranged on the circumferential side wall of the creep test section (1) along the axial direction of the full-length column, and each pair of the first strain terminals (10) is arranged in a direction parallel to the axial direction of the full-length column; a plurality of pairs of second strain terminals (11) are arranged on the circumferential side wall of the shrinkage control section (2) around the axial direction of the full-length column, and each pair of the second strain terminals (11) is arranged in a direction parallel to the axial direction of the full-length column.

7. The full-scale column for compression creep test according to claim 6, characterized in that: A pair of third strain terminals (12) is provided on each of the connecting members (5), and the pair of third strain terminals (12) are arranged in an axial direction parallel to the full-length column.

8. The full-scale column for compression creep test according to claim 7, characterized in that: A plurality of pairs of displacement meters are provided between the two loading parts (4), and the displacement meters are used to measure the displacement between the two loading parts (4).

9. A test method, characterized in that The full-scale column for compression creep test according to claim 8 comprises: Casting full-scale columns for the compression creep test of corresponding sizes according to test requirements; Recording a first distance between each pair of the first strain terminals (10) and a second distance between each pair of the second strain terminals (11); Apply loads to the two loading parts (4) respectively through a loading device, and tighten the threaded loading member (6) when the reading of the pressure sensor (7) meets the required load, so that the reading of the pressure sensor (7) remains at the required load after the loading device is removed; Standing for a set time to start a compression creep test, and after the compression creep test is completed, recording a third distance between each pair of the first strain terminals (10) and a fourth distance between each pair of the second strain terminals (11); The creep amount of the creep test area is calculated according to the difference between the first distance and the third distance and the difference between the second distance and the fourth distance.

10. The test method according to claim 9, characterized in that: The compression creep test results also include: Recording a fifth distance between each pair of the third strain terminals (12), and recording a sixth distance of the displacement meter; Transferring the full-scale column after the compression creep test to a multifunctional testing machine for a compression failure test until the creep test section (1) is destroyed; Recording the seventh distance between each pair of the third strain terminals and the eighth distance of the displacement meter; calculating the creep amount of the connecting member (5) according to the seventh distance and the fifth distance, and calculating the displacement difference between the two loading parts (4) before and after the compression creep full-size column failure according to the eighth distance and the sixth distance; The stress of the connecting member (5) in the compression failure test is calculated based on the creep amount of the connecting member (5) and the elastic modulus of the connecting member (5).