Method for determining Co and Cu in ferronickel by ICP-AES (inductively coupled plasma-atomic emission spectrometry)
Through ICP-AES technology, the complex and time-consuming problem of traditional detection methods is solved, and the rapid and accurate detection of Co and Cu in nickel iron is achieved, which simplifies operations, reduces pollution, and improves detection efficiency.
Patent Information
- Application Number
- CN202410802433.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The traditional chemical detection method is used for Co and Cu in nickel iron. The detection process is complex, time-consuming, large reagent consumption and serious pollution. There is serious interference in direct measurement of cobalt in a large amount of nickel and iron, and the procedures are cumbersome.
The content of Co and Cu in nickel iron was detected by ICP-AES (inductively coupled plasma spectroscopy), and the parameter setting and standard solution preparation were performed through a plasma emission spectrometer to shorten the detection time, simplify the operation steps, and reduce reagent consumption and environmental pollution.
It realizes rapid and accurate detection of Co and Cu content in nickel iron, improves detection efficiency, simplifies operational processes, reduces environmental pollution, and has high accuracy and application value.
Smart Images

Figure CN118914169A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of chemical detection and analysis, in particular to a method for determining Co and Cu in ferronickel by using ICP-AES. Background Art
[0002] Ferronickel is widely used in cast steel and cast iron industries. Its main components are nickel and iron, with a nickel content of 20%-60%. It also contains impurities such as Co and Cu. The quality of ferronickel depends not only on the nickel content, but also on the amount of impurities. Generally, the lower the impurity content, the better. For example, a high mass fraction of the impurity element Cu will cause hot brittleness during processing. Therefore, it is very important to detect the content of Co and Cu in ferronickel.
[0003] In traditional chemical detection methods, copper is detected by the chloroform extraction spectrophotometry of neocuproine, and the analysis of trace cobalt in nickel and iron is carried out by the R-nitroso salt spectrophotometry. Traditional detection methods are not only complicated and time-consuming, but also consume a lot of reagents and are costly. Direct measurement of cobalt in a large amount of nickel and iron by atomic absorption method has serious interference and must be separated by extraction with organic flux, which is also cumbersome and polluting.
[0004] Therefore, it is particularly important to study the determination method of Co and Cu in ferronickel, which can easily, quickly and accurately determine the Co and Cu content in ferronickel to evaluate the quality of ferronickel. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a method for determining Co and Cu in ferronickel by using ICP-AES, and the content of Co and Cu in ferronickel is detected by inductively coupled plasma spectroscopy, which shortens the detection time, simplifies the operation steps, reduces reagent consumption and environmental pollution, and improves the detection efficiency.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is:
[0007] A method for measuring Co and Cu in ferronickel by ICP-AES comprises the following steps:
[0008] Step 1, prepare the plasma emission spectrometer, debug and set parameters;
[0009] Step 2, preparing hydrochloric acid, nitric acid, perchloric acid, experimental water, high-purity nickel, high-purity iron powder, cobalt standard solution and copper standard solution;
[0010] Step 3, weigh 0.1000g of the nickel-iron sample and place it in a 100ml conical flask, add 10ml of nitric acid aqueous solution or dilute aqua regia, heat at low temperature to dissolve the nickel-iron sample, add 5ml of perchloric acid, continue to add until perchloric acid smoke comes out of the bottle mouth, take it off and cool it slightly, add 10ml of water, cool to room temperature, transfer it to a 100ml volumetric flask, dilute to the scale, and shake well;
[0011] Step 4, select Co and Cu element analysis lines; determine the analysis wavelength of Co to be 228.616nm; the analysis wavelength of Cu to be 324.752nm;
[0012] Step 5, selecting 0.0600g of high-purity iron powder and 0.0400g of high-purity nickel close to the content of the nickel-iron sample as a matrix, and preparing mixed standard solutions of different concentrations;
[0013] Step 6, measuring the prepared mixed standard solutions of different concentrations on a plasma emission spectrometer, and drawing a working curve with the mass fraction of Co and Cu as the horizontal axis and the emission intensity as the vertical axis;
[0014] Step 7, after the working curve is drawn, the Co and Cu in the nickel-iron sample are detected.
[0015] The further improvement of the technical solution of the present invention is that: in step 1, the resolution of the plasma emission spectrometer at 200nm is less than 0.006nm; the parameters are set as follows: RF power is 1150W; flushing pump speed is 100rpm; analysis pump speed is 50rpm; atomization chamber pressure is 30psi; atomization gas flow rate is 0.7L / min; auxiliary gas flow rate is 0.5L / min; flushing time is 30s; integration time is short wave 15s, long wave 5s; ambient temperature is 20-25 degrees Celsius; humidity is 20%-80%; liquid argon purity is ≥99.996%.
[0016] The further improvement of the technical solution of the present invention is that: in step 2, the hydrochloric acid, the nitric acid and the perchloric acid are all of high-grade purity, the experimental water complies with the provisions of GB / T6682; the purity of the high-purity nickel is 99.9%; the purity of the high-purity iron powder is 99.9%; the concentration of the cobalt standard solution is 100 μg / mL; and the concentration of the copper standard solution is 10 μg / mL.
[0017] A further improvement of the technical solution of the present invention is that in step 3, the volume ratio of nitric acid to experimental water in the nitric acid aqueous solution is 1:3; the dilute aqua regia is configured such that the volume ratio of hydrochloric acid: nitric acid: experimental water is 3:1:8.
[0018] The further improvement of the technical solution of the present invention is that in step 5, the specific preparation process is: select 0.0600g high-purity iron powder and 0.0400g high-purity nickel with a content close to that of the nickel-iron sample as the matrix, add corresponding volumes of Co standard solution: 0, 1ml, 5ml, 10ml, 15ml, Cu standard solution: 0, 0.5ml, 1ml, 10ml, 20ml, respectively, then process according to step 3, and supplement hydrochloric acid and nitric acid to make it have the same acidity as the solution dissolved with the nickel-iron sample to be tested, and finally obtain a series of mixed standard solutions with different concentrations.
[0019] A further improvement of the technical solution of the present invention is that in step 6, the specific method of drawing the working curve is: the prepared mixed standard solution of different concentrations is measured on a plasma emission spectrometer, the mass fraction of Co and Cu is used as the horizontal axis, and the emission intensity is used as the vertical axis, and the working curve is drawn, and the correlation coefficient of the working curve is calculated, and the correlation coefficient of each element is greater than 0.999.
[0020] A further improvement of the technical solution of the present invention is that in step 7, the specific detection process is: after the working curve is drawn, the dissolved nickel-iron sample to be tested is immediately detected using the working curve at Co, 228.616nm, and Cu, 324.752nm, respectively, and the computer automatically calculates the test results, and the obtained values are the contents of Co and Cu in the nickel-iron sample.
[0021] Due to the adoption of the above technical solution, the technical progress achieved by the present invention is:
[0022] The invention is a method for simultaneously analyzing and determining Co and Cu in ferronickel based on an ICP spectrometer, and can rapidly and accurately detect the contents of Co and Cu in ferronickel; the determination result can evaluate the product quality of ferronickel; the invention has the characteristics of convenience, rapidity and high accuracy, can replace a relatively complex standard method, improves the detection efficiency, and has good application value.
[0023] The present invention adopts inductively coupled plasma spectroscopy to detect the contents of Co and Cu in nickel iron, which shortens the detection time, simplifies the operation steps, reduces reagent consumption and environmental pollution, and improves the detection efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art are briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those of ordinary skill in the art, other drawings can be obtained based on these drawings without creative work.
[0025] Figure 1The present invention provides a method flow chart of determining Co and Cu in ferronickel by ICP-AES. DETAILED DESCRIPTION
[0026] It should be noted that the terms "including" and "having" and any variations thereof in the specification and claims of the present invention and the above-mentioned drawings are intended to cover non-exclusive inclusions. For example, a process, method, system, product or apparatus comprising a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or apparatus.
[0027] The present invention is further described in detail below with reference to the accompanying drawings and embodiments:
[0028] like Figure 1 As shown, a method for determining Co and Cu in ferronickel by ICP-AES comprises the following steps:
[0029] Step 1, prepare the plasma emission spectrometer, debug it and set the parameters;
[0030] The resolution of the plasma emission spectrometer at 200nm is less than 0.006nm;
[0031] The parameters were set as follows: RF power 1150W; flushing pump speed 100rpm; analysis pump speed 50rpm; nebulizer chamber pressure 30psi; nebulizer gas flow rate 0.7L / min; auxiliary gas flow rate 0.5L / min; flushing time 30s; integration time short wave 15s, long wave 5s; ambient temperature 20-25 degrees Celsius; humidity 20%-80%; liquid argon purity ≥99.996%;
[0032] Step 2, preparing hydrochloric acid, nitric acid, perchloric acid, experimental water, high-purity nickel, high-purity iron powder, cobalt standard solution and copper standard solution;
[0033] Hydrochloric acid, nitric acid and perchloric acid are all of high-grade purity, and the experimental water meets the requirements of GB / T6682; the purity of high-purity nickel is 99.9%; the purity of high-purity iron powder is 99.9%; the concentration of cobalt standard solution is 100μg / mL; the concentration of copper standard solution is 10μg / mL;
[0034] Step 3, weigh 0.1000g of the nickel-iron sample and place it in a 100ml conical flask, add 10ml of nitric acid aqueous solution or dilute aqua regia, heat at low temperature until the nickel-iron sample is dissolved, add 5ml of perchloric acid, continue to add until perchloric acid smoke comes out of the bottle mouth, take it out and cool it slightly, add 10ml of water, cool it to room temperature, transfer it to a 100ml volumetric flask, dilute to the scale, and shake it well; the volume ratio of nitric acid to experimental water in the nitric acid aqueous solution is 1:3; the configuration of dilute aqua regia is: V (hydrochloric acid): V (nitric acid): V (water) = 3:1:8;
[0035] Step 4, select Co and Cu element analysis lines; determine the analysis wavelength of Co to be 228.616nm; the analysis wavelength of Cu to be 324.752nm;
[0036] The selection of analytical spectral lines should be combined with the spectral line table to analyze and compare the interference and sensitivity of each spectral line of the measured element. The final selection should be based on the principle of high sensitivity and less interference.
[0037] Step 5, preparation of mixed standard solution;
[0038] In order to eliminate the interference of the matrix, 0.0600g high-purity iron powder and 0.0400g high-purity nickel, which are close to the content of the nickel-iron sample, are selected as the matrix, and the corresponding volumes of Co standard solution: 0, 1ml, 5ml, 10ml, 15ml, and Cu standard solution: 0, 0.5ml, 1ml, 10ml, 20ml are added respectively, and then the nickel-iron sample is dissolved according to the method of step 3, and hydrochloric acid and nitric acid are supplemented to make it have the same acidity as the solution to be tested. The mass fractions of Co in the mixed standard solution finally obtained are 0, 0.10, 0.50, 1.00, 1.50 respectively; the mass fractions of Cu are 0, 0.005, 0.010, 0.100, 0.200 respectively;
[0039] Step 6, drawing of working curve;
[0040] The prepared mixed standard solutions of different concentrations were measured on a plasma emission spectrometer, and a working curve was drawn with the mass fraction of Co and Cu as the horizontal axis and the emission intensity as the vertical axis. The correlation coefficient of the working curve was calculated, and it was found that the correlation coefficient of each element was greater than 0.999.
[0041] Step 7, after the working curve is drawn, Co and Cu in the ferronickel sample are detected;
[0042] After the working curve is drawn, the dissolved nickel-iron sample to be tested is immediately tested at Co, 228.616nm, and Cu, 324.752nm using the working curve. The computer automatically calculates the test results, and the obtained values are the contents of Co and Cu in the nickel-iron.
[0043] Detection limit experiment
[0044] A nickel iron sample was randomly selected and measured 10 times according to the selected spectral line, power, etc. The detection limits of Co and Cu elements were calculated through the intensity of the tested sample. Five times the detection limit of the element was taken as the lower limit of the determination of the element. The results are shown in Table 1:
[0045] Table 1 Analysis spectrum, detection limit and determination lower limit
[0046]
[0047] Precision experiment
[0048] The method precision and instrument precision were determined separately.
[0049] The precision experiment of the method used the same sample to perform 5 parallel dissolutions and measured on the same working curve to verify the reproducibility of the method. The results are shown in Table 2:
[0050] Table 2 Method precision test data
[0051]
[0052] As can be seen from Table 2, the results of the five measurements were well parallelized, indicating that the sample dissolution method can dissolve completely with good precision.
[0053] Another nickel-iron sample was taken and the same dissolved sample was measured six times in succession according to the selected dissolution method to verify the precision of the instrument. The specific results are shown in Table 3:
[0054] Table 3 Instrument precision test data
[0055]
[0056] It can be seen from Table 3 that the relative standard deviations of Co and Cu are both less than 0.7%, indicating that the instrument has good analytical accuracy for the determination of Co and Cu contents in ferronickel.
[0057] Spike recovery experiment
[0058] Take a certain amount of sample with known Co and Cu content, and add equal amount of standard solution respectively in proportion, measure its strength, and calculate the recovery rate of Co and Cu elements to be 96.0% to 103.0%. The results are shown in Table 4:
[0059] Table 4 Spike recovery experiment
[0060]
[0061] The above experiments prove that the method provided by the present invention for determining Co and Cu in ferronickel by ICP-AES is feasible, and the purpose of quickly and accurately detecting the content of Co and Cu in ferronickel by ICP-AES is achieved. The detection limits of Co and Cu are 0.0059 and 0.0045 μg / mL respectively, the recovery rate is 96.0% to 102.0%, the relative standard deviation of the sample dissolution method is less than 3.3%, and the relative deviation of the instrument determination is less than 0.7%. This proves that the method is stable and reliable, suitable for the detection of Co and Cu content in ferronickel, and can replace the more complicated standard method. The product quality of ferronickel can be better evaluated.
[0062] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for determining Co and Cu in ferronickel by ICP-AES, Features: The following steps are involved: Step 1, prepare the plasma emission spectrometer, debug and set parameters; Step 2, preparing hydrochloric acid, nitric acid, perchloric acid, experimental water, high-purity nickel, high-purity iron powder, cobalt standard solution and copper standard solution; Step 3, weigh 0.1000g of the nickel-iron sample and place it in a 100ml conical flask, add 10ml of nitric acid aqueous solution or dilute aqua regia, heat at low temperature to dissolve the nickel-iron sample, add 5ml of perchloric acid, continue to add until perchloric acid smoke comes out of the bottle mouth, take it off and cool it slightly, add 10ml of water, cool to room temperature, transfer it to a 100ml volumetric flask, dilute to the scale, and shake well; Step 4, select Co and Cu element analysis lines; determine the analysis wavelength of Co to be 228.616nm; the analysis wavelength of Cu to be 324.752nm; Step 5, selecting 0.0600g of high-purity iron powder and 0.0400g of high-purity nickel close to the content of the nickel-iron sample as a matrix, preparing mixed standard solutions of different concentrations; Step 6, measuring the prepared mixed standard solutions of different concentrations on a plasma emission spectrometer, and drawing a working curve with the mass fraction of Co and Cu as the horizontal axis and the emission intensity as the vertical axis; Step 7, after the working curve is drawn, the Co and Cu in the nickel-iron sample are detected.
2. A method for measuring Co and Cu in ferronickel by ICP-AES according to claim 1, Features: In step 1, the resolution of the plasma emission spectrometer at 200nm is less than 0.006nm; the parameters are set as follows: RF power is 1150W; flushing pump speed is 100rpm; analysis pump speed is 50rpm; nebulization chamber pressure is 30psi; nebulization gas flow rate is 0.7L / min; auxiliary gas flow rate is 0.5L / min; flushing time is 30s; integration time is short wave 15s, long wave 5s; ambient temperature is 20-25 degrees Celsius; humidity is 20%-80%; liquid argon purity is ≥99.996%.
3. A method for measuring Co and Cu in ferronickel by ICP-AES according to claim 1, Features: In step 2, the hydrochloric acid, the nitric acid and the perchloric acid are all of high-grade purity, and the experimental water complies with the provisions of GB / T6682; the purity of the high-purity nickel is 99.9%; the purity of the high-purity iron powder is 99.9%; the concentration of the cobalt standard solution is 100 μg / mL; and the concentration of the copper standard solution is 10 μg / mL.
4. A method for measuring Co and Cu in ferronickel by ICP-AES according to claim 1, Features: In step 3, the volume ratio of nitric acid to experimental water in the nitric acid aqueous solution is 1:3; the dilute aqua regia is configured such that the volume ratio of hydrochloric acid: nitric acid: experimental water is 3:1:
8.
5. A method for measuring Co and Cu in ferronickel by ICP-AES according to claim 1, Features: In step 5, the specific preparation process is: select 0.0600g high-purity iron powder and 0.0400g high-purity nickel with a content close to that of the nickel-iron sample as the matrix, add corresponding volumes of Co standard solution: 0, 1ml, 5ml, 10ml, 15ml, Cu standard solution: 0, 0.5ml, 1ml, 10ml, 20ml, respectively, and then process according to step 3, and supplement hydrochloric acid and nitric acid to make it have the same acidity as the solution dissolved with the nickel-iron sample to be tested, and finally obtain a series of mixed standard solutions of different concentrations.
6. A method for measuring Co and Cu in ferronickel by ICP-AES according to claim 1, Features: In step 6, the specific method for drawing the working curve is: measuring the prepared mixed standard solutions of different concentrations on a plasma emission spectrometer, drawing the working curve with the mass fraction of Co and Cu as the horizontal axis and the emission intensity as the vertical axis, calculating the correlation coefficient of the working curve, and obtaining a correlation coefficient of each element greater than 0.
999.
7. A method for measuring Co and Cu in ferronickel by ICP-AES according to claim 1, Features: In step 7, after the working curve is drawn, the dissolved nickel-iron sample to be tested is immediately tested at Co, 228.616nm, and Cu, 324.752nm using the working curve, and the computer automatically calculates the test results, and the obtained values are the contents of Co and Cu in the nickel-iron sample.
Citation Information
Patent Citations
Multi-element simultaneous determination method for trace elements in copper-chromium electrical contact material
CN113804672A
Inductively coupled plasma emission spectrum detection method for content of Al2O3 in silica sand
CN117825359A
Method for recovering and purifying nickel from ferronickel
US20230332268A1