Preparation method of metal interconnection structure
By adding a high-temperature thermal annealing process after the electrochemical plating process, the problem of stress migration failure in copper interconnect structures was solved, and the full reorganization of copper grains and the reliability of stress migration were improved.
Patent Information
- Application Number
- CN202410997130.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-08
AI Technical Summary
In copper interconnect structures, stress migration failure is a common problem in traditional fabrication processes, especially due to insufficient copper grain reorganization.
A high-temperature thermal annealing process is added after the electrochemical plating process, and high-temperature thermal annealing is performed before grinding to promote the recombination of copper grains and the release of vacancies. The high-temperature thermal annealing process enables the copper grains to grow fully and reduces the surface roughness.
It improves the stress migration reliability of copper interconnect structures, reduces the occurrence of stress migration, and enhances the stability of metal interconnect structures.
Smart Images

Figure CN118919487A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of semiconductor manufacturing technology, and in particular to a method for preparing a metal interconnection structure. Background Art
[0002] As VLSI (Very Large Scale Integration) develops to the ultra-deep submicron and nanometer stages, copper interconnects have successfully replaced aluminum interconnects and become the mainstream interconnect metal material. Stress migration or stress-induced vacancies in copper interconnects under thermal stress is an important factor affecting the reliability of copper interconnects.
[0003] The copper atomic grains in the copper interconnects generated after ECP (electrochemical plating) plating are small and have high energy. As time goes by, the grains swallow each other, transfer energy, and eventually grow into larger grains. The smaller the initial grains, the more vacancies are generated when growing into large grains, resulting in vacancy defects in certain areas. Although ECP has its own annealing process, the annealing temperature and time cannot complete the recombination of copper grains, and the grains cannot grow fully, so that the grains will continue to reorganize during the subsequent NDC (nitrogen-doped silicon carbide) deposition process, but the vacancies cannot be released due to the deposition of NDC, resulting in SM (stress migration) failure of the copper interconnect. Summary of the invention
[0004] The present application provides a method for preparing a metal interconnect structure, which can solve the problem of stress migration failure of copper interconnect in the traditional preparation process.
[0005] The present invention provides a method for preparing a metal interconnect structure, comprising:
[0006] A semiconductor structure is provided, wherein a metal interconnection layer is formed in the semiconductor structure, and a first barrier layer, a low-K dielectric layer, a buffer layer and a hard mask layer are sequentially stacked on the surface of the semiconductor structure, wherein the first barrier layer covers the metal interconnection layer;
[0007] Etching the hard mask layer, the buffer layer, the low-K dielectric layer, and the first barrier layer to the surface of the semiconductor structure to form a trench, wherein the metal interconnection layer is exposed at the bottom of the trench;
[0008] forming a diffusion suppression layer, wherein the diffusion suppression layer covers the sidewalls of the trench and the surface of the hard mask layer;
[0009] forming a main metal layer by an electrochemical plating process, wherein the main metal layer covers the diffusion suppression layer on the surface of the hard mask layer and fills the trench;
[0010] Conduct low-temperature thermal annealing process that comes with the electrochemical plating process;
[0011] Performing a high temperature thermal annealing process;
[0012] The main metal layer, the diffusion suppression layer, the hard mask layer and the buffer layer on the surface of the low-K dielectric layer and the main metal layer in the groove beyond the surface of the low-K dielectric layer are removed by grinding to obtain a metal interconnection structure, which is composed of the remaining main metal layer, the diffusion suppression layer and the metal interconnection layer.
[0013] Optionally, in the method for preparing the metal interconnect structure, the process temperature of the high-temperature thermal annealing process is 350° C. and the duration is 300 seconds.
[0014] Optionally, in the method for preparing the metal interconnect structure, the process temperature of the low-temperature thermal annealing process in the electrochemical plating process does not exceed 180° C., and the duration does not exceed 90 seconds.
[0015] Optionally, in the method for preparing the metal interconnect structure, after grinding and removing the main metal layer, the diffusion suppression layer, the hard mask layer and the buffer layer on the surface of the low-K dielectric layer and the main metal layer in the groove beyond the surface of the low-K dielectric layer to obtain the metal interconnect structure, the method for preparing the metal interconnect structure further comprises:
[0016] A second barrier layer is formed, wherein the second barrier layer covers the main metal layer in the trench and the low-K dielectric layer.
[0017] Optionally, in the method for preparing the metal interconnect structure, the first barrier layer and the second barrier layer are both made of nitrogen-doped silicon carbide.
[0018] Optionally, in the method for preparing the metal interconnect structure, the material of the buffer layer is SiON; the material of the hard mask layer is titanium nitride; and the material of the low-K dielectric layer is BD or BDII.
[0019] Optionally, in the method for preparing the metal interconnect structure, the diffusion suppression layer includes: a stacked tank nitride layer and a tank layer, and the tank nitride layer covers the sidewalls and the bottom wall of the trench.
[0020] Optionally, in the method for preparing the metal interconnect structure, the thickness of the diffusion suppression layer is
[0022] Optionally, in the method for preparing the metal interconnect structure, the main metal layer is made of copper.
[0023] The technical solution of this application has at least the following advantages:
[0024] The present application adds a high-temperature thermal annealing process after the electrochemical plating process and before the grinding process, so that the grains in the main metal layer can complete the grain reorganization before the subsequent deposition of the second barrier layer (NDC layer), the grains can fully grow, and the vacancies can be fully released to diffuse to the surface of the main metal layer and disappear, so as to improve the reliability of stress migration of the main metal layer; in addition, adding a high-temperature thermal annealing process before the grinding process can also reduce the surface roughness of the main metal layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0026] Figure 1 is a flow chart of a method for preparing a metal interconnect structure according to an embodiment of the present invention;
[0027] Figure 2-Figure 7 is a schematic diagram of a semiconductor structure in each process step of preparing a metal interconnect structure according to an embodiment of the present invention;
[0028] The reference numerals are described as follows:
[0029] 10-semiconductor structure, 11-metal interconnection layer, 12-diffusion suppression layer 1, 20-first barrier layer, 30-low-K dielectric layer, 40-buffer layer, 50-hard mask layer, 51-trench, 60-diffusion suppression layer 2, 70-main metal layer, 80-second barrier layer. DETAILED DESCRIPTION
[0030] The following will be combined with the accompanying drawings to clearly and completely describe the technical solutions in this application. Obviously, the described embodiments are part of the embodiments of this application, not all of them. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0031] In the description of the present application, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present application. In addition, the terms "first", "second", and "third" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.
[0032] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, it can also be the internal connection of two components, it can be a wireless connection, or it can be a wired connection. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0033] In addition, the technical features involved in the different embodiments of the present application described below can be combined with each other as long as they do not conflict with each other.
[0034] The present invention provides a method for preparing a metal interconnect structure. Figure 1 , Figure 1 1 is a flow chart of a method for preparing a metal interconnect structure according to an embodiment of the present invention. The method for preparing a metal interconnect structure includes:
[0035] Step S1: providing a semiconductor structure, wherein a metal interconnection layer is formed in the semiconductor structure, and a first barrier layer, a low-K dielectric layer, a buffer layer and a hard mask layer are sequentially stacked on the surface of the semiconductor structure, wherein the first barrier layer covers the metal interconnection layer;
[0036] Step S2: etching the hard mask layer, the buffer layer, the low-K dielectric layer, and the first barrier layer to the surface of the semiconductor structure to form a trench, wherein the metal interconnection layer is exposed at the bottom of the trench;
[0037] Step S3: forming a diffusion suppression layer, wherein the diffusion suppression layer covers the sidewalls and bottom wall of the trench and the surface of the hard mask layer;
[0038] Step S4: forming a main metal layer by an electrochemical plating process, wherein the main metal layer covers the diffusion suppression layer and fills the groove;
[0039] Step S5: performing a low-temperature thermal annealing process inherent in the electrochemical plating process;
[0040] Step S6: performing a high temperature thermal annealing process;
[0041] Step S7: Grind and remove the main metal layer, the diffusion suppression layer, the hard mask layer and the buffer layer on the surface of the low-K dielectric layer and the main metal layer in the groove beyond the surface of the low-K dielectric layer to obtain a metal interconnection structure, wherein the metal interconnection structure is composed of the remaining main metal layer, the diffusion suppression layer and the metal interconnection layer.
[0042] Specifically, refer to Figure 2-Figure 7 , Figure 2-Figure 7 Schematic diagram of semiconductor structure in each process step of preparing metal interconnect structure according to an embodiment of the present invention. Next, the preparation method of metal interconnect structure provided by the present application is specifically introduced.
[0043] First, perform step S1: refer to Figure 2 , Figure 2 1 is a schematic diagram of a semiconductor structure after a hard mask layer is formed according to an embodiment of the present invention, and provides a semiconductor structure 10, wherein an opening is formed in the semiconductor structure 10, a metal interconnection layer 11 is formed in the opening, and a diffusion suppression layer 12 for suppressing the diffusion of metal atoms is also formed on the sidewall of the metal interconnection layer. A first barrier layer 20, a low-K dielectric layer 30, a buffer layer 40 and a hard mask layer 50 are stacked in sequence on the surface of the semiconductor structure 10, and the first barrier layer 20 covers the metal interconnection layer 11.
[0044] In this embodiment, the material of the first barrier layer 20 is nitrogen-doped silicon carbide (NDC); the material of the low-K dielectric layer 30 is BD or BDII; the material of the buffer layer 40 is SiON; and the material of the hard mask layer 50 is titanium nitride.
[0045] Furthermore, the diffusion suppression layer 12 includes: a stacked tank nitride layer and a tank layer, and the tank nitride layer covers the sidewalls of the opening.
[0046] In this embodiment, the metal interconnection layer 11 is a copper interconnection layer.
[0047] Then, execute step S2: refer to Figure 3 , Figure 3 It is a schematic diagram of the semiconductor structure after the groove is formed according to an embodiment of the present invention. The hard mask layer 50, the buffer layer 40, the low-K dielectric layer 30, and the first barrier layer 20 are etched to the surface of the semiconductor structure 10 to form a groove 51, and the bottom of the groove 51 exposes the metal interconnection layer 11.
[0048] Next, execute step S3: refer to Figure 4 , Figure 4Schematic diagram of a semiconductor structure after a diffusion suppression layer is formed according to an embodiment of the present invention. A second diffusion suppression layer 60 is formed. The second diffusion suppression layer 60 covers the sidewalls and bottom wall of the trench 51 and the surface of the hard mask layer 50 .
[0049] Further, step S4 is performed: refer to Figure 5 , Figure 5 Schematic diagram of the semiconductor structure after the main metal layer is formed according to an embodiment of the present invention. The main metal layer 70 is formed by an electrochemical plating process. The main metal layer 70 covers the second diffusion suppression layer 60 and fills the groove 51.
[0050] In this embodiment, the main metal layer 70 is made of copper.
[0051] Next, step S5 is performed: performing a low-temperature thermal annealing process inherent in the electrochemical plating process.
[0052] Preferably, the process temperature of the low-temperature thermal annealing process in the electrochemical plating process does not exceed 180° C., and the duration does not exceed 90 seconds.
[0053] In this embodiment, although the electrochemical plating process has its own low-temperature annealing process, the annealing temperature and time cannot complete the reorganization of the copper grains in the main metal layer, so that new vacancies will be generated and diffused to the interface between the main metal layer and the second barrier layer after the subsequent deposition of the second barrier layer. However, at this time, the excess vacancies will be captured in the copper metal interconnect structure and cannot escape or be released, resulting in the stress migration at the interface between the copper metal interconnect structure (main metal layer) and the second barrier layer being prone to failure after the deposition of the second barrier layer.
[0054] Further, step S6 is performed: performing a high temperature thermal annealing process.
[0055] Preferably, the high temperature thermal annealing process has a process temperature of 350° C. and a duration of 300 seconds.
[0056] In the present application, by adding a high-temperature thermal annealing process after the low-temperature thermal annealing process of the electrochemical plating process and before the grinding process, the copper grains in the main metal layer can be completely reorganized before the subsequent deposition of the second barrier layer (NDC layer), the grains grow fully, the vacancies are fully released, diffuse to the surface of the main metal layer and disappear, and no new vacancies are formed in the subsequent main metal layer, so as to improve the reliability of stress migration of the main metal layer. In addition, adding a high-temperature thermal annealing process before the grinding process can also reduce the surface roughness of the main metal layer.
[0057] Finally, execute step S7: reference Figure 6 , Figure 61 is a schematic diagram of a semiconductor structure after a grinding process according to an embodiment of the present invention, wherein the main metal layer 70, the diffusion suppression layer 2 60, the hard mask layer 50 and the buffer layer 40 on the surface of the low-K dielectric layer 30 and the main metal layer 70 in the groove extending beyond the surface of the low-K dielectric layer 30 are removed by grinding to obtain a metal interconnect structure, wherein the metal interconnect structure is composed of the remaining main metal layer 70, the diffusion suppression layer 2 60 and the metal interconnect layer 11.
[0058] In this embodiment, a CMP (chemical mechanical polishing) process is used to polish and remove the main metal layer 70, the diffusion suppression layer 2 60, the hard mask layer 50 and the buffer layer 40 on the surface of the low-K dielectric layer 30, and the main metal layer 70 extending beyond the surface of the low-K dielectric layer 30 in the groove to obtain a metal interconnection structure.
[0059] For further reference, Figure 7 , Figure 7 1 is a schematic diagram of a semiconductor structure after forming a second barrier layer according to an embodiment of the present invention. After grinding and removing the main metal layer 70, the diffusion suppression layer 2 60, the hard mask layer 50 and the buffer layer 40 on the surface of the low-K dielectric layer 30 and the main metal layer 70 in the groove that exceeds the surface of the low-K dielectric layer 30 to obtain a metal interconnect structure, the method for preparing the metal interconnect structure also includes: forming a second barrier layer 80, and the second barrier layer 80 covers the main metal layer 70 in the groove 51 and the low-K dielectric layer 30.
[0060] In this embodiment, the second barrier layer 80 is made of nitrogen-doped silicon carbide.
[0061] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection created by this application.
Claims
1. A method for preparing a metal interconnect structure, characterized in that: include: A semiconductor structure is provided, wherein a metal interconnection layer is formed in the semiconductor structure, and a first barrier layer, a low-K dielectric layer, a buffer layer and a hard mask layer are sequentially stacked on the surface of the semiconductor structure, wherein the first barrier layer covers the metal interconnection layer; Etching the hard mask layer, the buffer layer, the low-K dielectric layer, and the first barrier layer to the surface of the semiconductor structure to form a trench, wherein the metal interconnection layer is exposed at the bottom of the trench; forming a diffusion suppression layer, wherein the diffusion suppression layer covers the sidewalls and bottom wall of the trench and the surface of the hard mask layer; forming a main metal layer by an electrochemical plating process, the main metal layer covering the diffusion suppression layer and filling the trench; Conduct low-temperature thermal annealing process that comes with the electrochemical plating process; Performing a high temperature thermal annealing process; The main metal layer, the diffusion suppression layer, the hard mask layer and the buffer layer on the surface of the low-K dielectric layer and the main metal layer in the groove beyond the surface of the low-K dielectric layer are removed by grinding to obtain a metal interconnection structure, which is composed of the remaining main metal layer, the diffusion suppression layer and the metal interconnection layer.
2. The method for preparing a metal interconnect structure according to claim 1, characterized in that: The high temperature thermal annealing process has a process temperature of 350° C. and a duration of 300 seconds.
3. The method for preparing a metal interconnect structure according to claim 1, characterized in that: The process temperature of the low-temperature thermal annealing process in the electrochemical plating process does not exceed 180° C., and the duration does not exceed 90 seconds.
4. The method for preparing a metal interconnect structure according to claim 1, characterized in that: After grinding and removing the main metal layer, the diffusion suppression layer, the hard mask layer and the buffer layer on the surface of the low-K dielectric layer and the main metal layer in the groove beyond the surface of the low-K dielectric layer to obtain a metal interconnect structure, the method for preparing the metal interconnect structure further includes: A second barrier layer is formed, wherein the second barrier layer covers the main metal layer in the trench and the low-K dielectric layer.
5. The method for preparing a metal interconnect structure according to claim 1, characterized in that: The first barrier layer and the second barrier layer are both made of nitrogen-doped silicon carbide.
6. The method for preparing a metal interconnect structure according to claim 1, characterized in that: The material of the buffer layer is SiON; the material of the hard mask layer is titanium nitride; and the material of the low-K dielectric layer is BD or BDII.
7. The method for preparing a metal interconnect structure according to claim 1, characterized in that: The diffusion suppression layer includes: a stacked tank layer and a tank layer, wherein the tank layer covers the sidewall and bottom wall of the trench.
8. The method for preparing a metal interconnect structure according to claim 1, characterized in that: The thickness of the diffusion suppression layer is 9. The method for preparing a metal interconnect structure according to claim 1, characterized in that: The main metal layer is made of copper.