Negative active material, negative plate, preparation method and battery

By constructing composite phosphorus carbon materials on the surface of phosphorus-based materials and combining the multi-dimensional conductive network structure of carbon nanotubes and graphene, the problem of poor volume expansion and solid electrolyte compatibility of phosphorus-based materials in lithium/sodium ion batteries is solved, and the battery is improved cycle life and electrochemical properties.

CN118919678APending Publication Date: 2024-11-08中汽新能(天津)电池科技有限公司
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410965890.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The high volume expansion rate of phosphorus-based materials in existing lithium/sodium ion batteries and the dissolution of reaction intermediates lead to rapid attenuation of battery capacity, and the low ionic conductivity and poor interface compatibility of solid electrolytes lead to large battery impedance, affecting cycle life.

Method used

Using composite phosphorus carbon material, the first solid electrolyte, carbon nanotube and graphene are attached to the surface of the phosphorus source and the second solid electrolyte cladding layer is coated to form a multi-dimensional conductive network structure, thereby improving the interface between the phosphorus-based material and the solid electrolyte Contact stability and conductivity.

Benefits of technology

It effectively reduces the internal resistance of the battery, improves the cycle life and Coulomb efficiency of the phosphorus-carbon material, prevents the powdering and volume expansion of the phosphorus-based material, and enhances the electrochemical performance of solid-state batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919678A_ABST
    Figure CN118919678A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of batteries, and particularly relates to a negative active material, a negative plate, a preparation method and a battery. The negative electrode active material comprises a composite phosphorus-carbon material core and a solid electrolyte coating layer coating the surface of the composite phosphorus-carbon material core; the composite phosphorus-carbon material comprises a first solid electrolyte, a phosphorus source, a carbon nanotube, graphene and a conductive polymer, and the solid electrolyte coating layer comprises a second solid electrolyte. The invention provides a negative active material, a negative plate, a preparation method and a battery, which meet the requirements of a high-specific-energy solid-state battery. A multi-dimensional conductive network structure is jointly constructed by introducing carbon nanotubes and graphene into a phosphorus-based material, and solid electrolyte particles are attached to the carbon nanotubes and the graphene, so that multi-site contact of the phosphorus-based material and a solid electrolyte is increased, interface resistance of the solid electrolyte and the phosphorus-carbon material can be effectively reduced, and the performance of the phosphorus-carbon material is improved. And a multi-dimensional channel for ion transmission is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of batteries, and in particular relates to a negative electrode active material, a negative electrode sheet, a preparation method and a battery. Background Art

[0002] Due to the shortage of oil resources and the increasing environmental pollution, there is an urgent need to vigorously develop clean energy technologies. Among them, secondary batteries have the advantages of long cycle life, no memory effect, and fast charging and discharging, and have been widely used in portable electronic products and electric vehicles. With the growing demand for new energy in the consumer market, it is necessary to develop secondary batteries with higher energy density. At present, the most widely used negative electrodes for lithium / sodium ion batteries are carbon-based materials, including artificial graphite, hard carbon, soft carbon, and mesophase carbon microspheres. However, the specific capacity of carbon-based materials is generally low. For example, the theoretical capacity of graphite is only 372mAh / g, which can no longer meet the requirements of higher energy density (>400Wh / kg) for secondary batteries. Therefore, the development of higher capacity negative electrode materials has become one of the current research and development focuses.

[0003] Phosphorus-based materials as alloy-type negative electrode materials have very high theoretical lithium / sodium storage capacity (2596 mAh / g) and suitable lithium / sodium deintercalation potential (~0.4 V vs. Na + / Na) can inhibit dendrite growth, and its reserves are abundant and the price is low. It is a very promising negative electrode material. However, its shortcomings hinder its application in secondary batteries. First, red / black phosphorus and its intermediate reactants have poor intrinsic electronic conductivity, which leads to very slow and lagging reactions; second, phosphorus-based materials have a high volume expansion rate after lithium / sodium insertion, which can easily lead to pulverization of negative electrode active materials and rupture of solid electrolyte interface film (SEI film), resulting in the exposed active sites constantly reacting with the electrolyte, causing the battery capacity to decay rapidly; third, the reaction intermediate product of phosphorus-based materials, polyphosphide, will dissolve in the electrolyte, resulting in low cycle coulomb efficiency and rapid capacity decay. Although liquid organic electrolytes have the advantages of high ionic conductivity and good wettability, they have poor thermal stability and are prone to flammability and leakage. At the same time, they are highly chemically active and are prone to many side reactions with the exposed active sites of the electrode, resulting in a continuous decline in battery performance. Based on the above reasons, researchers have proposed using solid electrolytes with low flammability, high thermal stability and high energy density to replace liquid electrolytes to reduce the occurrence of side reactions inside the battery and improve the safety performance and energy density of lithium / sodium ion batteries.

[0004] However, solid electrolytes have low ionic conductivity, poor wettability, and poor compatibility and stability at the electrode / solid electrolyte interface, resulting in large battery impedance and severe obstruction of the transmission and diffusion of lithium / sodium ions. The existing technical solution for solid-state batteries is to mechanically mix the negative electrode material with the solid electrolyte, binder, and conductive agent and then apply it, or to apply the slurry after the solid electrolyte and binder are mixed on the pole piece to form an integrated composite electrode, or to simply sinter the solid electrolyte and the negative electrode material and then mechanically mix them with the binder and conductive agent and then apply the slurry to prepare the negative electrode. The above solutions can only improve the point-to-point contact area between the negative electrode material and the solid electrolyte, but cannot improve the interface stability and compatibility between the solid electrolyte and the negative electrode material. In the process of continuous expansion / contraction of the material volume caused by continuous insertion / extraction of lithium at the negative electrode, it is still easy for the solid electrolyte to contact and separate from the negative electrode material, resulting in an increase in the internal resistance of the battery and a decrease in the cycle performance. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a negative electrode active material, a negative electrode sheet, a preparation method and a battery.

[0006] To achieve the above object, the technical solution adopted by the present invention is:

[0007] A negative electrode active material comprises a composite phosphorus-carbon material core and a solid electrolyte coating layer coated on the surface of the composite phosphorus-carbon material core; the composite phosphorus-carbon material comprises a first solid electrolyte, a phosphorus source, carbon nanotubes, graphene, and a conductive polymer; the solid electrolyte coating layer comprises a second solid electrolyte.

[0008] In the composite phosphorus-carbon material, the first solid electrolyte is attached to the surface of the phosphorus source, and the carbon nanotubes are dispersed between the phosphorus source particles; the graphene is coated on the surface of the inner core formed by the phosphorus source particles and the carbon nanotubes, and is connected to the solid electrolyte coating layer.

[0009] The thickness of the solid electrolyte coating layer is 50nm-1μm; preferably, the particle size of the composite phosphorus-carbon material inner shell is 1-20μm.

[0010] The mass ratio of the phosphorus source, carbon nanotubes, graphene, the first solid electrolyte, and the conductive polymer is (40-70):(1-20):(1-20):(2-30):(1-10), preferably 60:(5-13):(5-9):(5-10):5.

[0011] The diameter of the carbon nanotubes is ≤2 μm; preferably, the phosphorus source includes one or any combination of red phosphorus and black phosphorus;

[0012] Preferably, the first solid electrolyte and the second solid electrolyte independently include inorganic metal oxide solid electrolytes; preferably one or any combination of perovskite solid electrolyte materials, garnet solid electrolyte materials, NAS I CON solid electrolyte materials, and LISI CON solid electrolyte materials; the particle size is between 1-500 nm;

[0013] Preferably, the conductive polymer includes one or any combination of polythiophene, polypyrrole, polyaniline, PEDOT, and polyacetylene;

[0014] Preferably, the graphene is a few-layer graphene oxide, and the number of graphene oxide sheets is less than 5.

[0015] The present invention also includes a method for preparing the negative electrode active material, comprising the following steps: (1) adding a first solid electrolyte and a phosphorus source to carbon nanotubes washed to neutrality, and then ball milling to obtain nano-phosphorus-carbon particles coated with carbon nanotubes; (2) adding the ball-milled nano-phosphorus-carbon particles, graphene oxide, the first solid electrolyte, and a conductive polymer to a solvent for mixing; spray drying the mixed solution to obtain a composite phosphorus-carbon material; (3) adding a second solid electrolyte and a solvent to the composite phosphorus-carbon material obtained after the spray drying treatment, stirring evenly, and then drying; keeping the dried sample warm in a nitrogen atmosphere to obtain a negative electrode active material.

[0016] Specifically, the specific steps of step 1) are: mixing carbon nanotubes with a hydrochloric acid solution, and stirring evenly for 1-5 hours; filtering the carbon nanotube mixture and washing with water until the solution is neutral; adding the first solid electrolyte particles to the carbon nanotube slurry solution, stirring evenly, and then ultrasonically treating to obtain a composite solution; adding a phosphorus source to the above composite solution, stirring evenly, and then transferring to a ball milling jar, and ball milling for 1-10 hours under an inert atmosphere to obtain carbon nanotube-coated nano-phosphorus-carbon particles;

[0017] Preferably, the concentration of the hydrochloric acid solution is 0.1-10 mol / L;

[0018] Preferably, the spray drying process in step 2) is as follows: the solid content of the spray solution is 1wt%-20wt%, the spray drying temperature is 100-250°C, the fan frequency is 50-200Hz, and the feed flow rate is 100-1000mL / h;

[0019] Preferably, the insulation condition of step 3) is 200-300° C. for 1-2 h.

[0020] The present invention also includes a negative electrode sheet, including the negative electrode active material, a binder, and a conductive agent; preferably, the binder is PVDF; preferably, the conductive agent is Super-P.

[0021] The present invention also includes a method for preparing a negative electrode sheet, comprising the following steps: mixing the negative electrode active material with a binder and a conductive agent, homogenizing the mixture using N-methylpyrrolidone as a solvent, uniformly coating the mixture on a negative electrode current collector, and drying the mixture to obtain a negative electrode sheet.

[0022] The present invention also includes a battery, comprising the negative electrode sheet, the positive electrode sheet and the separator.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] (1) The solid electrolyte composite coating treatment of the phosphorus-carbon material can improve the interface contact stability and contact area between the phosphorus-carbon negative electrode and the solid electrolyte, reduce the internal resistance of the battery, and increase the cycle life of the solid-state battery;

[0025] (2) The present invention utilizes the advantages of the two-dimensional structure of carbon nanotubes and the three-dimensional structure of graphene to effectively improve the conductivity of phosphorus-based materials. The nano solid electrolyte is attached to the carbon nanotubes and graphene, which can improve the multi-directional site contact between the solid electrolyte and the phosphorus-based material and ensure the continuity of the ion transmission channel.

[0026] (3) The present invention utilizes a spray self-assembly method to coat the outer surface of the nano-phosphorus-based material with graphene, which not only acts as a protective net to inhibit the huge volume expansion of the phosphorus-based material when lithium / sodium is inserted, and prevents the pulverization of the phosphorus-based material and the subsequent electrical contact failure, but also acts to connect the inner core of the phosphorus-based material with the outer shell solid electrolyte, thereby improving the interface stability and compatibility between the negative electrode material and the solid electrolyte.

[0027] In summary, the present invention provides negative electrode active materials, negative electrode sheets, preparation methods and batteries that meet the requirements of high specific energy solid-state batteries. By introducing carbon nanotubes and graphene into phosphorus-based materials, a multi-dimensional conductive network structure is jointly constructed, and solid electrolyte particles are attached to carbon nanotubes and graphene, which increases the multi-site contact between the phosphorus-based material and the solid electrolyte, and can effectively reduce the interface resistance between the solid electrolyte and the phosphorus-carbon material, ensuring the multi-dimensional channel for ion transmission.

[0028] In addition, the graphene oxide sheet can also serve as a network protection layer to accommodate the volume expansion of phosphorus-based materials, inhibit the pulverization of phosphorus-based materials and the dissolution of polyphosphides, so as to ensure the best electrochemical performance of phosphorus-based materials. Graphene is coated between the inner core (phosphorus-carbon inner core) formed by phosphorus source particles and carbon nanotubes and the outer solid electrolyte coating layer, and can also effectively connect the phosphorus-carbon inner core with the outermost coated nano solid electrolyte layer to ensure the interface contact area between the two, improve the stability of the negative electrode / solid electrolyte contact interface, and the application of this composite phosphorus-carbon material in the negative electrode of solid-state batteries can effectively improve the battery's cycle performance and reduce battery impedance. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 A schematic diagram of the structure of the negative electrode active material according to an embodiment of the present invention;

[0030] Figure 2 Graph showing the cycle performance results of the embodiments of the present invention and the comparative examples. DETAILED DESCRIPTION

[0031] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and the best embodiments.

[0032] Figure 1 The negative electrode active material is shown, including a composite phosphorus-carbon material core and a solid electrolyte coating layer 1 coated on the surface of the composite phosphorus-carbon material core; the composite phosphorus-carbon material includes a first solid electrolyte, a phosphorus source 21, a carbon nanotube 23, a graphene 22, and a conductive polymer; the solid electrolyte coating layer 1 includes a second solid electrolyte. In the composite phosphorus-carbon material, the first solid electrolyte is attached to the surface of the phosphorus source 21, and the carbon nanotube 23 is dispersed between the particles of the phosphorus source 21; the graphene 22 is coated on the surface of the core formed by the phosphorus source 21 particles and the carbon nanotube 23, and is connected to the solid electrolyte coating layer 1.

[0033] The thickness of the solid electrolyte coating layer is 50nm-1μm, specifically 50nm, 100nm, 500nm, 1μm; the particle size of the composite phosphorus-carbon material inner shell is 1-20μm, specifically 1μm, 5μm, 10μm, 20μm;.

[0034] The mass ratio of phosphorus source, carbon nanotubes, graphene, first solid electrolyte and conductive polymer is (40-70):(1-20):(1-20):(2-30):(1-10); preferably 60:(5-13):(5-9):(5-10):5.

[0035] The diameter of the carbon nanotubes is ≤2 μm; preferably, the phosphorus source includes one or any combination of red phosphorus and black phosphorus;

[0036] Preferably, the first solid electrolyte and the second solid electrolyte independently include inorganic metal oxide solid electrolytes; preferably one or any combination of perovskite-type solid electrolyte materials, garnet-type solid electrolyte materials, NAS I CON-type solid electrolyte materials, and LISI CON-type solid electrolyte materials; and the particle size is between 1-500 nm.

[0037] Preferably, the conductive polymer includes one or any combination of polythiophene, polypyrrole, polyaniline, PEDOT, and polyacetylene;

[0038] Preferably, the graphene is a few-layer graphene oxide, and the number of graphene oxide sheets is less than 5.

[0039] The present invention also includes a method for preparing the negative electrode active material, comprising the following steps: (1) adding a first solid electrolyte and a phosphorus source to carbon nanotubes washed to neutrality, and then ball milling to obtain nano-phosphorus-carbon particles coated with carbon nanotubes; (2) adding the ball-milled nano-phosphorus-carbon particles, graphene oxide, the first solid electrolyte, and a conductive polymer to a solvent for mixing; spray drying the mixed solution to obtain a composite phosphorus-carbon material; (3) adding a second solid electrolyte and a solvent to the composite phosphorus-carbon material obtained after the spray drying treatment, stirring evenly, and then drying; keeping the dried sample warm in a nitrogen atmosphere to obtain a negative electrode active material.

[0040] Preferably, the mass ratio of the first solid electrolyte in step (1) to the first solid electrolyte in step (2) is (3-8):2; preferably 5:2;

[0041] Preferably, the mass ratio of the second solid electrolyte to the first solid electrolyte in step (2) is (9-20):2; preferably 15:2. Specifically, the specific steps of step 1) are: mixing the carbon nanotubes with the hydrochloric acid solution, and stirring evenly for 1-5 hours; filtering the carbon nanotube mixture with water, and washing with water until the solution is neutral; adding the first solid electrolyte particles to the carbon nanotube slurry solution, stirring evenly, and then ultrasonically treating to obtain a composite solution; adding the phosphorus source to the above composite solution, stirring evenly, and then transferring to a ball milling jar, and ball milling for 1-10 hours under an inert atmosphere to obtain carbon nanotube-coated nano-phosphorus-carbon particles;

[0042] Preferably, the concentration of the hydrochloric acid solution is 0.1-10 mol / L; specifically, it can be 0.1 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L, 5 mol / L, 10 mol / L.

[0043] Preferably, the spray drying process in step 2) is as follows: the solid content of the spray solution is 1wt%-20wt%, specifically 1wt%, 5wt%, 10wt%, 20wt%; the spray drying temperature is 100-250°C, specifically 100°C, 130°C, 200°C, 250°C; the fan frequency is 50-200Hz, specifically 50Hz, 70Hz, 100Hz, 200Hz; the feed flow rate is 100-1000mL / h; specifically 100mL / h, 500mL / h, 600mL / h, 1000mL / h;

[0044] Preferably, the insulation condition of step 3) is 200-300° C. for 1-2 h, specifically 300° C. for 1 h, 200° C. for 2 h, or 250° C. for 2 h.

[0045] The present invention also includes a negative electrode, including the negative electrode active material, a binder, and a conductive agent; preferably, the binder is PVDF; preferably, the conductive agent is Super-P.

[0046] The present invention also includes a method for preparing a negative electrode sheet, comprising the following steps: mixing the negative electrode active material with a binder and a conductive agent, homogenizing the mixture using N-methylpyrrolidone as a solvent, uniformly coating the mixture on a negative electrode current collector, and drying the mixture to obtain a negative electrode sheet.

[0047] The present invention also includes a battery, comprising the negative electrode sheet, the positive electrode sheet and the separator.

[0048] The following is an explanation with reference to specific embodiments.

[0049] Example 1

[0050] The method for preparing the negative electrode sheet comprises the following steps:

[0051] (1) Take 10g of single-walled carbon nanotubes, add 100mL of hydrochloric acid solution (molar concentration of 1.5mol / L), and stir evenly for 4h; filter and wash the carbon nanotube mixture several times until the solution pH = 7; add 3g of the first solid electrolyte Li with a particle size of 100nm 7 La 3 Zr 2 O 12 Add 50g of distilled water, stir evenly and then perform ultrasonic treatment;

[0052] (2) adding 60 g of red phosphorus to the composite solution, stirring again and transferring to a ball mill, and ball milling for 5 h under a nitrogen atmosphere to obtain a composite sample 1;

[0053] (3) The composite sample 1 prepared in step (2) was mixed with 5 g of single-layer graphene oxide, 5 g of polypyrrole, and 2 g of solid electrolyte Li with a particle size of 100 nm. 7 La 3 Zr 2 O 12 Adding into distilled water, stirring and strong ultrasonic mixing treatment, to obtain a mixed solution with a solid content of 5wt%; spraying self-assembly treatment on the mixed solution to obtain phosphorus carbon / graphene composite microspheres; the parameters in the spraying process are: air inlet temperature of 130°C, fan frequency of 70Hz, and feed rate of 600mL / h;

[0054] (4) The phosphorus-carbon / graphene composite microspheres obtained by the spray self-assembly are mixed with 15 g of nano-Li 7 La 3 Zr 2 O 12 The mixture was mixed, 50 g of distilled water was added, the mixture was stirred for 2 h and then dried. The dried sample was kept at 250° C. for 2 h under a nitrogen atmosphere to obtain a composite phosphorus-carbon negative electrode material coated with a solid electrolyte.

[0055] (5) 3.2 g of the composite phosphorus-carbon material (negative electrode active material) was mixed with 0.4 g of a binder (PVDF) and 0.4 g of a conductive agent Super-P, and slurried using N-methylpyrrolidone (NMP) as a solvent. The mixture was evenly coated on a copper foil and dried in an oven at 120°C for 12 h. The negative electrode sheet was then punched into a 13 mm diameter disc.

[0056] In a glove box filled with argon, a metal lithium sheet was used as the counter electrode and the electrolyte was 1.0 M Li PF 6 (EC / DEC = 1:1 volume ratio), the separator is a polyethylene separator, and assembled into a CR2032 button cell. At room temperature, the battery was tested using a blue battery tester, the test conditions were a current density of 20 mA / g, and the voltage range of the charge and discharge test was 0 to 2.5 V.

[0057] Example 2

[0058] The method for preparing the negative electrode sheet comprises the following steps:

[0059] (1) Take 10g of single-walled carbon nanotubes, add 100mL of hydrochloric acid solution (molar concentration of 1.5mol / L), and stir evenly for 4h; filter and wash the carbon nanotube mixture several times until the solution pH is 7; add 5g of the first solid electrolyte Li with a particle size of 100nm 7 La 3 Zr 2 O 12 Add 50g of distilled water, stir evenly and then perform ultrasonic treatment;

[0060] (2) adding 60 g of red phosphorus to the composite solution, stirring again and transferring to a ball mill, and ball milling for 5 h under a nitrogen atmosphere to obtain a composite sample 1;

[0061] (3) The composite sample 1 prepared in step (2) was mixed with 5 g of single-layer graphene oxide, 5 g of polypyrrole, and 2 g of solid electrolyte Li with a particle size of 100 nm. 7 La 3 Zr 2 O 12 Adding into distilled water, stirring and strong ultrasonic mixing treatment, to obtain a mixed solution with a solid content of 5wt%; spraying self-assembly treatment on the mixed solution to obtain phosphorus carbon / graphene composite microspheres; the parameters in the spraying process are: air inlet temperature of 130°C, fan frequency of 70Hz, and feed rate of 600mL / h;

[0062] (4) The phosphorus-carbon / graphene composite microspheres obtained by the spray self-assembly are mixed with 15 g of nano-Li 7 La 3 Zr 2 O 12 The mixture was mixed, 50 g of distilled water was added, the mixture was stirred for 2 h and then dried. The dried sample was kept at 250° C. for 2 h under a nitrogen atmosphere to obtain a composite phosphorus-carbon negative electrode material coated with a solid electrolyte.

[0063] (5) 3.2 g of the composite phosphorus-carbon material (negative electrode active material) was mixed with 0.4 g of a binder (PVDF) and 0.4 g of a conductive agent Super-P, and slurried using N-methylpyrrolidone (NMP) as a solvent. The mixture was evenly coated on a copper foil and dried in an oven at 120°C for 12 h. The negative electrode sheet was then punched into a 13 mm diameter disc.

[0064] In a glove box filled with argon, a lithium metal sheet was used as the counter electrode, the electrolyte was 1.0M Li PF6 (EC / DEC = 1:1 volume ratio), and the diaphragm was a polyethylene diaphragm to assemble a CR2032 button cell. The battery was tested at room temperature using a blue battery tester, with a current density of 20mA / g and a voltage range of 0 to 2.5V for charge and discharge tests.

[0065] Example 3

[0066] The method for preparing the negative electrode sheet comprises the following steps:

[0067] (1) Take 10 g of single-walled carbon nanotubes, add 100 mL of hydrochloric acid solution (molar concentration of 1.5 mol / L), and stir evenly for 4 h; filter and wash the carbon nanotube mixture several times until the solution pH = 7; add 8 g of the first solid electrolyte Li with a particle size of 100 nm;7 La 3 Zr 2 O 12 Add 50g of distilled water, stir evenly and then perform ultrasonic treatment;

[0068] (2) adding 60 g of red phosphorus to the composite solution, stirring again and transferring to a ball mill, and ball milling for 5 h under a nitrogen atmosphere to obtain a composite sample 1;

[0069] (3) The composite sample 1 prepared in step (2) was mixed with 5 g of single-layer graphene oxide, 5 g of polypyrrole, and 2 g of solid electrolyte Li with a particle size of 100 nm. 7 La 3 Zr 2 O 12 Adding into distilled water, stirring and strong ultrasonic mixing treatment, to obtain a mixed solution with a solid content of 5wt%; spraying self-assembly treatment on the mixed solution to obtain phosphorus carbon / graphene composite microspheres; the parameters in the spraying process are: air inlet temperature of 130°C, fan frequency of 70Hz, and feed rate of 600mL / h;

[0070] (4) The phosphorus-carbon / graphene composite microspheres obtained by the spray self-assembly are mixed with 15 g of nano-Li 7 La 3 Zr 2 O 12 The mixture was mixed, 50 g of distilled water was added, the mixture was stirred for 2 h and then dried. The dried sample was kept at 250° C. for 2 h under a nitrogen atmosphere to obtain a composite phosphorus-carbon negative electrode material coated with a solid electrolyte.

[0071] (5) 3.2 g of the composite phosphorus-carbon material (negative electrode active material) was mixed with 0.4 g of a binder (PVDF) and 0.4 g of a conductive agent Super-P, and slurried using N-methylpyrrolidone (NMP) as a solvent. The mixture was evenly coated on a copper foil and dried in an oven at 120°C for 12 h. The negative electrode sheet was then punched into a 13 mm diameter disc.

[0072] In a glove box filled with argon, a lithium metal sheet was used as the counter electrode, the electrolyte was 1.0M Li PF6 (EC / DEC = 1:1 volume ratio), and the diaphragm was a polyethylene diaphragm to assemble a CR2032 button cell. The battery was tested at room temperature using a blue battery tester, with a current density of 20mA / g and a voltage range of 0 to 2.5V for charge and discharge tests.

[0073] Example 4

[0074] The method for preparing the negative electrode sheet comprises the following steps:

[0075] (1) 5 g of single-walled carbon nanotubes were added to 100 mL of hydrochloric acid solution (molar concentration of 1.5 mol / L), and stirred evenly for 4 h; the carbon nanotube mixture was filtered and washed with water for multiple times until the solution pH was 7; 3 g of the first solid electrolyte Li with a particle size of 100 nm was added 7 La 3 Zr 2 O 12 Add 50g of distilled water, stir evenly and then perform ultrasonic treatment;

[0076] (2) adding 60 g of red phosphorus to the composite solution, stirring again and transferring to a ball mill, and ball milling for 5 h under a nitrogen atmosphere to obtain a composite sample 1;

[0077] (3) The composite sample 1 prepared in step (2) was mixed with 5 g of single-layer graphene oxide, 5 g of polypyrrole, and 2 g of solid electrolyte Li with a particle size of 100 nm. 7 La 3 Zr 2 O 12 Adding into distilled water, stirring and strong ultrasonic mixing treatment, to obtain a mixed solution with a solid content of 5wt%; spraying self-assembly treatment on the mixed solution to obtain phosphorus carbon / graphene composite microspheres; the parameters in the spraying process are: air inlet temperature of 130°C, fan frequency of 70Hz, and feed rate of 600mL / h;

[0078] (4) The phosphorus-carbon / graphene composite microspheres obtained after the above-mentioned spray self-assembly were mixed with 15 g of nano-Li 7La 3 Zr 2 O 12 of the second solid electrolyte, 50 g of distilled water was added, and the mixture was stirred for 2 h and then dried. The dried sample was kept at 250 ° C for 2 h under a nitrogen atmosphere to obtain a composite phosphorus-carbon negative electrode material coated with a solid electrolyte.

[0079] (5) 3.2 g of the composite phosphorus-carbon material (negative electrode active material) was mixed with 0.4 g of a binder (PVDF) and 0.4 g of a conductive agent Super-P, and slurried using N-methylpyrrolidone (NMP) as a solvent. The mixture was evenly coated on a copper foil and dried in an oven at 120°C for 12 h. The negative electrode sheet was then punched into a 13 mm diameter disc.

[0080] In a glove box filled with argon, a lithium metal sheet was used as the counter electrode, the electrolyte was 1.0M Li PF6 (EC / DEC = 1:1 volume ratio), and the diaphragm was a polyethylene diaphragm to assemble a CR2032 button cell. The battery was tested at room temperature using a blue battery tester, with a current density of 20mA / g and a voltage range of 0 to 2.5V for charge and discharge tests.

[0081] Example 5

[0082] The method for preparing the negative electrode sheet comprises the following steps:

[0083] (1) 13 g of single-walled carbon nanotubes were added to 100 mL of hydrochloric acid solution (molar concentration of 1.5 mol / L), and stirred evenly for 4 h; the carbon nanotube mixture was filtered and washed with water for multiple times until the solution pH was 7; 3 g of the first solid electrolyte Li with a particle size of 100 nm was added 7 La 3 Zr 2 O 12 Add 50g of distilled water, stir evenly and then perform ultrasonic treatment;

[0084] (2) adding 60 g of red phosphorus to the composite solution, stirring again and transferring to a ball mill, and ball milling for 5 h under a nitrogen atmosphere to obtain a composite sample 1;

[0085] (3) The composite sample 1 prepared in step (2) was mixed with 5 g of single-layer graphene oxide, 5 g of polypyrrole, and 2 g of solid electrolyte Li with a particle size of 100 nm. 7 La 3 Zr 2 O 12 Adding into distilled water, stirring and strong ultrasonic mixing treatment, to obtain a mixed solution with a solid content of 5wt%; spraying self-assembly treatment on the mixed solution to obtain phosphorus carbon / graphene composite microspheres; the parameters in the spraying process are: air inlet temperature of 130°C, fan frequency of 70Hz, and feed rate of 600mL / h;

[0086] (4) The phosphorus-carbon / graphene composite microspheres obtained after the above-mentioned spray self-assembly were mixed with 15 g of nano-Li 7La 3 Zr 2 O 12 of the second solid electrolyte, 50 g of distilled water was added, and the mixture was stirred for 2 h and then dried. The dried sample was kept at 250 ° C for 2 h under a nitrogen atmosphere to obtain a composite phosphorus-carbon negative electrode material coated with a solid electrolyte.

[0087] (5) 3.2 g of the composite phosphorus-carbon material (negative electrode active material) was mixed with 0.4 g of a binder (PVDF) and 0.4 g of a conductive agent Super-P, and slurried using N-methylpyrrolidone (NMP) as a solvent. The mixture was evenly coated on a copper foil and dried in an oven at 120°C for 12 h. The negative electrode sheet was then punched into a 13 mm diameter disc.

[0088] In a glove box filled with argon, a lithium metal sheet was used as the counter electrode, the electrolyte was 1.0M Li PF6 (EC / DEC = 1:1 volume ratio), and the diaphragm was a polyethylene diaphragm to assemble a CR2032 button cell. The battery was tested at room temperature using a blue battery tester, with a current density of 20mA / g and a voltage range of 0 to 2.5V for charge and discharge tests.

[0089] Example 6

[0090] The method for preparing the negative electrode sheet comprises the following steps:

[0091] (1) Take 10g of single-walled carbon nanotubes, add 100mL of hydrochloric acid solution (molar concentration of 1.5mol / L), and stir evenly for 4h; filter and wash the carbon nanotube mixture several times until the solution pH = 7; add 3g of the first solid electrolyte Li with a particle size of 100nm 7 La 3 Zr 2 O 12 Add 50g of distilled water, stir evenly and then perform ultrasonic treatment;

[0092] (2) adding 60 g of red phosphorus to the composite solution, stirring again and transferring to a ball mill, and ball milling for 5 h under a nitrogen atmosphere to obtain a composite sample 1;

[0093] (3) The composite sample 1 prepared in step (2) was mixed with 2 g of single-layer graphene oxide, 5 g of polypyrrole, and 2 g of solid electrolyte Li with a particle size of 100 nm. 7 La 3 Zr 2 O 12 Adding into distilled water, stirring and strong ultrasonic mixing treatment, to obtain a mixed solution with a solid content of 5wt%; spraying self-assembly treatment on the mixed solution to obtain phosphorus carbon / graphene composite microspheres; the parameters in the spraying process are: air inlet temperature of 130°C, fan frequency of 70Hz, and feed rate of 600mL / h;

[0094] (4) The phosphorus-carbon / graphene composite microspheres obtained after the above-mentioned spray self-assembly were mixed with 15 g of nano-Li 7La 3 Zr 2 O 12 of the second solid electrolyte, 50 g of distilled water was added, and the mixture was stirred for 2 h and then dried. The dried sample was kept at 250 ° C for 2 h under a nitrogen atmosphere to obtain a composite phosphorus-carbon negative electrode material coated with a solid electrolyte.

[0095] (5) 3.2 g of the composite phosphorus-carbon material (negative electrode active material) was mixed with 0.4 g of a binder (PVDF) and 0.4 g of a conductive agent Super-P, and slurried using N-methylpyrrolidone (NMP) as a solvent. The mixture was evenly coated on a copper foil and dried in an oven at 120°C for 12 h. The negative electrode sheet was then punched into a 13 mm diameter disc.

[0096] In a glove box filled with argon, a lithium metal sheet was used as the counter electrode, the electrolyte was 1.0M Li PF6 (EC / DEC = 1:1 volume ratio), and the diaphragm was a polyethylene diaphragm to assemble a CR2032 button cell. The battery was tested at room temperature using a blue battery tester, with a current density of 20mA / g and a voltage range of 0 to 2.5V for charge and discharge tests.

[0097] Example 7

[0098] The method for preparing the negative electrode sheet comprises the following steps:

[0099] (1) Take 10g of single-walled carbon nanotubes, add 100mL of hydrochloric acid solution (molar concentration of 1.5mol / L), and stir evenly for 4h; filter and wash the carbon nanotube mixture several times until the solution pH = 7; add 3g of the first solid electrolyte Li with a particle size of 100nm 7 La 3 Zr 2 O 12 Add 50g of distilled water, stir evenly and then perform ultrasonic treatment;

[0100] (2) adding 60 g of red phosphorus to the composite solution, stirring again and transferring to a ball mill, and ball milling for 5 h under a nitrogen atmosphere to obtain a composite sample 1;

[0101] (3) The composite sample 1 prepared in step (2) was mixed with 9 g of single-layer graphene oxide, 5 g of polypyrrole, and 2 g of solid electrolyte Li with a particle size of 100 nm. 7 La 3 Zr 2 O 12 Adding into distilled water, stirring and strong ultrasonic mixing treatment, to obtain a mixed solution with a solid content of 5wt%; spraying self-assembly treatment on the mixed solution to obtain phosphorus carbon / graphene composite microspheres; the parameters in the spraying process are: air inlet temperature of 130°C, fan frequency of 70Hz, and feed rate of 600mL / h;

[0102] (4) The phosphorus-carbon / graphene composite microspheres obtained after the above-mentioned spray self-assembly were mixed with 15 g of nano-Li 7La 3 Zr 2 O 12 of the second solid electrolyte, 50 g of distilled water was added, and the mixture was stirred for 2 h and then dried. The dried sample was kept at 250 ° C for 2 h under a nitrogen atmosphere to obtain a composite phosphorus-carbon negative electrode material coated with a solid electrolyte.

[0103] (5) 3.2 g of the composite phosphorus-carbon material (negative electrode active material) was mixed with 0.4 g of a binder (PVDF) and 0.4 g of a conductive agent Super-P, and slurried using N-methylpyrrolidone (NMP) as a solvent. The mixture was evenly coated on a copper foil and dried in an oven at 120°C for 12 h. The negative electrode sheet was then punched into a 13 mm diameter disc.

[0104] In a glove box filled with argon, a lithium metal sheet was used as the counter electrode, the electrolyte was 1.0M Li PF6 (EC / DEC = 1:1 volume ratio), and the diaphragm was a polyethylene diaphragm to assemble a CR2032 button cell. The battery was tested at room temperature using a blue battery tester, with a current density of 20mA / g and a voltage range of 0 to 2.5V for charge and discharge tests.

[0105] Example 8

[0106] The method for preparing the negative electrode sheet comprises the following steps:

[0107] (1) Take 10g of single-walled carbon nanotubes, add 100mL of hydrochloric acid solution (molar concentration of 1.5mol / L), and stir evenly for 4h; filter and wash the carbon nanotube mixture several times until the solution pH = 7; add 3g of the first solid electrolyte Li with a particle size of 100nm 7 La 3 Zr 2 O 12 Add 50g of distilled water, stir evenly and then perform ultrasonic treatment;

[0108] (2) adding 60 g of red phosphorus to the composite solution, stirring again and transferring to a ball mill, and ball milling for 5 h under a nitrogen atmosphere to obtain a composite sample 1;

[0109] (3) The composite sample 1 prepared in step (2) was mixed with 5 g of single-layer graphene oxide, 5 g of polypyrrole, and 2 g of solid electrolyte Li with a particle size of 100 nm. 7 La 3 Zr 2 O 12 Adding into distilled water, stirring and strong ultrasonic mixing treatment, to obtain a mixed solution with a solid content of 5wt%; spraying self-assembly treatment on the mixed solution to obtain phosphorus carbon / graphene composite microspheres; the parameters in the spraying process are: air inlet temperature of 130°C, fan frequency of 70Hz, and feed rate of 600mL / h;

[0110] (4) The phosphorus-carbon / graphene composite microspheres obtained by the spray self-assembly are mixed with 9g nano-Li 7 La 3 Zr 2 O 12The mixture was mixed, 50 g of distilled water was added, the mixture was stirred for 2 h and then dried. The dried sample was kept at 250° C. for 2 h under a nitrogen atmosphere to obtain a composite phosphorus-carbon negative electrode material coated with a solid electrolyte.

[0111] (5) 3.2 g of the composite phosphorus-carbon material (negative electrode active material) was mixed with 0.4 g of a binder (PVDF) and 0.4 g of a conductive agent Super-P, and slurried using N-methylpyrrolidone (NMP) as a solvent. The mixture was evenly coated on a copper foil and dried in an oven at 120°C for 12 h. The negative electrode sheet was then punched into a 13 mm diameter disc.

[0112] In a glove box filled with argon, a metal lithium sheet was used as the counter electrode and the electrolyte was 1.0 M LiPF 6 (EC / DEC = 1:1 volume ratio), the separator is a polyethylene separator, and assembled into a CR2032 button cell. At room temperature, the battery was tested using a blue battery tester, the test conditions were a current density of 20 mA / g, and the voltage range of the charge and discharge test was 0 to 2.5 V.

[0113] Example 9

[0114] The method for preparing the negative electrode sheet comprises the following steps:

[0115] (1) Take 10g of single-walled carbon nanotubes, add 100mL of hydrochloric acid solution (molar concentration of 1.5mol / L), and stir evenly for 4h; filter and wash the carbon nanotube mixture several times until the solution pH = 7; add 3g of the first solid electrolyte Li with a particle size of 100nm 7 La 3 Zr 2 O 12 Add 50g of distilled water, stir evenly and then perform ultrasonic treatment;

[0116] (2) adding 60 g of red phosphorus to the composite solution, stirring again and transferring to a ball mill, and ball milling for 5 h under a nitrogen atmosphere to obtain a composite sample 1;

[0117] (3) The composite sample 1 prepared in step (2) was mixed with 5 g of single-layer graphene oxide, 5 g of polypyrrole, and 2 g of solid electrolyte Li with a particle size of 100 nm. 7 La 3 Zr 2 O 12 Adding into distilled water, stirring and strong ultrasonic mixing treatment, to obtain a mixed solution with a solid content of 5wt%; spraying self-assembly treatment on the mixed solution to obtain phosphorus carbon / graphene composite microspheres; the parameters in the spraying process are: air inlet temperature of 130°C, fan frequency of 70Hz, and feed rate of 600mL / h;

[0118] (4) The phosphorus-carbon / graphene composite microspheres obtained by the spray self-assembly are mixed with 20 g of nano-Li 7 La 3 Zr 2 O 12 The mixture was mixed, 50 g of distilled water was added, the mixture was stirred for 2 h and then dried. The dried sample was kept at 250° C. for 2 h under a nitrogen atmosphere to obtain a composite phosphorus-carbon negative electrode material coated with a solid electrolyte.

[0119] (5) 3.2 g of the composite phosphorus-carbon material (negative electrode active material) was mixed with 0.4 g of a binder (PVDF) and 0.4 g of a conductive agent Super-P, and slurried using N-methylpyrrolidone (NMP) as a solvent. The mixture was evenly coated on a copper foil and dried in an oven at 120°C for 12 h. The negative electrode sheet was then punched into a 13 mm diameter disc.

[0120] In a glove box filled with argon, a metal lithium sheet was used as the counter electrode and the electrolyte was 1.0 M LiPF 6 (EC / DEC = 1:1 volume ratio), the separator is a polyethylene separator, and assembled into a CR2032 button cell. At room temperature, the battery was tested using a blue battery tester, the test conditions were a current density of 20 mA / g, and the voltage range of the charge and discharge test was 0 to 2.5 V.

[0121] Example 10

[0122] The method for preparing the negative electrode sheet comprises the following steps:

[0123] (1) Take 10g of single-walled carbon nanotubes, add 100mL of hydrochloric acid solution (molar concentration of 1.5mol / L), and stir evenly for 4h; filter and wash the carbon nanotube mixture several times until the solution pH = 7; add 3g of solid electrolyte Li with a particle size of 150nm 0.33 La 0.56 TiO 3 Add 50g of distilled water, stir evenly and then perform ultrasonic treatment;

[0124] (2) adding 60 g of black phosphorus to the composite solution, stirring evenly again, and then transferring to a ball milling jar, and ball milling for 5 h under a nitrogen atmosphere to obtain a composite sample 1;

[0125] (3) The composite sample 1 prepared in step (2) was mixed with 5 g of graphene oxide, 5 g of polyaniline, and 2 g of solid electrolyte Li with a particle size of 150 nm. 0.33 La 0.56 TiO 3Adding into distilled water, stirring and strong ultrasonic mixing treatment, to obtain a mixed solution with a solid content of 3wt%; spraying self-assembly treatment on the mixed solution to obtain phosphorus carbon / graphene composite microspheres; the parameters in the spraying process are: air inlet temperature of 130°C, fan frequency of 70Hz, and feed rate of 600mL / h;

[0126] (4) The phosphorus-carbon / graphene composite microspheres obtained by the spray self-assembly are mixed with 15 g of a second solid electrolyte Li with a particle size of 150 nm. 0.33 La 0.56 TiO 3 The mixture was mixed, 50 g of distilled water was added, and the mixture was dried after stirring for 2 h. The dried sample was kept at 200° C. for 2 h under a nitrogen atmosphere to obtain a composite phosphorus-carbon negative electrode material coated with a solid electrolyte.

[0127] (5) 3.2 g of the composite phosphorus-carbon material (negative electrode active material) was mixed with 0.4 g of a binder (PVDF) and 0.4 g of a conductive agent Super-P, and slurried using NMP as a solvent. The mixture was evenly coated on a copper foil and dried in an oven at 120°C for 12 h. The negative electrode sheet was then punched into a 13 mm diameter disc.

[0128] In a glove box filled with argon, a metal lithium sheet was used as the counter electrode and the electrolyte was 1.0 M LiPF 6 (EC / DEC = 1:1 volume ratio), the separator is a polyethylene separator, and assembled into a CR2032 button cell. At room temperature, the battery was tested using a blue battery tester, the test conditions were a current density of 20 mA / g, and the voltage range of the charge and discharge test was 0 to 2.5 V.

[0129] Embodiment 11

[0130] The method for preparing the negative electrode sheet comprises the following steps:

[0131] (1) 10 g of single-walled carbon nanotubes were added to 100 mL of hydrochloric acid solution (molar concentration of 3 mol / L), and stirred evenly for 5 h; the carbon nanotube mixture was filtered and washed with water for multiple times until the solution pH was 7; 3 g of the first solid electrolyte Li with a particle size of 150 nm was added 1.3 Al 0.3 Ti 1.7 (PO 4 ) 3 Add 50g of distilled water, stir evenly and then perform ultrasonic treatment;

[0132] (2) adding 60 g of red phosphorus to the composite solution, stirring again and transferring to a ball mill, and ball milling for 5 h under a nitrogen atmosphere to obtain a composite sample 1;

[0133] (3) The composite sample 1 prepared in step (2) was mixed with 5 g of graphene oxide, 5 g of polypyrrole, and 2 g of a first solid electrolyte Li having a particle size of 150 nm. 1.3 A l 0.3 T i 1.7 (PO 4 ) 3 Adding into distilled water, stirring and strong ultrasonic mixing treatment, to obtain a mixed solution with a solid content of 3wt%; spraying self-assembly treatment on the mixed solution to obtain phosphorus carbon / graphene composite microspheres; the parameters in the spraying process are: air inlet temperature of 130°C, fan frequency of 70Hz, and feed rate of 600mL / h;

[0134] (4) The phosphorus-carbon / graphene composite microspheres obtained by the spray self-assembly are mixed with 15 g of a second solid electrolyte Li with a particle size of 150 nm. 0.33 La 0.56 T i 3 Mix, add 50 g of distilled water, stir for 2 h and then dry, and keep the dried sample at 300 ° C for 1 h under a nitrogen atmosphere to obtain a composite phosphorus-carbon negative electrode material coated with a solid electrolyte;

[0135] (5) 3.2 g of the composite phosphorus-carbon material (negative electrode active material) was mixed with 0.4 g of a binder (PVDF) and 0.4 g of a conductive agent Super-P, homogenized using NMP solvent, and evenly coated on a copper foil. After drying in an oven at 120°C for 12 h, the negative electrode sheet was punched into a 13 mm diameter disc.

[0136] In a glove box filled with argon, a metal lithium sheet was used as the counter electrode and the electrolyte was 1.0 M Li PF 6 (EC / DEC = 1:1 volume ratio), the separator is a polyethylene separator, and assembled into a CR2032 button cell. At room temperature, the battery was tested using a blue battery tester, the test conditions were a current density of 20 mA / g, and the voltage range of the charge and discharge test was 0 to 2.5 V.

[0137] Example 12

[0138] The method for preparing the negative electrode sheet comprises the following steps:

[0139] (1) 10 g of single-walled carbon nanotubes were added to 100 mL of hydrochloric acid solution (molar concentration of 3 mol / L), and stirred evenly for 5 h; the carbon nanotube mixture was filtered and washed with water for multiple times until the solution pH was 7; 3 g of the first solid electrolyte Na with a particle size of 150 nm was added 2 Zr 2 P 2 O 12 Add 50g of distilled water, stir evenly and then perform ultrasonic treatment;

[0140] (2) adding 50 g of black phosphorus to the composite solution, stirring evenly again, transferring to a ball mill, and ball milling for 5 h under a nitrogen atmosphere to obtain a composite sample 1;

[0141] (3) The composite sample 1 prepared in step (2) is mixed with 5 g of graphene oxide, 5 g of polyacetylene, and 2 g of a first solid electrolyte Na with a particle size of 150 nm. 2 Zr 2 P 2 O 12 Adding into distilled water, stirring and strong ultrasonic mixing treatment, to obtain a mixed solution with a solid content of 3wt%; spraying self-assembly treatment on the mixed solution to obtain phosphorus carbon / graphene composite microspheres; the parameters in the spraying process are: air inlet temperature of 130°C, fan frequency of 70Hz, and feed rate of 600mL / h;

[0142] (4) The phosphorus-carbon / graphene composite microspheres obtained by the spray self-assembly are mixed with 15 g of a second solid electrolyte Na with a particle size of 150 nm. 2 Zr 2 P 2 O 12 The mixture was mixed, 50 g of distilled water was added, and the mixture was dried after stirring for 2 h. The dried sample was kept at 200° C. for 1.5 h under a nitrogen atmosphere to obtain a composite phosphorus-carbon negative electrode material coated with a solid electrolyte.

[0143] (5) 3.2 g of the composite phosphorus-carbon material (negative electrode active material) was mixed with 0.4 g of a binder (PVDF) and 0.4 g of a conductive agent Super-P, homogenized using NMP solvent, and evenly coated on a copper foil. After drying in an oven at 120°C for 12 h, the negative electrode sheet was punched into a 13 mm diameter disc.

[0144] In a glove box filled with argon, a sodium metal sheet was used as the counter electrode and the electrolyte was 1.0 M NaPF 6 (EC / DEC = 1:1 volume ratio), the separator is glass fiber (GF / F), assembled into CR2032 button cells. At room temperature, the battery was tested using a blue battery tester, the test conditions were a current density of 20mA / g, and the voltage range of the charge and discharge test was 0-2.5V.

[0145] Comparative Example 1

[0146] The method for preparing the negative electrode sheet comprises the following steps:

[0147] (1) Take 10g of single-walled carbon nanotubes, add 100mL of hydrochloric acid solution (molar concentration of 1.5mol / L), and stir evenly for 4h; filter and wash the carbon nanotube mixture several times until the pH of the solution is 7; add 60g of red phosphorus, stir evenly again, transfer to a ball mill, and ball mill for 9h under a nitrogen atmosphere to obtain a composite sample 1;

[0148] (2) adding the composite sample 1 prepared in step (1) together with 5 g of monolayer graphene oxide and 5 g of polypyrrole into distilled water, stirring and performing strong ultrasonic mixing treatment to obtain a mixed solution with a solid content of 5 wt%; spraying the mixed solution with self-assembly to obtain phosphorus carbon / graphene composite microspheres; the parameters during the spraying process are: the air inlet temperature is 130° C., the fan frequency is 70 Hz, and the feed rate is 600 mL / h;

[0149] (3) The phosphorus-carbon / graphene composite microspheres obtained after the above-mentioned spray self-assembly are kept at 250° C. for 2 h in a nitrogen atmosphere to obtain a composite phosphorus-carbon negative electrode material.

[0150] (4) 3.2 g of the composite phosphorus-carbon negative electrode material prepared above was mixed with 0.4 g of a binder (PVDF) and 0.4 g of a conductive agent Super-P, homogenized using NMP solvent, and evenly coated on a copper foil. After drying in an oven at 120° C. for 12 h, the negative electrode sheet was punched into a 13 mm diameter disc;

[0151] In a glove box filled with argon, a metal lithium sheet was used as the counter electrode and the electrolyte was 1.0 M NaPF 6 (EC / DEC = 1:1 volume ratio), the separator is glass fiber (GF / F), assembled into CR2032 button cells. At room temperature, the battery was tested using a blue battery tester, the test conditions were a current density of 20mA / g, and the voltage range of the charge and discharge test was 0-2.5V.

[0152] Comparative Example 2

[0153] The method for preparing the negative electrode sheet comprises the following steps:

[0154] (1) Take 10g of single-walled carbon nanotubes, add 100mL of hydrochloric acid solution (molar concentration of 1.5mol / L), and stir evenly for 4h; filter and wash the carbon nanotube mixture several times until the solution pH = 7; add 3g of the first solid electrolyte Li with a particle size of 100nm 7 La 3 Zr 2 O 12 Add 50g of distilled water, stir evenly and then perform ultrasonic treatment;

[0155] (2) adding 60 g of red phosphorus to the composite solution, stirring again and transferring to a ball mill, and ball milling for 5 h under a nitrogen atmosphere to obtain a composite sample 1;

[0156] (3) The ball-milled composite sample 1 was mixed with 17 g of nano-Li 7 La 3 Zr 2 O 12 The mixture was mixed, 50 g of distilled water was added, the mixture was stirred for 2 h and then dried. The dried sample was kept at 250° C. for 2 h under a nitrogen atmosphere to obtain a composite phosphorus-carbon negative electrode material coated with a solid electrolyte.

[0157] (4) 3.2 g of the composite phosphorus-carbon material was mixed with 0.4 g of a binder (PVDF) and 0.4 g of a conductive agent Super-P, and slurried using N-methylpyrrolidone (NMP) as a solvent. The mixture was evenly coated on a copper foil and dried in an oven at 120°C for 12 h. The negative electrode was then punched into a 13 mm diameter disc to obtain a negative electrode sheet.

[0158] In a glove box filled with argon, a metal lithium sheet was used as the counter electrode and the electrolyte was 1.0 M LiPF 6 (EC / DEC = 1:1 volume ratio), the separator is a polyethylene separator, and assembled into a CR2032 button cell. At room temperature, the battery was tested using a blue battery tester, the test conditions were a current density of 20 mA / g, and the voltage range of the charge and discharge test was 0 to 2.5 V.

[0159] Comparative Example 3

[0160] (1) Take 10g of single-walled carbon nanotubes, add 100mL of hydrochloric acid solution (molar concentration of 1.5mol / L), and stir evenly for 5h; filter and wash the carbon nanotube mixture several times until the pH of the solution is 7; add 60g of red phosphorus to the above composite solution, stir evenly again, transfer to a ball mill, and ball mill for 5h under a nitrogen atmosphere to obtain a composite sample 1;

[0161] (2) adding the composite sample 1 prepared in step (1) together with 5 g of monolayer graphene oxide and 5 g of polypyrrole into distilled water, stirring and performing strong ultrasonic mixing treatment to obtain a mixed solution with a solid content of 5 wt%; spraying the mixed solution with self-assembly to obtain phosphorus carbon / graphene composite microspheres; the parameters during the spraying process are: the air inlet temperature is 130° C., the fan frequency is 70 Hz, and the feed rate is 600 mL / h;

[0162] (3) The phosphorus-carbon / graphene composite microspheres obtained by the spray self-assembly are mixed with 15 g of solid electrolyte Li with a particle size of 150 nm. 0.33 La 0.56 T i 3The mixture was mixed, 50 g of distilled water was added, and the mixture was dried after stirring for 2 h. The dried sample was kept at 200° C. for 2 h under a nitrogen atmosphere to obtain a composite phosphorus-carbon negative electrode material coated with a solid electrolyte.

[0163] (4) 3.2 g of the composite phosphorus-carbon material was mixed with 0.4 g of a binder (PVDF) and 0.4 g of a conductive agent Super-P, and slurried using N-methylpyrrolidone (NMP) as a solvent. The mixture was evenly coated on a copper foil and dried in an oven at 120°C for 12 h. The negative electrode was then punched into a 13 mm diameter disc to obtain a negative electrode sheet.

[0164] In a glove box filled with argon, a metal lithium sheet was used as the counter electrode and the electrolyte was 1.0 M Li PF 6 (EC / DEC = 1:1 volume ratio), the separator is a polyethylene separator, and assembled into a CR2032 button cell. At room temperature, the battery was tested using a blue battery tester, the test conditions were a current density of 20 mA / g, and the voltage range of the charge and discharge test was 0 to 2.5 V.

[0165] The phosphorus-carbon negative electrode materials synthesized according to the methods of the above embodiments and comparative examples were assembled into button cells and the electrochemical performance was tested. The data are shown in Table 1 below.

[0166] Table 1 Battery performance test data

[0167] Serial number First cycle charge capacity (mAh / g) First coulombic efficiency (%) Example 1 1480 90.0% Example 2 1515 90.6% Example 3 1490 91.2% Example 4 1321 89.0% Example 5 1510 91.0% Example 6 1406 88.0% Example 7 1520 92.0% Example 8 1460 88.5% Example 9 1490 91.3% Example 10 1485 90.4% Embodiment 11 1550 92.0% Example 12 1410 91.8% Comparative Example 1 1030 82.7% Comparative Example 2 1165 89.0% Comparative Example 3 1250 85.0%

[0168] By the attached Figure 2 From the comparison results of the cycle performance of the batteries assembled with the composite phosphorus-carbon material prepared in Example 1 and the materials prepared in Comparative Examples 1 and 2, the composite phosphorus-carbon material of Example 1 has the best cycle performance. On the one hand, this is because the interface stability between the solid electrolyte and the phosphorus-carbon negative electrode is good, and on the other hand, graphene can effectively inhibit the expansion of the phosphorus-carbon material, ensuring a low electrode thickness expansion rate and improving the stability of the electrode structure.

[0169] It can be seen from the test data in Table 1 that, compared with Comparative Example 1, the solid electrolyte-coated phosphorus-carbon composite material provided in the embodiment of the present invention has better contact interface stability with the solid electrolyte and lower contact resistance, which is beneficial to improving the lithium / sodium insertion capacity of the phosphorus-carbon material; compared with Comparative Example 2, the graphene intermediate layer in the embodiment not only effectively connects the phosphorus-carbon inner core with the solid electrolyte outer layer, but also can effectively accommodate and inhibit the expansion of phosphorus-carbon, prevent more side reactions from occurring when phosphorus-carbon contacts the electrolyte, and effectively improve the cycle life of the phosphorus-carbon material; compared with Comparative Example 3, the solid electrolyte, carbon nanotubes and graphene jointly effectively construct an ion / electron conductive network system, which is beneficial to the internal transmission of ions and the conduction of electrons, and improves the cycle performance and coulombic efficiency of the composite phosphorus-carbon material.

[0170] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A negative electrode active material, characterized in that: It comprises a composite phosphorus-carbon material core and a solid electrolyte coating layer coated on the surface of the composite phosphorus-carbon material core; the composite phosphorus-carbon material comprises a first solid electrolyte, a phosphorus source, carbon nanotubes, graphene, and a conductive polymer; and the solid electrolyte coating layer comprises a second solid electrolyte.

2. The negative electrode active material according to claim 1, characterized in that In the composite phosphorus-carbon material, the first solid electrolyte is attached to the surface of the phosphorus source, and the carbon nanotubes are dispersed between the phosphorus source particles; the graphene is coated on the surface of the inner core formed by the phosphorus source particles and the carbon nanotubes, and is connected to the solid electrolyte coating layer.

3. The negative electrode active material according to claim 1, characterized in that The thickness of the solid electrolyte coating layer is 50nm-1μm; preferably, the particle size of the composite phosphorus-carbon material inner shell is 1-20μm.

4. The negative electrode active material according to claim 1, characterized in that The mass ratio of phosphorus source, carbon nanotubes, graphene, first solid electrolyte and conductive polymer is (40-70):(1-20):(1-20):(2-30):(1-10); preferably 60:(5-13):(5-9):(5-10):

5.

5. The negative electrode active material according to claim 1, characterized in that The diameter of the carbon nanotubes is ≤2 μm; preferably, the phosphorus source includes one or any combination of red phosphorus and black phosphorus; Preferably, the first solid electrolyte and the second solid electrolyte independently include inorganic metal oxide solid electrolytes; preferably one or any combination of perovskite solid electrolyte materials, garnet solid electrolyte materials, NASICON solid electrolyte materials, and LIS ICON solid electrolyte materials; preferably, the particle size is between 1-500 nm; Preferably, the conductive polymer includes one or any combination of polythiophene, polypyrrole, polyaniline, PEDOT, and polyacetylene; Preferably, the graphene is a few-layer graphene oxide, and the number of graphene oxide sheets is less than 5.

6. A method for preparing the negative electrode active material according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: (1) adding a first solid electrolyte and a phosphorus source to carbon nanotubes washed to be neutral, and then ball milling to obtain nano-phosphorus-carbon particles coated with carbon nanotubes; (2) adding the ball-milled nano-phosphorus-carbon particles, graphene oxide, a first solid electrolyte, and a conductive polymer to a solvent for mixing; spray drying the mixed solution to obtain a composite phosphorus-carbon material; (3) adding a second solid electrolyte and a solvent to the composite phosphorus-carbon material obtained after the spray drying, stirring evenly, and then drying; keeping the dried sample warm in a nitrogen atmosphere to obtain a negative electrode active material; Preferably, the mass ratio of the first solid electrolyte in step (1) to the first solid electrolyte in step (2) is (3-8):2; preferably 5:2; Preferably, the mass ratio of the second solid electrolyte to the first solid electrolyte in step (2) is (9-20):2; preferably 15:

2.

7. The method for preparing the negative electrode active material according to claim 6, characterized in that: The specific steps of step 1) are: mixing carbon nanotubes with hydrochloric acid solution, and stirring evenly for 1-5 hours; filtering the carbon nanotube mixture with water, and washing with water until the solution is neutral; adding the first solid electrolyte particles to the carbon nanotube slurry solution, stirring evenly, and then ultrasonically treating to obtain a composite solution; adding a phosphorus source to the above composite solution, stirring evenly, and then transferring to a ball milling jar, and ball milling for 1-10 hours under an inert atmosphere to obtain carbon nanotube-coated nano-phosphorus-carbon particles; Preferably, the concentration of the hydrochloric acid solution is 0.1-10 mol / L; Preferably, the spray drying process in step 2) is as follows: the solid content of the spray solution is 1wt%-20wt%, the spray drying temperature is 100-250°C, the fan frequency is 50-200Hz, and the feed flow rate is 100-1000mL / h; Preferably, the insulation condition of step 3) is 200-300° C. for 1-2 h.

8. A negative electrode sheet, characterized in that: The invention comprises the negative electrode active material according to any one of claims 1 to 5, a binder, and a conductive agent; preferably, the binder is PVDF; preferably, the conductive agent is Super-P.

9. A method for preparing a negative electrode sheet, characterized in that: The method comprises the following steps: mixing the negative electrode active material with a binder and a conductive agent, using N-methylpyrrolidone as a solvent for homogenization, uniformly coating the mixture on the negative electrode current collector, and drying the mixture to obtain the mixture.

10. A battery, characterized in that: It comprises the negative electrode sheet, the positive electrode sheet and the separator as claimed in claim 8.

Citation Information

Cited By

  • Preparation method of secondary battery with high energy density and high safety

    CN119695293A

  • Tin-carbon negative electrode material coated with mixed conductive polymer, preparation method of tin-carbon negative electrode material, negative electrode plate, sodium-ion battery and power-related equipment

    CN119764410A