Negative electrode composite material as well as preparation method and application thereof
By coating the graphite material with a hard carbon skeleton and depositing silicon in the pore structure, combined with the carbon cladding layer, the problems of high expansion and poor circulation stability of silicon materials are solved, significantly improving the energy density and rate performance of lithium-ion batteries, and extending the The service life of the battery.
Patent Information
- Application Number
- CN202410958488.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
AI Technical Summary
The existing silicon and graphite composite materials have problems such as high expansion and poor circulation stability, uneven dispersion, poor contact and low compaction in lithium-ion batteries, resulting in degradation of battery capacity and circulation performance.
A hard carbon skeleton is used to coat the graphite material, and silicon is deposited in the pore-like structure to form composite particles. The contact between silicon and the electrolyte is reduced through the carbon cladding layer, and the rate performance and cycling performance of the material are improved.
It effectively inhibits the expansion of silicon material, improves the fast charging and circulation performance of the material, improves the energy density and rate performance of lithium-ion batteries, extends the service life of the battery, and reduces the risk of side reactions.
Smart Images

Figure CN118919675A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to a negative electrode composite material and a preparation method and application thereof. Background Art
[0002] Graphite's low cost, high chemical stability and good processing performance make it the most commonly used commercial negative electrode material for lithium-ion batteries. However, with the development of electric vehicles and energy storage, the theoretical capacity of existing graphite materials has reached its limit, and the small theoretical interlayer spacing of graphite cannot meet the needs of high energy density and high-rate current charging. A large rate will cause surface lithium deposition and destruction of the graphite structure, resulting in a decrease in battery capacity and cycle performance. Silicon materials are abundant in resources and have extremely high theoretical specific capacity (4200mAh / g), and are expected to become a high-energy specific lithium-ion battery negative electrode material to replace graphite. However, silicon materials will undergo huge volume changes during the process of lithium insertion / extraction, resulting in the pulverization and shedding of active materials, which in turn leads to a sharp decrease in the capacity of silicon-based negative electrode batteries.
[0003] The currently commonly used optimization solution is to combine silicon material with a certain proportion of graphite material to prepare a silicon / graphite composite negative electrode. Although the energy density can be greatly improved, the problem of battery performance degradation caused by the poor conductivity of silicon material and the volume expansion of silicon is still serious.
[0004] Therefore, based on the problems existing in the current silicon and graphite composite materials, a new composite material still needs to be developed. Summary of the invention
[0005] The present invention aims to solve at least one of the above-mentioned technical problems existing in the prior art. To this end, the present invention provides a negative electrode composite material, which effectively solves the high expansion and extremely poor cycle stability of silicon materials, and also solves the technical problems of uneven dispersion, poor contact and low compaction of silicon materials and graphite.
[0006] The invention also provides a method for preparing the negative electrode composite material.
[0007] The invention also provides a negative electrode plate.
[0008] The invention also provides a lithium ion battery.
[0009] The invention also provides an electric device.
[0010] The first aspect of the present invention provides a negative electrode composite material, comprising composite particles and a carbon coating layer coating the composite particles, the composite particles comprising a graphite material and a hard carbon skeleton coating the graphite material, a porous structure distributed in the hard carbon skeleton, and silicon deposited in the porous structure.
[0011] One of the technical solutions of the present invention regarding the negative electrode composite material has at least the following beneficial effects:
[0012] Traditional silicon-carbon / graphite composite materials have a single graphite particle as the core, and nano-silicon-based materials are coated on the surface of the single graphite particle. This structure leads to poor dispersion uniformity of the silicon material in the active coating layer and poor contact with the graphite, resulting in uneven pore and current distribution.
[0013] The negative electrode composite material of the present invention structurally includes composite particles and a carbon coating layer coating the composite particles. Among them, the composite particles include graphite materials and a hard carbon skeleton coating the graphite materials. The composite particles are used as the core of the negative electrode composite material, which increases the anisotropy of the graphite core, controls the particle size of the graphite material, reduces the transmission distance of lithium ions inside a single particle, and improves the rate performance of the material. The carbon coating layer coating the composite particles reduces the direct contact between silicon and the electrolyte, reduces side reactions, and increases fast charging performance. Porous structures are distributed in the hard carbon skeleton, and silicon is deposited in these porous structures, thereby effectively suppressing the expansion of silicon.
[0014] The negative electrode composite material of the present invention has good interface contact and uniform dispersion between silicon carbon and graphite material. The hard carbon skeleton serves as a binding material for the composite particles and a skeleton for deposited silicon, which inhibits the expansion of the silicon material and effectively improves the fast charging performance and cycle performance of the material. The graphite material, as a primary particle, significantly improves the compaction of the composite material.
[0015] In summary, the negative electrode composite material of the present invention effectively solves the problems of high expansion and extremely poor cycle stability of silicon materials, and also solves the technical problems of uneven dispersion of silicon materials and graphite, poor contact, and low compaction. The negative electrode composite material has high gram capacity, excellent ion / electron transmission capacity, and high compaction. When it is used in lithium ion batteries, the obtained lithium ion batteries show high energy density, good rate performance, and cycle performance.
[0016] According to some embodiments of the present invention, the average particle size D of the negative electrode composite material is V 50 Range: 6μm≤D V 50≤25μm.
[0017] According to some embodiments of the present invention, the average particle size D of the negative electrode composite material is V 50 Range: 8μm≤D V 50≤20μm.
[0018] According to some embodiments of the present invention, the average particle size D of the negative electrode composite material is V50 can be any value among 8μm, 9μm, 10μm, 11m, 12μm, 13μm, 14μm, 15μm, 16μm, 17μm, 18μm, 19μm, and 20μm, or a range formed by any two of the values.
[0019] According to some embodiments of the present invention, the carbon coating layer has a thickness of 2 nm to 20 nm.
[0020] According to some embodiments of the present invention, the carbon coating layer has a thickness of 5 nm to 10 nm.
[0021] According to some embodiments of the present invention, the thickness of the carbon coating layer may be any value of 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, or a range formed by any two of them.
[0022] According to some embodiments of the present invention, the pore size of the porous structure is less than 5 nm.
[0023] According to some embodiments of the present invention, the pore diameter of the porous structure may be any value of 0.1 nm, 0.5 nm, 1.0 nm, 1.5 nm, 2.0 nm, 2.5 nm, 3.0 nm, 3.5 nm, and 4.0 nm.
[0024] According to some embodiments of the present invention, the mass percentage of the hard carbon skeleton in the negative electrode composite material is 9.7 wt % to 18.5 wt %.
[0025] According to some embodiments of the present invention, the mass percentage of silicon in the negative electrode composite material is 2.9 wt % to 7.4 wt %.
[0026] According to some embodiments of the present invention, the graphite material is not particularly limited and may be one or more of artificial graphite flakes, artificial graphite balls, artificial graphite blocks, natural flaky graphite, natural crystalline graphite, natural graphite balls and natural graphite blocks.
[0027] According to some embodiments of the present invention, the graphite material is one or more of artificial graphite sheets, artificial graphite balls, artificial graphite blocks, natural flaky graphite and natural graphite blocks.
[0028] According to some embodiments of the present invention, when the graphite material is in a granular form, the graphite particles are primary particles.
[0029] According to some embodiments of the present invention, the average particle size D of the graphite particles 1 50 Range: 3μm≤D 1 50≤10μm.
[0030] According to some embodiments of the present invention, the average particle size D of the graphite particles 1 50 Range: 4μm≤D 1 50≤8μm.
[0031] According to some embodiments of the present invention, the average particle size D of the graphite particles 1 50 can be any value among 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, or a range formed by any two of them.
[0032] The second aspect of the present invention provides a method for the negative electrode composite material of the present invention, comprising the following steps:
[0033] S1: wrapping the graphite material with a hard carbon skeleton precursor and carbonizing it to obtain a first precursor;
[0034] S2: heating the first precursor in a protective atmosphere, introducing a silicon source gas to perform silicon deposition, and obtaining a second precursor;
[0035] S3: thermally depositing the second precursor in a carbon source gas to obtain the negative electrode composite material.
[0036] A technical solution in the method for preparing the negative electrode composite material of the present invention has at least the following beneficial effects:
[0037] Traditional silicon-carbon / graphite composite materials are mainly synthesized in two ways: one method is to compound silicon-based (silicon / silicon-carbon / silicon-oxygen, etc.) nanoparticle powder materials and graphite powder materials through amorphous carbon coating. This method can better coat the silicon-based material on the graphite surface, but the carbonization of the coating layer requires a higher temperature, which will cause the silicon crystal to grow again, resulting in an increase in the volume expansion of the silicon material; another method is to compound silicon nanoparticle powder materials and graphite powder materials through ball milling. This method will cause uneven dispersion of silicon nanoparticles in graphite, and the silicon size cannot be controlled below 20nm, resulting in poor cycle performance and rate performance of the composite material.
[0038] The preparation method of the present invention first wraps the graphite material with a hard carbon skeleton precursor, then carbonizes it to obtain a first precursor, and then deposits silicon in the porous structure of the hard carbon skeleton of the composite particles by chemical vapor deposition, and finally performs carbon coating by thermal deposition, which effectively controls the size of the silicon crystal and makes the dispersion more uniform, thereby enhancing the cyclic stability of the material. The hard carbon skeleton can not only serve as a binder material for the composite material, but also as a conductive network for graphite and silicon materials, further enhancing the rate performance of the composite material.
[0039] The preparation method of the present invention does not require expensive equipment and complicated process control, has undemanding reaction conditions, has readily available raw materials, has low production costs, and is easy to industrialize.
[0040] In step S1:
[0041] Before wrapping the graphite material with the hard carbon skeleton precursor, the graphite material can be screened as needed to facilitate the average particle size D of the graphite material. 1 50Limited to 3μm≤D 1 In the range of 50≤10μm.
[0042] There are two methods for wrapping graphite materials with hard carbon skeleton precursors: solvent method and melting method:
[0043] The solvent method is to first dissolve the hard carbon skeleton precursor in a solvent, then add the graphite material, and perform carbonization treatment to achieve the wrapping of the graphite material by the hard carbon skeleton precursor. The hard carbon skeleton precursor is dissolved in a solvent, and the solvent includes ketones, alcohols and ether solvents, specifically including ethanol, propanol, butanol; methyl formate, methyl acetate; acetone, methyl ethyl ketone; chloroform, dichloromethane, etc.
[0044] The melting method is to first convert the hard carbon skeleton precursor into a molten state, and then add a graphite material to achieve the hard carbon skeleton precursor wrapped around the graphite material. To convert the hard carbon precursor into a molten state, the method can be to put the resin precursor into a heating device to ensure uniform distribution and avoid aggregation. Heating phenolic resin: Turn on the heating device and gradually increase the temperature until the phenolic resin is completely melted. During the heating process, pay attention to controlling the temperature to avoid overheating that causes the phenolic resin to burn or decompose. Remove impurities and bubbles: During the melting process, appropriate methods, such as stirring or vacuum treatment, can be adopted to remove impurities and bubbles in the phenolic resin. The melting temperature can be 130°C to 220°C. According to some embodiments of the present invention, the carbonization temperature is 1600°C to 2200°C.
[0045] According to some embodiments of the present invention, the carbonization temperature is 1900°C to 2000°C.
[0046] According to some embodiments of the present invention, the carbonization temperature can be any value of 1900°C, 1910°C, 1920°C, 1930°C, 1940°C, 1950°C, 1960°C, 1970°C, 1980°C, 1990°C, 2000°C or a range formed by any two of them.
[0047] According to some embodiments of the present invention, in the first precursor, the mass proportion of the hard carbon skeleton is ω 1 (The ratio of the coating mass of hard carbon to the first precursor) is 8wt% to 25wt%.
[0048] According to some embodiments of the present invention, in the first precursor, the mass proportion of the hard carbon skeleton is ω1 It is 10wt% to 20wt%.
[0049] According to some embodiments of the present invention, the mass of the hard carbon skeleton accounts for 9.7 wt% to 18.5 wt% of the finished graphite / silicon-carbon composite material particles.
[0050] The hard carbon skeleton precursor is not specifically limited and can be selected according to actual needs, for example, it can be styrene-butadiene rubber, polyfurfuryl alcohol, natural rubber, polyacrylonitrile, butadiene rubber, phenolic resin, furan resin, epoxy resin, furfural resin, furfural ketone resin, furfural alcohol resin.
[0051] In step S2:
[0052] Before the first precursor is heated in a protective atmosphere, the first precursor may be crushed as needed to make the silicon deposition more uniform.
[0053] After the first precursor is crushed, the average particle size D 2 The range of 50 is: 10μm≤D 2 50≤30μm.
[0054] After the first precursor is crushed, the average particle size D 2 The range of 50 is: 12μm≤D 2 50≤20μm.
[0055] After the first precursor is crushed, the average particle size D 2 The range of 50 can be any one of 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, and 20 μm, or a range formed by any two of the values.
[0056] The protective atmosphere may be an inert atmosphere.
[0057] Protective atmospheres include nitrogen and argon.
[0058] The first precursor is heated in a protective atmosphere at a temperature of 1600° C. to 2200° C.
[0059] The silicon source gas is not particularly limited and can be selected according to actual needs, such as one or more of monosilane, disilane, dichlorosilane and trichlorosilane.
[0060] A silicon source gas is introduced, and the hard carbon coating structure in the first precursor is used as a deposition skeleton / substrate for silicon.
[0061] According to some embodiments of the present invention, in the second precursor, the mass ratio of silicon (the ratio of the deposited mass of silicon to the total mass of the hard carbon coating layer and silicon) is 20 wt % to 45 wt %.
[0062] According to some embodiments of the present invention, in the second precursor, the mass ratio of silicon (the ratio of the deposited mass of silicon to the total mass of the hard carbon coating layer and silicon) is 30 wt % to 40 wt %.
[0063] According to some embodiments of the present invention, the mass of silicon accounts for 2.9 wt% to 7.4 wt% of the finished graphite / silicon-carbon composite material particles.
[0064] In step S3:
[0065] The carbon source gas is not particularly limited and can be selected according to actual needs. For example, the carbon source gas can be a hydrocarbon gas, specifically one of acetylene, ethylene and methane.
[0066] According to some embodiments of the present invention, the pyrolysis temperature is 200°C to 800°C.
[0067] According to some embodiments of the present invention, the pyrolysis temperature is any one of 200°C, 300°C, 400°C, 500°C, 600°C, 700°C, 800°C, or a range formed by any two of them.
[0068] According to some embodiments of the present invention, the pyrolysis temperature is 400°C to 500°C.
[0069] According to some embodiments of the present invention, the pyrolysis temperature is any one of 400°C, 410°C, 420°C, 430°C, 440°C, 450°C, 460°C, 470°C, 480°C, 490°C, and 500°C, or a range formed by any two of them.
[0070] The third aspect of the present invention provides a negative electrode plate, wherein the negative electrode plate is made from the negative electrode composite material described in the first aspect of the present invention or the negative electrode composite material prepared by the method described in the second aspect of the present invention.
[0071] The negative electrode plate of the present invention, because the negative electrode composite material of the present invention is used, has at least all the beneficial effects of the negative electrode composite material, specifically:
[0072] Since the negative electrode composite material has a high gram capacity and high compactness, the negative electrode plate can achieve a high energy density, allowing the lithium-ion battery to store more electrical energy at the same volume or weight. The structural design of the negative electrode composite material optimizes the transmission path and reactive area of lithium ions inside the battery, improving the rapid charge and discharge performance of the battery, that is, better rate performance. This allows the battery to maintain high efficiency and stability when rapid charge and discharge are required.
[0073] By effectively inhibiting the expansion of silicon materials and improving their cycle stability, the negative electrode plate can achieve long-term and stable recycling use, thereby extending the service life of the battery.
[0074] The carbon coating effectively reduces the possibility of direct contact between silicon materials and the electrolyte, reduces side reactions inside the battery, and thus improves the safety and stability of the battery.
[0075] In summary, the negative electrode plate prepared using the negative electrode composite material of the present invention can significantly improve the performance parameters of the lithium-ion battery, including energy density, rate performance and cycle stability, and is suitable for applications requiring high energy density and high-efficiency charging and discharging.
[0076] According to some embodiments of the present invention, in the negative electrode sheet, the type of current collector is not specifically limited and can be selected according to actual needs, such as copper foil and graphene paper.
[0077] A fourth aspect of the present invention provides a lithium-ion battery, comprising a positive electrode plate, a separator, an electrolyte, and the negative electrode plate described in the first aspect of the present invention.
[0078] The lithium-ion battery of the present invention uses the negative electrode sheet containing the negative electrode composite material of the present invention, and thus at least has all the beneficial effects of the negative electrode sheet. Specifically:
[0079] Since the negative electrode plate adopts the negative electrode composite material of the present invention, it has a high gram capacity and high compactness, and can achieve a higher energy density. This means that at the same volume or weight, the battery can store more electrical energy, thereby extending the use time of the device or reducing the volume and weight of the battery. The structure of the negative electrode composite material optimizes the transmission path and reactive area of lithium ions inside the battery, so that the battery can achieve better fast charging and discharging performance. This means that the battery can maintain high efficiency and stability when fast charging and discharging is required, and is suitable for high-power equipment and fast charging requirements. Furthermore, the negative electrode composite material effectively inhibits the expansion of the silicon material and improves its cycle stability, so that the battery can achieve long-term and stable cyclic use. This not only extends the service life of the battery, but also reduces the frequency of battery replacement and maintenance costs. In addition, the carbon coating effectively reduces the possibility of direct contact between the silicon material and the electrolyte, thereby reducing the side reactions inside the battery and improving the safety and stability of the battery. This is crucial to preventing thermal runaway of the battery and increasing the safety of the battery.
[0080] Therefore, the lithium-ion battery manufactured using the negative electrode plate of the present invention can be significantly improved in terms of energy density, rate performance, cycle life and safety, and is suitable for a wide range of applications requiring high energy density and high-efficiency charging and discharging, such as electric vehicles, portable devices and energy storage systems.
[0081] The fifth aspect of the present invention provides an electrical device, comprising the lithium-ion battery described in the fourth aspect of the present invention.
[0082] One of the technical solutions of the present invention regarding the electric device has at least the following beneficial effects:
[0083] The above-mentioned lithium-ion batteries have high energy density, excellent rate performance and long cycle life, and can provide a stable and long-lasting power supply for electrical devices. This is very important for applications such as electronic equipment, electric vehicles and energy storage systems, and can ensure that the equipment can operate efficiently for a long time. The excellent rate performance of lithium-ion batteries means that it can be charged quickly and discharged efficiently, and is suitable for fast charging equipment and applications that require frequent charging and discharging. This improves the convenience and efficiency of electrical devices such as new energy vehicles.
[0084] Due to high energy density and excellent cycle performance, the above batteries can store more electrical energy and maintain stable output for a long time, extending the service life of the equipment. This is especially important for equipment that relies on long-term use, such as new energy vehicles, mobile communication equipment, portable electronic devices, etc. Long cycle life and stability mean that the above batteries require less maintenance and replacement frequency, reducing maintenance costs and equipment downtime. This is particularly important for commercial and industrial applications, which can improve the reliability and economy of the equipment.
[0085] In addition, the carbon coating of the battery effectively reduces direct contact with the electrolyte, reducing the risk of side reactions and thermal runaway inside the battery, thereby improving the safety of electrical devices such as new energy vehicles. This is particularly important in applications that require high safety and reliability. BRIEF DESCRIPTION OF THE DRAWINGS
[0086] Figure 1 It is a schematic diagram of the structure of the negative electrode composite material of the present invention.
[0087] Reference numerals:
[0088] 1: graphite material; 2: hard carbon skeleton; 3: pore structure; 4: silicon; 5: carbon coating. DETAILED DESCRIPTION
[0089] The following are specific embodiments of the present invention, and the technical solutions of the present invention are further described in conjunction with the embodiments, but the present invention is not limited to these embodiments.
[0090] In the first aspect, some embodiments of the present invention provide a negative electrode composite material, including composite particles and a carbon coating layer coating the composite particles, the composite particles include graphite material and a hard carbon skeleton coating the graphite material, a porous structure is distributed in the hard carbon skeleton, and silicon is deposited in the porous structure.
[0091] It can be understood that the traditional silicon-carbon / graphite composite material has a single graphite particle as the core, and nano-silicon-based materials are coated on the surface of the single graphite particle. This structure leads to poor dispersion uniformity of the silicon material in the active coating layer and poor contact with the graphite, resulting in uneven pore and current distribution.
[0092] The negative electrode composite material of the present invention structurally includes composite particles and a carbon coating layer coating the composite particles. Among them, the composite particles include graphite materials and a hard carbon skeleton coating the graphite materials. The composite particles are used as the core of the negative electrode composite material, which increases the anisotropy of the graphite core, controls the particle size of the graphite material, reduces the transmission distance of lithium ions inside a single particle, and improves the rate performance of the material. The carbon coating layer coating the composite particles reduces the direct contact between silicon and the electrolyte, reduces side reactions, and increases fast charging performance. Porous structures are distributed in the hard carbon skeleton, and silicon is deposited in these porous structures, thereby effectively suppressing the expansion of silicon.
[0093] The negative electrode composite material of the present invention has good interface contact and uniform dispersion between silicon carbon and graphite materials. The hard carbon skeleton serves as a binding material for the composite particles and a skeleton for deposited silicon, which inhibits the expansion of the silicon material and effectively improves the fast charging performance and cycle performance of the particles. The graphite material, as a primary particle, significantly improves the compaction of the composite particles. The technical problems of high expansion and extremely poor cycle stability of silicon materials, uneven dispersion of silicon materials and graphite, poor contact, and low compaction are solved.
[0094] In summary, the negative electrode composite material of the present invention effectively solves the high expansion and extremely poor cycle stability of silicon materials, and also solves the technical problems of uneven dispersion of silicon materials and graphite, poor contact, and low compaction. The negative electrode composite material has high gram capacity, excellent ion / electron transmission capacity, and high compaction. When it is used in lithium ion batteries, the obtained lithium ion batteries show high energy density, good rate performance, and cycle performance.
[0095] In combination with the first aspect, in some embodiments of the present invention, the average particle size D of the negative electrode composite material is V 50 Range: 6μm≤D V 50≤25μm.
[0096] The appropriate particle size range helps to improve the rate performance and cycle stability of the battery. Smaller particles can increase the surface area of the battery, which is beneficial to the transmission of electrons and ions, thereby improving the power density and rapid charge and discharge performance of the battery. In an embodiment of the present invention, the particle size within this range helps to reduce the electron and ion transmission paths between particles, reduce the diffusion paths of lithium ions inside, and help improve the cycle stability and battery life. Too small a particle size (less than 6 μm) may increase the cost and difficulty of battery preparation, and may also cause the particles to be too sensitive, affecting the cycle life and safety of the battery. Furthermore, when D v 50 is too low. Due to the hard carbon coating and silicon deposition of the composite material, a small particle size will lead to an increase in specific surface area and increased silicon exposure, resulting in better fast charging performance of lithium-ion batteries, but low first efficiency and larger side reactions; a large particle size (greater than 25μm) may lead to a decrease in battery energy density, because large particles may be difficult to pack tightly, reducing the compactness of the battery and the electron / ion transmission efficiency. Furthermore, when D v 50 is too high. Due to the large particle size, the lithium ion transmission path is significantly increased, and the decreased porosity is not conducive to the infiltration of the electrolyte and the diffusion of ions, resulting in serious lithium deposition at the negative electrode of the lithium-ion battery, which seriously affects the cycle performance and fast charging performance of the lithium-ion battery.
[0097] In combination with the first aspect, in some embodiments of the present invention, the average particle size D of the negative electrode composite material is V 50 Range: 8μm≤D V 50≤20μm.
[0098] In combination with the first aspect, in some embodiments of the present invention, the average particle size D of the negative electrode composite material is V 50 can be any value among 8μm, 9μm, 10μm, 11m, 12μm, 13μm, 14μm, 15μm, 16μm, 17μm, 18μm, 19μm, and 20μm, or a range formed by any two of the values.
[0099] In combination with the first aspect, in some embodiments of the present invention, the thickness of the carbon coating layer is 2 nm to 20 nm.
[0100] The appropriate thickness of the carbon coating can effectively reduce the direct contact between the silicon material and the electrolyte, thereby reducing the occurrence of side reactions and improving the cycle stability and long-term performance of the battery. As a barrier layer, the carbon coating can effectively prevent the volume expansion of silicon, thereby reducing the structural damage of silicon particles, which is beneficial to improving the rapid charge and discharge capabilities of the battery. In addition, the appropriate thickness of the carbon coating helps to maintain the structural integrity of the silicon particles, reduce the mechanical stress of the electrode material, and improve the cycle life and stability of the battery. When the thickness of the carbon coating is too small (less than 2nm), it may lead to increased direct contact between the silicon particles and the electrolyte, weaken the barrier effect, and reduce the cycle life and stability of the battery; when the thickness of the carbon coating is too large (greater than 20nm), it may increase the cost and complexity of battery preparation, and may weaken the transmission performance of the carbon coating, affecting the electron and ion transmission efficiency of the battery, and reducing the power density and fast charging performance of the battery.
[0101] In combination with the first aspect, in some embodiments of the present invention, the thickness of the carbon coating layer is 5 nm to 10 nm.
[0102] In combination with the first aspect, in some embodiments of the present invention, the thickness of the carbon coating layer can be any value of 5nm, 6nm, 7nm, 8nm, 9nm, 10nm, or a range formed by any two of them.
[0103] In combination with the first aspect, in some embodiments of the present invention, the pore size of the porous structure is less than 5 nm.
[0104] The presence of the porous structure helps to optimize the electron transmission path of silicon particles, reduce resistance, and improve the power density and fast charging performance of the battery. The porous structure can effectively enhance the bonding strength between silicon particles and the hard carbon skeleton, which is beneficial to improve the compaction effect of the composite material and the cycle life of the battery. The porous structure smaller than 5nm can effectively limit the volume expansion of silicon, allowing it to be more evenly deposited inside the porous structure, thereby effectively inhibiting the expansion of silicon materials and improving the cycle stability and long-term performance of the battery. If the pore size of the porous structure is larger than 5nm, the larger pore size may not be able to effectively limit the volume expansion of silicon, causing the silicon particles to be prone to structural deformation and damage during the charge and discharge process, affecting the cycle stability and life of the battery. Excessively large pores may increase the length and resistance of the electron transmission path, reducing the power density and fast charging performance of the battery.
[0105] In combination with the first aspect, in some embodiments of the present invention, the pore diameter of the porous structure can be any value of 0.1 nm, 0.5 nm, 1.0 nm, 1.5 nm, 2.0 nm, 2.5 nm, 3.0 nm, 3.5 nm, and 4.0 nm.
[0106] In combination with the first aspect, in some embodiments of the present invention, the graphite material is not specifically limited and can be one or more of artificial graphite sheets, artificial graphite balls, artificial graphite blocks, natural flaky graphite, natural crystalline graphite, natural graphite balls and natural graphite blocks.
[0107] In combination with the first aspect, in some embodiments of the present invention, the graphite material is one or more of artificial graphite sheets, artificial graphite balls, artificial graphite blocks, natural flaky graphite and natural graphite blocks.
[0108] In combination with the first aspect, in some embodiments of the present invention, when the graphite material is in a granular form, the graphite particles are primary particles.
[0109] In combination with the first aspect, in some embodiments of the present invention, the average particle size D of the graphite particles is 1 50 Range: 3μm≤D 1 50≤10μm.
[0110] Moderate graphite particle size helps to improve the compaction effect of composite particles, thereby improving the energy density and cycle stability of the battery. The appropriate particle size range can also control the surface area and electron transfer path of the graphite particles, which is beneficial to improving the rapid charge and discharge performance and power density of the battery. In addition, the distribution of graphite particles within the particle size range is relatively uniform, which is beneficial to improving the uniformity and stability of silicon-carbon composite materials and reducing the unevenness during the charge and discharge process. If the average particle size of the graphite particles is D 1 50 is less than 3 μm or greater than 10 μm. Too small a particle size may increase the inter-particle gap, affect the compactness and stability of the battery material, and increase the complexity of the battery preparation process. Too large a particle size may cause the particles to be loosely packed, reduce the energy density and cycle stability of the battery, and increase the cost of battery preparation and waste of materials. Therefore, the average particle size D of the graphite particles is 1 50 is in the range of 3μm to 10μm, which can maximize its advantages in improving battery performance and stability while avoiding potential preparation and performance issues.
[0111] In combination with the first aspect, in some embodiments of the present invention, the average particle size D of the graphite particles is 1 50 Range: 4μm≤D 1 50≤8μm.
[0112] In combination with the first aspect, in some embodiments of the present invention, the average particle size D of the graphite particles is 1 50 can be any value among 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, or a range formed by any two of them.
[0113] In a second aspect, in some embodiments of the present invention, a method for preparing a negative electrode composite material of the present invention is provided, comprising the following steps:
[0114] S1: Wrapping the graphite material with a hard carbon skeleton precursor and carbonizing it to obtain a first precursor;
[0115] S2: heating the first precursor in a protective atmosphere, introducing a silicon source gas to perform silicon deposition, and obtaining a second precursor;
[0116] S3: thermally depositing the second precursor in a carbon source gas to obtain a negative electrode composite material.
[0117] It should be noted that traditional silicon-carbon / graphite composite materials are mainly synthesized in two ways: one method is to compound silicon-based (silicon / silicon-carbon / silicon-oxygen, etc.) nanoparticle powder materials and graphite powder materials through amorphous carbon coating. This method can better coat the silicon-based material on the graphite surface, but the carbonization of the coating layer requires a higher temperature, which will cause the silicon crystal to grow again, resulting in an increase in the volume expansion of the silicon material; another method is to compound silicon nanoparticle powder materials and graphite powder materials through ball milling. This method will cause uneven dispersion of silicon nanoparticles in graphite, and the silicon size cannot be controlled below 20nm, resulting in poor cycle performance and rate performance of the composite material.
[0118] The preparation method of the present invention is that hard carbon is uniformly coated on the outside of the graphite material as a binding material for secondary particles, and the pore structure of the hard carbon is used as a deposition site for silicon to deposit silicon, and finally the particles are carbon-coated by vapor deposition. Specifically, the graphite material is first wrapped with a hard carbon skeleton precursor, then carbonized to obtain a first precursor, and then silicon is deposited in the pore structure of the hard carbon coating layer of the composite particles by chemical vapor deposition, and finally carbon-coated by thermal deposition, thereby effectively controlling the size of the silicon crystals and dispersing them more evenly, thereby enhancing the cyclic stability of the material. The hard carbon coating structure can not only serve as a binder material for the composite particles, but also as a conductive network for graphite and silicon materials, further enhancing the rate performance of the composite material.
[0119] The preparation method of the present invention does not require expensive equipment and complicated process control, has undemanding reaction conditions, has readily available raw materials, has low production costs, and is easy to industrialize.
[0120] In step S1:
[0121] Before wrapping the graphite material with the hard carbon skeleton precursor, the graphite particles can be screened as needed to reduce the average particle size D of the graphite particles. 1 50Limited to 3μm≤D 1 In the range of 50≤10μm.
[0122] There are two methods for wrapping graphite materials with hard carbon skeleton precursors: solvent method and melting method:
[0123] The solvent method is to first dissolve the hard carbon skeleton precursor in a solvent, then add the graphite material, and perform carbonization treatment to achieve the encapsulation of the graphite material by the hard carbon skeleton precursor. The hard carbon skeleton precursor is dissolved in a solvent, and the solvent includes at least one of ethanol, propanol, butanol, methyl formate, methyl acetate, acetone, methyl ethyl ketone, chloroform and dichloromethane.
[0124] The melting method is to first convert the hard carbon skeleton precursor into a molten state, and then add the graphite material to achieve the hard carbon skeleton precursor wrapped around the graphite material. To convert the hard carbon precursor into a molten state, the method can be to place the hard carbon skeleton precursor into a heating device to ensure uniform distribution and avoid aggregation. Heating phenolic resin: Turn on the heating device and gradually increase the temperature until the phenolic resin is completely melted. During the heating process, pay attention to controlling the temperature to avoid overheating that causes the phenolic resin to burn or decompose. Remove impurities and bubbles: During the melting process, appropriate methods such as stirring or vacuum treatment can be adopted to remove impurities and bubbles in the phenolic resin. The melting temperature can be 130℃~220℃.
[0125] In combination with the second aspect, in some embodiments of the present invention, the carbonization temperature is 1600°C to 2200°C.
[0126] In combination with the second aspect, in some embodiments of the present invention, the carbonization temperature is 1900°C to 2000°C.
[0127] In combination with the second aspect, in some embodiments of the present invention, the carbonization temperature can be any value of 1900°C, 1910°C, 1920°C, 1930°C, 1940°C, 1950°C, 1960°C, 1970°C, 1980°C, 1990°C, 2000°C or a range formed by any two of them.
[0128] In combination with the second aspect, in some embodiments of the present invention, in the first precursor, the mass proportion of the hard carbon skeleton is 1 (The ratio of the coating mass of hard carbon to the first precursor) is 8wt% to 25wt%.
[0129] In combination with the second aspect, in some embodiments of the present invention, in the first precursor, the mass proportion of the hard carbon skeleton is 1 It is 10wt% to 20wt%.
[0130] The hard carbon skeleton precursor is not specifically limited and can be selected according to actual needs, for example, it can be styrene-butadiene rubber, polyfurfuryl alcohol, natural rubber, polyacrylonitrile, butadiene rubber, phenolic resin, furan resin, epoxy resin, furfural resin, furfural ketone resin, furfural alcohol resin.
[0131] In step S2:
[0132] Before the first precursor is heated in the protective atmosphere, the first precursor may be crushed as needed, for example, to make silicon deposition more uniform.
[0133] After the first precursor is crushed, the average particle size D 2 The range of 50 is: 10μm≤D 2 50≤30μm.
[0134] After the first precursor is crushed, the average particle size D 2 The range of 50 is: 12μm≤D 2 50≤20μm.
[0135] After the first precursor is crushed, the average particle size D 2 The range of 50 can be any one of 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, and 20 μm, or a range formed by any two of the values.
[0136] The protective atmosphere may be an inert atmosphere.
[0137] Protective atmospheres include nitrogen and argon.
[0138] The first precursor is heated in a protective atmosphere at a temperature of 1600° C. to 2200° C.
[0139] The silicon source gas is not particularly limited and can be selected according to actual needs, such as one or more of monosilane, disilane, dichlorosilane and trichlorosilane.
[0140] A silicon source gas is introduced, and the hard carbon coating structure in the first precursor is used as a deposition skeleton / substrate for silicon.
[0141] In combination with the second aspect, in some embodiments of the present invention, in the second precursor, the mass proportion of silicon (the proportion of the deposited mass of silicon to the total mass of the hard carbon coating layer and silicon) is 10wt% to 50wt%.
[0142] In combination with the second aspect, in some embodiments of the present invention, in the second precursor, the mass proportion of silicon (the proportion of the deposited mass of silicon to the total mass of the hard carbon coating layer and silicon) is 20wt% to 45wt%.
[0143] In step S3:
[0144] The carbon source gas is not particularly limited and can be selected according to actual needs. For example, the carbon source gas can be a hydrocarbon gas, specifically one of acetylene, ethylene and methane.
[0145] In combination with the second aspect, in some embodiments of the present invention, the pyrolysis temperature is 200°C to 800°C.
[0146] In a third aspect, in some embodiments of the present invention, a negative electrode plate is provided, wherein the negative electrode plate is made of the negative electrode composite material of the first aspect of the present invention or the negative electrode composite material prepared by the method of the second aspect of the present invention.
[0147] The negative electrode plate of the present invention, because the negative electrode composite material of the present invention is used, has at least all the beneficial effects of the negative electrode composite material, specifically:
[0148] Since the negative electrode composite material has a high gram capacity and high compactness, the negative electrode plate can achieve a high energy density, allowing the lithium-ion battery to store more electrical energy at the same volume or weight. The structural design of the negative electrode composite material optimizes the transmission path and reactive area of lithium ions inside the battery, improving the rapid charge and discharge performance of the battery, that is, better rate performance. This allows the battery to maintain high efficiency and stability when rapid charge and discharge are required.
[0149] By effectively inhibiting the expansion of silicon materials and improving their cycle stability, the negative electrode plate can achieve long-term and stable recycling use, thereby extending the service life of the battery.
[0150] The carbon coating effectively reduces the possibility of direct contact between silicon materials and the electrolyte, reduces side reactions inside the battery, and thus improves the safety and stability of the battery.
[0151] In summary, the negative electrode plate prepared using the negative electrode composite material of the present invention can significantly improve the performance parameters of the lithium-ion battery, including energy density, rate performance and cycle stability, and is suitable for applications requiring high energy density and high-efficiency charging and discharging.
[0152] In the third aspect, in some embodiments of the present invention, the method for preparing the negative electrode sheet is:
[0153] 1) mixing the negative electrode composite material, the conductive material, the binding material and water to obtain a negative electrode slurry;
[0154] 2) The negative electrode slurry obtained in the above steps is coated on the front and back surfaces of the current collector to form a coating layer on the current collector, and a composite negative electrode sheet containing carbon-coated silicon and carbon-coated graphite is obtained through drying, rolling and cutting.
[0155] In the third aspect, in some embodiments of the present invention, the specific process of step 1) comprises the following steps:
[0156] The carbon-coated silicon material, the carbon-coated graphite material and part of the conductive material are mixed as dry materials to obtain a premixed dry material; the binder material is stirred with deionized water at a low speed for 5 hours to obtain a binder solution; the premixed dry material, the remaining conductive material, the binder solution and deionized water are stirred at a high speed for 2 hours to obtain a first mixed solution; SBR and PAA are added to the first mixed solution, and the mixture is stirred at a low viscosity and low speed for 3 hours to obtain a composite negative electrode slurry. The solid content of the slurry is fixed at 50%.
[0157] The negative electrode active material accounts for 90-95% by weight in the negative electrode mixed slurry, the conductive material accounts for 2-5% by weight in the negative electrode mixed slurry, and the binder accounts for 3-6% by weight in the negative electrode mixed slurry.
[0158] In the third aspect, in some embodiments of the present invention, the conductive material includes one or more of conductive graphite, conductive carbon black, conductive carbon fiber, carbon nanotubes and graphene.
[0159] In the third aspect, in some embodiments of the present invention, the conductive material includes conductive graphite, conductive carbon black, conductive carbon fiber, carbon nanotube or graphene.
[0160] In the third aspect, in some embodiments of the present invention, in the negative electrode plate, the type of current collector is not specifically limited and can be selected according to actual needs, such as copper foil and graphene paper.
[0161] In a fourth aspect, in some embodiments of the present invention, a lithium-ion battery is provided, comprising a positive electrode plate, a separator, an electrolyte, and the negative electrode plate of the third aspect of the present invention.
[0162] Specifically, since the negative electrode plate adopts the negative electrode composite material of the present invention, it has a high gram capacity and high compactness, and can achieve a higher energy density. This means that at the same volume or weight, the battery can store more electrical energy, thereby extending the use time of the device or reducing the volume and weight of the battery. The structure of the negative electrode composite material optimizes the transmission path and reactive area of lithium ions inside the battery, so that the battery can achieve better fast charge and discharge performance. This means that the battery can maintain high efficiency and stability when fast charge and discharge are required, and is suitable for high-power equipment and fast charging requirements. Furthermore, the negative electrode composite material effectively inhibits the expansion of the silicon material and improves its cycle stability, so that the battery can achieve long-term and stable cycle use. This not only extends the service life of the battery, but also reduces the frequency of battery replacement and maintenance costs. In addition, the carbon coating effectively reduces the possibility of direct contact between the silicon material and the electrolyte, thereby reducing the side reactions inside the battery and improving the safety and stability of the battery. This is crucial to preventing thermal runaway of the battery and increasing the safety of the battery.
[0163] Therefore, the lithium-ion battery manufactured using the negative electrode plate of the present invention can be significantly improved in terms of energy density, rate performance, cycle life and safety, and is suitable for a wide range of applications requiring high energy density and high-efficiency charging and discharging, such as electric vehicles, portable devices and energy storage systems.
[0164] In a fifth aspect, in some embodiments of the present invention, there is provided an electrical device comprising the lithium-ion battery of the fourth aspect of the present invention.
[0165] It can be understood that the above-mentioned lithium-ion batteries have high energy density, excellent rate performance and long cycle life, and can provide a stable and long-lasting power supply for electrical devices. This is very important for applications such as electronic equipment, electric vehicles and energy storage systems, and can ensure that the equipment operates efficiently for a long time. The excellent rate performance of lithium-ion batteries means that it can be charged quickly and discharged efficiently, and is suitable for fast charging equipment and applications that require frequent charging and discharging. This improves the convenience and efficiency of electrical devices such as new energy vehicles.
[0166] Due to high energy density and excellent cycle performance, the above batteries can store more electrical energy and maintain stable output for a long time, extending the service life of the equipment. This is especially important for equipment that relies on long-term use, such as new energy vehicles, mobile communication equipment, portable electronic devices, etc. Long cycle life and stability mean that the above batteries require less maintenance and replacement frequency, reducing maintenance costs and equipment downtime. This is particularly important for commercial and industrial applications, which can improve the reliability and economy of the equipment.
[0167] In addition, the carbon coating of the battery effectively reduces direct contact with the electrolyte, reducing the risk of side reactions and thermal runaway inside the battery, thereby improving the safety of electrical devices such as new energy vehicles. This is particularly important in applications that require high safety and reliability.
[0168] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.
[0169] In the description of the present invention, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0170] Unless otherwise specified, "room temperature" in the present invention means 25°C±5°C.
[0171] Unless otherwise specified, "about" in the present invention means that the allowable error is within ±2%.
[0172] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.
[0173] Example 1
[0174] A negative electrode composite material is prepared, the structure of which includes composite particles and a carbon coating layer coating the composite particles. Figure 1 As shown, the composite particle includes a graphite material 1 and a hard carbon skeleton 2 coating the graphite material 1, a pore structure 3 is distributed in the hard carbon skeleton 2, and silicon 4 is deposited in the pore structure 3. The composite particle (equivalent to a secondary particle) formed by the graphite material 1, the hard carbon skeleton 2 and the silicon 4 is coated by a carbon coating layer 5.
[0175] Average particle size D of negative electrode composite material V 50About 10μm.
[0176] The thickness of the carbon coating layer is 10 nm.
[0177] The pore size of the porous structure is less than 5 nm.
[0178] The graphite material is specifically block-shaped artificial graphite.
[0179] The average particle size of artificial graphite balls D 1 50 is 10μm.
[0180] The preparation method of the negative electrode composite material is specifically as follows:
[0181] S1: Wrapping the graphite material with a hard carbon skeleton precursor and carbonizing it to obtain a first precursor;
[0182] S2: heating the first precursor in a protective atmosphere, introducing a silicon source gas to perform silicon deposition, and obtaining a second precursor;
[0183] S3: thermally depositing the second precursor in a carbon source gas to obtain a negative electrode composite material.
[0184] In step S1:
[0185] Before wrapping the graphite material with the hard carbon skeleton precursor, the graphite material is firstly screened.
[0186] As mentioned above, there are two methods for wrapping graphite material with hard carbon skeleton precursor: solvent method and melting method. In this embodiment, solvent method is specifically used. The method is: dissolving hard carbon precursor in solvent, the solvent is acetone, then adding artificial graphite balls, mixing, and carbonizing.
[0187] The carbonization temperature is 1800°C.
[0188] In the first precursor, the mass proportion of the hard carbon skeleton is ω 1 It is 15wt%.
[0189] The hard carbon skeleton precursor is specifically a phenolic resin.
[0190] In step S2:
[0191] Before the first precursor is heated in the protective atmosphere, the first precursor is first crushed to make the silicon deposition more uniform. It should be noted that if the first precursor prepared in step S1 has a small particle size, the first precursor can also be directly heated in the protective atmosphere.
[0192] In this embodiment, after the first precursor is crushed, the average particle size D 2 50 is 10μm.
[0193] The protective atmosphere is in particular nitrogen.
[0194] The first precursor is heated in a protective atmosphere at a temperature of 1900°C.
[0195] The silicon source gas is specifically silane.
[0196] A silicon source gas is introduced, and the hard carbon coating structure in the first precursor is used as a deposition skeleton / substrate for silicon.
[0197] In the second precursor, the mass proportion of silicon is ω 2 It is 35wt%.
[0198] In step S3:
[0199] The carbon source gas is specifically acetylene.
[0200] The pyrolysis temperature is 450°C.
[0201] In order to characterize the performance of the negative electrode composite material prepared in this example in a lithium secondary battery, the prepared negative electrode composite material is further prepared into a negative electrode plate, and then assembled with a positive electrode plate, an electrolyte and a separator into a lithium secondary battery.
[0202] It should be noted that the present invention does not limit the specific application of the negative electrode composite material, nor does it limit the specific preparation method of the negative electrode, positive electrode, electrolyte, separator and lithium secondary battery. They can be prepared by referring to the commonly used methods of technicians in this field and then characterized by conventional technical means.
[0203] The preparation method of the negative electrode sheet is as follows:
[0204] Carbon black (Super C65) and small-sized graphene are used as conductive agents, carboxymethyl cellulose (CMC), polyacrylic acid (PAA) and styrene-butadiene latex (SBR) are used as thickeners and binders, and composite negative electrodes are prepared by traditional coating methods. First, 90wt% of negative electrode composite materials, 2.0wt% of conductive carbon black and 2.0wt% of small-sized graphene, 2.0wt% of styrene-butadiene latex, 2.2wt% of polyacrylic acid and 1.8wt% of carboxymethyl cellulose are mixed to obtain a uniform slurry. The slurry is coated on the upper and lower surfaces of the copper foil, and finally placed in an oven to dry, and then cold pressed and cut to obtain a composite negative electrode sheet.
[0205] The preparation method of the positive electrode sheet is as follows:
[0206] High nickel ternary (NCM811) material is used as the positive electrode active material. Conductive carbon black (SuperC65) and conductive carbon nanotubes are used as conductive agents, polyvinylidene fluoride (PVDF) and N-methylpyrrolidine (NMP) are used as binders and solvents, and the positive electrode is prepared by a traditional coating method. Specifically: 96wt% of active material, 2.5wt% of conductive agent (1.5wt% carbon black, 1wt% carbon nanotubes), 1.5wt% of polyvinylidene fluoride and 37wt% of N-methylpyrrolidine are mixed, the mixture is placed in a homogenizer and homogenized twice to make the slurry completely uniform, and the slurry is filtered with a 200-mesh filter. The slurry with suitable viscosity is transferred to the coating machine, and it is coated on both sides of the aluminum foil according to the designed coating thickness. After drying, it is compacted and cut to obtain the positive electrode sheet.
[0207] The preparation method of the electrolyte is:
[0208] Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (EDC) were mixed in a volume ratio of 1:1:1, and then 1 mol / L LiPF 6 Mix well to prepare electrolyte.
[0209] A polypropylene film was used as a separator.
[0210] The preparation method of lithium secondary battery is as follows:
[0211] The negative electrode sheet, the isolation film, and the negative electrode sheet are stacked in sequence, so that the isolation film is between the positive and negative electrode sheets to play an isolating role, and a bare battery cell is obtained; the bare battery cell is placed in a battery casing, and after drying, an electrolyte is injected, and a lithium-ion battery is obtained through vacuum packaging, standing, forming, and shaping processes.
[0212] Examples 2 to 6, and Comparative Examples 1 to 4
[0213] The difference from Example 1 is that the average particle size D of the negative electrode composite material is V 50. Mass proportion of hard carbon skeleton ω 1 、Silicon mass proportionω 2 The details are shown in Table 1.
[0214] Comparative Example 5
[0215] The negative electrode material was prepared by dry material mixing method. Specifically:
[0216] Graphite material, silicon-carbon material and part of the conductive material are mixed in dry form to obtain a premixed dry material, wherein silicon-carbon accounts for 18% of the total mass of graphite and silicon-carbon; the above-mentioned binder material is stirred with deionized water, and stirred at a low speed for 5 hours to obtain a binder solution; the above-mentioned premixed dry material, the remaining conductive material, the binder solution and deionized water are stirred at a high speed for 2 hours to obtain a first mixed solution; SBR and PAA are added to the above-mentioned first mixed solution, and stirred at a low viscosity and low speed for 3 hours to obtain a composite negative electrode slurry. The solid content of the slurry is fixed at 50%.
[0217] The negative electrode slurry obtained in the above steps is coated on the front and back surfaces of the current collector to form a coating layer on the current collector, and a composite negative electrode sheet containing carbon-coated silicon and graphite is obtained through drying, rolling and cutting.
[0218] The negative electrode active material accounts for 95% by mass in the negative electrode mixed slurry, the conductive material accounts for 3% by mass in the negative electrode mixed slurry, and the binder accounts for 2% by mass in the negative electrode mixed slurry.
[0219] In the negative electrode preparation of Comparative Example 5, the graphite material is specifically artificial graphite.
[0220] Performance Testing
[0221] The performance of the lithium secondary batteries prepared in the examples and comparative examples was tested. Specifically, the following were performed:
[0222] (1) Mechanical properties test:
[0223] Lithium deposition degree test: At 25°C, the lithium secondary batteries prepared in the examples and comparative examples were fully charged and discharged at 1C, 2C, 3C and 4C rates, respectively. After each rate was repeated 10 times, the negative electrode plates were disassembled and the lithium deposition on the surface of the negative electrode plates was observed. Among them, the area of lithium deposition on the surface of the negative electrode plates is less than 5%, which is considered to be slight lithium deposition, the area of lithium deposition on the surface of the negative electrode plates is 5% to 40%, which is considered to be moderate lithium deposition, and the area of lithium deposition on the surface of the negative electrode plates is greater than 40%, which is considered to be severe lithium deposition.
[0224] 3C direct charge and fast charge cycle test: At 25°C, the lithium secondary batteries prepared in the examples and comparative examples were charged at a 3C rate and discharged at a 1C rate, and full charge and discharge cycle tests were performed until the capacity of the lithium secondary battery decayed to 80% of the initial capacity, and the number of cycles was recorded.
[0225] (2) Cyclic performance test:
[0226] At 25° C., the lithium secondary batteries prepared in the examples and comparative examples were charged at a 1C rate and discharged at a 1C rate for full charge and discharge cycle tests until the capacity of the lithium secondary batteries decayed to 80% of the initial capacity, and the number of cycles was recorded.
[0227] (3) Actual energy density test:
[0228] At 25°C, the lithium-ion battery is fully charged at a 0.33C rate and fully discharged at a 0.33C rate, and the actual discharge energy at this time is recorded; at 25°C, the lithium-ion battery is weighed using an electronic balance, and the weighing result is recorded as the weight of the lithium-ion battery; the energy density of the lithium-ion battery is the ratio of the actual discharge energy to the weight of the lithium-ion battery.
[0229] (4) Physical property tests of carbon-coated silicon and carbon-coated graphite:
[0230] The volume median particle size Dv50 of silicon-carbon / graphite composite material: obtained by using a laser diffraction particle size analyzer (MS2000). The sample particles are dispersed in a liquid medium at a concentration of 200-300 mg / L, and a monochromatic light beam is passed through. After the light is scattered by the particles, it is distributed at different angles. The regular multi-element detector receives the values of the relevant scattering diagram at many angles and records these values for analysis. Using the Rayleigh scattering formula, the scattering values are calculated to obtain the ratio of the volume of particles of each particle size level to the total volume, thereby obtaining the volume distribution of the particle size.
[0231] (5) Extreme compaction:
[0232] The negative electrode sheet was prepared according to 1.5, 1.52, 1.54, 1.58, 1.60, 1.62, 1.64, 1.66, 1.68, 1.7 g / cm 3A gradient roller compaction test was performed, and slight damage to the coating layer was identified as extreme compaction.
[0233] The results are shown in Tables 1 and 2.
[0234] Table 1
[0235]
[0236] Table 2
[0237]
[0238]
[0239] Table 3
[0240]
[0241] It can be seen from the test results in the embodiments and comparative examples that when the median particle size, hard carbon mass percentage, and silicon mass percentage of the composite material are within the value range of the present invention, the energy density, kinetic performance, and cycle performance of the lithium-ion battery are better.
[0242] When D v 50 is too low. Due to the hard carbon coating and silicon deposition of the composite material, too small a particle size will lead to an increase in specific surface area and increased silicon exposure, resulting in better fast charging performance of the lithium-ion battery, but low first efficiency and larger side reactions, as shown in Comparative Example 1.
[0243] When D v 50 is too high. As the particle size is too large, the lithium ion transmission path is significantly increased, and the decreased porosity is not conducive to the infiltration of the electrolyte and the diffusion of ions, resulting in serious lithium deposition at the negative electrode of the lithium ion battery, which seriously affects the cycle performance and fast charging performance of the lithium ion battery, as shown in Comparative Example 2.
[0244] When the proportion of hard carbon or silicon is too small, although the cycle stability is good, the material's specific capacity is too small and the fast charging performance is poor. This is because hard carbon materials have wider ion diffusion channels and active sites, which are beneficial to the material's rate performance; while silicon materials can improve the specific capacity of composite materials. Therefore, the small proportion of hard carbon or silicon leads to poor material specific capacity and rate performance, such as Comparative Example 3.
[0245] When the proportion of hard carbon or silicon is too large, the material has a high gram capacity and the battery cell has the highest energy density, but the cycle stability is poor and lithium plating is also serious. This is because as the silicon material increases, the material expansion gradually increases, resulting in a decrease in cycle performance; and as the silicon material increases, the material's conductivity and ion conductivity decrease, resulting in a deterioration in the material's rate performance, as shown in Comparative Example 4.
[0246] The battery cells prepared by using graphite in silicon-carbon / graphite composite materials as the negative electrode active material and mixed coating with commercial silicon-carbon materials show poor cycle performance and fast charging performance compared with the battery cells prepared using the silicon-carbon / graphite composite materials of this patent at the same energy density. This is because the graphite material and the silicon-based material are directly mixed and coated, the silicon material is unevenly dispersed in the composite negative electrode, resulting in uneven current density, and the silicon-based material fails in the negative electrode, resulting in poor cycle stability of the overall negative electrode material, as shown in Comparative Example 5. The silicon-carbon / graphite composite material to which this patent belongs has great structural advantages. Using hard carbon-coated graphite as the core to improve the compaction of the composite negative electrode, silicon is uniformly deposited in the hard carbon coating layer, and hard carbon is used as the carbon skeleton of the silicon material and the conductive network between silicon and graphite to effectively improve the cycle stability and fast charging performance of the battery cell.
[0247] Therefore, the hard carbon / silicon / graphite ratio and material size in silicon-carbon / graphite composites significantly affect the electrochemical properties of the material.
[0248] Finally, it should be noted that due to the excellent combination of silicon and graphite materials contained in the composite material structure of the present invention, the high gram capacity of silicon and the stability of graphite can be combined to significantly improve the energy density and power density of the battery. For new energy vehicles, this means longer driving range and better acceleration performance.
[0249] Traditional silicon-carbon / graphite composite materials often have poor cycle stability due to the high expansion of silicon materials. The hard carbon skeleton and porous structure in the composite material of the present invention effectively inhibit the expansion of silicon materials, thereby significantly improving the cycle life and stability of the battery and extending the service life of the battery. The carbon coating reduces the direct contact between silicon and the electrolyte, while the porous structure in the hard carbon skeleton effectively deposits silicon. These characteristics together improve the fast charging performance of the battery. New energy vehicles using batteries made of this composite material can complete charging more quickly, improving user convenience and satisfaction.
[0250] Furthermore, the hard carbon skeleton, as a bonding material for the composite particles and a skeleton for deposited silicon, helps optimize the electron transmission capacity. This means that the battery can release and store energy more efficiently, further improving the performance of the battery. The design and optimized structure of the composite material of the present invention can reduce the material cost of the battery during the manufacturing process, and improve the life and reliability of the battery, thereby reducing the overall battery system cost.
[0251] In summary, the lithium-ion battery manufactured using the negative electrode composite material of the present invention can not only improve the energy density and power density of the battery, but also improve the cycle stability and fast charging performance, so that the performance, endurance and ease of use of new energy vehicles are significantly improved, which meets the requirements of high performance and long life of future electric vehicles.
[0252] The present invention has been described in detail above in conjunction with the embodiments, but the present invention is not limited to the above embodiments, and various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.
Claims
1. A negative electrode composite material, It is characterized in that It comprises composite particles and a carbon coating layer coating the composite particles. The composite particles comprise graphite material and a hard carbon skeleton coating the graphite material. A pore structure is distributed in the hard carbon skeleton, and silicon is deposited in the pore structure.
2. The negative electrode composite material according to claim 1, It is characterized in that The average particle size D of the negative electrode composite material V 50 Range: 6μm≤D V 50≤25μm; and / or, the thickness of the carbon coating layer is 2nm-20nm; and / or, the pore size of the porous structure is less than 5nm.
3. The negative electrode composite material according to claim 1, It is characterized in that The mass proportion of the hard carbon skeleton in the negative electrode composite material is 9.7wt% to 18.5wt%.
4. The negative electrode composite material according to claim 1, It is characterized in that The mass proportion of silicon in the negative electrode composite material is 2.9 wt % to 7.4 wt %.
5. A method for preparing the negative electrode composite material according to any one of claims 1 to 4, It is characterized in that The following steps are involved: S1: wrapping the graphite material with a hard carbon skeleton precursor and carbonizing it to obtain a first precursor; S2: heating the first precursor in a protective atmosphere, introducing a silicon source gas to perform silicon deposition, and obtaining a second precursor; S3: thermally depositing the second precursor in a carbon source gas to obtain the negative electrode composite material.
6. The method according to claim 5, It is characterized in that The hard carbon skeleton precursor includes at least one of styrene-butadiene rubber, polyfurfuryl alcohol, natural rubber, polyacrylonitrile, butadiene rubber, phenolic resin, furan resin, epoxy resin, furfural resin, furfural ketone resin and furfural alcohol resin.
7. The method according to claim 5, It is characterized in that The carbonization temperature is 1600°C to 2200°C.
8. A negative electrode sheet, It is characterized in that The negative electrode plate is made of the negative electrode composite material according to any one of claims 1 to 4 or the negative electrode composite material prepared by the method according to any one of claims 5 to 7.
9. A lithium ion battery, It is characterized in that It comprises a positive electrode plate, a separator, an electrolyte and a negative electrode plate as claimed in claim 8.
10. An electrical device, It is characterized in that Includes the lithium ion battery as claimed in claim 9.