Preparation method of high-safety sodium storage material based on sodium vanadium fluorophosphate graphene composite structure

By adding polyvinyl alcohol to a sodium vanadium fluorophosphate and graphene composite material, a three-dimensional graphene conductive network was constructed, solving the problems of low conductivity and excessive volume change of NVPF, and realizing a sodium-ion battery material with high safety and high performance.

CN118919671APending Publication Date: 2024-11-08UESTC (SHENZHEN) ADVANCED RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410947262.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing sodium vanadium fluorophosphate (NVPF) cathode material for sodium-ion batteries has poor electronic conductivity, resulting in low capacity in the battery system. Furthermore, its volume change during charge-discharge cycles is too large, causing stress concentration and affecting the cycle stability and safety of the material.

Method used

By adding polyvinyl alcohol during the preparation of sodium vanadium fluorophosphate and graphene composite material, a three-dimensional graphene conductive network is constructed by utilizing the hydrogen bonding between polyvinyl alcohol and graphene oxide to encapsulate sodium vanadium fluorophosphate particles, forming an NVPF@PVA@rGO structure. This improves electronic conductivity and ion transport performance and restricts volume change.

Benefits of technology

It significantly improves the electronic conductivity and ion transport capacity of the material, enhances cycle stability and battery safety, improves the initial capacity, cycle stability and rate performance of sodium-ion batteries, and also improves the battery's heat dissipation capacity and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919671A_ABST
    Figure CN118919671A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a high-safety sodium storage material based on a sodium vanadium fluorophosphate graphene composite structure, and belongs to the technical field of preparation of sodium ion battery positive electrode materials. The invention aims to improve the electronic conductivity and ion transport performance of the material through the design of the sodium-ion battery positive electrode material structure, thereby improving the conductivity and solving the problem of stress concentration caused by overlarge volume change of the existing battery material in charge-discharge circulation at the same time. Adding graphene, a sodium source, a vanadium source, a phosphorus source and a fluorine source into the solution, then adding polyvinyl alcohol, carrying out solvothermal reaction, and then carrying out carbonization treatment in an argon atmosphere to obtain the graphene and sodium vanadium fluorophosphate composite material. The cubic special structure can shorten the diffusion path of sodium ions, and the synthesized three-dimensional graphene conductive network structure can limit the volume change of the material in the charge-discharge cycle and relieve the stress concentration in the charge-discharge cycle. Meanwhile, the electronic conductivity of the material can be improved, and the problem of low conductivity of NVPF is effectively relieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sodium ion battery electrode material preparation, and specifically relates to a method for preparing a high-safety sodium storage material based on a sodium vanadium fluorophosphate (NVPF) graphene composite structure. Background Art

[0002] Sodium-ion batteries are one of the most promising alternatives to lithium-ion batteries. They have the advantages of relatively low cost and excellent low-temperature performance, and are an indispensable part of energy storage power stations and low-speed electric vehicles. As an important component of batteries, positive electrode materials directly affect battery performance. Polyanionic compounds have a stable open three-dimensional framework and excellent structural stability, making them promising positive electrode materials for sodium-ion batteries.

[0003] Na3V2(PO4)3 (NVP) is the most typical NASICON cathode material and has been extensively studied by many researchers. However, the theoretical capacity of NVP is only 117.6 mA h g -1 , the operating voltage is 3.4V, resulting in a theoretical energy density of only 394Whkg -1 Na3V2(PO4)2F3(NVPF) can be regarded as the replacement of phosphate ions by F ions in NVP. Due to the stronger electronegativity of F ions, it can provide a higher operating voltage (3.6 V vs. 4.0 V) and a corresponding theoretical energy density (507 Wh kg-1). 1 ).

[0004] However, the electronic conductivity of NVPF is poor, only 10 -12 S cm -1 , which greatly reduces its capacity in the battery system. Combining NVPF with carbon materials to form a composite material is one of the most cost-effective methods, and many researchers have done this work, such as combining graphene, carbon nanotubes and porous carbon with NVPF. Among them, graphene is one of the materials with the best conductivity, and introducing it into the NVPF system is the most cost-effective method. However, the current work on combining graphene with NVPF only involves simple physical adsorption between graphene and NVPF, and does not fully utilize the excellent properties of graphene. Summary of the invention

[0005] The purpose of the present invention is to improve the electronic conductivity and ion transport performance of the material through the design of the positive electrode material structure of the sodium ion battery, thereby improving the conductivity, and at the same time solve the problem of stress concentration caused by excessive volume change of existing battery materials during the charge and discharge cycle.

[0006] To achieve the above object, the technical solution of the present invention is as follows:

[0007] A method for preparing a high-safety sodium storage material based on a sodium vanadium fluorophosphate graphene composite structure comprises the following steps:

[0008] Step 1: Dissolve 0-0.03 g of graphene oxide in 12.5 mL of deionized water, stir evenly, and ultrasonicate for 30 minutes;

[0009] Step 2: Add 0.35 g of ammonium metavanadate and 0.56 g of oxalic acid to the above solution;

[0010] Step 3: After stirring the solution on a magnetic stirrer for 10 minutes, the solution was transferred to an oil bath and heated at 70°C for 1 hour with stirring;

[0011] Step 4: Add 0.34 g of ammonium dihydrogen phosphate and 0.19 g of sodium fluoride to the solution, stir for 10 minutes, and add 12.5 mL of ethylene glycol dropwise to the solution;

[0012] Step 5: Add 0-0.2 g of polyvinyl alcohol to the above solution, then transfer the solution to a polytetrafluoroethylene reactor and react at 170° C. for 9 h.

[0013] Step 6: Wash the sample by centrifugation with water and anhydrous ethanol, and then calcine it at 450 degrees in an argon atmosphere in a tubular furnace for 3 hours at a heating rate of 2°C / min to finally obtain cubic sodium vanadium fluorophosphate with a three-dimensional conductive network.

[0014] Preferably, in the above technical solution, the amount of graphene oxide in step 1 is 0.03 g.

[0015] In the above technical solution, the amount of polyvinyl alcohol in step 5 is 0.2 g.

[0016] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0017] 1. In the present invention, polyvinyl alcohol is added to the solution system, and the graphene gel is constructed by utilizing the hydrogen bonding between polyvinyl alcohol and graphene oxide. 3+ ) interaction, providing sites for the crystallization of sodium vanadium fluorophosphate. After a high temperature and high pressure solvent thermal process, the cubic sodium vanadium fluorophosphate is evenly combined on the three-dimensional graphene conductive network, improving the problem of low conductivity of NVPF.

[0018] 2. In the present invention, the NVPF material is wrapped by a three-dimensional graphene conductive network, which limits its volume expansion, reduces the stress in the charge and discharge cycle and effectively improves the cycle stability of the material. In addition, the high thermal conductivity of graphene is utilized to increase the heat dissipation capacity of the battery material and improve the safety of the battery.

[0019] 3. NVPF@C@rGO is also disclosed in the prior art, but the NVPF@C@rGO of the prior art is only a surfactant added, which only acts as a carbon precursor, and is different from the sodium vanadium fluorophosphate particles by simply connecting the carbon network through simple physical adsorption. The present invention adds polyvinyl alcohol during the synthesis process, through the effect of hydrogen bonds between polyvinyl alcohol and graphene, and the hydroxyl groups in polyvinyl alcohol and metal ions (V 3+ ) interact with each other, and in the nucleation process, a three-dimensional conductive network is constructed and the sodium vanadium fluorophosphate particles are tightly combined with the conductive network, thereby improving the electronic conductivity and ion transport performance of the material, thereby effectively solving the problems of low conductivity and poor rate performance of NVPF. In addition, through the three-dimensional encapsulation of graphene and carbon materials, the carbon network is like a micron-scale "cage" that limits the volume change of the material during the charge and discharge cycle, alleviates the stress concentration during the charge and discharge cycle, and effectively enhances the cycle stability of the material. Compared with the prior art, the present invention has obvious advantages in terms of initial capacity, cycle stability and rate performance.

[0020] 4. Compared with the prior art, a NVPF@C@rGO structure is also provided, wherein the composite material has hollow NVPF microspheres, and the surface of the microspheres is coated with graphene (referred to as "hollow NVPF microspheres"). Compared with the three-dimensional graphene conductive network wrapped NVPF solution provided in the present application, the present application has the following advantages:

[0021] Electrical conductivity

[0022] Three-dimensional graphene conductive network: This structure can provide more electron transmission channels, significantly improving the electronic conductivity of the material, thereby improving rate performance and cycle stability.

[0023] Hollow NVPF microspheres: The hollow structure itself can increase the surface area of ​​the material, but the conductivity improvement effect of graphene wrapped on the surface of the microspheres is not as obvious as that of the three-dimensional graphene conductive network.

[0024] 4.2 Ion transport:

[0025] Three-dimensional graphene conductive network: During the carbonization process, the amorphous carbon formed by the decomposition of polyvinyl alcohol will fill the gaps between the NVPF cubes to form a three-dimensional conductive network, which is beneficial to ion transport, reduces ion transport resistance, and improves rate performance.

[0026] Hollow NVPF microspheres: The hollow structure can shorten the ion transmission path, but graphene is wrapped on the surface of the microspheres, the ion transmission channels are relatively few, and the ion transmission resistance may be higher.

[0027] 4.3 Structural stability:

[0028] Three-dimensional graphene conductive network: During the carbonization process, a strong interaction is formed between graphene and NVPF cubes, which can limit the volume expansion of NVPF cubes during the charge and discharge process, improve structural stability, and thus enhance cycle stability.

[0029] Hollow NVPF microspheres: The hollow structure can alleviate the volume expansion of NVPF microspheres during the charging and discharging process, but the graphene wrapped on the surface of the microspheres is not as effective in improving the structural stability as the three-dimensional graphene conductive network.

[0030] 4.4. Security:

[0031] Three-dimensional graphene conductive network: During the carbonization process, strong interactions are formed between graphene and NVPF cubes, which can improve the mechanical strength of the material and thus enhance battery safety.

[0032] Hollow NVPF microspheres (D0NJ02210A): The hollow structure can reduce the density of the material, but the graphene wrapped on the surface of the microspheres is not as effective in improving safety as the three-dimensional graphene conductive network. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is an electron microscope image of the sodium ion battery electrode material of the present invention;

[0034] Figure 2 This is a physical characterization diagram of the sodium ion battery electrode material of the present invention;

[0035] Figure 3 The X-ray diffraction patterns of Examples 4 and 5 of the present invention;

[0036] Figure 4 This is a test diagram of the electrochemical performance of the sodium ion battery electrode material of the present invention;

[0037] Figure 5 The cyclic voltammetry test diagram, constant current intermittent titration technology and corresponding fitting analysis of the sodium ion battery electrode material of the present invention;

[0038] Figure 6 The electrochemical performance diagram of a full battery assembled by combining the sodium ion battery electrode material of the present invention with hard carbon;

[0039] Figure 7 The graph shows the electrochemical data and temperature variation of the sodium ion battery electrode material of the present invention after the temperature sensor is added to the half-cell assembly. DETAILED DESCRIPTION

[0040] In order to make the objectives, technical solutions and advantages of the present invention more clear, the present invention is further described in detail below in conjunction with the implementation modes and the accompanying drawings.

[0041] A method for preparing a high-safety sodium ion battery material comprises the following steps:

[0042] Example 1

[0043] Step 1: Dissolve 0.03 g of graphene oxide in 12.5 mL of deionized water, stir evenly, and ultrasonicate for 30 minutes;

[0044] Step 2: Add 0.35 g of ammonium metavanadate and 0.56 g of oxalic acid to the above solution;

[0045] Step 3: After stirring the solution on a magnetic stirrer for 10 minutes, the solution was transferred to an oil bath and heated at 70°C for 1 hour with stirring;

[0046] Step 4: Add 0.34 g of ammonium dihydrogen phosphate and 0.19 g of sodium fluoride to the solution, stir for 10 minutes, and add 12.5 mL of ethylene glycol dropwise to the solution;

[0047] Step 5: Add 0.2 g of polyvinyl alcohol to the above solution, then transfer the solution to a polytetrafluoroethylene reactor and react at 170° C. for 9 h.

[0048] Step 6: Wash the sample by centrifugation with water and anhydrous ethanol, and then calcine it at 450 degrees in an argon atmosphere in a tube furnace for 3 hours with a heating rate of 2 degrees Celsius / min to finally obtain cubic sodium vanadium fluorophosphate (NVPF@PVA@rGO) with a three-dimensional conductive network.

[0049] Example 2

[0050] Step 1: Dissolve 0.03 g of graphene oxide in 12.5 mL of deionized water, stir evenly, and ultrasonicate for 30 minutes;

[0051] Step 2: Add 0.35 g of ammonium metavanadate and 0.56 g of oxalic acid to the above solution;

[0052] Step 3: After stirring the solution on a magnetic stirrer for 10 minutes, the solution was transferred to an oil bath and heated at 70°C for 1 hour with stirring;

[0053] Step 4: Add 0.34 g of ammonium dihydrogen phosphate and 0.19 g of sodium fluoride to the solution, stir for 10 minutes, and add 12.5 mL of ethylene glycol dropwise to the solution;

[0054] Step 5: The solution was transferred to a polytetrafluoroethylene reactor and reacted at 170°C for 9 hours.

[0055] Step 6: Wash the sample by centrifugation with water and anhydrous ethanol, and then calcine at 450 degrees in an argon atmosphere in a tube furnace for 3 hours with a heating rate of 2 degrees Celsius / min to finally obtain Example 2 (NVPF@rGO).

[0056] Example 3

[0057] Step 1: Add 0.35 g of ammonium metavanadate and 0.56 g of oxalic acid to 12.5 mL of deionized water solution;

[0058] Step 2: After stirring the solution on a magnetic stirrer for 10 minutes, the solution was transferred to an oil bath and heated at 70°C for 1 hour with stirring;

[0059] Step 3: Add 0.34 g of ammonium dihydrogen phosphate and 0.19 g of sodium fluoride to the solution, stir for 10 minutes, and add 12.5 mL of ethylene glycol dropwise to the solution;

[0060] Step 4: The solution was transferred to a polytetrafluoroethylene reactor and reacted at 170°C for 9 hours.

[0061] Step 5: Wash the sample by centrifugation with water and anhydrous ethanol, and then calcine it at 450 degrees in an argon atmosphere in a tube furnace for 3 hours with a heating rate of 2 degrees Celsius / min to finally obtain cubic sodium vanadium fluorophosphate (NVPF).

[0062] Example 4

[0063] The graphene oxide in step 1 of Example 1 was adjusted to 0.01 g, and the other aspects remained unchanged, to finally obtain cubic sodium vanadium fluorophosphate (NVPF@PVA@rGO) with a three-dimensional conductive network.

[0064] Example 5

[0065] The polyvinyl alcohol in step 5 of Example 1 was adjusted to 0.1 g, and the other contents remained unchanged, to finally obtain cubic sodium vanadium fluorophosphate (NVPF@PVA@rGO) with a three-dimensional conductive network.

[0066] Adding graphene increases conductivity. Too much graphene will cause a decrease in the ratio of cost to active substances, while too little will result in poor conductivity and poor performance. A content of 30 mg is just right. Polyvinyl alcohol uses hydrogen bonds to build a graphene network, and polyvinyl alcohol performs best at 200 mg.

[0067] Figure 1 The electron microscope image of Example 1 is shown in the figure. The precursor of the material is first synthesized by hydrothermal method, and then carbonized in an argon atmosphere to finally carbonize and generate a stable cubic sodium vanadium fluorophosphate with a three-dimensional conductive network (NVPF@PV A@rGO). Figure 1 Figures 1a, 1b and 1c show that sodium vanadium fluorophosphate wrapped by a three-dimensional conductive graphene network was successfully prepared. The rGO sheet shows a very thin thickness, wrapping a single NVPF particle. In the high-resolution image ( Figure 1e), visible lattice fringes can be observed, corresponding to three different interplanar spacings of different NVPF crystal planes. In the direct proximity of the NVPF particles, an amorphous layer of about 6 nm thick can be identified, which can be attributed to the amorphous carbon generated from the carbonization of PVA. In the outermost region, several layers of rGO can be observed, while PVA effectively connects NVPF and rGO together to form a NVPF@PVA@rGO structure. In the SAED pattern ( Figure 1 e), very bright and orderly diffraction spots exist, indicating that the prepared NVPF particles have a single crystal structure. Element mapping clearly shows the uniform distribution of different elements in the local area ( Figure 1 g), confirming the successful preparation of the nanocomposite.

[0068] Figure 2 is a physical characterization diagram of the battery material of the present invention, Figure 2 a and Figure 3 X-ray electron diffraction (XRD) patterns of five implementation cases. All identified peaks match the NVPF phase annotation cards, indicating high crystallinity, which is also consistent with the SAED data. Fourier transform infrared spectroscopy ( Figure 2 b) The results show that the vibration peak of NVPF@PVA@rGO is significantly red-shifted compared to NVPF@rGO before sintering, confirming the existence of hydrogen bonds in Example 1. The surface PVA and rGO form graphene hydrogels through hydrogen bonds, and a three-dimensional conductive network is formed during the subsequent carbonization process. These hydrogen bonds provide a strong interaction between PVA and carbon, allowing rGO to cover the surface of NVPF nanocubes. The high-resolution C 1s peak is decomposed into peaks at 284.8, 285.9 and 288.9 eV ( Figure 2 d), corresponding to CC(sp 2 ), CC(sp 2 ) and OC=O bonds, confirming the presence of graphene in the material. The high-resolution XPS spectrum of V 2p shows that V2p1 / 2 and V 2p 3 / 2 peaks are located at 517.6 and 524.7 eV respectively ( Figure 2 c), these peaks are attributed to V in NVPF@PVA@rG O 3+ , which is consistent with the result of Na3V2(PO4)2F3. Figure 2 e) The spectrum shows peaks at 684.7 and 687.3 eV, corresponding to VF and FC bonds, respectively. This indicates that there is a chemical connection between NVPF and amorphous carbon generated from PVA, resulting in a coating of PVA and rGO on the surface of NVPF.

[0069] In order to demonstrate the improvement of electrochemical performance of NVPF@PVA@rGO synthesized in Example 1 compared with Example 2 (NVPF@rGO) and Example 3 (NVPF), half-cells were assembled using metallic sodium as the counter electrode and the electrochemical performance of the three examples was tested. Figure 4 The charge-discharge curve shown in a shows that the capacity of NVPF@PVA@rGO is 125 mAh g -1 , close to the theoretical capacity of the material (128 mAh g -1 ), which is higher than NVPF@rGO (115mAh g -1 ) and NVPF (65mAh g -1 ). It is obvious that the two samples containing rGO have more obvious charge-discharge platforms at about 3.6V and 4.0V, showing a more obvious two-phase transition than pure NVPF. The surface rGO improves the electronic conductivity, thereby greatly promoting the transfer of sodium ions between Na3V2(PO4)2F3 and NaV2(PO4)2F3. Cyclic voltammetry (CV) curve at a scan rate of 1mV / s ( Figure 4 b) shows two distinct redox peaks, located at 3.6 V and 4.0 V, which can be attributed to the two Na + In V 4+ / V 5+ The two-step insertion / extraction of the redox couple is consistent with the above charge-discharge curves. In particular, the redox peaks of the NVPF sample are barely observable, indicating that the electronic conductivity is very low, resulting in a low degree of these electrochemical reactions. In contrast, the NVPF@PVA@rGO electrode shows a peak with a higher current density, indicating that V in NVPF@PVA@rGO 3+ / V 4+ The transformation kinetics are better than those of NVPF@rGO and NVPF. Figure 4 c and d compare the cycling stability of the three electrodes at current densities of 1 C and 10 C. The NVPF@PVA@rGO electrode shows excellent cycling performance, with almost no capacity decay (capacity retention of 99%) after 80 cycles at 1 C. It still maintains 112 mAh g after 500 cycles at a high current of 10 C. -1 The reversible capacity is equivalent to 98% capacity retention (initial capacity is 121 mAh g- 1 In contrast, the NVPF sample not only has a low initial capacity (90 mAh g at 1C), -1 , 17mAh g at 10C -1), and showed rapid capacity decay (only 72% after 100 cycles at 1C), probably due to slow ion diffusion and large particle size. NVPF@rGO has 107 mAh g -1 The capacity is still 100 mAh g after 100 cycles. -1 of capacity (capacity retention rate of 93%), and only 71 mAh g- 1 The capacity of the battery is 64 mAh g after 500 cycles. 1 of capacity (capacity retention rate is 90%). Figure 4 e shows the rate performance of the three implementation cases. As the current density increases from 0.5, 1, 2, 5, 10, 20, 50C to 70 and 100C, the reversible capacities of NVPF@PVA@rGO are 122, 120, 118, 115, 113, 108, 96, 85, and 64 mAh g, respectively. -1 . It is worth noting that even at an ultra-high rate of 100C, it can still provide a capacity of 64mAh g-1, equivalent to 53% of the initial capacity, and when the current drops back to 0.5C, the capacity is fully restored, indicating that the material still has high structural stability at extremely high currents. In contrast, the rate performance of NVPF@rGO and pure NVP F is significantly worse, with a retention rate of only 54% at 20C and a retention rate of only 5.9% at 100C, while NVP F can only reach 13.8mAh g-1 at 20C. 1 Obviously, compared with many NVPF composites using conductive substrates, such as graphene, mesoporous carbon, and electrospun fibers ( Figure 4 f), the performance of Example 1 has significant advantages. This advanced rate performance can be attributed to the excellent ionic / electronic conductivity and strong structural stability provided by the unique structure of NVPF@PVA@rGO, which ensures the rapid migration of sodium ions and rapid electronic conduction at ultra-high rates. Long-term cycling tests were then carried out ( Figure 4 Even after 700 cycles at a high rate of 50C, the capacity of the battery is still 104 mAh g-1, corresponding to a high retention rate of 98.3% (the initial capacity is 106 mAh g -1 ).

[0070] Subsequently, the three samples of the examples (NVPF@PVA@rGO, NVPF@rGO, NVPF) were subjected to cyclic voltammetry curve tests, constant current intermittent titration techniques and fitting analysis ( Figure 5 ), the analysis results are as follows Figure 5 As shown in Figure 2, CV analysis was performed at different scan rates (from 0.2 to 1 mV s -1 , Figure 5ac) to evaluate the dynamic performance of the prepared electrode. The CV curves of NVPF@PVA@rGO show consistent shapes at different scan rates, and the peak position only shifts slightly with the increase in scan rate, reflecting the good dynamic performance of the electrode. In contrast, the CV curves of NVPF@rGO and pure NVPF show obvious changes in peak position and shape at high scan rates, indicating that the two materials have higher polarizability. The relationship between current (i) and scan rate (v) can be described by the following equation:

[0071] i=av b (1)

[0072] log i=b logv+loga (2)

[0073] After fitting, we calculated that the b value of NVPF@PVA@rGO electrode is 0.65, NVPF@rGO is 0.85, and pure NVPF is 0.40. This indicates that the sodium ion storage process of NVPF@PVA@rGO and NVPF@rGO is mainly controlled by the capacitive effect, while the sodium ion storage process of NVPF is mainly controlled by the diffusion process.

[0074] To quantitatively evaluate the kinetic performance of the electrode, we used the Randles-Sevcik equation to calculate the diffusion coefficients of sodium ions during oxidation (A1, A2) and reduction (C1, C2) in the electrode system:

[0075] I p =269000n 3 / 2 A CD 1 / 2 v 1 / 2 (3)

[0076] In this equation, Ip represents the peak current, n is the number of electrons involved in the half reaction, and D is the diffusion coefficient (cm 2 / s), v is the scan rate (v / s), A is the electrode surface area (cm 2 ), c is the concentration of the measured substance (mol / cm 3 ). Therefore, we can get the value of Ip vs.v 12 picture( Figure 5 df), among which NVPF@PVA@rGO obviously shows the highest diffusion coefficient.

[0077] The galvanic intermittent titration technique (GITT) was used to measure ( Figure 5 g), it can be clearly seen that during the charge-discharge process, the diffusion coefficients of all electrodes change with different states, while the NVPF@PVA@rGO electrode -8 -10 -9 cm 2 / s, while NVPF@rGO and pure NVPF are 10 -9 -10 -10 cm 2 / s and 10 -9 -10 -11 cm 2 / s, indicating that the unique three-dimensional graphene conductive network in Example 1 promotes the Na + diffusion.

[0078] Finally, in order to verify the commercial potential of Example 1 (NVPF@PVA@rGO), the applicant used commercial hard carbon as the positive electrode and paired it with Example 1 to assemble a full battery (NVPF@PVA@rGO / / HC); Figure 6 The charge and discharge curves in b show that the voltage platform of the full battery is around 3.5 and 4.0 V. The full battery was tested for charge and discharge cycles at a current density of 1 C ( Figure 6 a), after 300 cycles, the battery showed 111.2 mAh g -1 The discharge capacity of 417.8Wh kg- 1 The energy density of Example 1 is (based on the mass of the positive electrode). This illustrates the application potential of Example 1 in sodium ion batteries.

[0079] Furthermore, by installing a temperature sensor in the half-cell at a current of 20C ( Figure 7 ) is used to test the temperature change of the battery during the cycle. It can be seen from the figure that compared with Example 3, Example 1 has a stable and regular temperature change during the charge and discharge process, and the change value is also within an acceptable range, which proves that Example 1 has higher safety and is suitable for large-scale production and application.

[0080] The present invention synthesizes a three-dimensional graphene conductive network loaded with sodium vanadium fluorophosphate to improve its conductivity, thereby improving the sodium storage performance and safety of the material. The present invention adds polyvinyl alcohol during the synthesis process, and through the action of hydrogen bonds between polyvinyl alcohol and graphene, a three-dimensional conductive network is constructed to improve the electronic conductivity and ion transport performance of the material, which embodies a more outstanding reversible capacity and high rate performance than simple graphene-loaded sodium vanadium fluorophosphate and pure phase sodium vanadium fluorophosphate, thereby solving the problem of low conductivity and poor rate of NVPF. In addition, by encapsulating graphene and carbon materials, not only the volume change of the material in the charge and discharge cycle is limited, the stress concentration in the charge and discharge cycle is alleviated, and the high thermal conductivity of graphene is utilized to increase the heat dissipation capacity of the battery material and improve the safety of the battery.

[0081] The above description is only a specific implementation mode of the present invention. Any feature disclosed in this specification, unless otherwise stated, can be replaced by other alternative features that are equivalent or have similar purposes; all the disclosed features, or all the steps in the methods or processes, except for mutually exclusive features and / or steps, can be combined in any way.

Claims

1. A method for preparing a high-safety sodium storage material based on a sodium vanadium fluorophosphate graphene composite structure, characterized in that: The following steps are involved: Step 1: Dissolve 0.01-0.03 g of graphene oxide in 12.5 mL of deionized water, stir evenly, and ultrasonicate for 30 minutes; Step 2: Add 0.35 g of ammonium metavanadate and 0.56 g of oxalic acid to the above solution; Step 3: After stirring the solution on a magnetic stirrer for 10 minutes, the solution was transferred to an oil bath and heated at 70 °C for 1 h. Step 4: Add 0.34 g of ammonium dihydrogen phosphate and 0.19 g of sodium fluoride to the solution, stir for 10 minutes, and add 12.5 mL of ethylene glycol dropwise to the solution; Step 5: Add 0.1-0.2 g of polyvinyl alcohol to the above solution, then transfer the solution to a polytetrafluoroethylene reactor and react at 170° C. for 9 h. Step 6: Wash the sample by centrifugation with water and anhydrous ethanol, and then calcine it at 450 degrees in an argon atmosphere in a tubular furnace for 3 hours at a heating rate of 2°C / min to finally obtain cubic sodium vanadium fluorophosphate with a three-dimensional conductive network.

2. The method for preparing a high-safety sodium storage material based on a sodium vanadium fluorophosphate graphene composite structure according to claim 1, characterized in that: The graphene oxide is 0.03g.

3. The method for preparing a high-safety sodium storage material based on a sodium vanadium fluorophosphate graphene composite structure according to claim 1, characterized in that: The polyvinyl alcohol is 0.2g.