Sodium battery positive electrode material and preparation method and application thereof

By introducing surfactant into the positive electrode material of sodium ion battery and optimizing the mixing method, the balance problem of material morphology and specific surface area is solved, cycle stability and rate performance are improved, and the performance of sodium ion battery is improved.

CN118919691APending Publication Date: 2024-11-08三一红象电池有限公司 +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411112142.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

There is room for improvement in the circulation stability and rate performance of existing sodium ion battery positive electrode materials, and the balance between material morphology and specific surface area is difficult to achieve.

Method used

By introducing surfactant as a stabilizer and optimizing the raw material mixing method, the sodium electropositive electrode material is prepared by step-by-step mixing and spray-drying method to form homogenized particles, and the morphology and chemical stability of the material are optimized.

Benefits of technology

It significantly improves the cycle stability, rate performance and volume energy density of sodium ion batteries. The material has good chemical and thermal stability and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919691A_ABST
    Figure CN118919691A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of secondary batteries, in particular to a sodium battery positive electrode material and a preparation method and application thereof. The preparation method of the sodium battery positive electrode material comprises the following steps: S1, mixing a carbon source, a vanadium source, a manganese source, a sodium source, a surfactant and water to obtain a solution A; preparing a solution B from a phosphorus source, a surfactant and water; mixing the solution A and the solution B for reaction to obtain mixed slurry; s2, carrying out spray drying on the mixed slurry to obtain a precursor; and S3, sequentially carrying out pre-sintering treatment and sintering treatment on the precursor to obtain the sodium battery positive electrode material. The surface active agent is introduced into a raw material system to serve as a stabilizer, meanwhile, the mixing mode of the raw materials is optimized, the morphology of the composite material can be improved, the stability of the material is improved, and the composite material finally has good conductivity, cycling stability and rate capability and has good application prospects in the field of sodium-ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of secondary batteries, and in particular to a sodium battery positive electrode material and a preparation method and application thereof. Background Art

[0002] In order to reduce the use of fossil fuels, it is of great significance to develop renewable energy and corresponding new power batteries and efficient energy storage systems. At present, lithium-ion batteries have undoubtedly received the most attention, but sodium-ion batteries are expected to compete with lithium-ion batteries in the future due to their abundant reserves and cost advantages, or they can complement lithium-ion batteries in terms of application.

[0003] The positive electrode of sodium ion batteries can be divided into two categories: layered oxides and polyanions. The advantages of layered oxides are high capacity and multiple voltage platforms, but their disadvantages are slightly lower voltage platforms and unstable structures during cycling. Compared with layered oxides, polyanion-type positive electrode materials with sodium superion conductor (NASICON) structures have more stable structures and wider ion channels, and the inductive effect of polyanions gives the materials an adjustable working voltage, so they are expected to become a new generation of positive electrode materials for sodium ion batteries. Among them, sodium manganese vanadium phosphate has the advantages of high reversible capacity, high energy density, high working voltage, low cost and low toxicity, and is a very promising positive electrode material for sodium ion batteries.

[0004] Patent application CN 117855451 A discloses a sodium vanadium manganese phosphate composite material, a preparation method thereof and a sodium ion battery, which improves the conductivity and cycle stability of the material to a certain extent through the cooperation of a carbon matrix with a network structure and a carbon coating layer on the surface of the sodium vanadium manganese phosphate material; however, in fact, there is still room for further improvement in the comprehensive performance of the battery. Summary of the invention

[0005] The present invention provides a sodium battery positive electrode material and a preparation method and application thereof, so as to solve the above-mentioned defects in the prior art and further improve the cycle stability and rate performance of the composite material.

[0006] In a first aspect, the present invention provides a method for preparing a sodium positive electrode material, comprising: S1: mixing a carbon source, a vanadium source, a manganese source, a sodium source, a surfactant and water to obtain liquid A; mixing a phosphorus source, a surfactant and water to obtain liquid B; and then mixing liquid A and liquid B to react to obtain a mixed slurry; S2: spray drying the mixed slurry to obtain a precursor; S3: performing a pre-sintering treatment and a sintering treatment on the precursor in sequence to obtain the sodium battery positive electrode material.

[0007] According to a method for preparing a sodium positive electrode material provided by the present invention, the surfactant consists of polyvinyl pyrrolidone and / or hexadecyltrimethylammonium bromide.

[0008] According to a method for preparing a sodium positive electrode material provided by the present invention, based on the amount of water in the mixed slurry, 0.1 to 1 gram of the surfactant is added to every 200 milliliters of water.

[0009] According to a method for preparing a sodium positive electrode material provided by the present invention, the mass ratio of the A solution to the B solution is (6-8): (2-4).

[0010] According to a method for preparing a sodium battery positive electrode material provided by the present invention, the amount of surfactant in the A solution is greater than the amount of surfactant in the B solution.

[0011] According to a method for preparing a sodium battery positive electrode material provided by the present invention, the mass ratio of the surfactant in the A solution to the surfactant in the B solution is (2-4):1.

[0012] According to a method for preparing a sodium positive electrode material provided by the present invention, the molar ratio of metal elements in the carbon source, vanadium source, manganese source and sodium source is (18-22): (1-2): (0.3-0.7): (3-4); and / or the molar ratio of metal elements in the sodium source and phosphorus source is 3.4-3.6:3.

[0013] According to a method for preparing a sodium positive electrode material provided by the present invention, the sodium source is one or more of sodium carbonate, sodium bicarbonate, sodium dihydrogen phosphate, sodium acetate and sodium oxalate.

[0014] According to a method for preparing a sodium battery positive electrode material provided by the present invention, the manganese source is one or more of manganese acetate, manganese oxalate and manganese carbonate.

[0015] According to a method for preparing a sodium battery positive electrode material provided by the present invention, the vanadium source is vanadium pentoxide and / or ammonium metavanadate.

[0016] According to a method for preparing a sodium positive electrode material provided by the present invention, the phosphorus source is one or more of ammonium dihydrogen phosphate, phosphoric acid and sodium dihydrogen phosphate.

[0017] According to a method for preparing a sodium positive electrode material provided by the present invention, the carbon source is one or more of citric acid, glucose, sucrose, oxalic acid and ascorbic acid.

[0018] According to a method for preparing a sodium positive electrode material provided by the present invention, in S2, during the spray drying, the outlet temperature is controlled to be 105 to 120 degrees Celsius.

[0019] According to a method for preparing a sodium positive electrode material provided by the present invention, S3 comprises: pre-sintering the precursor at 300-400 degrees Celsius in an inert gas atmosphere or a reducing gas atmosphere, and then sintering it at 800-900 degrees Celsius.

[0020] In a second aspect, the present invention provides a sodium positive electrode material, which is prepared by the above-mentioned preparation method.

[0021] According to a sodium battery positive electrode material provided by the present invention, the mass fraction of the amorphous carbon coating layer in the sodium battery positive electrode material is 5-10wt%, and the thickness of the amorphous carbon coating layer is 2-8 nanometers.

[0022] In a third aspect, the present invention provides a sodium ion battery comprising the above-mentioned positive electrode material.

[0023] A fourth aspect provides an electrical device comprising the sodium ion battery.

[0024] The sodium positive electrode material and its preparation method and application provided by the present invention can improve the morphology of the composite material and enhance the stability of the material by introducing a surfactant as a stabilizer into the raw material system and optimizing the mixing method of the raw materials, and finally take into account good conductivity, cycle stability, rate performance and volume energy density, and have good application prospects in the field of sodium ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0026] Figure 1 These are the XRD diagrams of NMVP@0.1gCTAB, NMVP@0.1gPVP and NMVP positive electrode materials obtained in Example 1, Example 4 and Comparative Example 1.

[0027] Figure 2 The amount of CTAB used in Example 1 is 0.1 g of Na 3.5 Mn 0.5 V 1.5 (PO 4 ) 3 @Scanning electron microscope image of C-CTAB positive electrode material.

[0028] Figure 3 The amount of CTAB used in Example 3 is 1 gram of Na 3.5 Mn 0.5 V1.5 (PO 4 ) 3 @Scanning electron microscope image of C-CTAB positive electrode material.

[0029] Figure 4 The amount of PVP used in Example 4 is 0.1 g of Na 3.5 Mn 0.5 V 1.5 (PO 4 ) 3 @Scanning electron microscope image of C-PVP positive electrode material.

[0030] Figure 5 The amount of PVP used in Example 6 is 1 gram of Na 3.5 Mn 0.5 V 1.5 (PO 4 ) 3 @Scanning electron microscope image of C-PVP positive electrode material.

[0031] Figure 6 The Na prepared by CTAB in Examples 1 to 3 3.5 Mn 0.5 V 1.5 (PO 4 ) 3 @C-CTAB positive electrode material half-cell cycle test curve at 0.2 coulomb, 1 coulomb, 5 coulomb current density; Figure 7 The Na prepared by PVP in Examples 4 to 6 3.5 Mn 0.5 V 1.5 (PO 4 ) 3 @C-PVP positive electrode material half-cell cycle test curve at 0.2 coulomb, 1 coulomb, 5 coulomb current density.

[0032] Figure 8 The Na prepared without surfactant in Comparative Example 1 3.5 Mn 0.5 V 1.5 (PO 4 ) 3 @C Cyclic test curve of half-cell prepared with positive electrode material at current density of 0.2 coulomb, 1 coulomb and 5 coulomb.

[0033] Fig. 9 The specific surface area test results of the sodium manganese vanadium phosphate composite materials prepared in the examples and comparative examples are shown. DETAILED DESCRIPTION

[0034] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the drawings of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] At present, existing technologies (such as patent application CN 117855451 A, etc.) have disclosed that the conductivity of the material is improved by forming a dense carbon coating layer, and the proportion of the raw metal source is adjusted to optimize the battery cycle performance. However, in fact, the above improvements have limited improvement in battery performance, and there is still room for further improvement in cycle stability, rate performance and volume energy density.

[0036] The present invention found that the reason why the performance of sodium-ion batteries is difficult to improve is related to the morphology of the material. Specifically, in order to maintain good cycle stability and high rate performance, the material is usually required to have a small or moderate particle size to provide a good ion diffusion path, which often means a large specific surface area; and in order to increase the compaction density of the positive electrode material or increase the loading of the positive electrode active material, the material is required to have a small specific surface area. There needs to be a trade-off between the two and a good balance.

[0037] The present invention further discovered that by introducing a surfactant as a stabilizer and optimizing the mixing method of the raw materials, it is possible to provide a good ion diffusion path and a smaller specific surface area to a certain extent, thereby improving the cycle stability, rate performance and volume energy density of the battery.

[0038] Based on this, the present invention has the following technical solutions: In a first aspect, the present invention provides a method for preparing a sodium positive electrode material, comprising: S1: mixing a carbon source, a vanadium source, a manganese source, a sodium source, a surfactant and water to obtain liquid A; mixing a phosphorus source, a surfactant and water to obtain liquid B; and then mixing liquid A and liquid B to react to obtain a mixed slurry; S2: spray drying the mixed slurry to obtain a precursor; S3: performing a pre-sintering treatment and a sintering treatment on the precursor in sequence to obtain the sodium battery positive electrode material.

[0039] The present invention finds that the raw materials are mixed in the above-mentioned step-by-step manner, combined with the synergistic effect between the above-mentioned constituent elements and the surfactant, and can be quickly adsorbed to the surface of the nanocrystal seeds during their initial formation, thereby effectively preventing the agglomeration of nanomaterials, thereby improving the material morphology and increasing the chemical stability and thermal stability of the nanomaterials.

[0040] Furthermore, the present invention finds that the conventional mixing method in the prior art, i.e., direct mixing of all elements, may affect battery performance due to uneven distribution of elements due to excessive local concentration; while the above-mentioned step-by-step mixing method, i.e., first mixing the carbon source, vanadium source, manganese source, sodium source and part of the surfactant, and then adding the phosphorus source and the remaining surfactant, because the addition of phosphate will form solid particles suspended in the solution with the aforementioned metal atoms, first forming a solution and then adding in steps can promote a more uniform mixing of the various elements, and can effectively control the grain growth process during the co-precipitation process, to obtain grains with a relatively concentrated / small particle size, which provides a good basis for the subsequent spray drying to prepare the precursor, and is conducive to obtaining a precursor with a uniform particle size.

[0041] In the present invention, when the carbon source, vanadium source, manganese source, sodium source, surfactant and water are mixed, and when the carbon source, surfactant and water are mixed, they are stirred at 60 to 150 degrees Celsius, the stirring speed is 300 to 1000 rpm, and the time is 1 to 6 hours. It should be noted that when mixing liquid A and liquid B, the temperature and speed of the two stirrings are independent of each other, and can be the same or different, and are not limited here.

[0042] In the present invention, when liquid A and liquid B are mixed for reaction, the reaction time is 3 to 5 hours.

[0043] According to a preferred embodiment provided by the present invention, the surfactant is composed of polyvinyl pyrrolidone (PVP for short) and / or cetyl trimethylammonium bromide (CTAB for short).

[0044] The present invention finds that when the introduced surfactant is hexadecyltrimethylammonium bromide, it can, to a certain extent, provide both a good ion diffusion path and a smaller specific surface area, and is particularly beneficial to the former, which can significantly improve the cycle stability and rate performance of the battery; and when the introduced surfactant is polyvinylpyrrolidone, it can, to a certain extent, provide both a good ion diffusion path and a smaller specific surface area, and is particularly beneficial to the latter, which can significantly improve the volume energy density of the battery.

[0045] According to a preferred embodiment provided by the present invention, based on the amount of water in the mixed slurry, 0.1 to 1 gram of the surfactant is added to every 200 milliliters of water. For example, 0.1 gram, 0.2 gram, 0.3 gram, 0.4 gram, 0.5 gram, 0.6 gram, 0.7 gram, 0.8 gram, 0.9 gram, or 1.0 gram of the surfactant can be added to every 200 milliliters of water.

[0046] Further preferably, based on the amount of water in the mixed slurry, 0.1 to 0.3 grams of the surfactant is added to every 200 milliliters of water.

[0047] According to a preferred embodiment provided by the present invention, the mass ratio of the liquid A to the liquid B is (6-8):(2-4).

[0048] The present invention finds that controlling the mass ratio of the liquid A to the liquid B within the above range is conducive to forming a uniform mixed liquid.

[0049] According to a preferred embodiment provided by the present invention, the amount of surfactant in the A liquid is greater than the amount of surfactant in the B liquid.

[0050] In the present invention, the amount of the surfactant added in steps is determined by the mass ratio of liquid A to liquid B; preferably, when the mass ratio of the surfactant in liquid A to the surfactant in liquid B is (2-4):1, it can help maintain an appropriate amount in the solution and promote uniform contact and mixing of the elements.

[0051] According to a preferred embodiment provided by the present invention, the molar ratio of the metal elements in the carbon source, vanadium source, manganese source and sodium source is (18~22):(1~2):(0.3~0.7):(3~4); and / or the molar ratio of the metal elements in the sodium source and phosphorus source is 3.4~3.6:3.

[0052] According to a preferred embodiment provided by the present invention, the sodium source is one or more of sodium carbonate, sodium bicarbonate, sodium dihydrogen phosphate, sodium acetate and sodium oxalate.

[0053] According to a preferred embodiment provided by the present invention, the manganese source is one or more of manganese acetate, manganese oxalate and manganese carbonate.

[0054] According to a preferred embodiment provided by the present invention, the vanadium source is vanadium pentoxide and / or ammonium metavanadate.

[0055] According to a preferred embodiment provided by the present invention, the phosphorus source is one or more of diammonium phosphate, phosphoric acid and sodium dihydrogen phosphate.

[0056] According to a preferred embodiment provided by the present invention, the carbon source is one or more of citric acid, glucose, sucrose, oxalic acid and ascorbic acid.

[0057] According to a preferred embodiment provided by the present invention, in S2, during the spray drying, the outlet temperature is controlled to be 105-120 degrees Celsius.

[0058] According to a preferred embodiment provided by the present invention, S3 includes: pre-sintering the precursor at 300-400 degrees Celsius in an inert gas atmosphere or a reducing gas atmosphere, and then sintering it at 800-900 degrees Celsius.

[0059] Further preferably, the inert gas atmosphere may be a nitrogen atmosphere and / or an argon atmosphere; the reducing gas atmosphere may be a nitrogen-hydrogen mixed gas or an argon-hydrogen mixed gas, wherein the volume fraction of hydrogen in the mixed gas is 3-20%.

[0060] More preferably, the pre-sintering time is 2 to 5 hours and the sintering time is 6 to 15 hours.

[0061] In the present invention, a composite material precursor is prepared by spray drying the mixed slurry, and then calcined at high temperature in a specific atmosphere to form an in-situ coated conductive carbon layer, thereby obtaining uniform particles. This method has the advantages of simple process and low cost, and is suitable for large-scale industrial production.

[0062] In a second aspect, the present invention provides a sodium positive electrode material, which is prepared by the above-mentioned preparation method.

[0063] According to a preferred embodiment provided by the present invention, the mass fraction of the amorphous carbon coating layer in the sodium battery positive electrode material is 5-10wt%, and the thickness of the amorphous carbon coating layer is 2-8 nanometers.

[0064] In a third aspect, the present invention provides a sodium ion battery comprising the above-mentioned positive electrode material.

[0065] A fourth aspect provides an electrical device comprising the sodium ion battery.

[0066] In the present invention, the sodium-ion positive electrode material is used as the positive electrode active material of a sodium-ion battery to prepare a sodium-ion battery. The phase change process is still stable under the electrochemical window of 2.5 to 3.8 volts, and the battery has excellent chemical stability and thermal stability.

[0067] In order to further illustrate the technical solution of the present invention, the present invention provides the following specific embodiments and comparative examples.

[0068] Unless otherwise specified, the various raw materials used in the examples and comparative examples are commercially available conventional raw materials, and the technical means used are conventional means well known to those skilled in the art.

[0069] Example 1

[0070] This embodiment provides a sodium positive electrode material, whose chemical formula is Na 3.5 Mn 0.5 V 1.5 (PO 4 )3 @C-CTAB, the preparation method thereof comprises: 22.22 g of citric acid monohydrate, 3.64 g of vanadium pentoxide, 3.27 g of manganese acetate tetrahydrate, 7.65 g of sodium acetate monohydrate and 0.07 g of CTAB were dissolved in 140 ml of a deionized water solution at 80 degrees Celsius, stirred for 1 hour to prepare liquid A, and 9.20 g of ammonium dihydrogen phosphate and 0.03 g of CTAB were dissolved in 60 ml of a deionized water solution at 80 degrees Celsius, stirred for 10 minutes to prepare liquid B. Liquid B was slowly added to liquid A and reacted for 3 hours before spray drying. The outlet temperature was adjusted to 105 degrees Celsius to obtain a light green precursor. Under an argon protective atmosphere, the precursor was pre-sintered at 350 degrees Celsius for 5 hours, and then sintered at 850 degrees Celsius for 10 hours to obtain the Na 3.5 Mn 0.5 V 1.5 (PO 4 ) 3 @C-CTAB positive electrode material, denoted as NMVP@0.1gCTAB.

[0071] Example 2

[0072] This embodiment provides a sodium positive electrode material, whose chemical formula is Na 3.5 Mn 0.5 V 1.5 (PO 4 ) 3 @C-CTAB, the preparation method thereof comprises: 22.22 g of citric acid monohydrate, 3.64 g of vanadium pentoxide, 3.27 g of manganese acetate tetrahydrate, 7.65 g of sodium acetate monohydrate and 0.28 g of CTAB were dissolved in 140 ml of a deionized water solution at 80 degrees Celsius, stirred for 1 hour to prepare liquid A, and 9.20 g of ammonium dihydrogen phosphate and 0.12 g of CTAB were dissolved in 60 ml of a deionized water solution at 80 degrees Celsius, stirred for 10 minutes to prepare liquid B. Liquid B was slowly added to liquid A and reacted for 3 hours, then spray-dried and the outlet temperature was adjusted to 105 degrees Celsius to obtain a light green precursor. Under an argon protective atmosphere, the precursor was pre-sintered at 350 degrees Celsius for 5 hours, and then sintered at 850 degrees Celsius for 10 hours to obtain the Na 3.5 Mn 0.5 V 1.5 (PO 4 ) 3 @C-CTAB positive electrode material, denoted as NMVP@0.4gCTAB.

[0073] Example 3

[0074] This embodiment provides a sodium positive electrode material, whose chemical formula is Na 3.5 Mn 0.5V 1.5 (PO 4 ) 3 @C-CTAB, the preparation method thereof comprises: 22.22 g of citric acid monohydrate, 3.64 g of vanadium pentoxide, 3.27 g of manganese acetate tetrahydrate, 7.65 g of sodium acetate monohydrate and 0.7 g of CTAB were dissolved in 140 ml of a deionized water solution at 80 degrees Celsius, stirred for 1 hour to prepare liquid A, and 9.20 g of ammonium dihydrogen phosphate and 0.3 g of CTAB were dissolved in 60 ml of a deionized water solution at 80 degrees Celsius, stirred for 10 minutes to prepare liquid B. Liquid B was slowly added to liquid A and reacted for 3 hours, then spray-dried, and the outlet temperature was adjusted to 105 degrees Celsius to obtain a light green precursor. Under an argon protective atmosphere, the precursor was pre-sintered at 350 degrees Celsius for 5 hours, and then sintered at 850 degrees Celsius for 10 hours to obtain the Na 3.5 Mn 0.5 V 1.5 (PO 4 ) 3 @C-CTAB positive electrode material, denoted as NMVP@1gCTAB.

[0075] Example 4

[0076] This embodiment provides a sodium positive electrode material, whose chemical formula is Na 3.5 Mn 0.5 V 1.5 (PO 4 ) 3 @C-PVP, the preparation method thereof comprises: 22.22 g of citric acid monohydrate, 3.64 g of vanadium pentoxide, 3.27 g of manganese acetate tetrahydrate, 7.65 g of sodium acetate monohydrate and 0.07 g of PVP were dissolved in 140 ml of a deionized water solution at 80 degrees Celsius, stirred for 1 hour to prepare liquid A, 9.20 g of ammonium dihydrogen phosphate and 0.03 g of PVP were dissolved in 60 ml of a deionized water solution at 80 degrees Celsius, stirred for 10 minutes to prepare liquid B. Liquid B was slowly added to liquid A and reacted for 3 hours, then spray-dried and the outlet temperature was adjusted to 105 degrees Celsius to obtain a light green precursor. Under an argon protective atmosphere, the precursor was pre-sintered at 350 degrees Celsius for 5 hours, and then sintered at 850 degrees Celsius for 10 hours to obtain the Na 3.5 Mn 0.5 V 1.5 (PO 4 ) 3 @C-PVP positive electrode material, denoted as NMVP@0.1gPVP.

[0077] Example 5

[0078] This embodiment provides a sodium positive electrode material, whose chemical formula is Na3.5 Mn 0.5 V 1.5 (PO 4 ) 3 @C-PVP, the preparation method thereof comprises: 22.22 g of citric acid monohydrate, 3.64 g of vanadium pentoxide, 3.27 g of manganese acetate tetrahydrate, 7.65 g of sodium acetate monohydrate and 0.28 g of PVP were dissolved in 140 ml of a deionized water solution at 80 degrees Celsius, stirred for 1 hour to prepare liquid A, 9.20 g of ammonium dihydrogen phosphate and 0.12 g of PVP were dissolved in 60 ml of a deionized water solution at 80 degrees Celsius, stirred for 10 minutes to prepare liquid B. Liquid B was slowly added to liquid A and reacted for 3 hours before spray drying. The outlet temperature was adjusted to 105 degrees Celsius to obtain a light green precursor. Under an argon protective atmosphere, the precursor was pre-sintered at 350 degrees Celsius for 5 hours, and then sintered at 850 degrees Celsius for 10 hours to obtain the Na 3.5 Mn 0.5 V 1.5 (PO 4 ) 3 @C-PVP positive electrode material, denoted as NMVP@0.4gPVP.

[0079] Example 6

[0080] This embodiment provides a sodium positive electrode material, whose chemical formula is Na 3.5 Mn 0.5 V 1.5 (PO 4 ) 3 @C-PVP, the preparation method thereof comprises: 22.22 g of citric acid monohydrate, 3.64 g of vanadium pentoxide, 3.27 g of manganese acetate tetrahydrate, 7.65 g of sodium acetate monohydrate and 0.7 g of PVP were dissolved in 140 ml of a deionized water solution at 80 degrees Celsius, stirred for 1 hour to prepare liquid A, 9.20 g of ammonium dihydrogen phosphate and 0.3 g of PVP were dissolved in 60 ml of a deionized water solution at 80 degrees Celsius, stirred for 10 minutes to prepare liquid B. Liquid B was slowly added to liquid A and reacted for 3 hours, then spray-dried and the outlet temperature was adjusted to 105 degrees Celsius to obtain a light green precursor. Under an argon protective atmosphere, the precursor was pre-sintered at 350 degrees Celsius for 5 hours, and then sintered at 850 degrees Celsius for 10 hours to obtain the Na 3.5 Mn 0.5 V 1.5 (PO 4 ) 3 @C-PVP positive electrode material, denoted as NMVP@1gPVP.

[0081] Comparative Example 1

[0082] This comparative example provides a sodium positive electrode material, the chemical formula of which is Na 3.5 Mn 0.5 V 1.5 (PO 4 ) 3 @C, the preparation method thereof comprises: 22.22 g of citric acid monohydrate, 3.64 g of vanadium pentoxide, 3.27 g of manganese acetate tetrahydrate, and 7.65 g of sodium acetate monohydrate were dissolved in 140 ml of 80 °C deionized water solution, stirred for 1 hour to prepare liquid A, and 9.20 g of ammonium dihydrogen phosphate was dissolved in 60 ml of 80 °C deionized water solution, stirred for 10 minutes to prepare liquid B. Liquid B was slowly added to liquid A and reacted for 3 hours, then spray dried, and the outlet temperature was adjusted to 105 °C to obtain a light green precursor. Under the protective atmosphere of argon, the precursor was pre-sintered at 350 °C for 5 hours, and then sintered at 850 °C for 10 hours to obtain the Na 3.5 Mn 0.5 V 1.5 (PO 4 ) 3 @C positive electrode material, denoted as NMVP.

[0083] Comparative Example 2

[0084] This comparative example provides a sodium positive electrode material, the chemical formula of which is Na 3.5 Mn 0.5 V 1.5 (PO 4 ) 3 @C-CTAB, the preparation method thereof comprises: 22.22 g of citric acid monohydrate, 3.64 g of vanadium pentoxide, 3.27 g of manganese acetate tetrahydrate, 7.65 g of sodium acetate monohydrate, 9.20 g of ammonium dihydrogen phosphate and 0.1 g of CTAB were dissolved in 200 ml of a deionized water solution at 80 degrees Celsius, stirred thoroughly, reacted for 3 hours, spray dried, and the outlet temperature was adjusted to 105 degrees Celsius to obtain a light green precursor. Under an argon protective atmosphere, the precursor was pre-sintered at 350 degrees Celsius for 5 hours, and then sintered at 850 degrees Celsius for 10 hours to obtain the Na 3.5 Mn 0.5 V 1.5 (PO 4 ) 3 @C-CTAB positive electrode material, denoted as NMVP-direct mixing.

[0085] Test Example 1

[0086] The composite materials obtained in some embodiments and comparative examples were characterized by XRD. Figure 1 shown.

[0087] The NMVP@0.1gCTAB prepared in Example 1, the NMVP@0.1gPVP obtained in Example 4, and the Na 3.5 Mn 0.5 V 1.5 (PO 4 ) 3 @C positive electrode material was characterized by XRD, such as Figure 1 shown.

[0088] It can be seen that the materials of the embodiment and the comparative example have good crystallinity, and no impurity peaks are detected, indicating that the synthesized materials have high purity. The composite material without surfactant and the composite material with 0.1 g of CTAB and PVP show extremely high consistency in the XRD test. The peak shape of the composite material is sharp, without obvious impurity peaks, and highly matched with the standard card, indicating that the material purity is extremely high.

[0089] Test Example 2

[0090] The scanned image of NMVP@0.1gCTAB prepared in Example 1 is as follows: Figure 2 As shown, the NMVP@1gCTAB prepared in Example 3 is as follows Figure 3 The scanning image of NMVP@0.1gPVP prepared in Example 4 is shown in Figure 4 As shown, the scanning image of NMVP@1gPVP prepared in Example 6 is as follows Figure 5 shown.

[0091] The results show that the addition of surfactants changes the material from spherical to a mixture of spherical and flaky structures, and the higher the additive content, the worse the regularity of the particle morphology. CTAB promotes the composite material to form spherical block particles, while PVP promotes the composite material to form long strip block particles, which are different from the irregular and unformed nanoparticle morphology in the prior art. Among them, spherical particles are particularly beneficial for shortening the ion diffusion path, improving structural stability and high-rate performance. Long strip block particles have a smaller specific surface area, which is beneficial for improving the volume energy density of the positive electrode.

[0092] Test Example 3

[0093] The materials provided in each embodiment and comparative example are assembled into a battery. The specific preparation method is as follows: the positive electrode material prepared in the embodiment, conductive carbon black (Super P) and polyvinylidene fluoride (PVDF) are weighed in a mass ratio of 7:2:1, and the mixture is fully ground and mixed, and then dissolved in an N-methylpyrrolidone (NMP) solution, stirred and ground to form a uniform slurry, and the slurry is evenly applied on an aluminum foil using a scraper method, dried at 80 degrees Celsius for 12 hours under a vacuum environment, and then cut into 12 mm diameter discs as the positive electrode of the battery; a 14 mm diameter sodium sheet is used as the negative electrode, and the electrolyte is 1M sodium perchlorate (NaClO 4 ) was dissolved in a 1:1 volume ratio of ethylene carbonate / diethyl carbonate (EC / DEC) system, and the separator was glass fiber. The button cells were assembled into 2032-type button cells in an argon-filled glove box. The button cells were tested for cycle performance in the voltage range of 2.5 to 3.8 volts and at different current densities (1 coulomb = 110 mA / g).

[0094] The three samples in Examples 1 to 3 were tested for cycle performance, and the results are as follows: Figure 6 As shown, by comparison, it can be found that the electrochemical performance of the material is improved after the addition of CTAB. The NMVP@0.1gCTAB positive electrode material has an initial capacity of 100.1 mAh / g at 0.2 coulomb, and can retain 83.4% of the reversible capacity after 800 cycles of 5 coulomb.

[0095] The three samples in Examples 4 to 6 were tested for cycle performance, and the results are as follows: Figure 7 As shown, by comparison, it can be found that the electrochemical performance of the material is reduced after the addition of PVP. The NMVP@0.1gPVP positive electrode material has an initial capacity of 90 mAh / g at 0.2 coulombs, and only 78% of the reversible capacity can be retained after 1000 cycles of 5 coulombs.

[0096] The sample in comparative example 1 was tested for cycle performance, and the results are as follows: Figure 8 As shown, it has an initial capacity of about 94 mAh / g at 0.2 coulomb, and retains 64% of the reversible capacity after 800 cycles of 5 coulomb.

[0097] The sample in comparative example 2 was tested for cycle performance, and the results are as follows: Figure 8 As shown, it has an initial capacity of about 95 mAh / g at 0.2 coulomb and retains 53% of the reversible capacity after 800 cycles of 5 coulomb.

[0098] Combination Figure 6 , Figure 7 , Figure 8The electrochemical performance of NMVP, NMVP@CTAB and NMVP@PVP can be compared, among which NMVP@0.1gCTAB in Example 4 shows the best electrochemical performance, with an initial capacity of 100.1 mAh / g in the voltage range of 2.5-3.8V, and 83.4% of the reversible capacity can be retained after 5 coulomb cycles of 800 cycles, with excellent cycle stability. At the same time, it can be seen that trace amounts of surfactants can have a great impact on the morphology and performance of the material. When using surfactants, it is necessary to select the appropriate dosage, otherwise it is difficult to achieve the ideal regulation effect and electrochemical performance.

[0099] Test Example 4

[0100] The present invention further tests the specific surface area of ​​the sodium manganese vanadium phosphate composite material obtained in the embodiment and the comparative example. The results are as follows: Fig. 9 As shown. The results show that Examples 1 to 3 have lower specific surface areas than Examples 4 to 6, among which NMVP@0.1gPVP corresponds to the smallest specific surface area, which is only 13.156 cubic centimeters per gram. In addition, the experimental results show that the specific surface areas of the sodium manganese vanadium phosphate composite materials prepared in Comparative Examples 1 and 2 are significantly higher than those of Examples 1 to 6.

[0101] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a sodium positive electrode material, characterized in that: include: S1: mixing a carbon source, a vanadium source, a manganese source, a sodium source, a surfactant and water to obtain liquid A; mixing a phosphorus source, a surfactant and water to obtain liquid B; and then mixing liquid A and liquid B to react to obtain a mixed slurry; S2: spray drying the mixed slurry to obtain a precursor; S3: performing a pre-sintering treatment and a sintering treatment on the precursor in sequence to obtain the sodium battery positive electrode material.

2. The method for preparing a sodium positive electrode material according to claim 1, characterized in that: The surfactant is composed of polyvinyl pyrrolidone and / or hexadecyl trimethyl ammonium bromide; Preferably, based on the amount of water in the mixed slurry, 0.1 to 1 gram of the surfactant is added to every 200 ml of water.

3. The method for preparing a sodium positive electrode material according to claim 1 or 2, characterized in that: The mass ratio of the A liquid to the B liquid is (6-8):(2-4).

4. The method for preparing a sodium positive electrode material according to claim 3, characterized in that: The amount of surfactant in the liquid A is greater than the amount of surfactant in the liquid B; preferably, the mass ratio of the surfactant in the liquid A to the surfactant in the liquid B is (2-4):

1.

5. The method for preparing a sodium positive electrode material according to any one of claims 1 to 4, characterized in that: The molar ratio of the metal elements in the carbon source, vanadium source, manganese source and sodium source is (18~22):(1~2):(0.3~0.7):(3~4); and / or the molar ratio of the metal elements in the sodium source and phosphorus source is (3.4~3.6):

3.

6. The method for preparing a sodium positive electrode material according to any one of claims 1 to 5, characterized in that: The sodium source is one or more of sodium carbonate, sodium bicarbonate, sodium dihydrogen phosphate, sodium acetate and sodium oxalate; And / or, the manganese source is one or more of manganese acetate, manganese oxalate and manganese carbonate; And / or, the vanadium source is vanadium pentoxide and / or ammonium metavanadate; And / or, the phosphorus source is one or more of ammonium dihydrogen phosphate, phosphoric acid and sodium dihydrogen phosphate; And / or, the carbon source is one or more of citric acid, glucose, sucrose, oxalic acid and ascorbic acid.

7. The method for preparing a sodium positive electrode material according to any one of claims 1 to 6, characterized in that: In S2, during the spray drying, the outlet temperature is controlled to be 105 to 120 degrees Celsius; And / or, S3 includes: pre-sintering the precursor at 300-400 degrees Celsius in an inert gas atmosphere or a reducing gas atmosphere, and then sintering it at 800-900 degrees Celsius.

8. A sodium positive electrode material, characterized in that: It is prepared by the preparation method according to any one of claims 1 to 7; preferably, the mass fraction of the amorphous carbon coating layer in the sodium positive electrode material is 5 to 10 wt%, and the thickness of the amorphous carbon coating layer is 2 to 8 nanometers.

9. A sodium ion battery, characterized in that: It contains the positive electrode material according to claim 8.

10. An electrical device, characterized in that: It contains the sodium ion battery according to claim 9.