Metal nanowire transparent conductive film with high stability and electronic device

By adding vanadium oxide compounds with valences of +2 to +5 as light stabilizers to a transparent conductive film of metal nanowires, a multilayer structure is formed, which solves the problem of poor stability of metal nanowires under light irradiation and realizes a highly stable transparent conductive film suitable for outdoor use and specific electronic devices.

CN118919128AActive Publication Date: 2024-11-08SICHUAN UNIV
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202411031638.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-08
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

Existing transparent conductive films made of metal nanowires have poor stability under light conditions, especially under ultraviolet light. Metal nanowires are prone to oxidation and migration, which can lead to failure of the conductive layer. Traditional encapsulation layers cannot effectively block light, resulting in increased resistance of the thin film and failure of the transparent electrode.

Method used

Vanadium oxides with valences of +2 to +5 are used as light stabilizers and added to the substrate, conductive layer and outer coating to form a multilayer transparent conductive film to improve the stability of metal nanowires, especially under ultraviolet irradiation conditions.

Benefits of technology

It significantly improves the stability of transparent conductive films made of metal nanowires, especially their ability to resist ultraviolet radiation, sweat and ethanol immersion in outdoor environments, and maintains excellent optical, thermal and chemical stability, thus expanding their application fields in outdoor applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919128A_ABST
    Figure CN118919128A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of transparent conductive films, and particularly discloses a metal nanowire transparent conductive film with high stability and an electronic device. The transparent conductive film comprises a substrate layer, a conductive layer and an outer coating layer, the conductive layer comprises metal nanowires, the transparent conductive film further comprises a light stabilizer, the light stabilizer comprises a vanadium oxide compound, the vanadium of the vanadium oxide compound is + 2-+ 5 and is not + 5, and the thickness of the conductive layer is smaller than that of the outer coating layer. The light stabilizer is included in at least one of the base layer, the conductive layer, and the outer coating layer. Compared with a traditional ITO conducting film, the transparent conducting film has the advantages of being high in transparency, high in bending resistance, good in stability, resistant to ultraviolet radiation and the like, and application of the transparent conducting film in the field of electronic devices such as outdoors, thin-film solar cells, transparent thin-film heaters, transparent electromagnetic shielding, vehicle-mounted photoelectric products and precise ultraviolet optical devices is expanded.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of transparent conductive films, and in particular relates to a metal nanowire transparent conductive film and an electronic device with high stability. Background Art

[0002] Transparent conductive film (TCF), also known as transparent electrode, refers to a thin film structure with high transparency and good conductivity in the visible light band (400nm ~ 800nm), which can be used in touch display screens, smart dimming films, LEDs, flexible displays, smart wearables, electronic skin, biosensors, transparent electromagnetic shielding, solar thin film batteries and transparent thin film heating devices. It is difficult for general conductive materials to have both good conductivity and light transmittance. The most widely used transparent conductive oxide is indium-doped tin oxide (ITO), which has a conductivity comparable to that of metals and a transmittance of more than 90% in the visible light region. However, due to its own ceramic brittleness, ITO needs to be deposited by sputtering, and the manufacturing efficiency is difficult to improve. In addition, the ceramic brittleness limits the application of ITO in curved, folding, flexible, electronic skin and smart wearable fields.

[0003] Metal nanowire transparent conductive film has the advantages of good conductivity, high light transmittance, resistance to bending and stretching, relatively stable physical and chemical properties, etc. It has the potential for application in multiple scenarios and irreplaceable advantages. Metal nanowires include but are not limited to at least one of gold, silver, copper, iron, cobalt, nickel, and aluminum, as well as composite metal nanowires (doped and core-shell types) composed of two or more metals. Due to the combined effects of high temperature, light (ultraviolet light irradiation), water vapor, and oxygen, metal oxidation and migration lead to reduced stability of metal nanowires and their conductive layers, or even rapid aging and failure. Therefore, the stability of metal nanowire transparent conductive films, their devices, and products is a difficult problem that needs to be overcome urgently.

[0004] At present, researchers believe that the most effective strategy is to encapsulate and protect the metal nanowire conductive layer, which can effectively block water and oxygen, thereby improving the stability of metal nanowire transparent conductive films and their devices and products in indoor application scenarios. However, under outdoor lighting conditions (especially ultraviolet light UV), the traditional encapsulation layer cannot effectively block light. The metal atoms on the surface of the metal nanowires that absorb UV photons are prone to plasma resonance, causing the metal atoms to diffuse and migrate, and the photothermal effect further accelerates the process, ultimately causing the transparent electrode to fail due to spherical fracture or short circuit of the metal nanowires.

[0005] The patent document with the publication number CN106660312B discloses an improved light stability of a nanowire-based transparent conductor, and discloses a light-stable optical stack, which includes a transparent conductive film formed by a silver nanostructure or a silver mesh, the conductive film includes silver nanowires and a light stabilizer, the light stabilizer includes a transition metal salt or a transition coordination complex of Fe, Co, Mn or V, the optical stack has a light exposure area, the metal atoms on the surface of the metal nanowires that absorb light undergo plasma resonance, so that photoactive species appear in the optical stack and the sheet resistance increases, and the light stabilizer acts as a catalyst to accelerate the reaction of the photoactive species with the organic material present in the optical stack, so that the photoactive species is consumed by the organic material before interacting with the silver nanowires. However, the light stabilizer does not effectively improve the absorption of light by the metal nanowires, but consumes the photoactive species using organic materials. Under the influence of external factors such as high temperature and light in outdoor application scenarios, it is easy to accelerate the oxidation reaction of the organic material, causing adverse effects such as aging of the organic material.

[0006] The patent document with the publication number CN109804439B discloses a stabilized sparse metal conductive film, which includes a substrate, a sparse metal conductive layer supported by the substrate, and a coating adjacent to the sparse metal conductive layer, wherein the sparse metal conductive layer includes a molten metal nanostructure network, and a stabilizer is contained in the coating adjacent to the sparse metal conductive layer, and the coating includes a polymer matrix and a vanadium + 5 stabilizing composition. However, since the presence of the vanadium + 5 stabilizing composition can inhibit the chemical melting process of the metal nanowires, the vanadium + 5 stabilizing composition cannot be applied to the sparse metal conductive layer, and the sparse metal conductive layer is also added with a complex of a transition metal salt Co, so that the photoactive species are consumed by the organic material before interacting with the silver nanowires to improve the photostability of the sparse metal conductive layer. For the same reason, the light stabilizer does not effectively improve the absorption of light by the metal nanowires.

[0007] In summary, there is an urgent need to provide a metal nanowire transparent conductive film with high stability and a preparation method, which can effectively improve the defect of increased sheet resistance caused by the absorption of light by the metal nanowires. Summary of the invention

[0008] The object of the present invention is to provide a metal nanowire transparent conductive film and an electronic device with high stability, which can effectively improve the defect that the metal nanowire absorbs light and causes an increase in sheet resistance.

[0009] In a first aspect, the present invention provides a transparent conductive film, comprising a base layer, a conductive layer and an outer covering layer, wherein the conductive layer comprises metal nanowires, and the transparent conductive film further comprises a light stabilizer, wherein the light stabilizer comprises a vanadium oxide compound, wherein the vanadium of the vanadium oxide compound has a valence of +2 to +5 and is not +5, and the light stabilizer is contained in at least one of the base layer, the conductive layer and the outer covering layer.

[0010] Optionally, the metal nanowires include at least one of gold, silver, copper, iron, cobalt, nickel, aluminum, indium, tin, platinum, palladium or titanium nanowires;

[0011] And / or, the metal nanowires include composite metal nanowires composed of at least two metals selected from the group consisting of gold, silver, copper, iron, cobalt, nickel, aluminum, indium, tin, platinum, palladium or titanium.

[0012] Optionally, the vanadium oxide compound includes at least one of strontium vanadate, lanthanum vanadate, cerium vanadate, calcium vanadate, yttrium vanadate, praseodymium vanadate, neodymium vanadate, vanadium dioxide or vanadium trioxide.

[0013] Optionally, the transparent conductive film further comprises an optically transparent adhesive layer and / or a top protective layer, and the light stabilizer is contained in at least one layer of the base layer, the conductive layer, the outer covering layer, the optically transparent adhesive layer or the top protective layer.

[0014] Optionally, the outer coating layer is composed of a composition including a polymer; and the light stabilizer is contained in at least one of the conductive layer and the outer coating layer.

[0015] Optionally, the conductive layer is prepared from a solution comprising the metal nanowires and the light stabilizer, and the content of the light stabilizer is 0.001 wt % to 3 wt % of the solution;

[0016] And / or, the outer coating layer is prepared from a solution including a polymer and the light stabilizer, and the content of the light stabilizer is 0.001 wt % to 3 wt % of the solution.

[0017] Optionally, the vanadium oxide compound is a micron or nanometer material, and the micron or nanometer material includes at least one of micron or nanometer particles, micron or nanometer fibers, micron or nanometer sheets, or micron or nanometer balls.

[0018] Optionally, the metal nanowires include silver nanowires.

[0019] Optionally, the sheet resistance of the transparent conductive film is no more than 40 ohms / square, the visible light transmittance is at least 85%, and the haze value is no more than 8%. After 1000 hours of ultraviolet irradiation, the sheet resistance of the transparent conductive film is no more than 100 ohms / square, the visible light transmittance is at least 85%, and the haze value is no more than 8%.

[0020] Optionally, the ultraviolet irradiation uses a UVB light source with a wavelength of 313 nm, the distance between the surface of the transparent conductive film and the light source is 5 cm, and the ultraviolet light energy density on the surface of the transparent conductive film reaches 0.5 mW / cm 2 .

[0021] In a second aspect, the present invention provides an electronic device, comprising the transparent conductive film as described in any one of the above items.

[0022] In summary, the present invention has at least one of the following beneficial effects:

[0023] The metal nanowire transparent conductive film provided by the present invention utilizes vanadium oxide compounds with a valence of +2 to +5 and not +5 to improve the stability of the metal nanowire transparent conductive film. The vanadium oxide compound is added to at least one of the key metal nanowire conductive layer and / or the base layer and the outer coating layer in the transparent conductive film. Compared with the metal nanowire transparent conductive film without adding the vanadium oxide compound, the overall stability of the transparent conductive film is improved, especially the stability of the resistance to UV radiation is improved. The vanadium oxide compound / metal nanowire transparent conductive film has a much better ability to resist UV radiation, sweat and ethanol immersion under room temperature conditions than commercial transparent conductive films, and is close to ITO. It has excellent optical, thermal and chemical stability, and expands its application in the fields of outdoor, thin-film solar cells, transparent film heaters, transparent electromagnetic shielding, vehicle-mounted optoelectronic products and precision ultraviolet optical devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0025] Figure 1 is a schematic structural diagram of a transparent conductive film according to an embodiment of the present invention;

[0026] Figure 2 This is a comparison chart of the photoelectric performance (square resistance Rs, visible light transmittance Tvis, haze H) of the silver nanowire transparent conductive film without adding strontium vanadate in Example 1 of the present invention and in Example 4 with adding strontium vanadate after ultraviolet irradiation for 1000 hours;

[0027] Figure 3This is a comparison chart of the photoelectric performance (square resistance Rs, visible light transmittance Tvis, haze H) of different types of vanadium oxide / silver nanowire composite transparent conductive films of Example 1 and Examples 4-8 of the present invention after ultraviolet irradiation for 1000 hours;

[0028] Figure 4 This is a comparison chart of the photoelectric performance (square resistance Rs, visible light transmittance Tvis, haze H) of different forms of strontium vanadate / silver nanowire composite transparent conductive films of Example 4 and Example 9 of the present invention after ultraviolet irradiation for 1000 hours;

[0029] Figure 5 This is a comparison chart of the photoelectric performance (square resistance Rs, visible light transmittance Tvis, haze H) of the composite transparent conductive films of strontium vanadate / silver nanowires with different addition amounts in Examples 1, 4, 10, and 11 of the present invention after ultraviolet irradiation for 500 hours;

[0030] Figure 6 This is a comparison chart of the photoelectric properties (square resistance Rs, visible light transmittance Tvis, haze H) of the silver nanowire transparent conductive films of Example 1 of the present invention without adding strontium vanadate, Example 4 adding strontium vanadate, and Comparative Examples 1 and 2 adding +5-valent vanadium oxide compounds (NaVO3 and SrV2O6) after ultraviolet irradiation for 1000 hours. DETAILED DESCRIPTION

[0031] The present invention provides a metal nanowire transparent conductive film and an electronic device with high stability. In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention. It should be noted that the directional terms such as up, down, left, right, front, back, inside, and outside that appear or will appear in the text of the present invention are based only on the drawings of the present invention, and are not specific limitations of the present invention.

[0032] Reference Figure 1, a typical transparent conductive film includes a multilayer structure, which generally includes a substrate 100, a conductive layer 110, an overcoat (OC) 120, an optional optically transparent adhesive layer (OCA) 130, and an optional top protective layer 140. It should be understood that not all embodiments include all layers. The overcoat 120 can be one or two layers, deposited on the upper side and / or lower side of the conductive layer 110 to protect the conductive layer 110. Optional means including or excluding the layer, for example, the optional optically transparent adhesive layer 130 may be included or not included, used to bond the adjacent upper and lower layers. The optional top protective layer 140 may be included or not included, used to protect the multilayer structure. The substrate 100 is used to provide support, and the conductive layer 110 includes metal nanowires of an interconnected structure or a mesh structure. The metal nanowires include but are not limited to at least one of gold, silver, copper, iron, cobalt, nickel, aluminum, indium, tin, platinum, palladium or titanium nanowires, as well as composite metal nanowires (doped type and core-shell type) composed of two or more of the aforementioned metals. Metal nanowire transparent conductive films are widely used in various electronic devices due to their high conductivity, transparency and flexibility, such as electronic displays (liquid crystal displays, touch screens and flexible displays), solar cells, optoelectronic devices (photoelectric conductive converters), organic light-emitting diodes (OLEDs), especially silver nanowire transparent conductive films, which have the best conductivity and are the most widely used.

[0033] The substrate 100 can be made of a material that is translucent to visible light, for example, a durable support layer is formed by one or more suitable materials such as quartz, sapphire, glass or plastic. Plastics can be listed as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polyimide (PI), polysulfone ether (PES), polycarbonate (PC), polyetherimide (PEI), polyacrylate (PA), polydimethoxysiloxane (PDMS), polyvinyl alcohol (PVA), their copolymers or their mixtures, and other suitable optically transparent polymers with high transparency, low haze and good protective support, all of which can be used as the material of the substrate 100 of the present invention. The thickness of the substrate 100 is not particularly limited and can be appropriately selected according to the purpose. In some embodiments of the present invention, the thickness of the substrate 100 can be 5μm to 1.5mm, further, 10μm to 1mm, and further 50μm to 500μm.

[0034] The conductive layer 110 is formed of a dispersion (solution) including metal nanowires, the dispersion includes a solvent, and conventional additives in the art may be added to improve the ability of the dispersion to form the conductive layer 110. The solvent used for the metal nanowire dispersion may include an aqueous solvent, an organic solvent, or a mixture thereof, which may be listed as: water, alcohol (ethanol, isopropanol, isobutanol, n-butanol, or tert-butanol), ketone (methyl ethyl ketone, methyl isobutyl ketone), ester (ethyl acetate, butyl acetate, ethyl lactate), ether (glycol ether), aromatic compound (toluene), alkane (hexane), etc., and mixtures thereof. The additives may be listed as: dispersants, surfactants, adhesives, thickeners, antioxidants, anti-settling agents, viscosity regulators, defoamers, ultraviolet light stabilizers, fillers, softeners, and mixtures thereof. In some embodiments of the present invention, the content of metal nanowires is 0.001wt% to 3wt% based on the mass of the dispersion, optionally, the content of metal nanowires is 0.003wt% to 2wt%, and further optionally, the content of metal nanowires is 0.005wt% to 1wt%. The content of the auxiliary agent is selected according to actual needs, and the addition amount of each auxiliary agent is usually not more than 3wt% of the dispersion, and there is no specific limitation. The metal nanowires can be made of gold, silver, copper, iron, cobalt, nickel, aluminum, indium, tin, platinum, palladium, titanium and alloys thereof. The average diameter of the metal nanowires is selected according to actual needs and is not specifically limited. Optionally, the average diameter of the metal nanowires in some embodiments of the present invention is below 300nm to provide good transparency and low haze. Further, the average diameter of the metal nanowires is below 200nm, and can be selected from 10nm to 150nm, and further, can be selected from 10nm to 100nm; similarly, the average length of the metal nanowires is selected according to actual needs and is not specifically limited. Optionally, the average length of the metal nanowires in some embodiments of the present invention is above 2μm to provide good conductivity. Further, the average length of the metal nanowires is above 5μm, and further, can be selected from 10μm to 100μm. In some embodiments of the present invention, the method of depositing the metal nanowire dispersion to form the conductive layer 110 can use conventional coating forming methods in the art, which can be listed as: drop coating, spin coating, spray coating, roll coating, dip coating, scraper coating, rod coating, printing, screen printing, blade coating, slot die coating, etc. After forming the coating, the sparse metal can be dried to remove the liquid, and the drying temperature is 45°C to 160°C. After drying, the coating can be washed with ethanol or isopropanol or other solvents and further dried to remove excess solids to reduce haze. It should be understood that the conductive layer 110 can also be patterned by selecting a conventional stripping process.The average thickness of the conductive layer 110 is selected according to actual needs, and is not specifically limited. Optionally, the average thickness of the conductive layer 110 formed in some embodiments of the present invention is less than 4 μm, further, less than 3 μm, and further, 10 to 800 nm. In some embodiments of the present invention, the metal nanowires in the conductive layer 110 overlap each other to form an interconnected structure or a mesh structure, and the mass per unit area of ​​the metal nanowires is 0.1 mg / m. 2 Up to 350 mg / m 2 , to improve transparency, conductivity and reduce haze, further, 1mg / m 2 Up to 280 mg / m 2 , further, 10mg / m 2 Up to 150 mg / m 2 , all are the qualities before patterning.

[0035] The outer coating 120 can be arranged on the upper side and / or the lower side of the conductive layer 110 to provide protection for the conductive layer 110, which can include mechanical, humidity, radiation, heat, oxygen and other protections, and is composed of a composition of polymers, also known as a polymer layer. The outer coating 120 is formed by a dispersion (solution) including a polymer, and the dispersion includes a solvent, and can be formed into the outer coating 120 by adding conventional additives in the art. The solvent and additives of the outer coating 120 and the amount of addition can refer to the solvent and additives and the amount of addition for forming the conductive layer 110 in the foregoing text, and will not be repeated here. The polymer of the outer coating 120 can be listed as: polyurethane (PU), acrylic resin (PA), acrylic acid (ester)-styrene-acrylonitrile copolymer (ASA), epoxy resin (EP), other polyesters, polyethers, cellulose polymers, polysaccharide polymers, and mixtures thereof. The polymer can be self-crosslinked under heating or irradiation, or can be crosslinked by adding a photoinitiator or other crosslinking agent. The content of the polymer is 0.001wt% to 10wt% based on the mass of the dispersion. Optionally, the content of the polymer is 0.01wt% to 8wt%. The preparation method of the outer coating 120 also refers to the preparation method of the conductive layer 110 described above, and will not be repeated here. The junction between the prepared outer coating 120 and the conductive layer 110 may be entangled or interwoven. The average thickness of the outer coating 120 is selected according to actual needs, and there is no specific limitation. Optionally, in some embodiments of the present invention, the outer coating 120 can have an average thickness of 10nm to 1.5μm, and further, it can be selected to be 10nm to 500nm.

[0036] The optically transparent adhesive layer 130 may be optionally disposed on the upper side and / or lower side of the conductive layer 110 or the outer covering layer 120, and the aforementioned component layers may be optionally coated or bonded in sequence through the optically transparent adhesive layer 130. The optically transparent adhesive layer 130 includes, for example, a liquid optically transparent adhesive or an adhesive tape coated thereon, and the liquid optically transparent adhesive may include a UV-curable coatable composition based on acrylic acid or polysiloxane chemical components. The average thickness of the optically transparent adhesive layer 130 is selected according to actual needs, and is not specifically limited. Optionally, in some embodiments of the present invention, the optically transparent adhesive layer 130 may have an average thickness of 10 nm to 300 μm, and further, may be selected to be 10 nm to 100 μm.

[0037] The suitable composition of the top protective layer 140 can refer to the composition of the substrate 100 described above, for example, polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polyimide (PI), polysulfone ether (PES), polycarbonate (PC), polyetherimide (PEI), polyacrylate (PA), polydimethoxysiloxane (PDMS), polyvinyl alcohol (PVA), their copolymers or their mixtures, and other suitable optically transparent polymers with high transparency, low haze and good protective support can all be used as the material of the top protective layer 140 of the present invention. The thickness of the top protective layer 140 is not particularly limited and can be appropriately selected according to the purpose. In some embodiments of the present invention, the thickness of the top protective layer 140 can be 5μm to 500μm, further, it can be selected to be 10μm to 300μm, and further, it can be selected to be 50μm to 150μm.

[0038] In some embodiments of the present invention, the light stabilizer adopts a vanadium oxide compound, and the vanadium of the vanadium oxide compound is +2 to +5 valence, and is not +5 valence, including but not limited to at least one of strontium vanadate, lanthanum vanadate, cerium vanadate, calcium vanadate, yttrium vanadate, praseodymium vanadate, neodymium vanadate, vanadium dioxide or vanadium trioxide. Optionally, the vanadium of the vanadium oxide compound is +2 to +4 valence, and further optionally, the vanadium of the vanadium oxide compound is +3 to +4 valence. Taking strontium vanadate as an example, it is a typical perovskite-type transition metal oxide, and its carrier concentration (2.2*10 22 cm -3 ) is higher than ITO(10 21 cm -3 ) is of the same magnitude, its resistivity (3.1*10 -7Ω·m) is only one order of magnitude higher than that of metallic silver, and has excellent conductivity similar to that of metal. At the same time, the optical bandgap width (4.3eV) of strontium vanadate is greater than that of indium-doped tin oxide (ITO, 3.7eV), and the light-transmitting window coverage is wider than that of ITO and silver. There is no strong absorption and reflection effect in Vis (visible light region), basically no intrinsic absorption in UV (ultraviolet region), and relatively little reflection in IR (infrared region), which can reduce the absorption of UV by metal nanowires, effectively alleviate the plasma resonance effect and photothermal effect of metal nanowires induced by UV, and inhibit the diffusion and migration of metal atoms, thereby improving the optical stability of the metal nanowire transparent conductive film. The light stabilizer can be incorporated into at least one of the substrate 100, the conductive layer 110, the optional overcoat (OC) 120, the optional optically transparent adhesive layer (OCA) 130, and the optional top protective layer 140 in the transparent conductive film multilayer structure as required. The light stabilizer can be incorporated into a dispersion-based composition, which can be coated to form any component layer of a given transparent conductive film. In some embodiments of the present invention, the light stabilizer is incorporated into a dispersion composition based on the conductive layer 110 and / or the overcoat 120 by a predetermined addition amount; further, in other embodiments of the present invention, the light stabilizer is incorporated into a dispersion (solution) based on the overcoat 120 by a predetermined addition amount; the amount of the light stabilizer added to the dispersion is 0.001 to 3 wt %, optionally, the amount of the light stabilizer added to the dispersion is 0.001 to 1 wt %, further optionally, the amount of the light stabilizer added to the dispersion is 0.005 to 0.08 wt %, and further optionally, the amount of the light stabilizer added to the dispersion is 0.008 to 0.06 wt %. In addition, the light stabilizer can also form a solution independently and be applied to any component layer in the transparent conductive film multilayer structure in a conventional manner such as immersion, spraying or coating. Optionally, the vanadium oxide compound is a micron or nano material, and the micron or nano material includes at least one of micron or nano particles, micron or nano fibers, micron or nano sheets or micron or nano balls. Further optionally, the vanadium oxide compound is at least one of micro balls, micro sheets, nano fibers or nano particles. Further optionally, the average diameter of the micro balls is 5 to 100 μm, optionally 10 to 50 μm, or optionally 10 to 30 μm; the average length of the nano fibers is 0.5 to 50 μm, optionally 0.5 to 30 μm, and the average diameter of the nano fibers is 10 to 500 nm, or optionally 30 to 300 nm; the sheet length of the micro sheets is 3 to 100 μm, optionally 5 to 50 μm, and the width is 0.5 to 10 μm, or optionally 1 to 5 μm; the average diameter of the nano particles is 5 to 500 nm, optionally 10 to 300 nm, or further optionally 10 to 100 nm.

[0039] Ultraviolet (UV) irradiation was used to evaluate the stability of the transparent conductive film. The UV irradiation used a UVB light source with a wavelength of 313nm. The distance between the film surface and the light source tube was set to be only 5cm, which can achieve close-range high-intensity irradiation, thereby causing strong metal atomic resonance on the surface of the metal nanowires, which has the effect of accelerating aging. The UV light energy density on the sample surface reached 0.5mW / cm 2 , irradiate for 500h or 1000h, compare the photoelectric properties of the transparent conductive film before and after irradiation, including the change rate of square resistance Rs, visible light transmittance Tvis, and haze H, take samples at each time point, and detect the values ​​of any three points on the transparent conductive film in parallel, and then take the average value to obtain the photoelectric performance data (square resistance Rs, visible light transmittance Tvis, haze H) of the transparent conductive film after UV irradiation for a certain period of time.

[0040] Among them, the four-probe method is used to test the square resistance Rs of the conductive film to characterize its conductivity. s The unit is ohm / square (Ω / □ or ohms / sq), and the test is carried out according to the standard ASTM D991-89 (2020). Different application scenarios and fields have different requirements for the square resistance of transparent conductive films. According to experience, the square resistance of transparent conductive films used in general optoelectronic products and devices does not exceed 500Ω / □. For example, the square resistance of transparent conductive films used in optoelectronic devices such as OLED and OPV does not exceed 50Ω / □, the square resistance of transparent conductive films used in large-size capacitive touch screens does not exceed 100Ω / □, and the square resistance of transparent conductive films used in optoelectronic devices such as PDLC smart dimming films does not exceed 500Ω / □.

[0041] The visible light transmittance Tvis is tested according to the standard ASTM D1003-21. At present, mainstream optoelectronic devices and products require the visible light transmittance Tvis of transparent conductive films to be no less than 80%, among which OLED and capacitive touch screens require Tvis to be no less than 85%. Infrared imaging optoelectronic devices have higher requirements for the visible light transmittance of transparent conductive films, generally requiring Tvis to be no less than 90%.

[0042] Haze H is another important optical performance indicator. Higher haze will cause the display of optoelectronic display products to be blurry, turbid, and have reduced clarity, affecting practical applications. It is tested according to standards ASTM D1003-21 or JIS K7105-1981.

[0043] The present invention requires that the square resistance Rs of each example sample after UV irradiation aging does not exceed 40Ω / □, the transmittance Tvis in the visible light region is at least 85%, and the haze H does not exceed 8.0%. The square resistance Rs after 1000 hours of UV irradiation does not exceed 100Ω / □, the transmittance Tvis in the visible light region is not less than 85%, and the haze H is not higher than 8.0%, indicating that the performance requirements of the actual application scenario are met. The three key optoelectronic performance parameters of the transparent conductive film incorporating the light stabilizer: the change rate of the square resistance Rs, the transmittance Tvis in the visible light region, and the haze H are compared with the change rate of the transparent conductive film of the blank sample to judge the effect of the light stabilizer on the stability of the transparent conductive film.

[0044] The present invention is further described below by means of specific examples. Unless otherwise specified, the raw materials in the specific examples of the present invention are commercially available or obtained by conventional preparation methods in the art.

[0045] Preparation example:

[0046] Preparation Example 1

[0047] Preparation Example 1 Silver nanowires are prepared, including the following steps: 600 mL of ethylene glycol is added to a clean 1L stainless steel reactor, and 200 mg of sodium chloride, 200 mg of sodium bromide and 2.0 g of polyvinyl pyrrolidone (PVP, K30) are added in sequence under stirring at 500 rpm; after complete dissolution, 50 mL of ethylene glycol solution containing 1.5 g of silver nitrate is evenly added dropwise for 30 min; then the temperature is raised to 180°C and maintained for 1.5 h; cooled to room temperature, the reaction solution is added to 3L of deionized water and dispersed evenly; then the silver nanowires are selectively precipitated by acetone and collected by centrifugal sedimentation, and the obtained pure silver nanowires are dispersed in 80 mL of anhydrous ethanol, stirred evenly to obtain a silver nanowire ethanol dispersion for standby use. The average length of the prepared silver nanowires is 30 μm, the average diameter is 25 nm, and the aspect ratio is 1200.

[0048] Preparation Example 2

[0049] Preparation Example 2 Strontium vanadate (SrVO3, nanofiber) is prepared, comprising the following steps: weighing 2 mmol of NH4VO3 to prepare 25 mL of a light yellow vanadium source solution; weighing 1 mmol of an acidifying agent H2C2O4 and adding the light yellow vanadium source solution to prepare an orange-red vanadium source solution; weighing 2 mmol of strontium nitrate (Sr(NO3)2, CAS: 10042-76-9) to prepare 20 mL of a strontium source solution; weighing 0.1 g of sodium dodecyl sulfate (SDS, CAS No.: 151-21-3) to prepare 5 mL SDS surfactant solution; mix the three solutions to obtain a stable homogeneous solution; transfer the homogeneous solution to a hydrothermal reactor with a polytetrafluoroethylene liner with a capacity of 100 mL, keep it warm at 180°C for 12 hours, and cool it to room temperature with the furnace; centrifugal drying is performed to obtain a strontium vanadium oxide SrV2O6 nanofiber precursor with an average length of 10 μm, an average diameter of 50 nm, and an aspect ratio of 200; the precursor is calcined in hydrogen in a tubular furnace at 800°C for 2 hours, and cooled to prepare strontium vanadate nanofibers with an average length of 10 μm, an average diameter of 50 nm, and an aspect ratio of 200.

[0050] Preparation Example 3

[0051] Preparation Example 3 prepares lanthanum vanadate (LaVO3). The difference between Preparation Example 3 and Preparation Example 2 is that an equal amount of lanthanum nitrate (La(NO3)3·6H2O, CAS: 10277-43-7) is used to replace the strontium nitrate (Sr(NO3)2) of Preparation Example 2, and the remaining preparation steps are the same as Preparation Example 2 to prepare lanthanum vanadate microspheres with an average diameter of 20 μm.

[0052] Preparation Example 4

[0053] Preparation Example 4 prepares cerium vanadate (CeVO3). The difference between Preparation Example 4 and Preparation Example 2 is that an equal amount of cerium nitrate (Ce(NO3)3·6H2O, CAS:10294-41-4) is used to replace the strontium nitrate (Sr(NO3)2) in Preparation Example 2, and the remaining preparation steps are the same as Preparation Example 2 to prepare cerium vanadate nanofibers with an average length of 1 μm, an average diameter of 100 nm, and an aspect ratio of 10.

[0054] Preparation Example 5

[0055] Preparation Example 5 prepares vanadium dioxide (VO2). The difference between Preparation Example 5 and Preparation Example 2 is that the strontium source solution in Preparation Example 2 is removed, and the remaining preparation steps are the same as Preparation Example 2 to prepare thin flake vanadium dioxide with a flake length of 10 μm, a width of 2 μm, and an aspect ratio of 5.

[0056] Preparation Example 6

[0057] Preparation Example 6 prepares vanadium trioxide (V2O3). The difference between Preparation Example 6 and Preparation Example 2 is that the strontium source solution in Preparation Example 2 is removed, and the 2mmol NH4VO3 of the vanadium source solution in Preparation Example 2 is adjusted to 4mmol NH4VO3. The remaining preparation steps are the same as Preparation Example 2. The prepared thin flake vanadium trioxide has a flake length of 20μm, a width of 1.5μm, and an aspect ratio of 13.33.

[0058] Preparation Example 7

[0059] Preparation Example 7: Strontium vanadate (SrVO3, nanoparticles) is prepared, comprising the following steps: weigh 2 mmol of NH4VO3, and prepare 25 mL of vanadium source solution; weigh 2 mmol of strontium nitrate (Sr(NO3)2, CAS:10042-76-9), and prepare 25 mL of strontium source solution; weigh 0.6 mL of dilute nitric acid, and add the strontium source solution; mix the above solutions to obtain a stable homogeneous solution; add 2 mL of 0.2 M KOH solution to the above homogeneous solution to obtain a precipitate; centrifugally dry the mixed solution after the precipitation reaction to obtain a strontium vanadium oxide precursor; calcine the precursor in a tubular furnace in hydrogen at 800°C for 2 h, and cool to prepare strontium vanadate nanoparticles, the average particle size of the strontium vanadate nanoparticles is 50 nm.

[0060] Example 1 (Silver nanowire transparent conductive film: blank control sample, comparative example)

[0061] The present invention provides a method for preparing a silver nanowire transparent conductive film, comprising the following steps:

[0062] S1. Preparation of silver nanowire dispersion: The silver nanowire ethanol dispersion prepared in Preparation Example 1 was ultrasonically dispersed for no more than 10 min, with an input power of 100 W and a frequency of 40 kHz to prepare a silver nanowire ethanol dispersion with a mass concentration of 1.0 wt%.

[0063] S2. Preparation of polymer dispersion: Disperse and dissolve waterborne polyurethane resin (WPU, 35 wt %, Anhui Anda Huatai New Materials) in ethanol to obtain a waterborne polyurethane resin ethanol dispersion with a mass concentration of 5.0 wt %.

[0064] S3. Prepare coating regulator solution: The coating regulator includes viscosity regulator hydroxypropyl methylcellulose (HPMC, CAS No.: 9004-65-3, viscosity 4000cps, Aladdin) and surface tension regulator FS-31 fluorocarbon surfactant (25wt%, DuPont, USA). The two regulators are dispersed and dissolved in ethanol to obtain coating regulator solutions A and B. The mass concentration of the viscosity regulator of coating regulator solution A is: HPMC 0.5wt%, and the mass concentration of the surface tension regulator of coating regulator solution B is: FS-31 2.5wt%.

[0065] S4. Prepare a silver nanowire coating solution: mix the silver nanowire ethanol dispersion in step S1 and the coating regulator solution in step S3 in a certain proportion, and then disperse them evenly by ultrasonic dispersion. The ultrasonic dispersion time does not exceed 10 min, the input power does not exceed 300 W, and the frequency is 40 kHz to prepare a silver nanowire coating solution. The mass concentrations of silver nanowires, HPMC and FS-31 in the silver nanowire coating solution are 0.18 wt%, 0.3 wt% and 0.05 wt%, respectively.

[0066] S5. Prepare a polymer coating liquid: mix the aqueous polyurethane resin ethanol dispersion prepared in step S2 and the coating regulator solution prepared in step S3 in a certain proportion, and then disperse them evenly by ultrasonic dispersion. The ultrasonic dispersion time does not exceed 10 min, the input power does not exceed 300 W, and the frequency is 40 kHz to prepare a polymer coating liquid. The mass concentrations of WPU and FS-31 in the polymer coating liquid are 0.8wt% and 0.03wt%, respectively.

[0067] S6. Primary coating: PET (thickness 125 μm, length 5 cm, width 5 cm, Toray, Japan) was used as a flexible substrate, which was placed on a desktop homogenizer after cleaning and drying, and fixed by adsorption with a vacuum pump. 1 mL of the silver nanowire coating liquid prepared in step S4 was accurately drawn with a micropipette, and evenly dropped on the PET substrate at a speed of 400 rpm and a spin coating time of 5 s. After coating, it was placed in an oven at 110°C and dried for 5 min to prepare a silver nanowire conductive layer on the PET substrate;

[0068] S7. Secondary coating: The same coating method as step S6 is used on the silver nanowire conductive layer prepared in step S6, and 1 mL of the polymer coating liquid prepared in step S5 is accurately aspirated with a micropipette again, and the polymer coating liquid prepared in step S5 is coated on the silver nanowire conductive layer, and a polymer layer (outer coating) is prepared on the silver nanowire conductive layer. The substrate / conductive layer / polymer layer constitutes a multilayer stacked structure of a transparent conductive film, and a silver nanowire transparent conductive film is prepared.

[0069] The square resistance Rs of the silver nanowire transparent conductive film prepared in Example 1 was measured to be 34.00Ω / □, the haze H was 3.39%, and the transmittance Tvis in the visible light region was 87.73%. After UV irradiation for 1000h, the square resistance Rs was 231.03Ω / □, an increase of 579.51%, the haze H was 3.49%, an increase of 2.95%, and the transmittance Tvis in the visible light region was 86.44%, a decrease of 1.47%.

[0070] Example 2 (Adding light stabilizer strontium vanadate to the conductive layer)

[0071] The difference between Example 2 and Example 1 is that, in step S1., a silver nanowire dispersion is prepared: the silver nanowire ethanol dispersion prepared in Preparation Example 1 and the strontium vanadate nanofiber prepared in Preparation Example 2 are ultrasonically dispersed to prepare a strontium vanadate / silver nanowire ethanol dispersion; in step S4., a silver nanowire coating liquid is prepared, and the mass concentrations of the silver nanowires, strontium vanadate nanofibers, HPMC and FS-31 in the silver nanowire coating liquid are 0.18wt%, 0.01wt%, 0.3wt% and 0.05wt%, respectively. The remaining preparation steps are the same as in Example 1, and a strontium vanadate / silver nanowire transparent conductive film is prepared.

[0072] The strontium vanadate / silver nanowire transparent conductive film of Example 2 was measured, and the Rs was 36.33Ω / □, the haze H was 3.33%, and the transmittance Tvis in the visible light region was 88.05%; compared with the silver nanowire transparent conductive film based on the same batch of silver nanowires and without adding strontium vanadate, the silver nanowire transparent conductive film without adding strontium vanadate had a square resistance Rs of 34.0Ω / □, a haze H of 3.39%, and a transmittance Tvis in the visible light region of 87.73%, and the square resistance Rs increased by 6.85%, the haze H decreased by 1.77%, and the transmittance in the visible light region increased by 0.36%. Adding strontium vanadate nanofibers to the conductive layer is beneficial to improving the transmittance of the transparent conductive film and reducing the haze, but because strontium vanadate is directly added to the silver nanowire conductive layer, its resistance value is slightly increased, but its square resistance value is only 36.33Ω / □, which is still far lower than the requirement for square resistance in actual application.

[0073] Example 3 (light stabilizer strontium vanadate is added to both the conductive layer and the polymer layer)

[0074] The difference between Example 3 and Example 1 is that the silver nanowire ethanol dispersion prepared in Preparation Example 1 and the strontium vanadate nanofibers prepared in Preparation Example 2 are ultrasonically dispersed to form a strontium vanadate / silver nanowire ethanol dispersion; S2. Preparing a polymer dispersion: ultrasonically dispersing an aqueous polyurethane resin and the strontium vanadate nanofibers prepared in Preparation Example 2 in ethanol to obtain a strontium vanadate / aqueous polyurethane resin ethanol dispersion; in step S4., a silver nanowire coating liquid is prepared, and the mass concentrations of silver nanowires, strontium vanadate nanofibers, HPMC and FS-31 in the silver nanowire coating liquid are 0.18wt%, 0.01wt%, 0.3wt% and 0.05wt%, respectively; in step S5., a polymer coating liquid is prepared, and the mass concentrations of WPU, FS-31 and strontium vanadate nanofibers in the polymer coating liquid are 0.8wt%, 0.03wt% and 0.01wt%, respectively. The remaining preparation steps are the same as those in Example 1, and a strontium vanadate / silver nanowire transparent conductive film is prepared.

[0075] The strontium vanadate / silver nanowire composite transparent conductive film of Example 3 was measured to have an Rs of 35.0Ω / □, a haze H of 3.44%, and a visible light transmittance Tvis of 87.83%; compared with the silver nanowire transparent conductive film based on the same batch of silver nanowires and without the addition of strontium vanadate, the silver nanowire transparent conductive film without the addition of strontium vanadate had a square resistance Rs of 34.0Ω / □, a haze H of 3.39%, and a visible light transmittance Tvis of 87.73%, and the square resistance Rs increased by 2.94%, the haze H increased by 1.47%, and the visible light transmittance increased by 0.11%.

[0076] Example 4 (Adding light stabilizer strontium vanadate to the polymer layer)

[0077] The difference between Example 4 and Example 1 is that, S2. prepares a polymer dispersion: ultrasonically disperses the aqueous polyurethane resin and the strontium vanadate nanofibers prepared in Preparation Example 2 in ethanol to obtain a strontium vanadate / aqueous polyurethane resin ethanol dispersion; in step S5., a polymer coating liquid is prepared, and the mass concentrations of WPU, FS-31 and strontium vanadate nanofibers in the polymer coating liquid are 0.8wt%, 0.03wt%, and 0.01wt%, respectively. The remaining preparation steps are the same as those in Example 1, and a strontium vanadate / silver nanowire transparent conductive film is prepared.

[0078] The strontium vanadate / silver nanowire composite transparent conductive film of Example 4 was measured to have an Rs of 33.62Ω / □, a haze H of 3.68%, and a visible light transmittance Tvis of 85.13%; compared with the silver nanowire transparent conductive film based on the same batch of silver nanowires and without adding strontium vanadate, the silver nanowire transparent conductive film without adding strontium vanadate had a square resistance Rs of 35.96Ω / □, a haze H of 4.04%, and a visible light transmittance Tvis of 85.73%, and the square resistance Rs was reduced by 6.51%, the haze H was reduced by 8.91%, and the visible light transmittance Tvis was reduced by 0.70%. After UV irradiation for 1000h, the square resistance Rs of the silver nanowire transparent conductive film of Example 4 was 85.09Ω / □, which increased by 153.09%, the haze H was 4.20%, which increased by 14.13%, and the transmittance Tvis in the visible light region was 85.54%, which increased by 0.48%.

[0079] refer to Figure 2 , Figure 2 The graph shows the comparison of the photoelectric performance of the silver nanowire transparent conductive film with strontium vanadate added to the polymer layer in Example 4 and the silver nanowire transparent conductive film without strontium vanadate added in Example 1 after ultraviolet irradiation for 1000 hours. Figure 2 It can be seen that: within the first 500 hours, the trends of the two are consistent, and the photoelectric performance data do not change much. However, as the irradiation time increases, the transparent conductive film in Example 4 with strontium vanadate added to the polymer layer only slowly increases to 85.09Ω / □ after 1000 hours of ultraviolet irradiation, the transmittance is 85.54%, which is slightly improved, and the haze value is 4.20%, which has a small change. The three key parameters are still within the requirements for practical applications. In Example 1, the transparent conductive film in which strontium vanadate is not added to the polymer layer has a resistance of 231.03Ω / □ after 1000 hours of irradiation, which increases by 579.51%, and the rate of change is much higher than that of the transparent conductive film with strontium vanadate added. It can be seen that strontium vanadate plays a role in significantly improving the photoelectric stability of the transparent conductive film.

[0080] Table 1. Effect of different addition positions of strontium vanadate on the photoelectric properties of transparent conductive films

[0081] <![CDATA[R / R0]]> <![CDATA[H / H0]]> <![CDATA[T / T0]]> Embodiment 2 (conductive layer) 1.069 0.982 1.004 Example 3 (Conductive layer and polymeric layer) 1.029 1.015 1.001 Example 4 (polymeric layer) 0.935 0.911 0.993

[0082] Referring to Table 1, Table 1 shows the effects of different addition positions of strontium vanadate in Examples 2-4 on the photoelectric properties of the strontium vanadate / silver nanowire transparent conductive film. It can be seen from Table 1 that adding strontium vanadate to different positions of the conductive film (respectively, the conductive layer, both at the same time, or the polymer layer) has slightly different effects on the square resistance Rs of the conductive film: Example 2 adds strontium vanadate to the conductive layer, and the square resistance increases slightly; Example 3 adds strontium vanadate to the conductive layer and the polymer layer, and the square resistance increases slightly; Example 4 adds strontium vanadate to the polymer layer, and the square resistance decreases slightly, which is beneficial to improving the conductive performance. The effects on the haze H and transmittance T of the transparent conductive film are small and can be ignored. Taking all factors into consideration, the subsequent examples all adopt the method of adding strontium vanadate or other light stabilizers to the polymer layer.

[0083] Example 5 (Different types of vanadium oxide compounds: lanthanum vanadate)

[0084] The difference between Example 5 and Example 4 is that the strontium vanadate in Example 4 is replaced by the lanthanum vanadate prepared in Preparation Example 3 of equal mass, and the remaining preparation steps are the same as those in Example 4 to prepare a lanthanum vanadate / silver nanowire transparent conductive film.

[0085] The lanthanum vanadate / silver nanowire transparent conductive film of Example 5 was measured to have a square resistance Rs of 26.92Ω / □, a haze H of 3.34%, and a visible light transmittance Tvis of 85.42%. After UV irradiation for 1000h, its square resistance Rs was 56.25Ω / □, an increase of 108.95%, a haze H of 3.93%, an increase of 17.66%, and a visible light transmittance Tvis of 86.75%, an increase of 1.56%.

[0086] Example 6 (Different types of vanadium oxide compounds: cerium vanadate)

[0087] The difference between Example 6 and Example 4 is that the cerium vanadate prepared in Preparation Example 4 with an equal mass is used to replace the strontium vanadate in Example 4, and the remaining preparation steps are the same as those in Example 4 to prepare a cerium vanadate / silver nanowire transparent conductive film.

[0088] The cerium vanadate / silver nanowire transparent conductive film of Example 6 was measured to have a square resistance Rs of 31.88Ω / □, a haze H of 2.86%, and a visible light transmittance Tvis of 86.80%. After UV irradiation for 1000h, its square resistance Rs was 84.56Ω / □, an increase of 165.24%, the haze H was 3.49%, an increase of 22.03%, and the visible light transmittance Tvis was 87.60%, an increase of 0.92%.

[0089] Example 7 (Different types of vanadium oxide compounds: vanadium dioxide)

[0090] The difference between Example 7 and Example 4 is that the strontium vanadate in Example 4 is replaced by vanadium dioxide prepared in Preparation Example 5 with an equal mass, and the remaining preparation steps are the same as in Example 4 to prepare a vanadium dioxide / silver nanowire transparent conductive film.

[0091] The vanadium dioxide / silver nanowire transparent conductive film of Example 7 was measured to have a square resistance Rs of 29.29Ω / □, a haze H of 3.31%, and a visible light transmittance Tvis of 85.56%. After UV irradiation for 1000h, its square resistance Rs was 62.64Ω / □, an increase of 113.86%, the haze H was 3.93%, an increase of 18.73%, and the visible light transmittance Tvis was 86.65%, an increase of 1.27%.

[0092] Example 8 (Different types of vanadium oxide compounds: vanadium trioxide)

[0093] The difference between Example 8 and Example 4 is that the strontium vanadate in Example 4 is replaced by vanadium trioxide prepared in Preparation Example 6 with an equal mass, and the remaining preparation steps are the same as in Example 4 to prepare a vanadium trioxide / silver nanowire transparent conductive film.

[0094] The vanadium trioxide / silver nanowire transparent conductive film of Example 8 was measured to have a square resistance Rs of 33.31Ω / □, a haze H of 3.25%, and a visible light transmittance Tvis of 85.55%. After UV irradiation for 1000h, its square resistance Rs was 76.65Ω / □, an increase of 130.11%, a haze H of 3.97%, an increase of 22.15%, and a visible light transmittance Tvis of 85.39%, a decrease of 0.19%.

[0095] refer to Figure 3 , Figure 3 The figure shows the changes in the photoelectric properties (square resistance Rs, visible light transmittance Tvis, haze H) of the transparent conductive films of Example 1 without adding a stabilizer and Examples 4 to 8 with adding different types of vanadium oxide compounds / silver nanowires after ultraviolet irradiation for 1000 hours. Figure 3 It can be seen that different types of vanadium oxide compounds, including +3-valent V2O3, lanthanum vanadate (LaVO3) and cerium vanadate (CeVO3), as well as +4-valent VO2 and strontium vanadate (SrVO3), are added to the polymer layer of the transparent conductive film as light stabilizers. After 1000 hours of ultraviolet irradiation, they all show good photoelectric properties. The square resistance Rs, visible light transmittance Tvis and haze H of the conductive film all change little and are within the allowable range for practical applications. In particular, the square resistance change has better stability than the blank sample of Example 1.

[0096] Example 9 (Different forms of strontium vanadate: nanoparticles)

[0097] The difference between Example 9 and Example 4 is that the strontium vanadate nanoparticles prepared in Preparation Example 7 of equal mass are used to replace the strontium vanadate nanofibers in Example 4, and the remaining preparation steps are the same as those in Example 4 to prepare a strontium vanadate / silver nanowire transparent conductive film.

[0098] The strontium vanadate / silver nanowire composite transparent conductive film of Example 9 was measured to have a square resistance Rs of 32.20Ω / □, a haze H of 2.98%, and a visible light transmittance Tvis of 85.20%. After UV irradiation for 1000h, its square resistance Rs was 55.06Ω / □, an increase of 70.99%, the haze H was 3.39%, an increase of 13.76%, and the visible light transmittance Tvis was 85.67%, an increase of 0.55%.

[0099] refer to Figure 4 , Figure 4 The photoelectric properties (square resistance Rs, visible light transmittance Tvis, haze H) of the composite transparent conductive film of strontium vanadate nanomaterial / silver nanowire with different forms added in Example 1 and Example 9 after ultraviolet irradiation for 1000h are shown. Figure 4 It can be seen that different forms of strontium vanadate have the effect of improving the photoelectric performance and stability of the transparent conductive film relative to the blank sample without adding light stabilizer. At the same time, when strontium vanadate nanoparticles are added in Example 9, after 1000 hours of ultraviolet irradiation, the photoelectric performance and stability of the transparent conductive film are better than those of the conductive film with strontium vanadate nanofibers added in Example 4, and the change rate of its square resistance Rs is smaller, and the stability is better.

[0100] Example 10 (Strontium vanadate nanofibers with different contents)

[0101] The difference between Example 10 and Example 4 is that 0.05 wt % strontium vanadate is used to replace 0.01 wt % strontium vanadate in Example 4, and the remaining preparation steps are the same as those in Example 4 to prepare a strontium vanadate / silver nanowire transparent conductive film.

[0102] The strontium vanadate / silver nanowire transparent conductive film of Example 10 was measured to have a square resistance Rs of 25.50Ω / □, a haze H of 7.28%, and a visible light transmittance Tvis of 86.45%; compared with the silver nanowire transparent conductive film without adding strontium vanadate, its square resistance Rs was reduced by 25%, the haze H was increased by 114.81%, and the visible light transmittance Tvis was reduced by 1.46%.

[0103] After UV irradiation for 500h, its square resistance Rs was 54.25Ω / □, which increased by 112.75%, its haze H was 7.52%, which increased by 3.29%, and its transmittance Tvis in the visible light region was 85.34%, which decreased by 1.29%.

[0104] Example 11 (Strontium vanadate nanofibers with different contents)

[0105] The difference between Example 11 and Example 4 is that 0.025 wt % strontium vanadate is used to replace 0.01 wt % strontium vanadate in Example 4, and the remaining preparation steps are the same as those in Example 4 to prepare a strontium vanadate / silver nanowire transparent conductive film.

[0106] The strontium vanadate / silver nanowire transparent conductive film of Example 11 was measured to have a square resistance Rs of 25.75Ω / □, a haze H of 4.86%, and a visible light transmittance Tvis of 86.43%; compared with the silver nanowire transparent conductive film without adding strontium vanadate, its square resistance Rs was reduced by 24.26%, the haze H was increased by 43.36%, and the visible light transmittance Tvis was reduced by 1.48%.

[0107] After UV irradiation for 500h, the square resistance Rs was 37.50Ω / □, which increased by 45.63%, the haze H was 5.40%, which increased by 11.01%, and the transmittance Tvis in the visible light region was 85.52%, which decreased by 1.05%.

[0108] refer to Figure 5 , Figure 5 The figure shows the changes in the photoelectric properties (square resistance Rs, visible light transmittance Tvis, haze H) of the conductive film after 500 hours of ultraviolet irradiation of the samples without strontium vanadate added in Example 1 and different amounts of strontium vanadate added in Examples 4, 10, and 11; Figure 5 It can be seen that by comparing the photoelectric performance data of samples with different amounts of strontium vanadate added and blank samples after 500 hours of ultraviolet irradiation, the photoelectric performance and stability of the transparent conductive film with added strontium vanadate are better than those of the blank control sample without added strontium vanadate. After adding strontium vanadate, the change rate of the square resistance Rs, visible light transmittance Tvis and haze H of the conductive film after ultraviolet irradiation is small, all within the allowable range of practical application, and the stability of adding 0.01wt% and 0.025wt% is significantly better than that of adding 0.05wt%.

[0109] Comparative Example 1 (Vanadium +5: NaVO3)

[0110] The difference between Comparative Example 1 and Example 4 is that an equal mass of +5-valent sodium metavanadate (NaVO3·2H2O, CAS: 13718-26-8) is used to replace the strontium vanadate in Example 4, and the remaining preparation steps are the same as those in Example 4 to prepare a NaVO3 / silver nanowire transparent conductive film.

[0111] The NaVO3 / silver nanowire composite transparent conductive film of Comparative Example 1 was measured to have a square resistance Rs of 28.54Ω / □, a haze H of 3.21%, and a visible light transmittance Tvis of 85.49%. After UV irradiation for 1000h, its square resistance Rs increased to infinity and could not be measured, the haze H was 3.66%, an increase of 14.02%, and the visible light transmittance Tvis was 82.43%, a decrease of 3.58%. When irradiated for 750h, Rs was 657.20Ω / □, an increase of 2202.73%.

[0112] Comparative Example 2 (Vanadium +5: SrV2O6)

[0113] The difference between Comparative Example 2 and Example 4 is that an equal mass of +5-valent SrV2O6 (see the SrV2O6 nanofiber precursor in Preparation Example 2, with an average length of 10 μm, an average diameter of 50 nm, and an aspect ratio of 200) is used to replace the strontium vanadate in Example 4, and the remaining preparation steps are the same as in Example 4 to prepare a SrV2O6 / silver nanowire transparent conductive film.

[0114] The SrV2O6 / silver nanowire transparent conductive film of Comparative Example 2 was measured to have a square resistance Rs of 33.93Ω / □, a haze H of 3.21%, and a visible light transmittance Tvis of 85.42%; after 1000h of UV irradiation, its square resistance Rs was 113.52Ω / □, an increase of 234.57%, the haze H was 3.87%, an increase of 20.56%, and the visible light transmittance Tvis was 86.48%, an increase of 1.24%.

[0115] refer to Figure 6 , Figure 6 The figure shows the comparison of the photoelectric performance (square resistance Rs, visible light transmittance Tvis, haze H) of the transparent conductive film of Example 4 with the addition of strontium vanadate, Comparative Examples 1 and 2 with the addition of +5-valent vanadium oxide (NaVO3 and SrV2O6), and the blank sample of Example 1 after ultraviolet irradiation for 1000 hours. Figure 6 It can be seen that: the two +5-valent vanadium oxide compounds (NaVO3 and SrV2O6) of Comparative Examples 1 and 2 are added to the conductive film as light stabilizers. After 1000 hours of ultraviolet irradiation, compared with the addition of strontium vanadate and the blank sample, their visible light transmittance Tvis and haze H are less affected, but the effect on the square resistance Rs is greater, and even has the effect of deteriorating its photoelectric performance. The square resistance Rs value is much higher than the range specified for practical applications, which will cause the transparent conductive film or the corresponding electronic device to fail to work normally, further highlighting the improvement of the photoelectric performance and stability of the conductive film by strontium vanadate as a light stabilizer.

[0116] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.

Claims

1. A transparent conductive film, comprising a base layer, a conductive layer and an outer covering layer, wherein the conductive layer comprises metal nanowires, characterized in that: The transparent conductive film further includes a light stabilizer, which includes a vanadium oxide compound, wherein the vanadium of the vanadium oxide compound has a valence of +2 to +5 and is not +5, and the light stabilizer is contained in at least one of the base layer, the conductive layer and the overcoat layer.

2. The transparent conductive film according to claim 1, characterized in that: The metal nanowires include at least one of gold, silver, copper, iron, cobalt, nickel, aluminum, indium, tin, platinum, palladium or titanium nanowires; And / or, the metal nanowires include composite metal nanowires composed of at least two metals selected from the group consisting of gold, silver, copper, iron, cobalt, nickel, aluminum, indium, tin, platinum, palladium or titanium.

3. The transparent conductive film according to claim 1, characterized in that: The vanadium oxide compound includes at least one of strontium vanadate, lanthanum vanadate, cerium vanadate, calcium vanadate, yttrium vanadate, praseodymium vanadate, neodymium vanadate, vanadium dioxide or vanadium trioxide.

4. The transparent conductive film according to claim 1, characterized in that: The transparent conductive film further includes an optically transparent adhesive layer and / or a top protective layer, and the light stabilizer is contained in at least one layer of the base layer, the conductive layer, the overcoat layer, the optically transparent adhesive layer or the top protective layer.

5. The transparent conductive film according to any one of claims 1 to 4, characterized in that The outer coating layer is composed of a composition including a polymer; and the light stabilizer is contained in at least one of the conductive layer and the outer coating layer.

6. The transparent conductive film according to claim 5, characterized in that: The conductive layer is prepared from a solution including the metal nanowires and the light stabilizer, wherein the content of the light stabilizer is 0.001 wt % to 3 wt % of the solution; And / or, the outer coating layer is prepared from a solution including a polymer and the light stabilizer, and the content of the light stabilizer is 0.001 wt % to 3 wt % of the solution.

7. The transparent conductive film according to any one of claims 1 to 4, characterized in that The vanadium oxide compound is a micron or nanometer material, and the micron or nanometer material includes at least one of micron or nanometer particles, micron or nanometer fibers, micron or nanometer sheets, or micron or nanometer balls.

8. The transparent conductive film according to any one of claims 1 to 4, characterized in that The metal nanowires include silver nanowires.

9. The transparent conductive film according to claim 8, characterized in that: The sheet resistance of the transparent conductive film does not exceed 40 ohms / square, the visible light transmittance is at least 85%, and the haze value does not exceed 8%. After 1000 hours of ultraviolet irradiation, the sheet resistance of the transparent conductive film does not exceed 100 ohms / square, the visible light transmittance is at least 85%, and the haze value does not exceed 8%.

10. An electronic device, characterized in that: The electronic device comprises the transparent conductive film according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Substrate for flexible light emitting device and fabrication method thereof

    CN102201549A

  • Substrate for flexible luminescent device and preparation method thereof

    CN102208563A

  • Heater based on transparent silver nanowire conducting thin film and preparation method thereof

    CN104053256A

  • Silver nanowire and M-phase vanadium dioxide nanoparticle composite film and preparation method thereof

    CN104228208A

  • Method for directly preparing metal oxide / silver nanowire composite conductive network

    CN104575864A