Nickel selenide nano material as well as preparation method and application thereof

By preparing Ni3Se4 nanomaterials and forming a spiral surface morphology under a high-intensity magnetic field, the problem of insufficient specific surface area of ​​nickel-based materials was solved, thus improving the capacitance performance of supercapacitors.

CN118919319APending Publication Date: 2024-11-08CHANGXING HUAQIANG ELECTRONICS +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411173805.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Nickel-based materials, when used as electrode materials for supercapacitors, suffer from a relatively low specific surface area, which limits the improvement of supercapacitor energy density.

Method used

A one-step hydrothermal synthesis wet chemical method was used to prepare selenide nickel nanomaterials with Ni3Se4 as the main phase. The surface morphology with spatial threads was formed by high-intensity magnetic field treatment to increase the specific surface area.

Benefits of technology

The specific surface area of ​​selenium-based nickel nanomaterials as electrode materials for supercapacitors was significantly increased, thereby improving their charge storage capacity and capacitance performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919319A_ABST
    Figure CN118919319A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of nickel selenide nano-materials, in particular to a nickel selenide nano-material and a preparation method and application thereof.The nickel selenide nano-material with Ni3Se4 as a main phase is prepared through a one-step hydrothermal synthesis wet chemical method, meanwhile, the nickel selenide nano-material has the shape of a nanorod, then the nanorod product is treated through energy, and the nickel selenide nano-material is obtained. The shape of the nickel selenide nano material is subjected to secondary modification to form a surface shape with spatial threads, and the specific surface area of Ni3Se4 is further increased, so that the problem that the specific surface area is relatively low when the nickel selenide nano material is used as a supercapacitor electrode material is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of selenium-based nickel nanomaterials, and in particular to a selenium-based nickel nanomaterial and a preparation method and application thereof. Background Art

[0002] The electrode material of supercapacitors is one of the key factors affecting their performance. The electrode materials that can be used for supercapacitors are mainly divided into three categories: carbon materials, transition metal oxides and conductive polymers. Compared with carbon materials, transition metal oxides have a variety of oxidation states and a wide working potential window, showing a large charge storage capacity, and therefore have attracted much attention. Nickel-based materials among transition metal oxides have become a popular choice for supercapacitor electrode materials because of their high theoretical capacitance and good thermal stability, and their abundance on Earth.

[0003] Based on existing research, the inventors of the present application found that nickel-based materials, as supercapacitor electrode materials, have a relatively low specific surface area, which limits the improvement of the supercapacitor energy density. Summary of the invention

[0004] In view of this, the purpose of the present invention is to propose the preparation of selenium-based nickel nanomaterials to solve the problem that nickel-based materials have a relatively low specific surface area when used as supercapacitor electrode materials.

[0005] Based on the above purpose, the present invention provides a method for preparing selenium-based nickel nanomaterials, the preparation method comprising the following steps:

[0006] Solution preparation: add selenium source to hydrazine hydrate, dissolve by ultrasonic to obtain uniform solution A; dissolve nickel source in deionized water to obtain solution B; pour solution B into solution A, and obtain suspension by ultrasonic;

[0007] Hydrothermal reaction, the suspension is subjected to high pressure sealed heating reaction by a one-step hydrothermal synthesis wet chemical method to obtain a reactant solution;

[0008] Washing and drying, filtering, washing and drying the reaction solution to obtain a preliminary sample;

[0009] Energy treatment, subjecting the preliminary sample to energy treatment to obtain a sample.

[0010] The present application uses a transition metal nickel source and a selenium source as precursors, and synthesizes a selenium-based nickel nanomaterial with Ni3Se4 as the main phase through a wet chemical method based on a hydrothermal reaction, and at the same time has the morphology of nanorods. Then, energy is used to treat the nanorod product to perform secondary modification on the morphology of the selenium-based nickel nanomaterial, thereby increasing the specific surface area of ​​Ni3Se4, thereby solving the problem of relatively low specific surface area of ​​selenium-based nickel nanomaterials as supercapacitor electrode materials.

[0011] In some embodiments, the selenium source is selenium powder, and the nickel source is nickel nitrate hexahydrate.

[0012] In some embodiments, the molar volume of the solution A is 1.5 to 2.2 L / mol, and the molar volume of the solution B is 1 to 1.6 L / mol.

[0013] In some embodiments, the ultrasound frequency is 200-500 Hz, and the time is 10-30 min.

[0014] In some embodiments, the molar ratio of the selenium source to the nickel source is 1-2.

[0015] In some embodiments, the temperature of the hydrothermal reaction is 180° C. and the time is 24 hours.

[0016] In some embodiments, the energy treatment is in the form of high-intensity magnetic field treatment.

[0017] In some embodiments, the high-intensity magnetic field treatment is a pulsed magnetic field, the magnetic field intensity S is 1.1-1.5T, the treatment time T1 is 20-30s, and the number of pulses satisfies t=log(S)*T1.

[0018] Since the 3d orbital energy level of Se is very close to the 3s and 3p orbitals, this structure makes the selenium element have more metallic properties when combined with transition metals. Under the action of a high-intensity magnetic field, the product prepared in this application undergoes energy level transitions and secondary changes in morphology, forming a surface morphology with spatial threads, further increasing the specific surface area of ​​the product.

[0019] A selenium-based nickel nanomaterial is prepared by adopting the above-mentioned preparation method.

[0020] An application of a selenium-based nickel nanomaterial, wherein the selenium-based nickel nanomaterial is applied in a supercapacitor electrode.

[0021] Beneficial effects of the present invention: The present application adopts a one-step hydrothermal synthesis wet chemical method to prepare a selenium-based nickel nanomaterial with Ni3Se4 as the main phase, which also has the morphology of nanorods. Then, the nanorod product is treated with energy to perform secondary modification on the morphology of the selenium-based nickel nanomaterial to form a surface morphology with spatial threads, thereby further increasing the specific surface area of ​​Ni3Se4, thereby solving the problem of relatively low specific surface area of ​​selenium-based nickel nanomaterials as supercapacitor electrode materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only for the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0023] Figure 1 This is a schematic flow chart of a wet chemical method for preparing selenium-based nickel nanomaterials by one-step hydrothermal method according to an embodiment of the present invention;

[0024] Figure 2 is an X-ray diffraction pattern of the nickel selenide material according to an embodiment of the present invention;

[0025] Figure 3 This is a morphology diagram of the nickel selenide material according to an embodiment of the present invention;

[0026] Figure 4 The figure is a schematic diagram of the cyclic voltammetry curve of the nickel selenide material in the potential range of 0 to 0.65 V according to an embodiment of the present invention;

[0027] Figure 5 This is a comparison diagram of the morphology of Ni3Se4 before and after energy treatment in an embodiment of the present invention;

[0028] Figure 6 Schematic diagram of cyclic voltammetry curves of Ni3Se4 in the potential range of 0 to 0.65 V before and after energy treatment in an embodiment of the present invention;

[0029] Figure 7 This is a long-term cycle stability test and specific capacitance attenuation diagram of the electrode material before and after Ni3Se4 energy treatment in an embodiment of the present invention. DETAILED DESCRIPTION

[0030] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.

[0031] It should be noted that, unless otherwise defined, the technical terms or scientific terms used in the present invention should be understood by people with ordinary skills in the field to which the present invention belongs. The "first", "second" and similar words used in the present invention do not indicate any order, quantity or importance, but are only used to distinguish different components. "Include" or "comprise" and similar words mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, without excluding other elements or objects. "Connect" or "connected" and similar words are not limited to physical or mechanical connections, but may include electrical connections, whether direct or indirect. "Up", "down", "left", "right" and the like are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may also change accordingly.

[0032] In order to solve the problem that nickel-based materials have a relatively low specific surface area when used as supercapacitor electrode materials, based on the above purpose, one or more embodiments of this specification provide a method for preparing selenium-based nickel nanomaterials, and the preparation method comprises the following steps:

[0033] Solution preparation: add selenium source to hydrazine hydrate, dissolve by ultrasonic to obtain uniform solution A; dissolve nickel source in deionized water to obtain solution B; pour solution B into solution A, and obtain suspension by ultrasonic;

[0034] Hydrothermal reaction, the suspension is subjected to high pressure sealed heating reaction by a one-step hydrothermal synthesis wet chemical method to obtain a reactant solution;

[0035] Washing and drying, filtering, washing and drying the reaction solution to obtain a preliminary sample;

[0036] Energy treatment, subjecting the preliminary sample to energy treatment to obtain a sample.

[0037] One or more embodiments of the present specification provide a selenium-based nickel nanomaterial, which is prepared using the above-mentioned preparation method.

[0038] One or more embodiments of the present specification provide an application of a selenium-based nickel nanomaterial, wherein the selenium-based nickel nanomaterial is applied in a supercapacitor electrode.

[0039] Specifically, an embodiment 1 of this specification provides a method for preparing a selenium-based nickel nanomaterial, such as Figure 1 As shown, including:

[0040] To prepare the solution, add 10 mL of hydrazine hydrate into a beaker, add 5.2 mmol of selenium powder (Sepowder), and dissolve it by ultrasonication for 10 min to obtain a black uniform solution A; at the same time, 3.9 mmol of nickel nitrate hexahydrate (Ni(NO3)2·6H2O) is dissolved in 5 mL of deionized water to obtain solution B; finally, pour solution B into solution A, ultrasonicate for 30 min, and obtain a black suspension.

[0041] After hydrothermal reaction, the obtained mixed black suspension was transferred into a 50 mL stainless steel polytetrafluoroethylene-lined autoclave. The autoclave was then sealed and heated to 180° C. and maintained at this temperature for 24 h.

[0042] Washing and drying: After the target reaction time is completed, the obtained sample is collected by filtration, and then carefully washed and centrifuged with deionized water 4 times. Finally, the obtained sample is dried in a vacuum oven at 60°C for 24h to obtain a preliminary sample.

[0043] Energy treatment, the preliminary sample is placed in the sample chamber of the pulse magnetic field treatment equipment, and then the magnetic field strength S is adjusted to 1.2T, the treatment time T1 is 25s, and the number of pulses satisfies t=log(S)*T1, which is 1.97 for energy treatment. After the treatment is completed, the sample is taken out after cooling to room temperature. The X-ray diffraction pattern is as follows Figure 2 b shows that the main component is Ni3Se4.

[0044] Specifically, Example 2 of this specification provides a method for preparing selenium-based nickel nanomaterials, as described in Example 1, except that the amounts of selenium powder and nickel nitrate hexahydrate are 4.5 mmol and 4.5 mmol, respectively. Figure 2 a shows that the main component is nickel selenide (NiSe).

[0045] Specifically, Example 3 of this specification provides a method for preparing selenium-based nickel nanomaterials, as described in Example 1, except that the amounts of selenium powder and nickel nitrate hexahydrate are 6.6 mmol and 3.3 mmol respectively. Figure 2 c shows that the main component is nickel selenide (NiSe2).

[0046] The samples of Examples 1 to 3 were subjected to morphological analysis, and the results were as follows: Figure 3 As shown, Figure 3 As shown in a, nickel selenide (NiSe) has a nanoparticle morphology with an average particle size of 15.1 nm. Figure 3 As shown in b, nickel selenide (Ni3Se4) has a nanorod morphology with a length of 35.2nm and a diameter of 9.2nm. Figure 3 As shown in c, nickel diselenide (NiSe2) is an octahedron with an edge length of 212.5 nm.

[0047] The preparation method of selenium-based nickel nanomaterials has the advantages of uniform morphology, adjustable phase, simple synthesis method, and low cost. This simple material synthesis method and its excellent performance have broad prospects in sustainable energy and environmental applications.

[0048] To measure the capacitive properties of these three types of selenium-based nickel nanomaterials, we used an electrochemical workstation and connected a three-electrode system, using a glassy carbon electrode as the working electrode, a Pt wire as the counter electrode, and Hg / HgO as the reference electrode. The process for preparing the working electrode slurry is as follows: 5 mg of nickel selenide nanoparticle sample and 10 mg of carbon black are dissolved in 1 mL of water, 1 mL of ethanol, and 0.1 mL of Nafion, and ultrasonically stirred for 1 hour. 5 uL of the newly prepared electrocatalyst slurry is extracted with a pipette and dropped on a glassy carbon electrode with a diameter of 5 mm, and the sample is allowed to dry naturally.

[0049] First, the cyclic voltammetry (CV) curves of NiSe, Ni3Se4 and NiSe2 nanomaterials in 1 mol KOH aqueous electrolyte. Figure 4 The cyclic voltammetry curves obtained at the same scan rate of 50mV / s in the potential range of 0-0.65V were compared. With the increase of selenium content, the redox peak shifted significantly. At the same scan rate, Ni3Se4 has the highest redox peak area, which is higher than NiSe2 and NiSe materials.

[0050] Secondly, a galvanostatic charge-discharge (GCD) curve is usually used to evaluate the supercapacitor performance of different nickel selenide nanoparticles. Figure 4 bcd show the charge and discharge curves of NiSe, Ni3Se4, and NiSe2 electrode materials in 1 mol KOH aqueous electrolyte in the Hg / HgO potential window of 0-0.6 V at a variable current of 0.05-1.0 mA. According to the GCD curve, the specific capacity (C) can be calculated using the following equation: C = IΔt / mΔV

[0051] Where I is the charge or discharge current, Δt is the charge and discharge time, m is the mass of Ni-Co nanoparticles deposited on the electrode, and ΔV is the potential window used for the test.

[0052] According to the GCD curve and the above formula, the specific capacity of Ni3Se4 electrode ( Figure 4 b) 1531.2, 838.8, 689.9, 612.0, 562.5 and 506.9 F g respectively -1. Both are higher than the other two electrode materials, such as NiSe ( Figure 4 c) 932.8, 560.1, 478.5, 438.9, 562.5 and 408.0F g -1 , and NiSe2( Figure 4 d) 572.4, 573.7, 489.6, 451.3, 424.1 and 395.6 F g of electrode materials -1 .

[0053] Based on the above research, the product synthesized in Example 1 was finally selected as the raw material for energy treatment.

[0054] Specifically, an embodiment 4 of the present specification provides a method for preparing selenium-based nickel nanomaterials, as described in embodiment 1, except that the magnetic field intensity S is adjusted to 1.1T, the processing time T1 is 25s, and the number of pulses satisfying t=log(S)*T1 is 1.03.

[0055] Specifically, an embodiment 5 of the present specification provides a method for preparing selenium-based nickel nanomaterials, as described in embodiment 1, except that the magnetic field intensity S is adjusted to 1.5T, the processing time T1 is 25s, and the number of pulses satisfying t=log(S)*T1 is 4.4.

[0056] Specifically, an embodiment 6 of the present specification provides a method for preparing selenium-based nickel nanomaterials, as described in embodiment 1, except that the magnetic field intensity S is adjusted to 1.2T, the processing time T1 is 20s, and the number of pulses satisfying t=log(S)*T1 is 1.58.

[0057] Specifically, an embodiment 7 of the present specification provides a method for preparing selenium-based nickel nanomaterials, as described in embodiment 1, except that the magnetic field intensity S is adjusted to 1.2T, the processing time T1 is 30s, and the number of pulses satisfying t=log(S)*T1 is 2.37.

[0058] The samples of Examples 4 to 7 were subjected to morphological analysis, and the results were as follows: Figure 5 As shown, the Ni3Se4 nanorods after energy treatment have a threaded shape, and the specific surface area of ​​Ni3Se4 is greatly improved, providing more ion diffusion channels and active sites.

[0059] The supercapacitor performance of Ni3Se4 after energy treatment was evaluated using constant current charge and discharge curves. Figure 6 As shown, the specific capacity of the Ni3Se4 electrode after treatment is higher than that before treatment.

[0060] Cycling performance is another important parameter of supercapacitors. Figure 7The specific capacity of Ni3Se4 electrode before and after energy treatment at 0.5mA charge and discharge current for 3000 consecutive cycles (the first 100 cycles were activated at 0.1mA charge and discharge current). Figure 7 It can be seen from the two figures in the upper middle part that the specific capacity of Ni3Se4 before and after treatment quickly stabilizes after the first 10 cycles, mainly due to the activation and deactivation of the electrode, but the specific capacity of Ni3Se4 treated with energy is ultimately higher than that of the untreated one. Figure 7 As shown in the lower middle part, compared with the initial value, the specific capacity of untreated Ni3Se4 was maintained at 84.7%, 75.2%, 67.9%, 63.5%, 59.1% and 55.5% of the initial value at the 500th, 1000th, 1500th, 2000th, 2500th and 3000th cycles, respectively, while the specific capacity after treatment was maintained at 89.1%, 85.2%, 78.4%, 71.2%, 68.7% and 66.1% of the initial value, respectively.

[0061] Through comparison, it was found that under the same charging and discharging conditions, energy processing can effectively adjust the morphology and electronic structure of the material to obtain the optimal supercapacitor performance.

[0062] This may be because the 3d orbital energy level of Se is very close to the 3s and 3p orbitals. This structure makes the selenium element have more metallic properties when combined with transition metals. Under the action of a high-intensity magnetic field, the product prepared in this application undergoes energy level transitions and secondary changes in morphology, forming a surface morphology with spatial threads, further increasing the specific surface area of ​​the product.

[0063] In the process of analyzing the samples of Examples 4 to 7, it was found that only when the pulse number satisfies the condition of t=log(S)*T1, a threaded structure will be formed on the surface and inside the Ni3Se4 nanotube structure, and the double-plane threaded structure has a larger specific surface area than the single-plane threaded structure, which is more conducive to Ni3Se4 as a supercapacitor electrode material. The pulse number satisfies t=log(S)*T1 because it basically conforms to the Bigelow dynamic model, which is conducive to generating a stable blasting point during pulse processing, forming continuous destruction, and finally forming a threaded structure.

[0064] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention (including the claims) is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.

[0065] The present invention is intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing a selenium-based nickel nanomaterial, characterized in that: The preparation method comprises the following steps: Solution preparation: add selenium source to hydrazine hydrate, dissolve by ultrasonic to obtain uniform solution A; dissolve nickel source in deionized water to obtain solution B; pour solution B into solution A, and obtain suspension by ultrasonic; Hydrothermal reaction, the suspension is subjected to high pressure sealed heating reaction by a one-step hydrothermal synthesis wet chemical method to obtain a reactant solution; Washing and drying, filtering, washing and drying the reaction solution to obtain a preliminary sample; Energy treatment, subjecting the preliminary sample to energy treatment to obtain a sample.

2. The preparation method according to claim 1, characterized in that: The selenium source is selenium powder, and the nickel source is nickel nitrate hexahydrate.

3. The preparation method according to claim 1, characterized in that: The molar volume of the solution A is 1.5 to 2.2 L / mol, and the molar volume of the solution B is 1 to 1.6 L / mol.

4. The preparation method according to claim 1, characterized in that: The ultrasonic frequency is 200-500 Hz, and the time is 10-30 minutes.

5. The preparation method according to claim 1, characterized in that: The mass ratio of the selenium source to the nickel source is 1-2.

6. The preparation method according to claim 1, characterized in that: The temperature of the hydrothermal reaction is 180° C. and the time is 24 hours.

7. The preparation method according to claim 1, characterized in that: The energy treatment method is high-intensity magnetic field treatment.

8. The preparation method according to claim 7, characterized in that: The high-intensity magnetic field treatment is a pulsed magnetic field, the magnetic field intensity S is 1.1-1.5T, the treatment time T1 is 20-30s, and the number of pulses satisfies t=log(S)*T1.

9. A selenium-based nickel nanomaterial, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 8.

10. An application of the selenium-based nickel nanomaterial according to claim 9, characterized in that: The selenium-based nickel nanomaterial is used in supercapacitor electrodes.

Citation Information

Cited By

  • Method for preparing high-quality two-dimensional nickel-selenium nano island by utilizing molecular beam epitaxial growth technology, high-quality two-dimensional nickel-selenium nano island and application of high-quality two-dimensional nickel-selenium nano island

    CN122215067A