Positive electrode material, preparation method and positive electrode plate
By covering the microporous carbon layer in the positive electrode material of lithium iron phosphate or lithium manganese iron phosphate and filling the inert salt microcrystalline particles, the problem of insufficient conductivity and diffusion coefficient is solved, and the specific capacity, magnification and cycling performance of the battery are improved. , a high-performance battery positive electrode material is formed.
Patent Information
- Application Number
- CN202410957781.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
AI Technical Summary
Lithium iron phosphate and lithium manganese iron phosphate as the positive electrode materials of lithium-ion batteries have problems such as low electronic conductivity, small lithium ion diffusion coefficient, and poor rate performance and cycle performance, which limits their development in power batteries.
A positive electrode material is used, including a shell layer of the core coated with microporous carbon layer and filled with inert salt microcrystalline particles in the micropores. The Raman spectroscopy test ensures that ID/IG ≥0.8, and the particle size distribution meets specific conditions. The preparation method includes iron source, phosphorus source mixing, heating and stirring, ball milling and bio-oil mixing, and high-temperature insulation to form a positive electrode material with excellent conductivity and ion transport capability.
It improves the specific capacity, rate performance and cycling performance of lithium iron phosphate or lithium iron manganese iron phosphate-based batteries, enhances the stability of the material and ion transmission capabilities, and is suitable for the preparation of high-performance battery positive electrode sheets.
Smart Images

Figure CN118919674A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of water treatment, and in particular to a positive electrode material, a preparation method and a positive electrode sheet. Background Art
[0002] As a vital functional component of secondary batteries, cathode materials play a key role in improving the performance of secondary batteries. As a traditional cathode material for lithium-ion batteries, lithium iron phosphate has good safety performance, good thermal stability, stable voltage platform and low cost. However, the structural characteristics of lithium iron phosphate cause it to have problems such as low electronic conductivity and small lithium ion diffusion coefficient, which hinders its development in power batteries.
[0003] Compared with lithium iron phosphate, lithium manganese iron phosphate has a higher voltage platform and energy density, but lithium manganese iron phosphate currently also has problems such as poor electronic conductivity, low lithium ion diffusion coefficient, poor rate performance and cycle performance. Summary of the invention
[0004] The present invention provides a positive electrode material, which can improve the specific capacity, rate performance and cycle performance of lithium iron phosphate or lithium iron manganese phosphate batteries.
[0005] The present invention also provides a method for preparing a positive electrode material, which can prepare the positive electrode material and has a simple process.
[0006] The present invention also provides a positive electrode sheet. Since the positive electrode sheet comprises the positive electrode material, the positive electrode sheet is used in a battery to improve the specific capacity, rate performance and cycle performance of the battery.
[0007] In a first aspect, the present invention provides a positive electrode material, comprising a core and a shell layer at least partially covering the core; the chemical composition of the core is LiM x Fe 1-x PO4, where 0≤x≤0.6;
[0008] The shell layer is a carbon layer including a plurality of micropores, the pore size of the micropores is y, and y satisfies: 0.6nm≤y<2nm; at least part of the micropores include inert salt microcrystalline particles.
[0009] Furthermore, the inert salt microcrystalline particles include one or more of potassium salt, sodium salt, calcium salt and magnesium salt.
[0010] Furthermore, the content of inert salt microcrystals is ≤60 mg / g.
[0011] Furthermore, through Raman spectroscopy testing, the positive electrode material satisfies: I D / I G ≥0.8.
[0012] Furthermore, the particle size distribution of the primary particles of the positive electrode material meets the following conditions: D50 is 1-2 μm, 5 μm≤D90-D10≤9.5 μm.
[0013] In a second aspect, the present invention provides a method for preparing the above-mentioned positive electrode material, comprising the following steps:
[0014] S1, adding an oxidant, a surfactant, and a precipitant to a mixed solution containing an iron source and a phosphorus source, making the pH of the mixed system ≤ 1.6, and reacting to obtain a first precursor, wherein the chemical composition of the first precursor is M x Fe 1-x PO4·nH2O, where M is a non-ferrous transition metal, 0≤x≤0.6, n>0;
[0015] S2, the first precursor is added to the phosphorus-containing liquid, heated and stirred, and after the water evaporates, a second precursor is obtained; wherein the phosphorus-containing liquid includes PO4 3- , K + , Ca 2+ 、Na + Mg 2+ , Cl - 、SO4 2- and CO3 2- , among which PO4 3- The concentration of K is ≥10mg / L, + , Ca 2+ 、Na + Mg 2+ , Cl - 、SO4 2- and CO3 2- The sum of the concentrations of ≤300mg / L;
[0016] S3. The lithium source and the second precursor are ball-milled or ground to obtain a third precursor, and the third precursor is mixed with bio-oil. The obtained mixed system is heated to 500-800°C at a heating rate of 1-10°C / min in a protective atmosphere, and is kept warm for 2-12 hours. Then, the temperature is lowered to 200-350°C, and the mixture is kept warm for 0.2-1h in air or oxygen atmosphere for a second time. Then, the mixture is kept warm for 0.5-1h in a protective atmosphere for a third time to prepare the positive electrode material.
[0017] Furthermore, the bio-oil is prepared by a method comprising the following processes:
[0018] The biomass material is heated to 500-1600° C. at a heating rate of 1-20° C. / min in a protective atmosphere, and kept warm for 0.1-12 hours to prepare crude bio-oil, and the crude bio-oil is cleaned, distilled and dried to obtain the bio-oil.
[0019] Furthermore, the mass ratio of the bio-oil to the third precursor is 5%-20%.
[0020] Furthermore, after step S3, the method further includes washing the positive electrode material with ethanol and deionized water, and then drying the positive electrode material.
[0021] Furthermore, the solid-liquid ratio of the first precursor and the phosphorus-containing liquid is 1:5-20.
[0022] In a third aspect, the present invention provides a positive electrode sheet comprising the positive electrode material described in the first aspect.
[0023] The positive electrode material provided by the present invention not only has excellent stability but also has high conductivity and ion transmission capacity because it includes a carbon layer with pores filled with inert salt microcrystalline particles. Therefore, it is used to prepare battery positive electrode sheets, which helps to improve the specific capacity, rate capability and cyclability of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.
[0025] Figure 1 This is a SEM image of the positive electrode material prepared in Example 1;
[0026] Figure 2 XRD pattern of the positive electrode material prepared in Example 1;
[0027] Figure 3 The Raman graph of the positive electrode material prepared in Example 1;
[0028] Figure 4 The particle size distribution diagram of the positive electrode material prepared in Example 1;
[0029] Figure 5 The constant current charge and discharge curve of the battery including the positive electrode material prepared in Example 1 is shown.
[0030] The above drawings have shown clear embodiments of the present invention, which will be described in more detail below. These drawings and text descriptions are not intended to limit the scope of the present invention in any way, but to illustrate the concept of the present invention for those skilled in the art by referring to specific embodiments. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the application embodiments will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of them. Based on the embodiments in the application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] In a first aspect, the present invention provides a positive electrode material, comprising a core and a shell layer at least partially covering the core; the chemical composition of the core is LiM x Fe 1-x PO4, where 0≤x≤0.6;
[0033] The shell layer is a carbon layer including a plurality of micropores, the pore size of the micropores is y, and y satisfies: 0.6nm≤y<2nm; at least part of the micropores include inert salt microcrystalline particles.
[0034] In the present invention, a specific carbon layer is coated on the surface of the inner core to form a conductive network, thereby increasing the conductivity and stability of the lithium iron phosphate / lithium iron manganese phosphate material, and the inert salt microcrystalline particles in the micropores of the carbon layer can enhance the conductivity and ion transmission capacity of the lithium iron phosphate / lithium iron manganese phosphate material, shorten the migration and diffusion distance of lithium ions, and thus improve the rate performance of the positive electrode material.
[0035] In a specific embodiment, the inert salt microcrystalline particles include one or more of potassium salt, sodium salt, calcium salt, and magnesium salt.
[0036] In a specific embodiment, the content of the inert salt microcrystals is ≤60 mg / g.
[0037] Preferably, the content of the inert salt microcrystals is 10-60 mg / g; if the content of the inert salt microcrystals is too much, the capacity of the positive electrode material becomes low, and if the content of the inert salt microcrystals is too little, the improvement on the conductivity and ion transport capacity of the positive electrode material is limited.
[0038] Illustratively, the content of the inert salt microcrystals is any value in the ranges of 10-55 mg / g, 15-50 mg / g, 20-45 mg / g, 25-40 mg / g, 30-35 mg / g, etc.
[0039] In one embodiment, the positive electrode material satisfies the following requirements through Raman spectroscopy test: D / I G ≥0.8.
[0040] Among them, the carbon layer of the positive electrode material of the above embodiment has certain defects, which is not only more conducive to the fixation of the inert salt microcrystalline particles, but also more conducive to the construction of a conductive network with better conductivity on the surface of the positive electrode material. D It means that the phosphorus adsorption material is shifted at 1300cm in Raman spectrum test. -1 Up to 1400cm -1 The peak intensity in the range, I G It means that the phosphorus adsorption material is shifted at 1550cm in Raman spectrum test. -1 Up to 1650cm -1 Peak intensity in the range.
[0041] In a specific embodiment, the particle size distribution of the primary particles of the positive electrode material meets the following conditions: D50 is 1-2 μm, 5 μm≤D90-D10≤9.5 μm.
[0042] In the present invention, the expression "primary particle" refers to a primary structure of a single particle, and correspondingly "secondary particle" refers to an aggregate of primary particles aggregated by physical or chemical bonding between primary particles, that is, a secondary structure.
[0043] In the present invention, the expressions "D10, D50 and D90" refer to the particle size values when the particle content (by volume) is 3%, 10%, 50% and 90% respectively, starting from the maximum particle size; for example: D50 means, in the primary particles of the positive electrode material, the particle size value when the volume content is 50% calculated from the maximum particle size; D10 and D90 are deduced by analogy; D90-D10 represents the difference between D90 and D10 of the primary particles of the positive electrode material.
[0044] The above-mentioned embodiment limits the particle size distribution of the primary particles of the positive electrode material so that it is not easily crushed during actual use, which helps to reduce the residual alkali and gas production of the assembled battery, and helps to further improve the cycle performance and safety performance of the assembled battery.
[0045] In a second aspect, the present invention provides a method for preparing the above-mentioned positive electrode material, comprising the following steps:
[0046] S1, adding an oxidant, a surfactant, and a precipitant to a mixed solution containing an iron source and a phosphorus source, making the pH of the mixed system ≤ 1.6, and reacting to obtain a first precursor, wherein the chemical composition of the first precursor is M x Fe 1-x PO4·nH2O, where M is a non-ferrous transition metal, 0≤x≤0.6, n>0;
[0047] S2, the first precursor is added to the phosphorus-containing liquid, heated and stirred, and after the water evaporates, a second precursor is obtained; wherein the phosphorus-containing liquid includes PO43- , K + , Ca 2+ 、Na + Mg 2+ , Cl - 、SO4 2- and CO3 2- , among which PO4 3- The concentration of K is ≥10mg / L, + , Ca 2+ 、Na + Mg 2+ , Cl - 、SO4 2- and CO3 2- The sum of the concentrations of ≤300mg / L;
[0048] S3. The lithium source and the second precursor are ball-milled or ground to obtain a third precursor. The third precursor is mixed with bio-oil, and the obtained mixed system is heated to 500-800°C at a heating rate of 1-10°C / min in a protective atmosphere, and kept warm for 2-12h, then cooled to 200-350°C, kept warm for 0.2-1h in air or oxygen atmosphere for a second time, and then kept warm for 0.5-1h in a protective atmosphere for a third time to prepare the positive electrode material.
[0049] In the above preparation method, step S1 uses a surfactant or the like to assist in obtaining a first precursor with relatively uniform particles and relatively regular and uniform morphology. Step S2 heats and stirs the first precursor in a phosphorus-containing liquid. During the evaporation of water, K in the phosphorus-containing liquid + , Ca 2+ 、Na + Mg 2+ , Cl - 、SO4 2- 、CO3 2- Uniformly precipitated in the form of salt microcrystals x Fe 1-x PO4·nH2O surface, and a certain concentration of PO4 3-The presence of the second precursor grains can inhibit agglomeration; in step S3, the lithium source, the second precursor and the bio-oil are mixed and heated to 500-800°C at a heating rate of 1-10°C / min. During the first heat preservation process, the salt microcrystals are dissolved in the bio-oil and uniformly exist between the grains of the second precursor, which can avoid the growth and agglomeration of the second precursor grains during the calcination process; when the temperature drops to 200-350°C, air or oxygen is switched to the second heat preservation process. At this time, due to the etching and oxidation of oxygen and air, the excess coated carbon layer becomes gas and volatilizes, which is not only conducive to obtaining a thin coated carbon layer, but also forms micropores on the surface of the coated carbon layer, and some salt microcrystals will be deposited and filled in the micropores. After that, in a protective atmosphere, three heat preservations are performed to obtain the positive electrode material with excellent conductivity and ion transmission capacity of the present invention.
[0050] In addition, the above preparation method uses bio-oil as the carbon source for preparing lithium iron phosphate. On the one hand, it can form a uniform and thin layer of coated carbon on the surface of the positive electrode material, improve the ion transport and charge conduction capabilities of the material, enhance the chemical stability and mechanical strength of the material, and on the other hand, it can also play a reducing role, making Fe 3+ Reduction to Fe 2+ .
[0051] Non-iron transition metal salt is M x Fe 1-x The source of M in the PO4·nH2O material can be adjusted by technicians according to the type of the desired positive electrode material, and preferably, the non-ferrous transition metal salt is a manganese salt.
[0052] Illustratively, the phosphorus-containing liquid involved in the present invention can be any one of biogas slurry, aquaculture wastewater, brewing wastewater, domestic sewage, municipal tail water, phosphate fertilizer production wastewater, slaughtering wastewater, meat product processing wastewater, etc.
[0053] In one embodiment, the bio-oil is prepared by a method comprising the following steps:
[0054] The biomass material is heated to 500-1600° C. at a heating rate of 1-20° C. / min in a protective atmosphere, and kept warm for 0.1-12 hours to prepare crude bio-oil, and the crude bio-oil is cleaned, distilled and dried to obtain the bio-oil.
[0055] In a specific embodiment, the mass ratio of the bio-oil to the third precursor is 5%-20%.
[0056] In a specific embodiment, a surfactant is added to the mixed system according to 1%-5% of the mass of the phosphate; wherein the mass of the phosphate can be obtained by theoretical calculation based on the content of phosphate and cation when the raw materials are added.
[0057] In a specific embodiment, step S3 further includes the steps of washing the positive electrode material with ethanol and deionized water, and then drying.
[0058] In a specific embodiment, the solid-to-liquid ratio of the first precursor to the phosphorus-containing liquid is 1:5-20.
[0059] Exemplarily, before adding the surfactant, an oxidant may be added, and the oxidant may be selected from hydrogen peroxide, etc. Exemplarily, after adding the oxidant for oxidation, the mixed solution may be heated to 60-100°C and reacted for 0.5-2h to completely decompose the hydrogen peroxide, and then the mixed solution may continue to be heated while adding the surfactant.
[0060] Illustratively, the surfactant is any one of cetyltrimethylammonium bromide, cis-oleyl primary amine, ascorbic acid, and the like.
[0061] Exemplarily, the precipitant may be selected from sodium hydroxide or aqueous ammonia.
[0062] For example, after the reaction in step S3, the generated precipitate is repeatedly washed with deionized water and ethanol and vacuum dried, and then an appropriate amount of deionized water is added to the vacuum dried solid particles, and spray dried at 140-260° C. to finally obtain the Mn x Fe 1-x PO4·nH2O.
[0063] Illustratively, the lithium source can be selected from any one of lithium carbonate, lithium phosphate, lithium hydroxide, lithium oxalate, lithium acetate, lithium nitrate, lithium chloride, and lithium sulfate.
[0064] In a third aspect, the present invention provides a positive electrode sheet comprising the positive electrode material described in the first aspect.
[0065] In a specific embodiment of the present invention, the positive electrode sheet includes a current collector and a positive electrode material layer disposed on the current collector, and the positive electrode material layer includes the positive electrode material of the first aspect described above, and may also include a conductive agent, a binder, and the like.
[0066] Exemplarily, the conductive agent includes at least one of carbon nanotubes, carbon black and graphene.
[0067] Exemplarily, the binder can be selected from one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl alcohol (PVA), styrene-butadiene rubber (SBR), polyimide (PI), polyacrylic acid (PAA), polyacrylonitrile (PAN), polyacrylate, sodium carboxymethyl cellulose (CMC), polyolefin, and sodium alginate.
[0068] Exemplarily, the method for preparing the positive electrode sheet includes the following steps: mixing a positive electrode material, a binder, a conductive agent, and a solvent into a slurry, and coating the slurry on at least one surface of a current collector to prepare a positive electrode sheet.
[0069] Furthermore, the use of the above-mentioned positive electrode sheet to assemble a lithium-ion button battery comprises the following steps:
[0070] The biomass carbon, binder, conductive agent and copper foil produced in the bio-oil preparation process are prepared into a negative electrode sheet; the positive electrode sheet, negative electrode sheet, separator, electrolyte and battery shell are assembled into a lithium-ion button battery.
[0071] The present invention is described in detail below in conjunction with specific embodiments:
[0072] Example 1
[0073] This example provides a positive electrode material, including a core and a shell layer at least partially covering the core; the chemical composition of the core is LiM 0.35 Fe 0.65 PO4; the shell layer is a carbon layer including a plurality of micropores, the pore size of the micropores is 1.3 nm; at least part of the micropores include inert salt microcrystalline particles; the inert salt microcrystalline particles include potassium salt, sodium salt, calcium salt, and magnesium salt; the content of the inert salt microcrystalline particles is 26 mg / g; the primary particle size distribution of the positive electrode material satisfies the following conditions: D50 is 1.484 μm, D90-D10 is about 9 μm; I D / I G It is 0.92.
[0074] The preparation method thereof comprises the following steps:
[0075] S1. The straw biomass material was heated to 800°C at a heating rate of 5°C / min in an argon atmosphere and kept warm for 2 hours. The obtained solid product was repeatedly washed with hydrochloric acid, ethanol, and deionized water, dried and sieved to prepare bio-oil and porous carbon; 5g of bio-oil was dissolved in 50mL of ethanol at 80°C to obtain a mixed solution containing bio-oil;
[0076] S2, ferric chloride, manganese chloride, and phosphoric acid are dissolved in water, and the molar ratio of the sum of Fe and Mn elements to P is 0.96-1.1. Then, hydrogen peroxide solution is added to ensure that Fe 2+ All oxidized to Fe 3+ The mixed solution was then heated to 60°C and reacted for 2 hours to completely decompose the hydrogen peroxide. The mixed solution was then heated further and a surfactant, hexadecyltrimethylammonium bromide, was added to the mixed solution at a rate of 2% of the mass of the phosphate. Then, a precipitant, sodium hydroxide, was added to the mixed solution to ensure that the real-time pH of the mixed solution was ≤1.6. After reacting for 12 hours, the first precursor Mn was obtained.0.35 Fe 0.65 PO4·nH2O, n>0;
[0077] S3, the first precursor is added to the phosphorus-containing liquid (solid-liquid ratio is 1:10, PO4 3- The concentration is 63.1 mg / L, K + , Ca 2+ 、Na + Mg 2+ , Cl - 、SO4 2- 、CO3 2- The sum of the concentrations of ≤300 mg / L), heating and stirring, and after the water evaporates, a second precursor is obtained;
[0078] S4, lithium carbonate and the second precursor are mixed evenly according to the ratio of the amount of substance of 1-1.1:1, a small amount of deionized water is added, and the mixture is ball-milled and dried to obtain a third precursor; the third precursor is mixed with a mixed liquid containing bio-oil (the mass ratio of bio-oil to the third precursor is 5%), and the mixture is heated to 650°C at a heating rate of 5°C / min in an argon atmosphere, and kept warm for 6 hours, and then cooled to 350°C, kept warm for 1 hour in an air atmosphere, and then changed to an argon atmosphere, kept warm for 1 hour three times, and cooled to room temperature to prepare a positive electrode material LiMn 0.35 Fe 0.65 PO4 / C, where Figure 1 The positive electrode material in this example is LiMn 0.35 Fe 0.65 SEM image of PO4 / C, Figure 2 The positive electrode material in this example is LiMn 0.35 Fe 0.65 XRD pattern of PO4 / C, Figure 3 The positive electrode material in this example is LiMn 0.35 Fe 0.65 Raman graph of PO4 / C, Figure 4 The positive electrode material in this example is LiMn 0.35 Fe 0.65 Particle size distribution of PO4 / C.
[0079] Example 2
[0080] The difference from Example 1 is that the concentration of the phosphorus-containing liquid is adjusted so that the content of the inert salt microcrystalline particles in the positive electrode material is 58 mg / g.
[0081] Example 3
[0082] This example provides a positive electrode material, including a core and a shell layer at least partially covering the core; the chemical composition of the core is LiMn 0.55 Fe0.45 PO4; the shell layer is a carbon layer including a plurality of micropores, the pore size of the micropores is 1.6 nm; at least part of the micropores include inert salt microcrystalline particles; the content of the inert salt microcrystalline particles is 41 mg / g; the primary particle size distribution of the positive electrode material satisfies the following conditions: D50 is 1.736 μm, D90-D10 is about 9.4 μm; I D / I G It is 0.89.
[0083] The preparation method is different from that of Example 1 in that the ratio of Fe and Mn in the eluent of step S4 is adjusted, and step S6 is adjusted as follows: heating to 800°C at a heating rate of 10°C / min, keeping the temperature for 12 hours, then cooling to 250°C, keeping the temperature for 0.5 hours in an air atmosphere, changing to an argon atmosphere, keeping the temperature for 0.5 hours three times, and cooling to room temperature to prepare a positive electrode material LiMn 0.55 Fe 0.45 PO4 / C.
[0084] Example 4
[0085] This example provides a positive electrode material, including a core and a shell layer at least partially covering the core; the chemical composition of the core is LiM 0.35 Fe 0.65 PO4; the shell layer is a carbon layer including a plurality of micropores, the pore size of the micropores is 0.8 nm; at least part of the micropores include inert salt microcrystalline particles; the inert salt microcrystalline particles include potassium salt, sodium salt, calcium salt, and magnesium salt; the content of the inert salt microcrystalline particles is 13 mg / g; the primary particle size distribution of the positive electrode material satisfies the following conditions: D50 is 1.152 μm, D90-D10 is about 5.3 μm; I D / I G is 1.01.
[0086] The preparation method thereof comprises the following steps:
[0087] S1. The straw biomass material was heated to 800°C at a heating rate of 5°C / min in an argon atmosphere and kept warm for 2h. The obtained solid product was repeatedly washed with hydrochloric acid, ethanol, and deionized water, dried and sieved to prepare bio-oil and porous carbon; 5g of bio-oil was dissolved in 50mL of ethanol at 80°C to obtain a mixed solution;
[0088] S2, ferric chloride, manganese chloride, and phosphoric acid are dissolved in water, and the molar ratio of the sum of Fe and Mn elements to P is 0.96-1.1. Then, hydrogen peroxide solution is added to ensure that Fe 2+ All oxidized to Fe 3+The mixed solution was then heated to 60°C and reacted for 2 hours to completely decompose the hydrogen peroxide. The mixed solution was then heated further and a surfactant, hexadecyltrimethylammonium bromide, was added to the mixed solution at a rate of 2% of the mass of the phosphate. Then, a precipitant, sodium hydroxide, was added to the mixed solution to ensure that the real-time pH of the mixed solution was ≤1.6. After reacting for 12 hours, the first precursor Mn was obtained. 0.35 Fe 0.65 PO4·nH2O, n>0;
[0089] S3, the first precursor is added again to the phosphorus-containing liquid consistent with Example 1 (solid-to-liquid ratio is 1:10), heated and stirred, and after the water evaporates, a second precursor is obtained;
[0090] S4, lithium carbonate and the second precursor are mixed evenly according to the ratio of the amount of substance of 1-1.1:1, a small amount of deionized water is added, ball milling is performed and then dried to obtain a third precursor; the third precursor is mixed with a mixed solution containing bio-oil (the mass ratio of bio-oil to the third precursor is 5%), the mixture is heated to 800°C at a heating rate of 10°C / min in an argon atmosphere, and is kept warm for 12 hours, then cooled to 250°C, kept warm for 0.5 hours in an air atmosphere, and then changed to an argon atmosphere, kept warm for 0.5 hours three times, and cooled to room temperature to prepare a positive electrode material LiMn 0.35 Fe 0.65 PO4 / C.
[0091] Comparative Example 1
[0092] This example provides a positive electrode material, which is different from Example 1 in that: the shell layer is a carbon layer including a plurality of micropores, the pore size of the micropores is 2.2 nm; at least part of the micropores include inert salt microcrystalline particles; the inert salt microcrystalline particles include potassium salt, sodium salt, calcium salt, and magnesium salt; the content of the inert salt microcrystalline particles is 6 mg / g; the primary particle size distribution of the positive electrode material meets the following conditions: D50 is 4.253 μm, D90-D10 is about 16 μm; I D / I G It is 0.86.
[0093] The preparation method thereof is different from that of Example 1 in that the bio-oil in step S4 is replaced by sucrose.
[0094] Comparative Example 2
[0095] This example provides a positive electrode material, and the preparation method thereof is different from that of Example 1 in that: the mixture in step S4 is heated to 650°C at a heating rate of 5°C / min in an argon atmosphere, kept at this temperature for 8 hours, and cooled to room temperature to prepare a positive electrode material LiMn 0.35 Fe 0.65PO4 / C, after testing, the carbon layer of the positive electrode material did not form micropores including inert salt microcrystalline particles.
[0096] Comparative Example 3
[0097] This example provides a positive electrode material, which is different from Example 1 in that: the shell layer is a carbon layer including a plurality of micropores, the pore size of the micropores is 0.4 nm; the pores do not include inert salt microcrystalline particles; the primary particle size distribution of the positive electrode material meets the following conditions: D50 is 2.71 μm, D90-D10 is about 12 μm; I D / I G is 0.95.
[0098] The preparation method thereof is different from that of Example 1 in that step S3 is not performed.
[0099] Application Example 1
[0100] The positive electrode sheet is prepared by using the positive electrode material, comprising the following steps:
[0101] The positive electrode materials of the above-mentioned Examples 1-4 and Comparative Examples 1-3 were assembled into positive electrode sheets, and the process was as follows: the positive electrode material, acetylene black, and polyvinylidene fluoride were dissolved in N-methylpyrrolidone at a mass ratio of 8:1:1, and stirred to form a slurry. The slurry was then coated on the surface of the aluminum foil with a scraper. The positive electrode sheet was then dried at 80°C for 4 hours, and then vacuum dried at 120°C for 12 hours, and then pressed and cut with a tablet press to obtain a positive electrode sheet.
[0102] Application Example 2
[0103] Assembling a battery using the above-mentioned positive electrode sheet includes the following steps:
[0104] In the glove box, ensure that the moisture and oxygen content are not higher than 0.1ppm, place the positive electrode sheet in the middle of the positive electrode shell, then soak the positive electrode sheet with electrolyte (1mol / L LiPF6 dissolved in EC and DEC with a volume ratio of 1:1), then place the Celgard diaphragm on the positive electrode sheet, then soak the diaphragm with electrolyte, then place the lithium sheet in the middle of the diaphragm, then place the gasket and spring on top of the lithium sheet in turn, and then cover the negative electrode shell. Finally, the battery is compacted at 10MPa with a battery sealing machine to obtain a finished button battery.
[0105] Test Case
[0106] Test the performance of the battery of Application Example 2: The specific capacity, rate performance and cycle performance of the battery were tested by constant current charge and discharge test. The test results are shown in Table 1. The charge and discharge voltage was 2.0-4.5V, the current density of the capacity and rate performance tests was set to 0.2C, 0.5C, 1C, 2C, 5C, 10C (1C = 170mA / g), and the current density of the cycle performance test was set to 5C. The constant current charge and discharge curve of the battery including the positive electrode material prepared in Example 1 is shown in Table 1. Figure 5 .
[0107] Table 1 Performance test results
[0108]
[0109] It can be seen from Table 1 that, compared with the comparative example, the positive electrode material of the embodiment is used to assemble the battery, and has higher specific capacity, rate performance and better cycle performance.
[0110] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application.
Claims
1. A positive electrode material, characterized in that: It comprises a core and a shell layer at least partially covering the core; the chemical composition of the core is LiM x Fe 1-x PO4, where 0≤x≤0.6; The shell layer is a carbon layer including a plurality of micropores, the pore size of the micropores is y, and y satisfies: 0.6nm≤y<2nm; at least part of the micropores include inert salt microcrystalline particles.
2. The positive electrode material according to claim 1, characterized in that The inert salt microcrystalline particles include one or more of potassium salt, sodium salt, calcium salt and magnesium salt; And / or, in the positive electrode material, the content of the inert salt microcrystals is ≤60 mg / g.
3. The positive electrode material according to claim 1 or 2, characterized in that Through Raman spectroscopy testing, the positive electrode material meets the following requirements: D / I G ≥0.
8.
4. The positive electrode material according to any one of claims 1 to 3, characterized in that: The particle size distribution of the primary particles of the positive electrode material meets the following conditions: D50 is 1-2 μm, 5 μm≤D90-D10≤9.5 μm.
5. A method for preparing a positive electrode material according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1, adding a surfactant and a precipitant to a mixed solution containing an iron source and a phosphorus source, making the pH of the mixed system ≤ 1.6, and reacting to obtain a first precursor, wherein the chemical composition of the first precursor is M x Fe 1-x PO4·nH2O, where M is a non-ferrous transition metal, 0≤x≤0.6, n>0; S2, the first precursor is added to the phosphorus-containing liquid, heated and stirred, and after the water evaporates, a second precursor is obtained; wherein the phosphorus-containing liquid includes PO4 3- , K + , Ca 2+ 、Na + Mg 2+ , Cl - 、SO4 2- and CO3 2- , among which PO4 3- The concentration of K is ≥10mg / L, + , Ca 2+ 、Na + Mg 2+ , Cl - 、SO4 2- and CO3 2- The sum of the concentrations of ≤300mg / L; S3. The lithium source and the second precursor are ball-milled or ground to obtain a third precursor, and the third precursor is mixed with bio-oil. The obtained mixed system is heated to 500-800°C at a heating rate of 1-10°C / min in a protective atmosphere, and is kept warm for 2-12h, cooled to 200-350°C, and kept warm for 0.2-1h in air or oxygen atmosphere for a second time, and then kept warm for 0.5-1h in a protective atmosphere for a third time to prepare the positive electrode material.
6. The preparation method according to claim 5, characterized in that: The bio-oil is prepared by a method comprising the following steps: The biomass material is heated to 500-1600° C. at a heating rate of 1-20° C. / min in a protective atmosphere, and kept warm for 0.1-12 hours to prepare crude bio-oil, and the crude bio-oil is cleaned, distilled and dried to obtain the bio-oil.
7. The preparation method according to claim 5 or 6, characterized in that: The mass ratio of the bio-oil to the third precursor is 5%-20%.
8. The preparation method according to claim 5 or 6, characterized in that: After step S3, the method further includes washing the positive electrode material with ethanol and deionized water, and then drying the positive electrode material.
9. The preparation method according to claim 5 or 6, characterized in that: The solid-to-liquid ratio of the first precursor to the phosphorus-containing liquid is 1:5-20.
10. A positive electrode sheet, characterized in that: The invention comprises the positive electrode material described in any one of claims 1 to 4, or the positive electrode material prepared by the preparation method described in any one of claims 5 to 9.