Metal element progressive fitting vibration fatigue performance characterization method

Through the principle of gradual fitting and damage equivalent, the real stress of metal components in the resonant environment is gradually obtained, which solves the problem of inaccurate vibration fatigue performance testing in the existing technology, and realizes more accurate vibration fatigue life analysis and design of helicopter structure .

CN118917086APending Publication Date: 2024-11-08CHINA HELICOPTER RES & DEV INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411003437.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art has failed to effectively characterize the true stress performance of metal components in resonant environments, resulting in inaccurate vibration fatigue performance test results, affecting the safety of the helicopter structure.

Method used

Using the progressive fitting method, through the principle of damage equivalent and data fitting, the equivalent true stress of the metal element in the resonant environment is gradually obtained, and the S-N curve is iteratively fitted until the conditional fatigue limit error of N iterations and N-1 iterations is smaller than that of 0.5% to ensure accuracy.

Benefits of technology

It improves the accuracy of vibration fatigue performance characterization, can truly reflect the vibration fatigue characteristics of the material, improves the vibration fatigue life analysis and design of the helicopter structure, and improves structural safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118917086A_ABST
    Figure CN118917086A_ABST
Patent Text Reader

Abstract

The invention relates to the field of material-level performance characterization, in particular to a progressive fitting vibration fatigue performance characterization method for a metal element. The method comprises the following steps: firstly, fitting according to initial excitation stress and failure life of each test piece to obtain an initial S-N curve; according to the recorded value of the real stress of the dangerous section of each test piece along with the change of the test times, adopting a damage equivalence principle and combining with the initial S-N curve to obtain equivalent primary real stress; fitting is carried out according to the equivalent primary true stress and the failure life of each test piece to obtain a primary iteration S-N curve; the equivalent secondary true stress is repeatedly obtained by adopting the damage equivalence principle, and compared with the previous vibration fatigue performance research, the accuracy of the description of the fatigue performance characterization method can be improved, and the vibration fatigue characteristics of the material can be reflected more truly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of material-level performance characterization, and in particular to a method for characterizing the progressive fitting vibration fatigue performance of a metal component. Background Art

[0002] In order to conduct fatigue reliability design, probabilistic damage tolerance design, reliability life assessment and failure analysis of helicopter structures, measure the fatigue performance of materials, and provide relevant data for the compilation of load spectra, fatigue performance tests of various materials are required. At the same time, the helicopter structure is subjected to complex aerodynamic alternating loads and structural vibration loads during flight. Vibration fatigue failures caused by conventional fatigue superimposed on structural body resonance have occurred frequently on many types of domestic helicopters in recent years. They mostly appear on secondary load-bearing and locally resonant structures, seriously affecting the structural safety of helicopter platforms. Therefore, for typical metal materials of helicopters, component-level vibration fatigue tests are required to obtain the vibration fatigue SN curve performance of the material. HB5277-2021 "Vibration Fatigue Test Methods for Engine Blades and Materials" gives the specimen form, test process and SN curve test method for vibration fatigue tests.

[0003] However, due to the change in the dynamic characteristics of the specimen in a resonant environment, the stiffness of the dangerous position will decrease, and the true stress will continue to increase as the test progresses. HB5277-2021 does not provide a method for characterizing the vibration fatigue performance of the true stress of the specimen. Summary of the invention

[0004] Purpose of the Invention

[0005] The present invention proposes a new progressive fitting vibration fatigue performance characterization method to obtain the real stress performance characterization of the dangerous position of the metal component in a resonance environment.

[0006] Technical Solution

[0007] The purpose of the present invention is to provide a method for characterizing the vibration fatigue performance of metal components by progressive fitting, including damage equivalent process, data fitting and other aspects. First, the initial SN curve is obtained by fitting according to the initial excitation stress and failure life of each test piece; the equivalent primary true stress is obtained according to the recorded value of the true stress of the dangerous section of each test piece changing with the number of tests, using the damage equivalent principle, combined with the initial SN curve; then, the first iteration SN curve is obtained by fitting according to the equivalent primary true stress and failure life of each test piece; the equivalent secondary true stress is repeatedly obtained by using the damage equivalent principle, and then the secondary iteration SN curve is obtained by fitting... The fatigue limit error under the conditions of N iterations and N-1 iterations is less than 0.5% as the iteration criterion.

[0008] The specific steps include:

[0009] Step 1: Get the initial SN curve by fitting the initial stress results of the group method and lift method tests;

[0010] Step 2: According to the initial SN curve, obtain the equivalent primary true stress of a single specimen;

[0011] Step 3: Fit the equivalent first-time true stress results of the group method and lift method tests to obtain a first-time iterative SN curve;

[0012] Step 4: According to the first iteration SN curve, the equivalent quadratic true stress of a single specimen is obtained;

[0013] Step 5: According to the test equivalent quadratic true stress results of the group method and the lifting method, the quadratic iterative SN curve is obtained by fitting;

[0014] Step 6: Similarly, iterate sequentially until the fatigue limit error is less than 0.5% after N iterations and N-1 iterations.

[0015] Furthermore, step one is as follows: the test piece is placed on a vibration table, and a vibration fatigue test is performed by providing basic excitation through the vibration table. Calibration is performed before the formal test to obtain the relationship between the response acceleration of the test piece and the true stress at the dangerous position. During the test, the response acceleration of each test piece and the corresponding number of cycles are recorded. The initial SN curve is fitted by the stress value corresponding to the initial excitation acceleration of each test piece by the grouping method and the lifting method. The expression of the sample SN curve is usually given by a three-parameter power function fitting:

[0016] lgN=a0-b0×lg(S max -S ∞0 ) (1)

[0017] Among them, a0 and b0 are material parameters, which vary according to the material and state of the sample, S ∞0 is the material fatigue limit corresponding to an infinite number of cycles, N is the failure life of the specimen, S max is the maximum stress, that is, the initial stress at the dangerous position of the specimen.

[0018] Furthermore, step 2 is specifically as follows: for a single specimen, under constant amplitude cyclic stress S i The number of test cycles recorded below is n i According to equation (1), at this stress S i The fatigue life under the action is N i (S i ), after experiencing the stress level S i n i The damage after the second cycle D i (S i ) can be defined as:

[0019]

[0020] When the specimen is cycled to failure, the total number of cycles n is recorded. i A total of k stress levels S i The total damage D1 it suffers can be defined as:

[0021]

[0022] According to equation (1), the equivalent primary true stress S of the specimen is a1 The fatigue life is N(S a1 ), the damage under the total number of cycles can be defined as:

[0023]

[0024] According to the damage equivalence principle, D1=D a1 , the equivalent primary true stress S of the specimen can be obtained a1 .

[0025] Furthermore, step three is as follows: adopt the method of step two to obtain the equivalent primary true stress of each specimen, and then combine the test results of the group method and the lifting method to obtain the first iteration SN curve by fitting as follows:

[0026] lgN=a0′-b0′×lg(S max -S ∞0 ′) (5)

[0027] Further, step 4 is specifically as follows: according to formula (5), repeat step 2, according to the constant amplitude cyclic stress S i The number of test cycles recorded below is n i The equivalent secondary true stress S of a single specimen can be obtained by using the damage equivalence a2 ;

[0028] Furthermore, step five is as follows: using the method of step two, the equivalent secondary true stress of each specimen is obtained, and then combining the test results of the group method and the lifting method, the secondary iterative SN curve is obtained by fitting as follows:

[0029] lgN=a0″-b0″×lg(S max -S ∞0 ″) (6)

[0030] Furthermore, step six is ​​as follows: repeat the iterative process, taking N = 1 × 10 7 cycle, obtain the fatigue limit error of N iterations and N-1 iterations, and take the error value less than 0.5% as the iteration termination condition.

[0031] Furthermore, the metal element is 35Cr2Ni4MoA alloy steel, 40CrNiMoA alloy steel, 7050 aluminum alloy or 2A14 aluminum alloy.

[0032] Furthermore, the grouping method in step 1 preliminarily selects a failure life of 1×10 5 times, 5×10 5 times, 1×10 6 The test load is set at the corresponding stress level.

[0033] Furthermore, the lifting method in step 1 is performed at 1×10 7 The conditional fatigue limit of the material is determined again.

[0034] Furthermore, the calibration test in step 1 is to obtain the corresponding relationship between the strain on the test piece and the response acceleration. When the formal test is carried out, the strain gauge may deform and fail due to the change in the stiffness of the test piece.

[0035] Furthermore, the SN curve in step 1 may be fitted in the form of a power function or an exponential function.

[0036] Furthermore, the damage accumulation in step 2 adopts Miner's linear cumulative damage theory. The beneficial effects of this application are:

[0037] (1) Since the current vibration fatigue performance characterization method for metal components is based on fitting according to input load and damage life, the real stress changes in dangerous positions of the specimen are not considered. The progressive fitting vibration fatigue performance characterization method provided by the present invention can obtain the equivalent real stress of the component through the damage equivalence principle, and then perform vibration fatigue performance fitting characterization based on the real stress and damage life. Compared with previous vibration fatigue performance research, it can improve the accuracy of the fatigue performance characterization method description and ensure a more realistic reflection of the vibration fatigue characteristics of the material.

[0038] (2) Local vibration fatigue problems frequently occur in helicopter secondary load-bearing structures. The present invention provides a method for characterizing vibration fatigue performance using real stress that takes into account changes in the stiffness of metal components. This method can truly reflect the structural vibration fatigue characteristics and improve the existing method for analyzing the vibration fatigue life of typical helicopter structures. At the same time, it can be widely used in vibration fatigue life assessment of various types of helicopters and in the vibration fatigue resistance design and analysis of structural parts of various types of helicopters. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 is a schematic diagram of the test piece;

[0040] Figure 2 It is a schematic diagram of the calibration relationship;

[0041] 1-Clamping end; 2-Strain gauge pasting; 3-Fixed response accelerometer. DETAILED DESCRIPTION

[0042] In order to make the purpose, technical scheme and advantages of the implementation of the present invention clearer, the technical scheme in the embodiment of the present invention will be described in more detail below in conjunction with the drawings in the embodiment of the present invention. In the drawings, the same or similar reference numerals throughout represent the same or similar originals or elements with the same or similar functions. The described embodiments are part of the embodiments of the present invention, not all of the embodiments. The embodiments described below with reference to the drawings are exemplary and intended to be used to explain the present invention, and should not be construed as limitations on the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. The embodiments of the present invention are described in detail below in conjunction with the drawings.

[0043] (1) The present invention proposes characterizing the real stress at the dangerous position based on the damage equivalence principle for the component-level vibration fatigue test of metal materials, which can more realistically reflect the material properties;

[0044] (2) Considering the SN curve test of vibration fatigue of metal materials, the fitting method is gradually iterated. The present invention provides a method for characterizing the real stress performance of vibration fatigue, which can provide the vibration fatigue characteristic parameters of metal materials.

[0045] The progressive fitting vibration fatigue performance characterization method of metal components includes the damage equivalent process, data fitting and other aspects. First, the initial SN curve is obtained by fitting according to the initial excitation stress and failure life of each test piece; according to the recorded value of the true stress of the dangerous section of each test piece changing with the number of tests, the damage equivalent principle is used, combined with the initial SN curve, to obtain the equivalent primary true stress; then, according to the equivalent primary true stress and failure life of each test piece, the first iteration SN curve is obtained by fitting; the damage equivalent principle is also used to repeatedly obtain the equivalent secondary true stress, and then the secondary iteration SN curve is obtained by fitting... The fatigue limit error under the conditions of N iterations and N-1 iterations is less than 0.5% as the iteration criterion.

[0046] The specific steps include:

[0047] Step 1: Get the initial SN curve by fitting the initial stress results of the group method and lift method tests;

[0048] Step 2: According to the initial SN curve, obtain the equivalent primary true stress of a single specimen;

[0049] Step 3: Fit the equivalent first-time true stress results of the group method and lift method tests to obtain a first-time iterative SN curve;

[0050] Step 4: According to the first iteration SN curve, the equivalent quadratic true stress of a single specimen is obtained;

[0051] Step 5: According to the test equivalent quadratic true stress results of the group method and the lifting method, the quadratic iterative SN curve is obtained by fitting;

[0052] Step 6: Similarly, iterate sequentially until the fatigue limit error is less than 0.5% after N iterations and N-1 iterations.

[0053] The present invention is further described in detail below by taking the metal component level progressive fitting vibration fatigue performance characterization method as an example in conjunction with the accompanying drawings:

[0054] Step 1: Test piece Figure 1 The vibration fatigue test is carried out by placing it on a vibration table and providing basic excitation through the vibration table. Calibration is performed before the formal test to obtain the relationship between the test piece's response acceleration and the actual stress at the hazardous position. Figure 2 During the test, the response acceleration of each specimen and the corresponding number of cycles are recorded. The initial SN curve is fitted by the stress value corresponding to the initial excitation acceleration of each specimen by the grouping method and the lifting method. The expression of the specimen SN curve is usually given by a three-parameter power function fitting:

[0055] lgN=a0-b0×lg(S max -S ∞0 ) (1)

[0056] Among them, a0 and b0 are material parameters, which vary according to the material and state of the sample, S ∞0 is the material fatigue limit corresponding to an infinite number of cycles, N is the failure life of the specimen, S max is the maximum stress, that is, the initial stress at the dangerous position of the specimen.

[0057] Step 2: For a single specimen, under constant amplitude cyclic stress S i The number of test cycles recorded below is n i According to equation (1), at this stress S i The fatigue life under the action is N i (S i ), after experiencing the stress level S i n i The damage after the second cycle D i (S i ) can be defined as:

[0058]

[0059] When the specimen is cycled to failure, the total number of cycles n is recorded. i A total of k stress levels Si The total damage D1 it suffers can be defined as:

[0060]

[0061] According to equation (1), the equivalent primary true stress S of the specimen is a1 The fatigue life is N(S a1 ), the damage under the total number of cycles can be defined as:

[0062]

[0063] According to the damage equivalence principle, D1=D a1 , the equivalent primary true stress S of the specimen can be obtained a1 .

[0064] Step 3: Using the method in step 2, the equivalent primary true stress of each specimen can be obtained. Combining the test results of the group method and the lifting method, the first iteration SN curve is fitted as follows:

[0065] lgN=a0′-b0′×lg(S max -S ∞0 ′) (5)

[0066] Step 4: According to formula (5), repeat step 2 and calculate the constant amplitude cyclic stress S i The number of test cycles recorded below is n i The equivalent secondary true stress S of a single specimen can be obtained by using the damage equivalence a2 ;

[0067] Step 5: Using the method in step 2, the equivalent secondary true stress of each specimen can be obtained. Combining the test results of the group method and the lifting method, the secondary iterative SN curve is fitted as follows:

[0068] lgN=a0″-b0″×lg(S max -S ∞0 ″) (6)

[0069] Step 6: Repeat the iterative process, taking N = 1 × 10 7 cycle, obtain the fatigue limit error of N iterations and N-1 iterations, and take the error value less than 0.5% as the iteration termination condition.

[0070] In a certain implementation case of the present invention, the metal element is a typical material used in the secondary load-bearing structure of a helicopter, specifically: 35Cr2Ni4MoA alloy steel, 40CrNiMoA alloy steel, 7050 aluminum alloy, 2A14 aluminum alloy, etc.

[0071] In a certain embodiment of the present invention, the grouping method in step 1 preliminarily selects a failure life of 1×10 5 times, 5×10 5 times, 1×10 6 The test load is set at the corresponding stress level.

[0072] In one embodiment of the present invention, the lifting method in step 1 is performed at 1×10 7 The conditional fatigue limit of the material is determined again.

[0073] In a certain implementation case of the present invention, the calibration test in step one is to obtain the corresponding relationship between the strain on the test piece and the response acceleration. When conducting a formal test, the strain gauge may deform and fail due to changes in the stiffness of the test piece, so it is only necessary to record the response acceleration under the corresponding number of tests.

[0074] In a certain implementation case of the present invention, the SN curve in the step 1 may also be fitted in the form of a power function or an exponential function.

[0075] In a certain implementation case of the present invention, the damage accumulation in the step 2 adopts Miner's linear cumulative damage theory, ignoring the influence of the order of load cycles, and linearly superimposes the damage under each level of load to obtain the total damage.

[0076] It is understood by those skilled in the art that, unless otherwise defined, all terms (including technical terms and scientific terms) used herein have the same meaning as the general understanding of ordinary technicians in the field to which the present invention belongs. It should also be understood that terms such as those defined in general dictionaries should be understood to have the same meaning as in the context of the prior art, and unless defined as here, will not be interpreted with idealized or overly formal meanings. The specific implementation methods described above further describe the purpose, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the present invention. Within the spirit and principle of the present invention, any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment of equivalent changes for application in other fields, but any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the technical solution content of the present invention, any modification, equivalent replacement, improvement, etc., made according to the technical essence of the present invention, should be included in the protection scope of the present invention.

Claims

1. A method for characterizing the vibration fatigue performance of metal components by progressive fitting, characterized in that: It includes damage equivalent process and data fitting; firstly, the initial SN curve is obtained by fitting according to the initial excitation stress and failure life of each test piece; according to the recorded value of the true stress of the dangerous section of each test piece changing with the number of tests, the damage equivalent principle is adopted, combined with the initial SN curve, to obtain the equivalent primary true stress; then, according to the equivalent primary true stress and failure life of each test piece, a first-order SN curve is obtained by fitting; the damage equivalent principle is also used to repeatedly obtain the equivalent secondary true stress, and then the secondary iterative SN curve is obtained by fitting... The fatigue limit error under the conditions of N iterations and N-1 iterations is less than 0.5% as the iteration criterion.

2. The method according to claim 1, characterized in that The specific steps include: Step 1: Get the initial SN curve by fitting the initial stress results of the group method and lift method tests; Step 2: According to the initial SN curve, obtain the equivalent primary true stress of a single specimen; Step 3: Fit the equivalent first-time true stress results of the group method and lift method tests to obtain a first-time iterative SN curve; Step 4: According to the first iteration SN curve, the equivalent quadratic true stress of a single specimen is obtained; Step 5: According to the test equivalent quadratic true stress results of the group method and the lifting method, the quadratic iterative SN curve is obtained by fitting; Step 6: Similarly, iterate sequentially until the fatigue limit error is less than 0.5% after N iterations and N-1 iterations.

3. The method according to claim 2, characterized in that Step 1 is as follows: the test piece is placed on a vibration table, and a vibration fatigue test is performed by providing basic excitation through the vibration table. Calibration is performed before the formal test to obtain the relationship between the response acceleration of the test piece and the true stress at the hazardous position. The response acceleration of each test piece and the corresponding number of cycles are recorded during the test. The initial SN curve is fitted by the stress value corresponding to the initial excitation acceleration of each test piece by the grouping method and the lifting method. The expression of the sample SN curve is usually given by a three-parameter power function fitting: lgN=a0-b0×lg(S max -S ∞0 ) (1) Among them, a0 and b0 are material parameters, which vary according to the material and state of the sample, S ∞0 is the material fatigue limit corresponding to an infinite number of cycles, N is the failure life of the specimen, S max is the maximum stress, that is, the initial stress at the dangerous position of the specimen.

4. The method according to claim 2, characterized in that Step 2 is as follows: for a single specimen, under constant amplitude cyclic stress S i The number of test cycles recorded below is n i According to equation (1), at this stress S i The fatigue life under the action is N i (S i ), after experiencing the stress level S i n i The damage after the second cycle D i (S i ) can be defined as: When the specimen is cycled to failure, the total number of cycles n is recorded. i A total of k stress levels S i The total damage D1 it suffers can be defined as: According to equation (1), the equivalent primary true stress S of the specimen is a1 The fatigue life is N(S a1 ), the damage under the total number of cycles can be defined as: According to the damage equivalence principle, D1=D a1 , the equivalent primary true stress S of the specimen can be obtained a1 .

5. The method according to claim 2, characterized in that Step 3 is as follows: Use the method in step 2 to obtain the equivalent primary true stress of each specimen, and then combine the test results of the group method and the lifting method to fit and obtain the first iteration SN curve as follows: lgN=a0′-b0′×lg(S max -S ∞0 ′) (5)。 6. The method according to claim 2, characterized in that Step 4 is as follows: According to formula (5), repeat step 2, and according to the constant amplitude cyclic stress S i The number of test cycles recorded below is n i The equivalent secondary true stress S of a single specimen can be obtained by using the damage equivalence a2 .

7. The method according to claim 2, characterized in that Step 5 is as follows: Use the method in step 2 to obtain the equivalent secondary true stress of each specimen, and then combine the test results of the group method and the lifting method to fit the secondary iterative SN curve as follows: lgN=a0″-b0″×lg(S max -S ∞0 ″) (6)。 8. The method according to claim 2, characterized in that Step 6 is as follows: Repeat the iterative process, taking N = 1 × 10 7 cycle, obtain the fatigue limit error of N iterations and N-1 iterations, and take the error value less than 0.5% as the iteration termination condition.

9. The method according to claim 2, characterized in that The metal element is 35Cr2Ni4MoA alloy steel, 40CrNiMoA alloy steel, 7050 aluminum alloy or 2A14 aluminum alloy.

10. The method according to claim 3, characterized in that The grouping method in step 1 preliminarily selects a failure life of 1×10 5 times, 5×10 5 times, 1×10 6 The test load is set at the corresponding stress level; the lifting method in step 1 is at 1×10 7 The conditional fatigue limit of the material is measured for the second time; the calibration test in step one is to obtain the corresponding relationship between the strain on the test piece and the response acceleration. When conducting a formal test, the strain gauge may deform and fail due to the change in the stiffness of the test piece; the SN curve in step one can be fitted in the form of a power function or an exponential function.