Advanced integrated circuit wafer recovery method of super-lens advanced integrated circuit sensor
By filling the bubble defects of the ultra-lens wafer and two-step wet etching steps, the recycling of advanced integrated circuit wafers in the ultra-lens advanced integrated circuit sensor is achieved, solving the scrapping problem caused by bonded bubbles, and improving utilization rate and capacity, and reduce costs.
Patent Information
- Application Number
- CN202410967125.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
AI Technical Summary
The prior art is difficult to effectively recover advanced integrated circuit wafers in ultra-lens advanced integrated circuit sensors that need to be scrapped due to the existence of bonded bubbles, resulting in low output rates and high cost.
By filling the bubble defects of the ultralens wafer, combined with a two-step wet etching step, we ensure that the advanced integrated circuit wafer is not damaged and its recycling is achieved through surface planarization.
It saves the advanced integrated circuit wafer that is about to be scrapped, reduces factory costs, improves wafer utilization and production capacity, and has a simple process and low cost, which is suitable for industrial production.
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor technology, and in particular to a method for recovering advanced integrated circuit wafers of a superlens advanced integrated circuit sensor. Background Art
[0002] The superlens advanced integrated circuit sensor is a sensor that integrates superlens technology. It uses the planar structure of the superlens and its ability to precisely control light waves, combined with advanced integrated circuit sensors, to achieve efficient photoelectric conversion and signal processing. This integrated technology can significantly improve the performance of the sensor, including improving imaging resolution, enhancing sensing sensitivity, expanding the field of view, and achieving a more compact system design. The advantages of superlens advanced integrated circuit sensors lie in their ultra-thin, ultra-light, and highly integrated characteristics. They can be widely used in 3D sensing, medical imaging, smart devices and other fields. With the advancement of manufacturing technology and the innovation of design methods, it is expected that superlens advanced integrated circuit sensors will play an important role in more fields in the future and promote the development of sensor technology to a higher level.
[0003] At present, the process of superlens advanced integrated circuit sensor is to integrate the superlens structure of silicon substrate with advanced integrated circuit wafer through oxide melt bonding method, and then use silicon thinning and removal process to completely remove the silicon substrate of superlens structure, that is, use bonding process to transfer superlens structure to advanced integrated circuit wafer. After the bonding process, in order to reduce the post-bonding bubble detection and measurement machine, a few pieces will be sampled to characterize the bonding situation of the same batch of products. Wafers that have not been inspected may also have the risk of bonding bubbles. If the bubbles are larger than a certain specification, the wafer needs to be scrapped in the subsequent thinning process, thereby losing another bonded advanced integrated circuit wafer. Due to the high cost of advanced integrated circuit wafer process, direct scrapping will not only lead to low output rate, but also increase factory cost. Therefore, recycling advanced integrated circuit wafers can improve their utilization rate and reduce costs.
[0004] CN 117133646A discloses a method for repairing bubble defects in a wafer bonding structure, the method comprising: providing a wafer bonding structure, the wafer bonding structure comprising a first wafer and a second wafer bonded together, the bonding interface between the first wafer and the second wafer comprising a bubble defect located on one side of the second wafer; thinning the second wafer to a set thickness to expose the bubble defect; forming a repair layer on the surface of the second wafer and in the bubble defect, the repair layer filling the bubble defect; using a chemical mechanical grinding process to remove the repair layer above the surface of the second wafer, and making the surface of the second wafer flat.
[0005] CN 112735964A discloses a wafer surface defect detection and surface repair method, which forms a bonding structure between two adjacent wafers by bonding at least two wafers, and after judging that the bubble defect is caused by the design structure, breaks the bonding structure to separate at least two bonded wafers, and determines the design structure causing the bubble defect according to the position of the bubble defect on the wafer, and repairs the wafer surface.
[0006] The above inventions all repair bonded wafers with bubble defects to avoid the problem of reduced yield. However, the above methods are obviously not applicable when the bubbles are larger than a certain size and the wafers with bubble defects need to be scrapped.
[0007] Therefore, in view of the shortcomings of the existing technology, it is urgently necessary to provide a method that can recycle advanced integrated circuit wafers of superlens advanced integrated circuit sensors and improve the utilization rate of advanced integrated circuit wafers. Summary of the invention
[0008] The purpose of the present invention is to provide a method for recovering advanced integrated circuit wafers of a superlens advanced integrated circuit sensor, thereby realizing the recovery of advanced integrated circuit wafers in a superlens advanced integrated circuit sensor with bubble defects and improving the utilization rate of advanced integrated circuit wafers.
[0009] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0010] The present invention provides a method for recycling advanced integrated circuit wafers of a superlens advanced integrated circuit sensor, the advanced integrated circuit wafer recycling method comprising the following steps:
[0011] A superlens advanced integrated circuit sensor structure is provided, wherein the superlens advanced integrated circuit sensor structure comprises a bonded superlens wafer and an advanced integrated circuit wafer, wherein a bonding interface between the superlens wafer and the advanced integrated circuit wafer has a bubble defect located on one side of the superlens wafer;
[0012] A first wet etching is performed on the silicon substrate of the superlens wafer, and the bubble defects are filled before or after the first wet etching; then a second wet etching is performed on the superlens structure layer of the superlens wafer and the filler at the bubble defects, and the obtained advanced integrated circuit wafer is recycled after surface flattening.
[0013] The advanced integrated circuit wafer recycling method of the super lens advanced integrated circuit sensor provided by the present invention fills the bubble defects of the super lens wafer and combines the two-step wet etching process to achieve the removal of the super lens wafer while ensuring that the advanced integrated circuit wafer is not damaged. The advanced integrated circuit wafer can be recycled after further surface flattening. The advanced integrated circuit wafer recycling method saves the advanced integrated circuit wafer that is about to be scrapped due to the presence of bonding bubbles, reduces factory costs, improves the utilization rate of advanced integrated circuit wafers, and increases production capacity. The process method is simple and low-cost, and is suitable for industrial production.
[0014] Preferably, the advanced integrated circuit wafer includes any one of a logic device, a memory, an analog device, an image sensor or a silicon optical sensor.
[0015] Preferably, the image sensor comprises a CIS.
[0016] The CIS refers to a complementary metal oxide semiconductor image sensor (CMOS Image Sensor, CIS), which, combined with the miniaturized optical technology of the super lens, can achieve higher optical resolution and faster imaging speed.
[0017] Preferably, the resistivity of the silicon substrate of the superlens wafer is 0.5-100Ω·cm, for example, it can be 0.5Ω·cm, 10Ω·cm, 30Ω·cm, 50Ω·cm, 80Ω·cm or 100Ω·cm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0018] Preferably, the thickness of the silicon substrate of the superlens wafer is 15-30 μm, for example, 15 μm, 20 μm, 25 μm or 30 μm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0019] Preferably, the etching solution used in the first wet etching includes TMAH solution.
[0020] The etching solution used in the first wet etching needs to be selected for Si / SiO 2 The solution with high etching selectivity can ensure that the SiO2 exposed on the advanced integrated circuit wafer will not be removed while removing the silicon substrate. 2 layer.
[0021] Preferably, the concentration of tetramethylammonium hydroxide in the TMAH solution is 2.375-2.38%, for example, 2.375%, 2.376%, 2.378%, 2.379% or 2.38%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0022] Preferably, the etching rate of the TMAH solution on the silicon substrate is For example it could be or However, it is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0023] Preferably, the etching temperature of the silicon substrate by the TMAH solution is 60-80°C, for example, 60°C, 65°C, 70°C, 75°C or 80°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0024] Preferably, the etching time of the silicon substrate with the TMAH solution is 50-120 min, for example, 50 min, 60 min, 80 min, 100 min or 120 min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0025] Preferably, the specific step of filling the bubble defects after the first wet etching comprises: depositing SiO on the surface of the superlens wafer; 2 .
[0026] Preferably, the SiO 2 The deposition thickness is For example it could be or However, it is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0027] Preferably, the deposited SiO 2 Afterwards, SiO 2 Flattening is performed.
[0028] Preferably, the planarization grinding amount is For example it could be or However, it is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0029] Preferably, the total thickness of the superlens structure layer is For example it could be or However, it is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0030] Preferably, the specific step of filling the bubble defects before the first wet etching comprises: manually dropping and spin-coating photoresist on the bubble defects.
[0031] Preferably, the photoresist thickness is 1-5 μm, for example, 1 μm, 2 μm, 3 μm, 4 μm or 5 μm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0032] Preferably, the filler used to fill the bubble defects after the first wet etching is SiO 2 When the etching solution used for the second wet etching includes a spinD solution, the spinD solution is a mixed solution of phosphoric acid with a concentration of 18-22%, nitric acid with a concentration of 38-42%, sulfuric acid with a concentration of 8-12%, and hydrofluoric acid with a concentration of 3-4%.
[0033] The spinD solution has good stability on Si and SiO 2 Both have etching capabilities and can directly and effectively remove superlens structures containing silicon pillars.
[0034] The concentration of phosphoric acid in the spinD solution is 18-22%, for example, 18%, 20% or 22%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0035] The concentration of nitric acid in the spinD solution is 38-42%, for example, 38%, 40% or 42%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0036] The concentration of sulfuric acid in the spinD solution is 8-12%, for example, 8%, 10% or 12%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0037] The concentration of hydrofluoric acid in the spinD solution is 3-4%, for example, 3%, 3.5% or 4%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0038] Preferably, the etching rate of the spinD solution on the superlens structure layer is 6-8 μm / min, for example, it can be 6 μm / min, 6.5 μm / min, 7 μm / min, 7.5 μm / min or 8 μm / min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0039] Preferably, the spinD solution is 2 The etching rate is For example it could be or However, it is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0040] Preferably, the temperature of the second wet etching is 20-25°C, for example, 20°C, 21°C, 23°C, 24°C or 25°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0041] Preferably, the second wet etching time is 1-5 min, for example, 1 min, 2 min, 3 min, 4 min or 5 min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0042] Preferably, when the filler used to fill the bubble defects before the first wet etching is photoresist, the etching solution used in the second wet etching further includes SPM solution.
[0043] Preferably, when the filler at the bubble defect is photoresist, the specific steps of the second wet etching include: etching the superlens structure layer with a spinD solution, and then etching the photoresist with a SPM solution.
[0044] The process parameters of etching the super lens structure layer using the spinD solution and the filling material at the bubble defect is SiO 2 The process parameters for the second wet etching are the same.
[0045] Preferably, the SPM solution comprises a mixed solution of sulfuric acid and hydrogen peroxide in a volume ratio of (2-8):1, for example, 2:1, 4:1, 5:1, 6:1 or 8:1, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0046] Preferably, the etching temperature of the SPM solution on the photoresist is 100-190°C, for example, 100°C, 120°C, 150°C, 170°C or 190°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0047] Preferably, the etching time of the photoresist by the SPM solution is 1-5 min, for example, 1 min, 2 min, 3 min, 4 min or 5 min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0048] Preferably, the grinding amount for surface flattening is For example it could be or However, it is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0049] Compared with the prior art, the present invention has the following beneficial effects:
[0050] The advanced integrated circuit wafer recycling method of the super lens advanced integrated circuit sensor provided by the present invention fills the bubble defects of the super lens wafer and combines the two-step wet etching process to achieve the removal of the super lens wafer while ensuring that the advanced integrated circuit wafer is not damaged. The advanced integrated circuit wafer can be recycled after further surface flattening. The advanced integrated circuit wafer recycling method saves the advanced integrated circuit wafer that is about to be scrapped due to the presence of bonding bubbles, reduces factory costs, improves the utilization rate of advanced integrated circuit wafers, and increases production capacity. The process method is simple and low-cost, and is suitable for industrial production. DETAILED DESCRIPTION
[0051] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only used to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0052] Example 1
[0053] This embodiment provides a method for recycling advanced integrated circuit wafers of a superlens advanced integrated circuit sensor, the advanced integrated circuit wafer recycling method comprising the following steps:
[0054] A superlens advanced integrated circuit sensor structure is provided, wherein the superlens advanced integrated circuit sensor structure comprises a bonded superlens wafer and a CIS wafer, wherein a bonding interface between the superlens wafer and the CIS wafer has a bubble defect located on one side of the superlens wafer;
[0055] A photoresist with a thickness of 2 μm was manually drop-coated on the bubble defect, and then the silicon substrate of the superlens wafer was first wet-etched using TMAH solution at an etching rate of The temperature is 70° C., the time is 80 min, the concentration of tetramethylammonium hydroxide in the TMAH solution is 2.378%; the resistivity of the silicon substrate of the superlens wafer is 50Ω·cm, and the thickness is 20 μm;
[0056] Then the total thickness of the superlens wafer was 1000 mm / s by using spinD solution. The super lens structure layer is etched at an etching rate of 7 μm / min, a temperature of 23° C., and a time of 1 min, wherein the spinD solution is a mixed solution of 20% phosphoric acid, 40% nitric acid, 10% sulfuric acid, and 3.5% hydrofluoric acid;
[0057] Then, the photoresist was etched with SPM solution at an etching temperature of 150°C for 2 min. The SPM solution included a mixed solution of sulfuric acid and hydrogen peroxide in a volume ratio of 4:1. The obtained CIS wafer was ground by The surface is flattened and then recycled.
[0058] Example 2
[0059] This embodiment provides a method for recycling advanced integrated circuit wafers of a superlens advanced integrated circuit sensor, the advanced integrated circuit wafer recycling method comprising the following steps:
[0060] A superlens advanced integrated circuit sensor structure is provided, wherein the superlens advanced integrated circuit sensor structure comprises a bonded superlens wafer and a CIS wafer, wherein a bonding interface between the superlens wafer and the CIS wafer has a bubble defect located on one side of the superlens wafer;
[0061] A photoresist with a thickness of 1 μm was manually drop-coated on the bubble defect, and then the silicon substrate of the superlens wafer was first wet-etched using TMAH solution at an etching rate of The temperature is 60° C., the time is 120 min, the concentration of tetramethylammonium hydroxide in the TMAH solution is 2.375%; the resistivity of the silicon substrate of the superlens wafer is 100 Ω·cm, and the thickness is 30 μm;
[0062] Then the total thickness of the superlens wafer was 1000 mm / s by using spinD solution. The super lens structure layer is etched at an etching rate of 6 μm / min, a temperature of 20° C., and a time of 1 min, wherein the spinD solution is a mixed solution of 18% phosphoric acid, 38% nitric acid, 8% sulfuric acid, and 3% hydrofluoric acid;
[0063] Then, the photoresist was etched with SPM solution at an etching temperature of 100°C for 1 min. The SPM solution included a mixed solution of sulfuric acid and hydrogen peroxide in a volume ratio of 2:1. The obtained CIS wafer was ground by The surface is flattened and then recycled.
[0064] Example 3
[0065] This embodiment provides a method for recycling advanced integrated circuit wafers of a superlens advanced integrated circuit sensor, the advanced integrated circuit wafer recycling method comprising the following steps:
[0066] A superlens advanced integrated circuit sensor structure is provided, wherein the superlens advanced integrated circuit sensor structure comprises a bonded superlens wafer and a CIS wafer, wherein a bonding interface between the superlens wafer and the CIS wafer has a bubble defect located on one side of the superlens wafer;
[0067] A photoresist with a thickness of 5 μm was manually drop-coated on the bubble defect, and then the silicon substrate of the superlens wafer was first wet-etched using TMAH solution at an etching rate of The temperature is 80° C., the time is 50 min, the concentration of tetramethylammonium hydroxide in the TMAH solution is 2.38%; the resistivity of the silicon substrate of the superlens wafer is 0.5Ω·cm, and the thickness is 15 μm;
[0068] Then the total thickness of the superlens wafer was 1000 mm / s by using spinD solution. The super lens structure layer is etched at an etching rate of 8 μm / min, a temperature of 25° C., and a time of 5 min, wherein the spinD solution is a mixed solution of 22% phosphoric acid, 42% nitric acid, 12% sulfuric acid, and 4% hydrofluoric acid;
[0069] Then, the photoresist was etched with SPM solution at an etching temperature of 190°C for 5 min. The SPM solution included a mixed solution of sulfuric acid and hydrogen peroxide in a volume ratio of 8:1. The obtained CIS wafer was ground by The surface is flattened and then recycled.
[0070] Example 4
[0071] This embodiment provides a method for recycling advanced integrated circuit wafers of a superlens advanced integrated circuit sensor, the advanced integrated circuit wafer recycling method comprising the following steps:
[0072] A superlens advanced integrated circuit sensor structure is provided, wherein the superlens advanced integrated circuit sensor structure comprises a bonded superlens wafer and a CIS wafer, wherein a bonding interface between the superlens wafer and the CIS wafer has a bubble defect located on one side of the superlens wafer;
[0073] The silicon substrate of the superlens wafer is first wet-etched using TMAH solution at an etching rate of The temperature is 80° C., the time is 50 min, the concentration of tetramethylammonium hydroxide in the TMAH solution is 2.38%; the resistivity of the silicon substrate of the superlens wafer is 0.5Ω·cm, and the thickness is 15 μm;
[0074] The thickness of the deposition on the surface of the superlens wafer is SiO 2 , then SiO 2 For planarization, the grinding amount is
[0075] Then the total thickness of the superlens wafer was 1000 mm / s by using spinD solution. The super lens structure layer is made of SiO 2 The etching rate of the super lens structure layer is 6μm / min, and the etching rate of SiO 2 The etching rate is The temperature is 20°C, the time is 2.5 min, and the spinD solution is a mixed solution of 18% phosphoric acid, 38% nitric acid, 8% sulfuric acid and 3% hydrofluoric acid; the obtained CIS wafer is ground with a grinding amount of The surface is flattened and then recycled.
[0076] Example 5
[0077] This embodiment provides a method for recycling advanced integrated circuit wafers of a superlens advanced integrated circuit sensor, the advanced integrated circuit wafer recycling method comprising the following steps:
[0078] A superlens advanced integrated circuit sensor structure is provided, wherein the superlens advanced integrated circuit sensor structure comprises a bonded superlens wafer and a CIS wafer, wherein a bonding interface between the superlens wafer and the CIS wafer has a bubble defect located on one side of the superlens wafer;
[0079] The silicon substrate of the superlens wafer is first wet-etched using TMAH solution at an etching rate of The temperature is 60° C., the time is 120 min, the concentration of tetramethylammonium hydroxide in the TMAH solution is 2.375%; the resistivity of the silicon substrate of the superlens wafer is 100 Ω·cm, and the thickness is 30 μm;
[0080] The thickness of the deposition on the surface of the superlens wafer is SiO 2 , then SiO 2 For planarization, the grinding amount is
[0081] Then the total thickness of the superlens wafer was 1000 mm / s by using spinD solution. The super lens structure layer is made of SiO 2 The etching rate of the super lens structure layer is 8μm / min, and the etching rate of SiO 2 The etching rate is The temperature is 25°C, the time is 5 minutes, and the spinD solution is a mixed solution of 22% phosphoric acid, 42% nitric acid, 12% sulfuric acid and 4% hydrofluoric acid; the obtained CIS wafer is ground by The surface is flattened and then recycled.
[0082] The advanced integrated circuit wafer recycling method provided in Examples 1-5 is used to recycle the advanced integrated circuit wafer of the super lens advanced integrated circuit sensor, and the SiO2 on the surface of the advanced integrated circuit wafer is measured by a film thickness measuring machine. 2 Thickness is tested. If SiO 2 thickness It is considered that the structure at the bottom of the advanced integrated circuit wafer is not damaged, which is indicated as "qualified". The results are shown in Table 1.
[0083] Table 1
[0084] Advanced IC Wafer Qualification Status Example 1 qualified Example 2 qualified Example 3 qualified Example 4 qualified Example 5 qualified
[0085] It can be seen from Table 1 that the advanced integrated circuit wafer recycling method provided by the present invention is used to recycle the advanced integrated circuit wafer of the superlens advanced integrated circuit sensor, and the structure at the bottom of the advanced integrated circuit wafer is not damaged, so the advanced integrated circuit wafer that is about to be scrapped due to the presence of bonding bubbles is saved, the factory cost is reduced, and it can be suitable for industrial production.
[0086] In summary, the advanced integrated circuit wafer recycling method of the superlens advanced integrated circuit sensor provided by the present invention fills the bubble defects of the superlens wafer and combines the two-step wet etching process to achieve the removal of the superlens wafer while ensuring that the advanced integrated circuit wafer is not damaged. The advanced integrated circuit wafer can be recycled after further surface flattening. The advanced integrated circuit wafer recycling method saves the advanced integrated circuit wafer that is about to be scrapped due to the presence of bonding bubbles, reduces factory costs, improves the utilization rate of advanced integrated circuit wafers, and increases production capacity. The process method is simple and low-cost, and is suitable for industrial production.
[0087] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.
Claims
1. A method for recycling advanced integrated circuit wafers of metalens advanced integrated circuit sensors, It is characterized in that The advanced integrated circuit wafer recycling method comprises the following steps: A superlens advanced integrated circuit sensor structure is provided, wherein the superlens advanced integrated circuit sensor structure comprises a bonded superlens wafer and an advanced integrated circuit wafer, wherein a bonding interface between the superlens wafer and the advanced integrated circuit wafer has a bubble defect located on one side of the superlens wafer; A first wet etching is performed on the silicon substrate of the superlens wafer, and the bubble defects are filled before or after the first wet etching; then a second wet etching is performed on the superlens structure layer of the superlens wafer and the filler at the bubble defects, and the obtained advanced integrated circuit wafer is recycled after surface flattening.
2. The advanced integrated circuit wafer recycling method according to claim 1, It is characterized in that The advanced integrated circuit wafer includes any one of a logic device, a memory, an analog device, an image sensor or a silicon optical sensor; Preferably, the image sensor comprises a CIS; Preferably, the resistivity of the silicon substrate of the superlens wafer is 0.5-100Ω·cm; Preferably, the thickness of the silicon substrate of the superlens wafer is 15-30 μm.
3. The advanced integrated circuit wafer recycling method according to claim 1 or 2, It is characterized in that The etching solution used in the first wet etching includes a TMAH solution; Preferably, the concentration of tetramethylammonium hydroxide in the TMAH solution is 2.375-2.38%.
4. The advanced integrated circuit wafer recycling method according to claim 3, It is characterized in that The etching rate of the TMAH solution on the silicon substrate is Preferably, the etching temperature of the TMAH solution on the silicon substrate is 60-80°C; Preferably, the etching time of the silicon substrate by the TMAH solution is 50-120 min.
5. The advanced integrated circuit wafer recycling method according to any one of claims 1 to 4, It is characterized in that The specific steps of filling the bubble defects after the first wet etching include: depositing SiO 2 ; Preferably, the SiO 2 The deposition thickness is 6. The advanced integrated circuit wafer recycling method according to claim 5, It is characterized in that The deposited SiO 2 Afterwards, SiO 2 Flattening is performed; Preferably, the planarization grinding amount is Preferably, the total thickness of the superlens structure layer is 7. The advanced integrated circuit wafer recycling method according to any one of claims 1 to 6, It is characterized in that The specific steps of filling the bubble defects before the first wet etching include: manually dropping and spin-coating photoresist on the bubble defects; Preferably, the photoresist has a thickness of 1-5 μm.
8. The advanced integrated circuit wafer recycling method according to any one of claims 1 to 7, It is characterized in that The filler filling the bubble defects after the first wet etching is SiO 2 When the etching solution used for the second wet etching includes a spinD solution, the spinD solution is a mixed solution of phosphoric acid with a concentration of 18-22%, nitric acid with a concentration of 38-42%, sulfuric acid with a concentration of 8-12%, and hydrofluoric acid with a concentration of 3-4%; Preferably, the etching rate of the spinD solution on the superlens structure layer is 6-8 μm / min; Preferably, the spinD solution is 2 The etching rate is Preferably, the temperature of the second wet etching is 20-25°C; Preferably, the second wet etching time is 1-5 minutes.
9. The advanced integrated circuit wafer recycling method according to claim 8, It is characterized in that When the filler used to fill the bubble defects before the first wet etching is photoresist, the etching solution used in the second wet etching further includes an SPM solution; Preferably, when the filler at the bubble defect is photoresist, the specific steps of the second wet etching include: etching the superlens structure layer with a spinD solution, and then etching the photoresist with a SPM solution.
10. The advanced integrated circuit wafer recycling method according to claim 9, It is characterized in that The SPM solution includes a mixed solution of sulfuric acid and hydrogen peroxide in a volume ratio of (2-8):1; Preferably, the etching temperature of the SPM solution on the photoresist is 100-190°C; Preferably, the etching time of the SPM solution on the photoresist is 1-5 min; Preferably, the grinding amount for surface flattening is