Electrode for lithium secondary battery and lithium secondary battery comprising same
By using PVDF-HFP as the adhesive for the primer in the lithium secondary battery electrode, the interface resistance between the electrode current collector and the active material layer is increased, and the explosion problem caused by nail stings is solved and the safety of the battery is improved and thermal safety.
Patent Information
- Application Number
- CN202411278578.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2018-08-08
- Filing Date
- 2019-07-31
- Publication Date
- 2024-11-08
AI Technical Summary
In the process of high energy density and output development, lithium secondary batteries have reduced safety, especially the explosion problem caused by nail stings, which is mainly due to local IR heating caused by short-circuit current between the electrode active material layer and the current collector.
Introducing a base coat containing poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP) into the electrode of the lithium secondary battery, as a binder, to increase the electrode current collector and the electrode active material layer Interface resistance reduces the short circuit current when nailing.
By increasing the interface resistance, the short-circuit current during nail stabbing is reduced, the battery's safety is improved, and the temperature caused by IR heating is reduced by improving the thermal safety of the adhesive, enhancing the overall safety performance of the battery.
Smart Images

Figure CN118919649A_ABST
Abstract
Description
[0001] This application is a divisional application. The international application number of the original application is PCT / KR2019 / 009574, the application number of the Chinese national phase is 201980049126.9, the application date is July 31, 2019, and the name of the invention is "Electrode for lithium secondary battery and lithium secondary battery containing the electrode". Technical Field
[0002] This application claims the priority of Korean Patent Application No. 10-2018-0092536 filed in Korea on August 8, 2018. The present disclosure relates to an electrode for a lithium secondary battery and a lithium secondary battery including the electrode. More specifically, the present disclosure relates to an electrode for a lithium secondary battery that can provide improved nail puncture safety and a lithium secondary battery including the electrode. Background Art
[0003] Recently developed lithium secondary batteries for vehicles are required to have high energy density and high output. However, the development of lithium secondary batteries towards high energy density and output has led to a decrease in battery safety. In addition, with the increasing demand for lithium secondary batteries, the demand for safety has increased significantly. In particular, when the battery pack is penetrated due to external impact or appearance deformation, an explosion of manual devices such as vehicles may occur. Therefore, in the safety evaluation items of lithium secondary batteries for vehicles, penetration safety is considered an important item, and many attempts have been made to improve this.
[0004] In particular, it is known that the explosion caused by nail penetration is caused by local IR heating due to a short-circuit current caused by the contact between the nail and the electrode current collector or the contact between the electrode active material layer and the electrode current collector.
[0005] In order to solve the problems related to such nail puncture safety, it is important to increase the interfacial resistance between the electrode active material layer and the electrode current collector. This is because a high-rate current flows due to the short circuit caused by the nail puncture, and at this time, electrons are transferred from the electrode active material to the electrode current collector and the nail. In this case, when the resistance increases, the short-circuit current of the nail puncture decreases, so IR heating can be reduced. Summary of the invention
[0006] [Technical issues]
[0007] The present disclosure is designed to solve the problems in the related art, and thus the present disclosure aims to provide an electrode for a lithium secondary battery that can provide improved nail penetration safety and a lithium secondary battery including the electrode.
[0008] [Technical solution]
[0009] According to a first embodiment of the present disclosure, an electrode for a lithium secondary battery is provided, comprising: an electrode current collector; a primer layer disposed on at least one surface of the electrode current collector and comprising a binder and a conductive material; and an electrode active material layer disposed on the primer layer, wherein the binder comprises poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP), which contains repeating units derived from vinylidene fluoride (VDF) and repeating units derived from hexafluoropropylene (HFP), the content of the repeating units derived from HFP in the PVDF-HFP is 2 wt % to 13 wt %, and the thickness of the primer layer is 0.8 μm to 5 μm.
[0010] According to a second embodiment of the present disclosure, there is provided the lithium secondary battery electrode as described in the first embodiment, wherein the undercoat layer includes the binder in an amount of 10 to 80 parts by weight based on 100 parts by weight of the conductive material.
[0011] According to a third embodiment of the present disclosure, there is provided the lithium secondary battery electrode as described in the second embodiment, wherein the undercoat layer includes the binder in an amount of 35 to 65 parts by weight based on 100 parts by weight of the conductive material.
[0012] According to a fourth embodiment of the present disclosure, there is provided the electrode for a lithium secondary battery as described in any one of the first to third embodiments, wherein the content of the HFP-derived repeating unit in the PVDF-HFP polymer is 3 wt % to 10 wt %.
[0013] According to a fifth embodiment of the present disclosure, there is provided the electrode for a lithium secondary battery as described in any one of the first to fourth embodiments, wherein the thickness of the undercoat layer is 1 μm to 2 μm.
[0014] According to a sixth embodiment of the present disclosure, there is provided the electrode for a lithium secondary battery as described in any one of the first to fifth embodiments, wherein the thickness of the undercoat layer is 0.01 to 0.05 times the thickness of the electrode active material layer.
[0015] According to a seventh embodiment of the present disclosure, there is provided the lithium secondary battery electrode as described in the sixth embodiment, wherein the thickness of the undercoat layer is 0.01 to 0.03 times the thickness of the electrode active material layer.
[0016] According to an eighth embodiment of the present disclosure, there is provided the electrode for a lithium secondary battery as described in any one of the first to seventh embodiments, wherein the binder includes PVDF-HFP in an amount of 50 wt % or more based on 100 wt % of the binder.
[0017] According to a ninth embodiment of the present disclosure, there is provided an electrode for a lithium secondary battery as described in any one of the first to seventh embodiments, wherein the electrode active material layer contains an electrode binder, and the amount of PVDF-HFP used is 5 wt % or less based on 100 wt % of the electrode binder.
[0018] In another aspect of the present disclosure, a lithium secondary battery is provided, including a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, wherein the positive electrode or the negative electrode is the electrode according to any one of the first to ninth embodiments.
[0019] [Beneficial Effects]
[0020] The electrode for a lithium secondary battery of an embodiment of the present disclosure includes a primer layer comprising PVDF-HFP as a binder and a conductive material between an electrode current collector and an electrode active material layer, thereby increasing the interfacial resistance between the electrode current collector and the electrode active material layer, and reducing the amount of short-circuit current flowing through the nail even when a nail puncture occurs, thereby ultimately improving the safety of the battery.
[0021] In addition, HFP contained in PVDF-HFP can improve the thermal safety of the adhesive, and thus can reduce the temperature within the battery due to IR heating. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The accompanying drawings illustrate preferred embodiments of the present disclosure, and together with the foregoing disclosure, are used to provide a further understanding of the technical features of the present disclosure. Therefore, the present disclosure is not interpreted as being limited to the accompanying drawings.
[0023] Figure 1 Schematic diagram showing the structure of an electrode for a lithium secondary battery according to an embodiment of the present disclosure. DETAILED DESCRIPTION
[0024] Hereinafter, preferred embodiments of the present disclosure will be described in detail with reference to the accompanying drawings. Before the description, it should be understood that, based on the principle of allowing the inventor to appropriately define terms for the best interpretation, the terms used in the specification and the appended claims should not be interpreted as limited to the general meaning and dictionary meaning, but should be interpreted based on the meaning and concept corresponding to the technical aspects of the present disclosure.
[0025] Therefore, the descriptions presented herein are merely preferred examples for illustrative purposes and are not intended to limit the scope of the present disclosure. It should be appreciated that other equivalent substitutions and modifications may be made thereto without departing from the scope of the present disclosure.
[0026] In one aspect of the present disclosure, a negative electrode 100 for a lithium secondary battery is provided. Figure 1The negative electrode 100 for a lithium secondary battery includes: an electrode current collector 10; an undercoat layer 20 disposed on at least one surface of the electrode current collector and containing a binder and a conductive material; and an electrode active material layer 30 disposed on the undercoat layer.
[0027] According to one embodiment of the present disclosure, the electrode current collector 10 is not specifically limited as long as it has conductivity and does not cause any chemical changes in the battery. For example, the electrode current collector that can be used includes copper, stainless steel, aluminum, nickel, titanium, fired carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., or aluminum-cadmium alloy, etc.
[0028] The thickness of the electrode current collector is not particularly limited, but may be 3 μm to 500 μm as conventionally used in the art.
[0029] According to one embodiment of the present disclosure, the primer layer 20 may include poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP) as a binder, which contains repeating units derived from vinylidene fluoride (VDF) and repeating units derived from hexafluoropropylene (HFP). According to one embodiment of the present disclosure, based on 100 wt % of the binder, the content of PVDF-HFP may be 50 wt % or more, 80 wt % or more, 90 wt % or more, or 99 wt % or more.
[0030] HFP contained in PVDF-HFP characteristically shows an increase in absorbency for organic electrolyte, so the swelling degree of the PVDF-HFP binder can be controlled according to the HFP content. In other words, as the HFP content increases, the swelling of the PVDF-HFP binder also increases.
[0031] When PVDF-HFP is used as a binder contained in the electrode active material layer, the cycle characteristics may be deteriorated, and the swelling of the battery may be deteriorated, resulting in reduced battery performance. In contrast, in the present invention, PVDF-HFP as a binder is contained in the undercoat layer rather than the electrode active material layer, so the above-mentioned side effects are not a problem.
[0032] In other words, the primer layer containing PVDF-HFP as a binder is disposed between the electrode current collector and the electrode active material layer, thereby increasing the interfacial resistance between the electrode current collector and the electrode active material layer while substantially not affecting the swelling of the entire electrode. Therefore, even if a nail puncture occurs, the amount of short-circuit current flowing into the nail can be reduced, thereby ultimately improving battery safety.
[0033] In addition, HFP improves the thermal safety of the adhesive, thus reducing the temperature inside the battery due to IR heating.
[0034] For these reasons, according to the present disclosure, the primer layer disposed between the electrode current collector and the electrode active material layer comprises a PVDF-HFP binder, the amount of the HFP-derived repeating unit contained in it being 2 wt % to 13 wt %, particularly 3 wt % to 10 wt %, and more particularly 3 wt % to 7 wt %. When the content of the repeating unit derived from HFP is less than 2 wt %, the binder may not swell sufficiently when using HFP, and thermal safety cannot be fully ensured. When the content of HFP exceeds 13 wt %, the adhesive exhibits reduced adhesion (which is the main function of the binder), and excessive swelling occurs, resulting in excessive increase in the resistance of the primer layer, which reduces the life characteristics.
[0035] According to the present disclosure, the content of the repeating unit based on weight can be 1 H-NMR, for example, Varian 500.
[0036] In addition, the undercoat layer should have a thickness significantly smaller than that of the electrode active material layer so that it can have little effect on the swelling of the entire electrode. In other words, the thickness of the undercoat layer is preferably 0.8 μm to 5 μm, particularly 1 μm to 2 μm, and more particularly 1 μm to 1.5 μm. When the thickness of the undercoat layer is less than 0.8 μm, the effect of sufficiently increasing resistance and swelling cannot be provided. When the thickness of the undercoat layer is greater than 10 μm, resistance and swelling are excessively increased, causing a problem of reduced life characteristics.
[0037] Specifically, the thickness of the undercoat layer is preferably controlled to be 0.01 to 0.05 times, particularly 0.01 to 0.03 times, the thickness of the electrode active material layer.
[0038] Meanwhile, based on 100 parts by weight of the conductive material, the content of the PVDF-HFP binder of the primer layer may be 10 to 80 parts by weight, particularly 35 to 65 parts by weight, and more particularly 40 to 50 parts by weight. When the content of the PVDF-HFP binder satisfies the above range, the amount of short-circuit current during nail penetration can be reduced while maintaining adhesion to the battery (which is the essential purpose of the binder), thereby providing an effect of improving safety.
[0039] The primer layer may be formed by dispersing PVDF-HFP as a binder and a conductive material in a solvent to obtain slurry, and applying the obtained slurry to at least one surface of the electrode current collector.
[0040] Here, the conductive material can be the conductive material currently used for the electrode active material layer. For example, the conductive material may include any one selected from the following or a mixture of two or more thereof: graphite, such as natural graphite or artificial graphite; carbon black, such as acetylene black, Ketjen black, channel black, furnace black, lamp black, or thermal black; conductive fibers, such as carbon fibers or metal fibers; metal powders, such as aluminum or nickel powders; conductive whiskers, such as zinc oxide or potassium titanate; conductive metal oxides, such as titanium dioxide; and conductive materials such as polyphenylene derivatives.
[0041] According to one embodiment of the present disclosure, the electrode active material layer 30 can be formed as follows: an electrode slurry is obtained by dispersing an active material, an electrode binder, and a conductive material in a solvent, the electrode slurry is coated on the undercoat layer 20, and then dried and pressed.
[0042] Here, when the electrode for a lithium secondary battery according to one embodiment of the present disclosure is a positive electrode, the positive electrode active material can be any material commonly used as the positive electrode active material for a lithium secondary battery. For example, the positive electrode active material may include, but is not limited to: layered compounds, such as lithium cobalt oxide (LiCoO2) and lithium nickel oxide (LiNiO2), or these compounds substituted with one or more transition metals; lithium manganese oxides, such as lithium manganese oxides represented by the chemical formula Li 1+x Mn 2-x O4 (where x is 0 - 0.33), LiMnO3, LiMn2O3, and LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides, such as LiV3O8, LiV3O4, V2O5, or Cu2V2O7; nickel-site type lithium nickel oxides represented by the chemical formula LiNi 1-x M x O2 (where M is Co, Mn, Al, Cu, Fe, Mg, B, or Ga, and x is 0.01 - 0.3); lithium manganese composite oxides represented by the chemical formula LiMn 2-x M x O2 (where M = Co, Ni, Fe, Cr, Zn, or Ta, x = 0.01 - 0.1), Li2Mn3MO8 (where M = Fe, Co, Ni, Cu, or Zn), or Li a Ni x Co y Mn z O2 (0.5 < a < 1.5, 0 < x, y, z < 1, x + y + z = 1); lithium manganese composite oxides having a spinel structure and represented by the chemical formula LiNi x Mn 2-x O4; LiMn2O4 partially substituted with alkaline earth metal ions; disulfides; Fe2(MoO4)3; or LiNi 0.8 Co 0.1 Mn0.1 such as O2.
[0043] Meanwhile, when the electrode for a lithium secondary battery according to an embodiment of the present disclosure is a negative electrode, the negative electrode active material can be any material commonly used as the negative electrode active material of a lithium secondary battery. For example, the negative electrode active material may include, but is not limited to: carbon, such as non-graphitized carbon or graphitic carbon (natural graphite, artificial graphite), etc.; metal composite oxides, such as Li x Fe2O3 (0 ≤ x ≤ 1), Li x WO2 (0 ≤ x ≤ 1), Sn x Me 1-x Me' y O z (Me: Mn, Fe, Pb or Ge; Me': Al, B, P, Si, Group 1, Group 2 or Group 3 elements in the periodic table, or halogen; 0 < x ≤ 1; 1 ≤ y ≤ 3; 1 ≤ z ≤ 8); lithium metal; lithium alloy; silicon-based alloy; tin-based alloy; metal oxides, such as SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4 or Bi2O5, etc.; conductive polymers, such as polyacetylene; Li-Co-Ni-based materials; titanium dioxide; and lithium titanium oxides, etc. According to an embodiment of the present disclosure, the negative electrode active material may include a carbonaceous material and / or Si.
[0044] There is no specific limitation on the conductive material as long as it does not cause chemical changes in the corresponding battery and has conductivity. For example, the conductive material includes any one selected from the following or a mixture of two or more thereof: graphite, such as natural graphite or artificial graphite; carbon black, such as acetylene black, Ketjen black, channel black, furnace black, lamp black or thermal cracking carbon black; conductive fibers, such as carbon fibers or metal fibers; metal powders, such as aluminum or nickel powders; conductive whiskers, such as zinc oxide or potassium titanate; conductive metal oxides, such as titanium dioxide; and conductive materials such as polyphenylene derivatives. Based on the total weight of the electrode active material layer, the amount of the conductive material can be 0.1 wt% to 20 wt%, particularly 1 wt% to 10 wt%.
[0045] In addition, the electrode binder may include at least one selected from the following: polyvinylidene fluoride (PVDF), polyvinylidene fluoride-co-trichloroethylene, polymethyl methacrylate, polyethylhexyl acrylate, polybutyl acrylate, polyacrylonitrile, polyvinyl pyrrolidone, polyvinyl acetate, polyethylene-co-vinyl acetate, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan, styrene-butadiene rubber (SBR) or carboxymethyl cellulose, etc., but the scope of the present disclosure is not limited thereto. At the same time, due to the problem of battery swelling, PVDF-HFP is not suitable as an adhesive for an electrode. Based on the gross weight of the electrode active material layer, the amount of the binder may be less than 20% by weight, less than 10% by weight, less than 5% by weight or less than 1% by weight. For example, the amount of the binder may be less than 0.1% by weight. Specifically, the electrode binder may include PVDF-HFP in an amount of 5 wt % or less, 1 wt % or less, or 0.1 wt % or less, based on 100 wt % of the entire electrode binder.
[0046] In another aspect of the present disclosure, a lithium secondary battery is provided, which includes a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, wherein the positive electrode or the negative electrode is an electrode for a lithium secondary battery according to an embodiment of the present disclosure.
[0047] Specifically, the lithium secondary battery electrode of the embodiment of the present disclosure can be a positive electrode. When preparing the coating slurry, the binder for the primer layer can be used together with an organic solvent, and compared to the negative electrode, the organic solvent is more frequently used when manufacturing the positive electrode. Therefore, it is more suitable to use the lithium secondary battery electrode for the positive electrode.
[0048] The separator is interposed between the positive electrode and the negative electrode and plays a role in allowing lithium ions to pass through while electrically insulating the positive electrode and the negative electrode from each other. The separator may be any separator commonly used in the field of lithium secondary batteries, and is not particularly limited.
[0049] The lithium secondary battery of the present invention can be used as a unit cell in a battery module. The battery module can be used in a battery pack or a device including the battery pack as a power source. Specific examples of the device include, but are not limited to: an electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, or a power storage system.
[0050] The embodiments will be described more fully below so that the present disclosure can be easily understood. However, the following embodiments are for illustrative purposes only, and the scope of the present disclosure is not limited thereto.
[0051] Example 1: Manufacturing positive electrode
[0052] (Step 1)
[0053] First, 50 parts by weight of PVDF-HFP (HFP content: 3 wt%) as a binder was dissolved in acetonitrile as a solvent to prepare a binder solution. Next, 100 parts by weight of carbon black (Super C65) as a conductive material was introduced into the binder solution to obtain a slurry for forming an undercoat layer.
[0054] Then, the slurry for forming an undercoat layer was applied to an aluminum current collector having a thickness of 20 μm to a thickness of 2.4 μm, and then vacuum dried at 120° C. for 24 hours to form an undercoat layer.
[0055] (Step 2)
[0056] First, 4 parts by weight of PVDF as a binder was dissolved in acetonitrile as a solvent to obtain a binder solution, and then 6 parts by weight of carbon black (Super C65) as a conductive material and 90 parts by weight of NCM811 (LiNi 0.8 Co 0.1 Mn 0.1 O2) to obtain a homogeneous positive electrode slurry.
[0057] The positive electrode slurry was applied to the undercoat layer formed by step 1 until the thickness was 140 μm, and vacuum dried at 120° C. for 24 hours to form a positive electrode active material layer. Then, pressing was performed to complete the positive electrode (the thickness of the positive electrode active material layer after pressing: 70 μm, the thickness of the undercoat layer after pressing: 1.2 μm, the ratio of the thickness of the undercoat layer in the completed positive electrode to the thickness of the positive electrode active material layer: 0.017).
[0058] Embodiment 2:
[0059] A positive electrode was obtained in the same manner as in Example 1, except that PVDF-HFP (HFP content: 7 wt %) was used as the binder in Step 1.
[0060] Comparative Example 1:
[0061] A positive electrode was obtained in the same manner as in Example 1, except that PVDF (HFP content: 0 wt %) was used as the binder in Step 1.
[0062] Comparative Example 2:
[0063] A positive electrode was obtained in the same manner as in Example 1, except that PVDF-HFP (HFP content: 20 wt %) was used as the binder in Step 1.
[0064] Comparative Example 3:
[0065] A positive electrode was obtained in the same manner as in Example 1, except that the thickness of the undercoat layer after pressing was 0.3 μm, and the thickness of the positive electrode active material layer after pressing was 70 μm.
[0066] Comparative Example 4:
[0067] A positive electrode was obtained in the same manner as in Example 1, except that the thickness of the undercoat layer after pressing was 10 μm, and the thickness of the positive electrode active material layer after pressing was 70 μm.
[0068] Test example:
[0069] A polyethylene film (Celgard: thickness 20 μm) was placed between each positive electrode obtained from the embodiment and the comparative example and the negative electrode described below. Then, an electrolyte containing 1M LiPF6 dissolved in a mixed solvent was injected to obtain a lithium secondary battery, wherein the mixed solvent contained ethylene carbonate, dimethylene carbonate, and diethyl carbonate in a ratio of 1:2:1. The performance of each lithium secondary battery was evaluated.
[0070] The negative electrode was obtained as follows: 96.3 wt % of artificial graphite as a negative electrode active material, 1.0 wt % of carbon black (Super P) as a conductive material, and 2.7 wt % of PVDF as a binder were dispersed in NMP as a solvent to prepare a negative electrode slurry, and the negative electrode slurry was coated on a copper foil with a thickness of 10 μm until the thickness was 160 μm, and then dried and pressed. The final thickness of the negative electrode was 90 μm.
[0071] <Nail puncture safety evaluation>
[0072] Five samples of each battery were prepared, and each sample was buffered at 4.25 V. Then, a nail penetration tester (KSG-103, KYOUNGSUNG testing machine Co., Ltd.) was used to make an iron nail with a diameter of 6 mm pass through the center of each battery from the top of each battery. Here, the nail penetration rate was always set to 12 m / min.
[0073] Whether the five samples passed the nail penetration safety test was judged according to the following evaluation criteria. The number of samples that passed the test is shown in Table 1 below.
[0074] <Evaluation Criteria>
[0075] Pass: Although smoke was observed, no combustion occurred during the nailing process
[0076] Failure: Burning occurs immediately during nail penetration or delayed burning occurs within 5 minutes or less after nail penetration
[0077] (Combustion: the production of flames or fire visible to the naked eye)
[0078] <Lifespan Characteristics>
[0079] Each battery was charged / discharged by applying a current equivalent to 1 C (40 Ah) at a voltage ranging from 3 V to 4.25 V. After a total of 100 charge / discharge cycles were performed, the capacity retention ratio was calculated by the following formula to evaluate the life characteristics.
[0080] Capacity retention rate (%) = (discharge capacity after 100 cycles / discharge capacity at the first cycle) × 100
[0081] Table 1
[0082]
[0083] As can be seen from Table 1, both Examples 1 and 2 ensure nail puncture safety and high capacity retention. In Examples 1 and 2, the primer layer provided between the electrode current collector and the electrode active material layer comprises PVDF-HFP and has a thickness of 0.8 μm to 5 μm, and the content of HFP-derived repeating units of the PVDF-HFP is 2 wt % to 13 wt %.
[0084] In contrast, Comparative Examples 1 to 4, which failed to satisfy the above-mentioned ranges of HFP content and primer layer thickness, provided inferior results in terms of nail penetration safety or high capacity retention rate.
[0085] The present disclosure has been described in detail. However, it should be understood that the detailed description and specific examples, while indicating preferred embodiments of the present disclosure, are given by way of illustration only, since various changes and modifications within the scope of the present disclosure will become apparent to those skilled in the art from this detailed description.
Claims
1. An electrode for a lithium secondary battery, comprising: Electrode current collector; a primer layer disposed on at least one surface of the electrode current collector and comprising a binder and a conductive material; and an electrode active material layer disposed on the undercoat layer, The adhesive comprises poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP), wherein the PVDF-HFP contains repeating units derived from vinylidene fluoride (VDF) and repeating units derived from hexafluoropropylene (HFP), The content of HFP-derived repeating units in PVDF-HFP is 2 wt % to 13 wt %, and The thickness of the primer layer is 0.8 μm to 5 μm; The thickness of the undercoat layer is 0.01 to 0.05 times the thickness of the electrode active material layer.
2. The lithium secondary battery electrode according to claim 1, wherein The primer layer may include the binder in an amount of 10 to 80 parts by weight based on 100 parts by weight of the conductive material.
3. The lithium secondary battery electrode according to claim 2, wherein: The primer layer includes the binder in an amount of 35 parts by weight to 65 parts by weight based on 100 parts by weight of the conductive material.
4. The lithium secondary battery electrode according to claim 1, wherein The content of the HFP-derived repeating units in the PVDF-HFP polymer is 3 to 10 wt %.
5. The lithium secondary battery electrode according to claim 1, wherein The primer layer has a thickness of 1 μm to 2 μm.
6. The lithium secondary battery electrode according to claim 1, wherein The thickness of the undercoat layer is 0.01 to 0.03 times the thickness of the electrode active material layer.
7. The lithium secondary battery electrode according to claim 1, wherein The adhesive includes PVDF-HFP in an amount of 50 wt % or more based on 100 wt % of the adhesive.
8. The lithium secondary battery electrode according to claim 1, wherein The electrode active material layer includes an electrode binder, and the amount of PVDF-HFP is 5 wt % or less based on 100 wt % of the electrode binder.
9. The electrode for lithium secondary battery according to claim 8, wherein The electrode binder includes at least one selected from the group consisting of polyvinylidene fluoride (PVDF), polyvinylidene fluoride-co-trichloroethylene, polymethyl methacrylate, polyethylhexyl acrylate, polybutyl acrylate, polyacrylonitrile, polyvinyl pyrrolidone, polyvinyl acetate, polyethylene-co-vinyl acetate, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan, styrene-butadiene rubber (SBR) and carboxymethyl cellulose. 10 . A lithium secondary battery comprising a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, wherein the positive electrode or the negative electrode is the electrode according to claim 1 .
Citation Information
Patent Citations
Personal ion skin massager
KR1020180092536A
KR2019/009574