Measurement and calculation method for active-inert ratio of mixed coal

Through weighted statistical points and component calculations, combined with repeatability limits and reproducibility limits, the problem of slower calculation speed and poor accuracy of mixed coal compounding in the existing technology is solved, and the rapid and accurate calculation and results of live-in ratios are achieved. reliability.

CN118914179APending Publication Date: 2024-11-08BENXI BEIYING IRON & STEEL GROUP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410948411.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art cannot quickly and accurately calculate the live-in ratio of mixed coal, and the traditional method takes 8 hours to complete, which cannot meet the continuous production needs, and there are large differences in the measurement results, making it difficult to judge the accuracy.

Method used

The live-in ratio of mixed coal is quickly and accurately calculated by weighted statistical points calculation, calculation of active and inert components, and the introduction of repeatability limits and reproducibility limits to ensure the accuracy of the calculation results.

Benefits of technology

The operation-inert ratio of mixed coal is quickly and accurately calculated, meets production needs, and ensures the reliability and accuracy of the measurement results through precision judgment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004946399240000031
    Figure BDA0004946399240000031
  • Figure BDA0004946399240000032
    Figure BDA0004946399240000032
  • Figure BDA0004946399240000041
    Figure BDA0004946399240000041
Patent Text Reader

Abstract

The invention relates to a method for measuring and calculating the active-inert ratio of mixed coal. The method comprises the following steps: (1) the weighted statistical point number of the mixed coal is the sum of the weighted statistical point numbers of single coals; (2) the measured value of the active component of the single coal = the statistical point number of the single coal * the volume percentage of the active component of the single coal * the ratio of the single coal; the measured and calculated value of the active components of the mixed coal is equal to the sum of the measured and calculated values of the active components of each single coal / (100 * weighted statistical point number of the mixed coal); (3) the inertia component measurement and calculation value of the mixed coal is equal to the sum of the inertia component measurement and calculation values of the single coals / (100 * weighted statistical point number of the mixed coal); and 4) the active-inert ratio of the mixed coal = the active component measurement value of the mixed coal / the inert component measurement value of the mixed coal. The method has the advantages that the active-inert ratio of the mixed coal can be quickly measured without repeated measurement, and the accuracy of determining the active-inert ratio of the mixed coal is realized by introducing a repeatability limit and a reproducibility limit.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of coking production in the coking industry, and in particular relates to a method for calculating the active-inactive ratio of mixed coal. Background Art

[0002] The active-to-inert ratio usually refers to the ratio of active components to inert components. Specifically, it is the content of vitrinite and exinite divided by the content of inertite. This ratio can characterize the strength of coke to a certain extent. The quality of coke is closely related to the properties of coking coal. Each type of coking coal is mixed together in a certain proportion to make coke. These mixed coking coals are called "mixed coal". The active-to-inert ratio of mixed coal has a great influence on the quality of coke. The determination method is mainly to sample at different locations, then prepare, grind, measure, and finally take the average value. During the measurement process, the measurement results will be different due to the different measurement statistical points and measurement personnel. The repeated measurement method cannot well judge whether the measurement results are accurate. In addition, when the results need to be obtained quickly, it takes about 8 hours to sample, deliver, dry, prepare, grind, and measure, which cannot meet the needs of continuous production. Summary of the invention

[0003] The purpose of the present invention is to provide a method for calculating the active-inertia ratio of mixed coal, which can quickly and accurately calculate the active-inertia ratio of mixed coal to meet production needs.

[0004] To achieve the above object, the present invention is implemented through the following technical solutions:

[0005] A method for calculating the active-inert ratio of mixed coal comprises the following steps:

[0006] 1) Calculation of weighted statistical points for blended coal

[0007] Weighted statistical points of a single type of coal = statistical points of a single type of coal × volume percentage of active components of a single type of coal;

[0008] The weighted statistical points of blended coal are the sum of the weighted statistical points of each single type of coal;

[0009] 2) Calculation of active components of blended coal

[0010] The calculated value of active components of a single type of coal = the number of statistical points of a single type of coal × the volume percentage of active components of a single type of coal × the proportion of a single type of coal;

[0011] The calculated value of active components of blended coal = the sum of the calculated values ​​of active components of each single type of coal / (100×weighted statistical points of blended coal);

[0012] 3) Calculation of inert components of blended coal

[0013] The calculated value of the inert component of a single type of coal = the number of statistical points of a single type of coal × the volume percentage of the inert component of a single type of coal × the proportion of a single type of coal;

[0014] The calculated value of inert components of blended coal = the sum of the calculated values ​​of inert components of each single type of coal / (100×weighted statistical points of blended coal);

[0015] 4) Calculation of active and inert ratio of blended coal

[0016] The active-to-inert ratio of blended coal = the calculated value of active components in the blended coal / the calculated value of inert components in the blended coal.

[0017] The active components of the mixed coal are the vitrinite of each single type of coal and the exinite of each single type of coal;

[0018] The inert components of the mixed coal are the inert components of each single type of coal and the minerals of each single type of coal.

[0019] The mineral is at least one of clay minerals, sulfide minerals, carbonate minerals, silicon oxide minerals and other minerals.

[0020] The method for determining the calculation precision of the active-inert ratio of the blended coal comprises the following steps:

[0021] 1) Calculation

[0022] P=|P 实测 -P 测算 | (1)

[0023] In formula (1): P 实测 is the volume fraction of a certain micro-component measured in the blended coal; P 测算 is the volume fraction of a certain micro-component of the blended coal; P is the absolute value of the difference between the measured value and the calculated value of the volume fraction of a certain micro-component of the blended coal;

[0024] 2) P and repeatability limit P 重复 and reproducibility limit P 再现 Make a comparison

[0025] When P≤P 重复 , then the precision of a certain microscopic component of the blended coal is good;

[0026] When P 重复 <P≤P 再现 , then the precision of a certain microscopic component of the blended coal is acceptable;

[0027] When P>P 再现 , then the precision of a certain microscopic component of the blended coal is insufficient;

[0028] 3) When the precision of each microscopic component of the blended coal is good or acceptable, the activity-inertness ratio of the blended coal can be accurately calculated.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] The present invention can quickly measure the active-inertness ratio of the mixed coal without repeated measurement, and can directly calculate the active-inertness ratio of the mixed coal when necessary, and can realize the accuracy of the active-inertness ratio determination of the mixed coal by introducing repeatability limit and reproducibility limit. DETAILED DESCRIPTION

[0031] The present invention is described in detail below, but it should be noted that the implementation of the present invention is not limited to the following embodiments.

[0032] Example 1

[0033] A mixed coal is composed of 15% Hongling, 25% Hengshan, 30% Malan and 30% Xinfa. The proportions, volume fractions of microscopic components, statistical points, active components, inert components and active-inert ratios of the above-mentioned single coals are shown in Table 1.

[0034] Table 1 Proportions of each type of coal and volume fraction of its microscopic components (%)

[0035]

[0036]

[0037] As shown in Table 1, the active component volume fraction of Hongling is 56.6%, and the inert component volume fraction is 43.4%; the active component volume fraction of Hengshan is 83.4%, and the inert component volume fraction is 16.6%; the active component volume fraction of Malan is 55.8%, and the inert component volume fraction is 44.2%; the active component volume fraction of Xinfa is 83.7%, and the inert component volume fraction is 16.3%. The active-inert ratio of the blended coal is calculated as follows:

[0038] The weighted statistical points of blended coal = (15×500+25×500+30×500+30×515) / 100=505.

[0039] The calculated value of active components of blended coal = (56.6×15×500+83.4×25×500+55.8×30×500+83.7×30×515) / (100×505) = 71.3%.

[0040] The calculated value of inert components in blended coal = (43.4×15×500+16.6×25×500+44.2×30×500+16.3×30×515) / (100×505) = 28.7%.

[0041] Calculated value of active-inert ratio of blended coal = 71.3 / 28.7 = 2.48

[0042] The method for calculating the volume fraction of each microscopic component of the blended coal also uses the above-mentioned weighted algorithm, and the various calculated values ​​of the above-mentioned blended coal are shown in Table 2.

[0043] Table 2 Calculated values ​​of maceral components and active-inert ratio of blended coal

[0044]

[0045] Determine the precision of measured value of activity-inertness ratio of blended coal

[0046] Volume fraction P of each microscopic component measured in blended coal 实测 Calculate the volume fraction P of each microscopic component with mixed coal 测算 Absolute value of difference P and repeatability limit P 重复 (See Table 3) and reproducibility limit P 再现 (See Table 4) for comparison. If P≤P 重复 , then the precision of a certain microscopic component of the blended coal is good; if P 重复 <P≤P 再现 , then the precision of a certain microscopic component of the blended coal is acceptable; if P>P 再现 , then the precision of some microscopic components of the mixed coal is insufficient.

[0047] Table 3 Repeatability limits of microscopic components

[0048] Volume fraction of a certain micro-component P / % P≤10 10<P≤30 30<P≤60 60<P≤90 P>90 Repeatability limit / % 2.0 3.0 4.0 4.5 4.0

[0049] Table 4 Reproducibility limits of microscopic components

[0050] Volume fraction of a certain micro-component P / % P≤10 10<P≤30 30<P≤60 60<P≤90 P>90 Reproducibility limit / % 3.0 4.5 6.0 6.8 6.0

[0051] The same repeatability limit and reproducibility limit are applied to the mineral components, whether they are subdivided into clay minerals, sulfide minerals, carbonate minerals, silicon oxide minerals, other minerals, or the microscopic components are counted by the major mineral categories. The present invention counts the microscopic components by the major mineral categories.

[0052] For example, the measured value, calculated value, absolute value of difference, repeatability limit and precision determination of the above-mentioned blended coal are shown in Table 5.

[0053] Table 5 Measured value, calculated value, absolute value of difference, repeatability limit and precision judgment of blended coal

[0054]

[0055] It can be seen from Table 5 that the calculated values ​​of the volume fractions of the vitrinite, exinite, inertinite and minerals in the blended coal calculated by the above-mentioned weighted algorithm are all within the repeatability limit and have good precision compared with the measured values ​​of the volume fractions of the corresponding components. That is, the active-inertinite ratio of the blended coal calculated by the weighted algorithm to be 2.48 is accurate.

[0056] Example 2

[0057] A mixed coal is composed of 50% Dongqu and 50% Hengshan. The proportions, volume fractions of microscopic components, statistical points, active components, inert components and active-inert ratios of the above-mentioned single coals are shown in Table 6.

[0058] Table 6 Proportions of each type of coal and volume fraction of its microscopic components (%)

[0059]

[0060] From Table 6, we can see that the volume fraction of active components in Dongqu is 60%, and the volume fraction of inert components is 40%; the volume fraction of active components in Hengshan is 84.9%, and the volume fraction of inert components is 15.1%. The active-inert ratio of the blended coal is calculated as follows:

[0061] The weighted statistical points of blended coal = (50×500+50×521) / 100 = 510.5.

[0062] The calculated value of active components of blended coal = (60×50×500+84.9×50×521) / (100×510.5) = 72.7%.

[0063] The calculated value of inert components in blended coal = (40×50×500+15.1×50×521) / (100×510.5) = 27.3%.

[0064] Calculated value of active-inert ratio of blended coal = 72.7 / 27.3 = 2.66

[0065] The method for calculating the volume fraction of each microscopic component of the blended coal also uses the above-mentioned weighted algorithm, and the various calculated values ​​of the above-mentioned blended coal are shown in Table 7.

[0066] Table 7 Calculated values ​​of maceral components and active-inert ratio of blended coal

[0067]

[0068] Determine the precision of measured value of activity-inertness ratio of blended coal

[0069] The measured values, calculated values, absolute values ​​of differences, repeatability limits and precision determinations of the above-mentioned blended coals are shown in Table 8.

[0070] Table 8 Measured value, calculated value, absolute value of difference, repeatability limit and precision determination of blended coal

[0071]

[0072] As can be seen from Table 8, the calculated values ​​of the volume fractions of the vitrinite, exinite and inertinite of the mixed coal calculated by the above-mentioned weighted algorithm are all within the repeatability limit compared with the measured values ​​of the volume fractions of the corresponding components, and the precision is good; the calculated value of the mineral volume fraction is not within the repeatability limit compared with the actual measured value, but within the reproducibility limit, and the precision of the mineral volume fraction of this mixed coal is acceptable. In this case, it is determined whether the active-inert ratio of the mixed coal calculated by the weighted algorithm is accurate by judging whether the total active components and the total inert components meet the repeatability limit. As can be seen from Table 8, the calculated values ​​of the volume fractions of the total active components and the total inert components of the mixed coal are all within the repeatability limit compared with the actual measured values, and the precision is good, that is, the active-inert ratio of the mixed coal calculated by the weighted algorithm is 2.66, which is accurate.

Claims

1. A method for calculating the active-inactive ratio of mixed coal, characterized in that: The following steps are involved: 1) Calculation of weighted statistical points for blended coal Weighted statistical points of a single type of coal = statistical points of a single type of coal × volume percentage of active components of a single type of coal; The weighted statistical points of blended coal are the sum of the weighted statistical points of each single type of coal; 2) Calculation of active components of blended coal The calculated value of active components of a single type of coal = the number of statistical points of a single type of coal × the volume percentage of active components of a single type of coal × the proportion of a single type of coal; The calculated value of active components of blended coal = the sum of the calculated values ​​of active components of each single type of coal / (100×weighted statistical points of blended coal); 3) Calculation of inert components of blended coal The calculated value of the inert component of a single type of coal = the number of statistical points of a single type of coal × the volume percentage of the inert component of a single type of coal × the proportion of a single type of coal; The calculated value of inert components of blended coal = the sum of the calculated values ​​of inert components of each single type of coal / (100×weighted statistical points of blended coal); 4) Calculation of active and inert ratio of blended coal The active-to-inert ratio of blended coal = the calculated value of active components in the blended coal / the calculated value of inert components in the blended coal.

2. The method for calculating the active-inactive ratio of blended coal according to claim 1, characterized in that: The active components of the mixed coal are the vitrinite of each single type of coal and the exinite of each single type of coal; The inert components of the mixed coal are the inert components of each single type of coal and the minerals of each single type of coal.

3. The method for calculating the active-inactive ratio of blended coal according to claim 2, characterized in that: The mineral is at least one of clay minerals, sulfide minerals, carbonate minerals, silicon oxide minerals and other minerals.

4. The method for calculating the active-inactive ratio of blended coal according to claim 1, characterized in that: The method for determining the calculation precision of the active-inert ratio of the blended coal comprises the following steps: 1) Calculation P=|P 实测 -P 测算 | (1) In formula (1): P 实测 is the volume fraction of a certain micro-component measured in the blended coal; P 测算 is the volume fraction of a certain micro-component of the blended coal; P is the absolute value of the difference between the measured value and the calculated value of the volume fraction of a certain micro-component of the blended coal; 2) P and repeatability limit P 重复 and reproducibility limit P 再现 Make a comparison When P≤P 重复 , then the precision of a certain microscopic component of the blended coal is good; When P 重复 <P≤P 再现 , then the precision of a certain microscopic component of the blended coal is acceptable; When P>P 再现 , then the precision of a certain microscopic component of the blended coal is insufficient; 3) When the precision of each microscopic component of the blended coal is good or acceptable, the activity-inertness ratio of the blended coal can be accurately calculated.