Method for accurately detecting water absorption rate of artificial silicate functional aggregate

CN118913987APending Publication Date: 2024-11-08NO 7 ENG CO OF CHINA RAILWAY NO 8 ENG GRP CO LTD +1
-1 Cites -1 Cited by

Patent Information

Application Number
CN202410988688.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-08

Smart Images

  • Figure CN118913987A_ABST
    Figure CN118913987A_ABST
Patent Text Reader

Abstract

The invention discloses a method for accurately detecting the water absorption rate of an artificial silicate functional aggregate, which comprises the following steps: S1, drying the artificial silicate functional aggregate to constant weight, cooling and weighing; s2, putting the artificial silicate functional aggregate in the step S1 into a liquid medium which is lighter than the artificial silicate functional aggregate and can be solidified after cooling, and keeping the environmental condition at 60 DEG C or above, so that the artificial silicate functional aggregate is fully sucked into the liquid medium; and S3, after the liquid medium is solidified through low-temperature cooling, stripping off the external liquid medium, then weighing the mass of the artificial silicate functional aggregate, and calculating the water absorption rate of the artificial silicate functional aggregate. According to the method, the calculated water absorption rate is accurate, and the scheme confidence coefficient ranges from 0.95 to 0.99; meanwhile, the problem of errors caused by saturated surface dryness and the problem of large-area floating of the aggregate in the detection process are avoided, operation is easy, detection is rapid and accurate, and the method is suitable for application and popularization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of performance index detection of artificial silicate aggregate for concrete, and in particular to a method for accurately detecting the water absorption rate of artificial silicate functional aggregate. Background Art

[0002] The statements in this section merely provide background information related to the present disclosure and may not constitute prior art.

[0003] Concrete is one of the most widely used building materials. With the increase in the amount of concrete used, the demand for coarse aggregate, which accounts for the largest volume in the concrete system, has increased dramatically. However, natural aggregate resources are very limited. In order to protect the environment and achieve sustainable development of resources, many artificial aggregates with excellent performance are gradually entering the market, such as ceramsite coarse aggregate, recycled coarse aggregate, silicate functional aggregate, etc.

[0004] Artificial silicate functional aggregate is the latest artificial coarse aggregate product developed and produced in China. It uses low-quality solid waste such as slag, fly ash, tailings, steel slag, red mud, carbide slag, gasified slag as the main raw materials, adopts appropriate proportions of calcium raw materials and silicon raw materials, and is made into spherical particles through batching, balling and shelling processes. It is prepared under autoclaving conditions (steam pressure of about 1MPa, temperature of 180-240℃) with tobermorite (CaO-SiO-HO, CSH) as the main product. The stable phase has a spherical shell structure (such as Figure 1 As shown in the figure, it stabilizes the cylinder and improves the fluidity of concrete. The most important point is that the artificial silicate functional aggregate has a capillary honeycomb structure inside, which has good water absorption, water storage and water release capabilities, and can solve the contradiction that the concrete is insufficient in water and cannot be intervened by the outside during the hardening process of concrete due to hydration reaction and evaporation. According to the performance indicators specified in the current international standard "Light Aggregate and Its Test Methods Part 1: Light Aggregate" GB / T17431.1-2010, silicate functional aggregate belongs to light coarse aggregate, and bulk density, apparent density, cylinder compressive strength and water absorption are the four most basic indicators of light coarse aggregate.

[0005] Due to the important influence of the water absorption, water storage and water release capacity of silicate functional aggregate, especially the water absorption rate, on the mixture performance and durability of concrete, it is very important to accurately control the water absorption rate of silicate functional aggregate in the actual batching process.

[0006] The current national standard "Lightweight Aggregate and Its Test Methods Part 1: Lightweight Aggregate" GB / T17431.1-2010 stipulates that functional aggregate belongs to artificial industrial waste and has a density of 600-1200 kg / m 3The light aggregate has a water absorption rate of ≤10% in 1 hour. The test method is based on the provisions of "Light Aggregate and Its Test Method Part 2: Test Method" GB / T17431.2-2010:

[0007] Take 4 liters of the sample and sieve it with a sieve with a mesh size of 2.36 mm. Take the sieve residue and dry it to a constant weight for later use; mix the sample evenly, divide it into three equal parts, weigh m1 respectively, and then put it into a container filled with water. If there are particles floating on the water, they should be pressed into the water. After the sample is soaked in water for 1 hour, pour it on a wrung wet towel, hold the two ends of the towel with your hands to make it into a groove shape, let the aggregate roll back and forth on the towel 8 to 10 times, make the sample saturated and dry, and then weigh m0.

[0008] Calculation formula: w = (m0-m1) / m1×100, and the arithmetic mean of the three test values ​​is taken as the test result.

[0009] In addition, the current standards such as the national standard ("Pebbles and Crushed Stones for Construction" GB / T 14685-2022), the construction standard ("Standard for Quality and Inspection Methods of Sand and Stone for Ordinary Concrete" JGJ 52-2006) and the highway standard ("Highway Engineering Aggregate Test Procedure" JTG 3432-2024) have all made provisions for the test method of water absorption of coarse aggregate, and the results are all expressed as the percentage of water absorption of saturated surface dry crushed stone. The only difference is that the aggregate is dried to constant weight after being saturated with water. In short, the current standard for testing water absorption relies on the calculation of water absorption by saturated surface dry.

[0010] However, the saturated surface dryness of aggregate itself has the problem of large errors caused by operational factors. It is difficult to fully dry 4L aggregate by simply rolling it back and forth on a towel. This is highly random, making the water absorption data obtained by measuring it inaccurate, which in turn affects the actual mix design and leads to unstable mixture performance.

[0011] Moreover, there are some problems when this standard is used for artificial silicate functional aggregates: artificial silicate functional aggregates are light coarse aggregates with low density. The bulk density of 2.36-10 mm aggregates is generally in the range of 950-1050 kg / m 3 , apparent density is 1800~2100kg / m 3 , which means that a large amount of aggregate cannot sink into the water during the test. The floating particles can be pressed into the water manually, but a large area of ​​particles floating in the water greatly increases the burden on the test personnel and significantly increases the experimental error; and there will be errors in the measurement of saturated surface dryness. It is difficult for 4L of aggregate to reach the saturated surface dry state by rolling it back and forth on a towel 8 to 10 times. Different testers, different water temperatures and different judgment methods will bring large errors to the experimental results, which brings considerable trouble to the mix design of lightweight aggregate concrete.

[0012] The inventors of this application found in experiments that the water content measured according to the above standard method is inaccurate, which makes it difficult to control the water-binder ratio, and ultimately leads to unstable performance of the mixture, which seriously hinders the development and application of new environmentally friendly concrete materials. Through further analysis, it is found that the water absorption rate of aggregates must be accurately mastered in order to effectively control the water content of the concrete mix and determine the water-binder ratio. Summary of the invention

[0013] The purpose of the present invention is to provide a method for accurately detecting the water absorption rate of artificial silicate functional aggregate in view of the problem of inaccurate measurement of the water absorption rate of artificial silicate functional aggregate at present, avoid the error problem caused by saturated surface drying and the problem of large-area floating of aggregate during the detection process, realize adapting to the properties of artificial silicate functional aggregate, based on simple operation, quickly and accurately detecting the water absorption rate of artificial silicate functional aggregate, effectively solving key problems, and promoting the development and application of new environmentally friendly concrete materials.

[0014] The technical solution of the present invention is as follows:

[0015] A method for accurately detecting the water absorption rate of artificial silicate functional aggregate comprises the following steps:

[0016] Step S1: drying the artificial silicate functional aggregate to constant weight, cooling and weighing;

[0017] Step S2: placing the artificial silicate functional aggregate of step S1 into a liquid medium which is lighter than the artificial silicate functional aggregate and changes from liquid phase to solid phase upon cooling, and maintaining the environmental condition above 60° C. so that the artificial silicate functional aggregate can fully absorb the liquid medium;

[0018] Step S3: Cooling at low temperature until the liquid medium solidifies, peeling off the external liquid medium, and then weighing the mass of the artificial silicate functional aggregate to calculate the water absorption rate of the artificial silicate functional aggregate.

[0019] According to a preferred embodiment, the liquid medium which is lighter than the artificial silicate functional aggregate and changes from liquid phase to solid phase upon cooling can be paraffin. The melting point of paraffin is 50-80°C, and the density of liquid paraffin is 880-950 kg / m 3 , which is less dense than water and has a longer setting time. It is conducive to the full absorption of artificial silicate functional aggregate.

[0020] According to a preferred embodiment, the environmental conditions in step S2 also include being set as a vacuum environment to promote the artificial silicate functional aggregate to fully absorb the liquid medium, and the vacuum environment has an environmental vacuum degree greater than 0.06 MPa and less than 0.1 MPa.

[0021] According to a preferred embodiment, the vacuum environment in step S2 is maintained for 60-150 minutes to allow the artificial silicate functional aggregate to fully absorb the liquid medium.

[0022] In the present application, the time for sucking the liquid medium can be adjusted according to the size of the environmental vacuum degree. Under a higher vacuum degree, saturated suction can be achieved by sucking for a shorter time, while under a lower vacuum degree, saturated suction can be achieved by sucking for a longer time. It can be adjusted according to actual conditions.

[0023] Preferably, the environmental conditions in step S2 specifically include: maintaining the environmental vacuum degree at 0.06 MPa for at least 150 minutes.

[0024] Preferably, the environmental conditions in step S2 specifically include: absorbing for 90 minutes under the condition of an environmental vacuum degree of 0.08 MPa.

[0025] According to a preferred embodiment, the environmental conditions in step S2 specifically include: absorbing for 60 minutes under the condition of an environmental vacuum degree of 0.08 MPa, so that the artificial silicate functional aggregate fully absorbs the liquid medium.

[0026] According to a preferred embodiment, the vacuum environment can be provided by a vacuum water saturation machine.

[0027] According to a preferred embodiment, in step S3, the low temperature cooling temperature is: 0-5°C.

[0028] According to a preferred embodiment, the water absorption rate of the aggregate is calculated as follows:

[0029] W = Δm / m × 100%;

[0030] Where W is the water absorption rate; Δm is the mass difference of artificial silicate functional aggregate before and after saturated absorption;

[0031] m is the mass of artificial silicate functional aggregate before absorption.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] 1. A method for accurately detecting the water absorption rate of artificial silicate functional aggregate to avoid errors. After the aggregate is saturated with liquid paraffin and cooled and solidified, a spherical shell will be formed on the surface of the aggregate. The saturated surface dry state of the aggregate can be obtained by peeling off the shell, which avoids the errors caused by the human judgment of saturated surface dryness in the prior art. The saturated surface dry state obtained by different operators is consistent, which improves the accuracy of aggregate moisture content detection;

[0034] 2. A method for accurately detecting the water absorption rate of artificial silicate functional aggregates. The innovative vacuum saturation method is used to allow the paraffin liquid to be completely and quickly absorbed into the aggregates, directly replacing the existing technical indicators of 1-hour water absorption rate and 24-hour water absorption rate, which accelerates the detection process. Aggregates with lower density can also sink into liquid paraffin, without the need for artificial auxiliary aggregate immersion, simplifying the test operation process.

[0035] 3. A method for accurately detecting the water absorption rate of artificial silicate functional aggregates, which is very easy to operate, control and use, and promotes the application of new low-carbon and environmentally friendly concrete materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 This is a physical picture of artificial silicate functional aggregate;

[0037] Figure 2 The present invention is a flow chart of a method for accurately detecting the water absorption rate of artificial silicate functional aggregate. DETAILED DESCRIPTION

[0038] The specific embodiments listed in the present invention are only examples of the present invention, and the present invention is not limited to the specific embodiments described below. For those skilled in the art, any equivalent modifications and substitutions to the embodiments described below are also within the scope of the present invention. Therefore, the equal transformations and modifications made without departing from the spirit and scope of the present invention should be included in the scope of the present invention. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturers are not specified for all reagents or instruments, they are all conventional products that can be purchased commercially. In order to better illustrate the present invention, numerous specific details are given in the specific embodiments below. It should be understood by those skilled in the art that the present invention can also be implemented without certain specific details. In other embodiments, the methods, means, equipment and steps well known to those skilled in the art are not described in detail in order to highlight the purport of the present invention.

[0039] Unless otherwise defined, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art. Unless otherwise specified, the units used in this specification are all international standard units, and the numerical values ​​and numerical ranges appearing in the present invention should be understood to include the inevitable systematic errors in industrial production.

[0040] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0041] Example 1 A method for accurately detecting the water absorption rate of artificial silicate functional aggregate

[0042] 1. Instruments and equipment:

[0043] Vacuum water saturation machine: maintain the air pressure at (0-0.1)Mpa; drying oven: 0-200℃, temperature accurate to 0.1℃; electronic balance: sensitivity 0.01g, range 5000g; electric heating furnace; low temperature box; vibrating screen; ceramic container, sand and gravel screen (sieve hole is 4.75mm), tray, thermometer, etc.; semi-refined paraffin: 58#.

[0044] 2. Technical methods and steps:

[0045] 2.1 Preliminary preparation

[0046] 2.1.1 Paraffin test

[0047] Put the block of 58# paraffin wax into a ceramic container, and then put it on an electric heating furnace, set the temperature to 100℃, and measure the temperature with a thermometer when it is heated to liquid state. After it is completely melted, continue heating for 30 minutes to discharge the water and other impurities in the paraffin wax. After heating is completed, cool it down and record the time. The final result is:

[0048] Test environment temperature (℃) Melting point temperature (℃) Solidification time (hours and minutes) 23 58.2 3 hours 20 minutes

[0049] 2.1.2 Determination of aggregate vacuum saturation time and pressure.

[0050] Take 6 ceramic containers, put 5 artificial silicate functional aggregates with a particle size of 10mm and a small amount of heat-treated paraffin in each container (to ensure that the liquid paraffin can submerge the aggregate), and then put them in a drying oven with the temperature set to 60°C. After the paraffin is completely dissolved into liquid, put it in a vacuum saturator. In order to allow the paraffin to be completely absorbed into the aggregate, set different pressures and different saturation times for the saturator to determine the pressure and time for the next test. The pressures are set to normal pressure, 0.02MPa, 0.04MPa, 0.06MPa, 0.08MPa, and 0.1MPa; the time is set to 30min, 60min, 90min, 120min, and 150min. After the test is completed, take out the cooled aggregate, peel off the paraffin shell, and weigh it. The difference between the mass of the aggregate before saturation is the mass of liquid paraffin absorbed by the aggregate. The results of the test for the mass of paraffin absorbed are as follows: (unit: g)

[0051]

[0052] From the results in the above table, it can be found that the maximum mass of paraffin solution absorbed by aggregate in the vacuum saturator is about 0.30g, and the peak value can be reached when saturated for 90min at a pressure of 0.08MPa or 60min at a pressure of 0.10MPa. However, in order to ensure that the aggregate is fully absorbed by the liquid paraffin, this test method determines the saturation condition to be 0.08MPa, 90min.

[0053] 2.2 Experiment

[0054] According to Figure 2 The steps shown are as follows:

[0055] Step S1: The sample is 5-10 mm silicate functional aggregate produced by Zhejiang Zhongjin Company, as shown in the figure. Figure 1 As shown, take a 4L sample according to the standard, pass it through a 2.36mm sieve, put it in a drying oven to dry until constant weight, and then put it in a dryer to cool for later use. After the aggregate cools to room temperature, take it out and divide it into three parts, and weigh their masses respectively (recorded as m1, m2, and m3).

[0056] Step S2: Three portions of aggregate are placed in three ceramic containers respectively, and a certain amount of processed paraffin blocks are placed in each container, and then placed in an oven set at 60°C to ensure that the dissolved liquid paraffin can submerge the aggregate surface by 10 mm. If it is found that the paraffin is insufficient, sufficient paraffin can be added at any time during the oven heating process. After the aggregate is completely submerged in the liquid paraffin, the ceramic container is taken out of the oven and placed in a vacuum saturation machine, the pressure is set to 0.08 MPa, and it is operated under vacuum conditions for 90 minutes.

[0057] Step S3: After the vacuum saturation is completed, the ceramic container is taken out and the aggregate is poured onto the tray, which is immediately placed in a low temperature box at 0-5°C for solidification for 30 minutes. After the low temperature treatment, the tray is taken out, and the aggregate has become a small white ball. Then the sample is placed in a vibrating screen machine. Under the action of vibration, the paraffin shell wrapped on the surface of the aggregate is completely peeled off, and the mass is weighed respectively (recorded as m1', m2', m3').

[0058] 2.3 Result processing

[0059] 2.3.1 Calculation of mass change of three aggregate samples

[0060] Δm1=m1'-m1=1.45-1.29=0.16kg;

[0061] Δm2=m2'-m2=1.44-1.29=0.15kg;

[0062] Δm3=m3'-m3=1.46-1.29=0.17kg.

[0063] 2.3.2 Calculation of water absorption of three parts of aggregate

[0064] W1=Δm1 / m1×100%=0.16 / 1.29×100%=12.4%;

[0065] W2=Δm2 / m2×100%=0.15 / 1.29×100%=11.6%;

[0066] W3=Δm3 / m3×100%=0.17 / 1.29×100%=13.2%.

[0067] 2.3.3 Calculate the water absorption rate of the batch of silicate functional aggregate

[0068] Wl=W1+W2+W3 / 3=12.4+11.6+13.2=12.4%, the calculation result is accurate to 0.1%.

[0069] 3 Repeatability test uncertainty

[0070] The test method of the above technical solution was used to conduct a repeatability test on the water absorption rate of silicate functional aggregate. The Wl data after 10 tests are shown in the following table: (unit: %)

[0071] Wl 12.3 11.9 12.4 11.7 12.0 11.6 12.7 13.2 12.6 11.9

[0072] According to Class A uncertainty assessment:

[0073] average value

[0074] Standard Deviation

[0075] The standard uncertainty introduced by the reading

[0076] Standard uncertainty U introduced by electronic balance (Rn) =0.08%;

[0077] The combined uncertainty

[0078] The coverage factor k is 2, and the expanded uncertainty U = Uc*k = 1.02% < 2.0%.

[0079] The confidence probability P is between 0.95 and 0.99, so the detection scheme is credible.

[0080] 4. Result Verification

[0081] While conducting the above repetitive test, the vacuum saturation method (0.08MPa, 90min) and the test method specified in the prior art method ("Light Aggregate and Its Test Method Part 2: Test Method" GB / T17431.2-2010) were used to conduct 24-hour saturation tests respectively. The water absorption rate Ws1 of the silicate functional aggregate under 10 vacuum saturation conditions and the water absorption rate Ws2 of 10 normal pressure 24-hour saturation conditions are shown in the following table: (Unit %)

[0082] Ws1 12.0 12.2 9.7 11.2 9.2 8.8 12.4 11.2 9.3 11.6 Ws2 11.2 10.0 10.9 8.1 10.2 9.0 10.7 11.8 10.1 9.2

[0083] It can be seen from the test results that the vacuum saturation water absorption rate Ws1 is generally larger than the 24-hour normal pressure water absorption rate Ws2, and smaller than Wl, indicating that the aggregate can absorb the liquid more thoroughly through vacuum saturation. However, it can also be found from the data that the data of Ws1 and Ws2 vary greatly, indicating that when using water as the absorption medium, the saturated surface dry state is difficult to grasp, resulting in uncontrollable errors.

[0084] It can be seen that the test method of the technical solution of the present invention can not only effectively detect the water absorption rate of silicate functional aggregate, but also has the advantages of simplicity, efficiency and accuracy compared with the existing technology. It is more instructive for the selection of unit water consumption of aggregate in concrete mix design, which is beneficial to the development, promotion and application of new concrete materials.

[0085] The above-mentioned embodiments only express the specific implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the protection scope of the present application. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the technical solution concept of the present application, and these all belong to the protection scope of the present application.

Claims

1. A method for accurately detecting the water absorption rate of artificial silicate functional aggregate, characterized in that: The steps include: Step S1: drying the artificial silicate functional aggregate to constant weight, cooling and weighing; Step S2: placing the artificial silicate functional aggregate of step S1 into a liquid medium which is lighter than the artificial silicate functional aggregate and changes from liquid phase to solid phase upon cooling, and maintaining the environmental condition above 60° C. so that the artificial silicate functional aggregate can fully absorb the liquid medium; Step S3: Cooling at low temperature until the liquid medium solidifies, peeling off the external liquid medium, and then weighing the mass of the artificial silicate functional aggregate to calculate the water absorption rate of the artificial silicate functional aggregate.

2. The method for accurately detecting the water absorption rate of artificial silicate functional aggregate according to claim 1, characterized in that: In step S2, the liquid medium is paraffin.

3. The method for accurately detecting the water absorption rate of artificial silicate functional aggregate according to claim 2, characterized in that: The environmental conditions in step S2 also include setting a vacuum environment to promote the artificial silicate functional aggregate to fully absorb the liquid medium, and the vacuum environment has an environmental vacuum degree of 0.06MPa-0.1MPa.

4. The method for accurately detecting the water absorption rate of artificial silicate functional aggregate according to claim 3, characterized in that: In step S2, the vacuum environment is maintained for 60-150 minutes to allow the artificial silicate functional aggregate to fully absorb the liquid medium.

5. The method for accurately detecting the water absorption rate of artificial silicate functional aggregate according to claim 4, characterized in that: The environmental conditions in step S2 specifically include: maintaining the environmental vacuum degree at 0.06 MPa for at least 150 minutes.

6. The method for accurately detecting the water absorption rate of artificial silicate functional aggregate according to claim 4, characterized in that: The environmental conditions in step S2 specifically include: maintaining the environmental vacuum degree at 0.08 MPa for at least 90 minutes.

7. The method for accurately detecting the water absorption rate of artificial silicate functional aggregate according to claim 4, characterized in that: The environmental conditions in step S2 specifically include: maintaining the environmental vacuum degree at 0.10 MPa for at least 60 minutes.

8. The method for accurately detecting the water absorption rate of artificial silicate functional aggregate according to claim 3, characterized in that: The vacuum environment can be provided by a vacuum water saturation machine.

9. The method for accurately detecting the water absorption rate of artificial silicate functional aggregate according to claim 1, characterized in that: In step S3, the temperature of low temperature cooling is 0-5°C.

10. The method for accurately detecting the water absorption rate of artificial silicate functional aggregate according to claim 1, characterized in that: The water absorption rate of the aggregate in step S3 is calculated as: W = Δm / m × 100%; Where W is the water absorption rate; Δm is the mass difference of the artificial silicate functional aggregate before and after saturation absorption of liquid medium; m is the mass of artificial silicate functional aggregate before absorbing liquid medium.