Lithium supplement material and preparation method thereof, positive electrode material and secondary battery
By using one-dimensional carbon materials in lithium-ion batteries to load lithium-rich materials and catalysts, and combining the structure of two-dimensional carbon materials, the problems of poor conductivity and high deliquency potential of the positive electrode materials are solved, and the capacity, energy density and Security.
Patent Information
- Application Number
- CN202410880148.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-11-08
AI Technical Summary
The poor conductivity and high deliquency potential of the positive electrode material in existing lithium-ion batteries lead to low capacity and energy density of lithium-ion batteries, and degradation of safety and performance.
One-dimensional carbon material is used to load lithium-rich materials and catalysts, and the conductivity and catalytic effect are improved through the conductive network structure of one-dimensional carbon material, reducing the deliquification voltage of lithium-rich materials, and ensuring gas is present through the hole structure of two-dimensional carbon material. Sequential flow protects material structure and battery safety.
It significantly improves the conductivity and catalytic effect of lithium supplement materials, reduces the deliquency potential of lithium-rich materials, enhances the capacity and energy density of the battery, and improves the safety and performance of the battery.
Smart Images

Figure CN118919707A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of secondary batteries, and in particular to a lithium supplement material and a preparation method thereof, a positive electrode material and a secondary battery. Background Art
[0002] During the first charging process of a lithium-ion battery, the negative electrode material permanently consumes more active Li from the positive electrode. + , forming a SEI film on the surface of the negative electrode, reducing the capacity and energy density of the lithium-ion battery. In order to make up for the lithium consumed in forming the SEI film, lithium replenishment technology can be used in lithium-ion batteries. Compared with negative electrode lithium replenishment, positive electrode lithium replenishment can directly add lithium replenishment materials into the positive electrode slurry without additional process improvements, and the cost is relatively low.
[0003] Reported positive electrode lithium supplement materials such as Li 3 N, Li 3 P, Li 2 S, Li 2 O 2 etc., have a high theoretical specific capacity, but are very sensitive to air and humidity, making it difficult to achieve large-scale industrial application. 2 C 2 O 4 , Li 2 C 4 O 4 and Li 2 C 6 O 6 However, due to their poor conductivity, the delithiation potential of the materials is high (>4.7V), which cannot match that of most commercial cathode materials, which greatly hinders their commercial application. Summary of the invention
[0004] The purpose of the present invention is to provide a lithium supplement material and a preparation method thereof, a positive electrode material and a secondary battery, so as to solve the problems of poor conductivity and high lithium desorption potential of lithium-rich materials.
[0005] To achieve the purpose of this application, this application provides the following technical solutions:
[0006] In a first aspect, the present invention provides a lithium supplement material, comprising a one-dimensional carbon material, a lithium-rich material and a catalyst, wherein at least part of the lithium-rich material and at least part of the catalyst are loaded on the one-dimensional carbon material.
[0007] The lithium-supplementing material provided by the present invention uses a one-dimensional carbon material as a carrier, and uses the one-dimensional carbon material to load a large amount of catalyst and lithium-rich material. The advantages of the lithium-supplementing material include: 1) the one-dimensional carbon material has strong conductivity, and using the one-dimensional carbon material as a carrier can improve the overall conductivity of the lithium-supplementing material; 2) the one-dimensional carbon material provides abundant active sites for the catalyst, which is beneficial to enhance the catalytic effect of the catalyst, thereby significantly reducing the lithium decomposition voltage of the lithium-rich material; 3) the linear structure of the one-dimensional carbon material is beneficial to ensure the orderly flow and escape of the gas after the lithium-rich material produces gas, thereby protecting the structural integrity and stability of the lithium-supplementing material and the safety of the battery.
[0008] In one embodiment, the one-dimensional carbon material is in multiple numbers, and the multiple one-dimensional carbon materials are stacked to form a conductive wire bundle structure; and / or the multiple one-dimensional carbon materials are interwoven to form a conductive network structure.
[0009] In one embodiment, the lithium-supplementing material further comprises a two-dimensional carbon material, and a portion of the lithium-rich material and a portion of the catalyst are combined with a surface of the two-dimensional carbon material.
[0010] In one embodiment, the two-dimensional carbon material is in multiple pieces, and the multiple pieces of the two-dimensional carbon material are stacked.
[0011] In one embodiment, at least one of the one-dimensional carbon materials is inserted into a gap between two adjacent pieces of the two-dimensional carbon material.
[0012] In one embodiment, the two-dimensional carbon material has holes, and at least part of the one-dimensional carbon material is interspersed in the holes.
[0013] In one embodiment, the one-dimensional carbon material and / or the two-dimensional carbon material is doped with a non-metallic element, and the non-metallic element includes at least one of O, N, and S.
[0014] In one embodiment, the catalyst is grown in situ on the one-dimensional carbon material and / or on the two-dimensional carbon material.
[0015] In one embodiment, the two-dimensional carbon material comprises carbon nanosheets.
[0016] In one embodiment, the porosity of the two-dimensional carbon material is 30% to 70%.
[0017] In one embodiment, the mass ratio of the one-dimensional carbon material to the two-dimensional carbon material is 1:(1-10).
[0018] In one embodiment, the specific surface area of the one-dimensional carbon material and the two-dimensional carbon material is 200 m 2 / g~800m 2 / g.
[0019] In one embodiment, the catalyst includes at least two different metal compounds, and the two metal compounds are interconnected to form a heterojunction.
[0020] In one embodiment, at least a portion of the lithium-rich material and at least a portion of the catalyst are in contact with each other.
[0021] In one embodiment, part of the lithium-rich material is coated on the outer surface of the catalyst.
[0022] In one embodiment, at least a portion of the one-dimensional carbon material has gaps, so that the interior of the one-dimensional carbon material is connected to the external space.
[0023] In one embodiment, the one-dimensional carbon material includes carbon nanotubes.
[0024] In one embodiment, the particle size of the lithium-rich material is 10 nm to 3 μm.
[0025] In one embodiment, the particle size of the catalyst is 2 nm to 100 nm.
[0026] In one embodiment, the mass ratio of the lithium-rich material to the catalyst is 100:(1-15).
[0027] In one embodiment, the chemical formula of the lithium-rich material is Li x1 C y1 O z1 , where 0<x1≤2,y1> 0,z1>0.
[0028] In a second aspect, the present invention provides a method for preparing a lithium-supplementing material, comprising: mixing a catalyst raw material with a one-dimensional carbon material for reaction so that at least part of the catalyst is loaded on the one-dimensional carbon material; mixing a lithium-rich material with the one-dimensional carbon material loading the catalyst so that at least part of the lithium-rich material is loaded on the one-dimensional carbon material to obtain a lithium-supplementing material.
[0029] In a third aspect, the present invention further provides a positive electrode material, which includes a positive electrode active material and a lithium supplement material, wherein the lithium supplement material includes the lithium supplement material described in the first aspect, or the positive electrode material includes the lithium supplement material obtained by the preparation method of the lithium supplement material described in the second aspect.
[0030] In a fourth aspect, the present invention further provides a secondary battery, comprising a positive electrode, a negative electrode and a separator arranged between the positive electrode and the negative electrode, wherein the positive electrode comprises the positive electrode material described in the third aspect. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0032] Figure 1 is a schematic structural diagram of a lithium supplement material according to an embodiment;
[0033] Figure 2 is a schematic structural diagram of a lithium supplement material according to another embodiment;
[0034] Figure 3 is a schematic diagram of a preparation process of a lithium supplement material according to an embodiment;
[0035] Figure 4 is a schematic diagram of a preparation process of a catalyst having a heterojunction according to an embodiment;
[0036] Figure 5 is a schematic diagram of a preparation process of a lithium supplement material according to another embodiment;
[0037] Figure 6 The present invention is a schematic diagram of the preparation process of one-dimensional carbon materials and two-dimensional carbon materials according to an embodiment. DETAILED DESCRIPTION
[0038] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0039] It should be noted that when a component is said to be "fixed to" another component, it can be directly on the other component or there can be a central component. When a component is said to be "connected to" another component, it can be directly connected to the other component or there can be a central component at the same time.
[0040] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used in this application and in the specification are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used in this application includes any and all combinations of one or more of the related listed items.
[0041] In conjunction with the accompanying drawings, some embodiments of the present application are described in detail below. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.
[0042] In the first aspect, the present invention provides a lithium supplement material, please refer to Figure 1 , including a one-dimensional carbon material 21, a lithium-rich material 10 and a catalyst 30, at least part of the lithium-rich material 10 and at least part of the catalyst 30 are loaded on the one-dimensional carbon material 21.
[0043] Among them, the lithium-rich material 10 is the main body for lithium supplementation, which can contribute a large amount of lithium ions. During the first charging process, the lithium (Li) in the lithium-rich material 10 can be released and migrated to the negative electrode of the battery to offset the irreversible lithium loss caused by the formation of the SEI film, thereby improving the total capacity and energy density of the battery. However, most of the existing high-capacity lithium-rich materials 10 have problems with poor conductivity and high detachment potential, which makes such lithium-rich materials 10 unable to match most commercial positive electrode materials, which greatly hinders their commercial application. In addition, the higher voltage also causes the lithium-rich material 10 to produce gas when the lithium-ion battery is charged and discharged for the first time. The generated gas cannot be discharged in time, resulting in reduced safety and performance of the lithium-ion battery. Therefore, how to solve the poor conductivity and high detachment potential of the lithium-rich material 10 has become the key.
[0044] The catalyst 30 has a catalytic effect and is used to catalytically reduce the delithiation potential of the lithium-rich material 10. It should be explained that among the existing commercial lithium-rich materials 10, most of the lithium-rich materials 10 have a higher energy density, but because the delithiation potential of the lithium-rich material 10 does not match the voltage of the existing commercial positive electrode materials, the lithium-rich material 10 cannot fully release its capacity during the use of the battery. Therefore, by adding a catalyst 30 to the lithium-supplementing material to reduce the activation energy of the reaction, the reaction activity is improved. The addition of the catalyst 30 can reduce the delithiation potential of the lithium-rich material 10 to varying degrees, so that it can match the existing commercial positive electrode materials.
[0045] The one-dimensional carbon material 21 is the main body for loading the lithium-rich material 10 and the catalyst 30. Since the one-dimensional carbon material 21 is essentially a carbon material, the one-dimensional carbon material 21 has excellent electrical conductivity, and the lithium-rich material 10 loaded on the one-dimensional carbon material 21 can improve its conductivity.
[0046] In one embodiment, the chemical formula of the lithium-rich material 10 is Li x1 C y1 O z1 , where 0<x1≤2,y1> 0, z1>0. In some embodiments of the present application, the lithium-rich material 10 may be Li 2 C 3 O 3 , Li2 C 4 O 4 , Li 2 C 6 O 6 , Li 2 C 3 O 5 , Li 2 C 2 O 4 and Li 2 C 4 O 6 It can be understood that the lithium-rich material 10 of lithium oxalate has a higher theoretical capacity (>525 mAhg -1 ) and good air stability, it is considered to be an attractive cathode pre-lithiation additive. However, it has a high delithiation potential (>4.7V), which cannot match most commercial cathode materials, and its poor conductivity greatly hinders its commercial application.
[0047] In one embodiment, the lithium-rich material 10 also includes other lithium-supplementing materials with a higher decomposition voltage, mainly including lithium-supplementing materials with a lithium decomposition potential of more than 4V, such as Li 2 O (lithiation potential 4.5V), Li 2 O 2 (delithiation potential 4.3V), LiOH (delithiation potential 4.8V), Li 4 SiO 4 (lithiation potential 4.5V), Li 3 PO 4 (lithiation potential exceeds 4V), Li 2 CO 3 (lithiation potential 4.7V), Li 5 FeO 4 (Delithiation potential 4V). These lithium-rich materials 10 also have a high capacity, but these lithium-rich materials 10 require a higher charging voltage for delithiation, and there is a technical problem of high platform voltage. At the same time, the higher voltage also causes the lithium-rich material 10 to produce oxygen when the lithium-ion battery is first charged and discharged. The generated oxygen is further oxidized to cause the electrolyte to oxidize and decompose, thereby resulting in reduced safety and performance of the lithium-ion battery. These lithium-rich materials 10 with higher decomposition voltages are also difficult to compound with conventional positive electrode materials (such as lithium iron phosphate with a delithiation potential of about 3.5V), which limits the wide application of lithium-supplementing materials. Therefore, the present invention provides a one-dimensional carbon material 21, loads the lithium-rich material 10 and the catalyst 30 on the one-dimensional carbon material 21, and the catalyst 30 is combined with the lithium-rich material 10 to enhance the catalytic effect, which can effectively reduce the decomposition voltage of the lithium-rich material 10 and improve the utilization rate of the lithium-rich material 10.
[0048] Optionally, the lithium-rich material 10 may further include a binary lithium supplement and / or a ternary lithium supplement. The general chemical formula of the lithium-rich material 10 corresponding to the binary lithium supplement is Li x2 K y2 , where K is at least one element among S, P, N, F, B, Se, Te, 1≤x2≤5, 0<y2. The binary lithium supplement includes but is not limited to Li 3 N, Li 2 S, LiF, Li 3 P, Li 2 Se, etc.
[0049] Optionally, the chemical formula of the lithium-rich material 10 corresponding to the ternary lithium supplement is Li a M b O c , where M is at least one element among Fe, Ni, Mn, Cu, Zn, Co, Cr, Zr, Sb, Ti, V, Mo, Sn, etc., 1≤a≤8, 0<b, 0<c<7. In a specific embodiment, the lithium-rich material 10 may be Li 5 FeO 4 , Li 6 MnO 4 , Li 6 CoO 4 , Li 6 ZnO 4 , Li 2 NiO 2 , Li 2 CuO 2 , Li 2 CoO 2 , Li 2 MnO 2 , Li 2 Ni 0.5 Mn 1.5 O 4 , Li 2 Ni d Cu (1-d) O 2 (0<d<1), etc.
[0050] Optionally, the chemical formula of the lithium-rich material 10 may also be Li 1+x3 A y3 O z3 , where 0<x3≤1.2, 1≤y3<3, z3>0, and A includes at least one of Ni, Fe, Mn, Co, Cr, V, Mo, Ti, Nb, Zr, Cu, Mg. These lithium-rich materials 10 can be used as both lithium supplements and directly as cathode materials. Exemplarily, the lithium-rich material 10 includes Li 2 CuO2 , Li 2 NiO 2 , Li 2 MnO 2 At least one of .
[0051] The lithium-rich material 10 mentioned above may be undoped or modified by doping, or may be surface coated, pre-lithiated, etc. These lithium-rich materials 10 have high theoretical capacity and structural stability, can provide sufficient lithium ions, effectively supplement the irreversible lithium ions consumed by the formation of SEI film in the negative electrode, and improve the initial efficiency and overall electrochemical performance of the battery.
[0052] The lithium-supplementing material provided by the present invention uses a one-dimensional carbon material 21 as a carrier, and uses the one-dimensional carbon material 21 to load a large amount of catalyst 30 and lithium-rich material 10. The advantages of the lithium-supplementing material include: 1) The one-dimensional carbon material 21 has strong conductivity, and using the one-dimensional carbon material 21 as a carrier can improve the overall conductivity of the lithium-supplementing material; 2) The one-dimensional carbon material 21 provides abundant active sites for the catalyst 30, and increases the contact area between the catalyst 30 and the one-dimensional carbon material 21, further increasing the catalytic effect of the catalyst 30 and the conductive effect of the one-dimensional carbon material 21; 3) The linear structure of the one-dimensional carbon material 21 is beneficial to the lithium-rich material 10 after gas production, ensuring the orderly flow and escape of gas, thereby protecting the structural integrity and stability of the material and the safety of the battery.
[0053] In one implementation, please refer to Figure 1 , the number of the one-dimensional carbon materials 21 is multiple, and the multiple one-dimensional carbon materials 21 are stacked to form a conductive wire bundle structure; and / or, the multiple one-dimensional carbon materials 21 are interwoven to form a conductive network structure.
[0054] Specifically, in this aspect, the one-dimensional carbon material 21 includes one or more of carbon nanotubes, carbon nanorods, and carbon nanofibers. In a specific embodiment, the one-dimensional carbon material 21 can be carbon nanotubes (CNTs). Multiple one-dimensional carbon materials 21 are interwoven into a conductive network structure, that is, interwoven into a porous mesh structure. Therefore, the three-dimensional network structure in this aspect has holes, and the holes are meshes formed by the one-dimensional carbon materials 21 interweaving. In other embodiments, multiple one-dimensional carbon materials 21 extend in the same direction and are stacked on each other, thereby forming a conductive wire bundle structure, and gaps are also formed between the one-dimensional carbon materials 21.
[0055] Therefore, a large number of gaps (holes or gaps) are formed between the multiple one-dimensional carbon materials 21, and part of the lithium-rich material 10 and the catalyst 30 are contained in the gaps, which can improve the stability of the lithium-rich material 10 and the catalyst 30 loaded on the one-dimensional carbon material 21. On the other hand, the conductive network structure brings a larger specific surface area, thereby increasing the loading amount of the lithium-rich material 10 and the catalyst 30. At the same time, the gaps divided by the conductive network structure on the one-dimensional carbon material 21 can guide the gas generated by the lithium-rich material 10 after discharge, and avoid the gas generated by the lithium-rich material 10 from gathering in the material, thereby reducing the impact of gas production on the battery, and ultimately achieving the purpose of improving battery performance.
[0056] The advantages of setting the one-dimensional carbon material as a conductive wire bundle structure or a conductive network structure are: 1) increasing the overall specific surface area of the one-dimensional carbon material, which is conducive to loading catalysts and lithium-rich materials, and the large specific surface area provides active sites for the catalyst, which can enhance the connection stability between the catalyst and the one-dimensional carbon material; 2) enhancing the overall flexibility of the one-dimensional carbon material. Compared with other carbon materials, the one-dimensional carbon material can be interwoven into a conductive network structure by bending, winding, folding, etc., and the "fishing net" (or "wire bundle")-like structure can provide a large number of gaps, which can increase the loading amount of both lithium-rich materials and catalysts, and limit the growth of lithium-rich materials and catalysts, reduce the particle size of the two, and increase the contact area between the two, thereby enhancing the catalytic effect of the catalyst and further reducing the decomposition voltage of the lithium-rich material.
[0057] In one embodiment, the catalyst 30 and the lithium-rich material 10 are both grown in situ on the one-dimensional carbon material 21. The one-dimensional carbon material 21 may be provided in advance, and then the one-dimensional carbon material 21 and the catalyst raw material are mixed, the catalyst raw material is attached to the one-dimensional carbon material 21 to form a catalyst precursor, and finally the catalyst precursor is converted into the catalyst 30 by sintering.
[0058] By in-situ growing the catalyst 30 on the surface of the one-dimensional carbon material 21, the catalyst 30 can fully contact the one-dimensional carbon material 21 and obtain a larger contact area, thereby exposing more active sites on the one-dimensional carbon material 21 and improving the overall conductivity of the one-dimensional carbon material 21 and the catalyst 30, thereby improving the catalytic activity of the catalyst 30; and the in-situ grown catalyst 30 has a smaller particle size, which is conducive to fully exerting the catalytic performance of the catalyst 30.
[0059] In one embodiment, the length of the one-dimensional carbon material 21 is 10 μm to 50 μm. Optionally, the length of the one-dimensional carbon material 21 may be 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, or 50 μm.
[0060] Satisfying the length of the one-dimensional carbon material 21 within the above range can ensure that the one-dimensional carbon material 21 has a larger specific surface area, thereby providing higher conductivity and higher carrying capacity for the lithium-rich material 10 and the catalyst 30. When the length of the one-dimensional carbon material 21 is less than the above range, the one-dimensional carbon material 21 is shorter, resulting in fewer attachment points provided by the one-dimensional carbon material 21 to the lithium-rich material 10 and the catalyst 30, making the bonding of the lithium-rich material 10, the catalyst 30 and the one-dimensional carbon material 21 poor. When the length of the one-dimensional carbon material 21 is greater than the above range, the one-dimensional carbon material 21 is longer, resulting in an increase in the conduction path of electrons in the one-dimensional carbon material 21, which is not conducive to improving the conductive efficiency of the lithium-supplementing material, and the longer one-dimensional carbon material 21 is easily entangled together to form a sphere, which increases the difficulty of dispersing the one-dimensional carbon material 21, which is not conducive to the uniform distribution of the lithium-rich material 10 and the catalyst 30 on the one-dimensional carbon material 21.
[0061] In one embodiment, the diameter of the one-dimensional carbon material 21 is 8 nm to 15 nm. Optionally, the diameter of the one-dimensional carbon material 21 can be 8 nm, 9 nm, 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, or 15 nm.
[0062] When the diameter of the one-dimensional carbon material 21 is within the above range, it can ensure that the one-dimensional carbon material 21 has a larger specific surface area, thereby providing higher conductivity, and the one-dimensional carbon material 21 has higher strength. When the diameter of the one-dimensional carbon material 21 is smaller than the above range, the one-dimensional carbon material 21 is thinner, resulting in the deterioration of the strength of the one-dimensional carbon material 21, and it is easy to break and fall off. When the diameter of the one-dimensional carbon material 21 is larger than the above range, the one-dimensional carbon material 21 is coarser, resulting in a decrease in the specific surface area of the one-dimensional carbon material 21, which is not conducive to improving conductivity.
[0063] In one embodiment, the catalyst 30 includes at least two different metal compounds, and the two metal compounds are interconnected to form a heterojunction.
[0064] In a specific embodiment, the catalyst 30 in the lithium supplement material includes a metal oxide and a metal sulfide, and at least a portion of the metal oxide and the metal sulfide are connected to form a heterojunction. The chemical formula of the metal oxide includes D1 n1 O m1 The chemical formula of metal sulfides includes D1 n2 S m2 , wherein D1 is a transition metal element, D1 includes at least one of Co, Mo, W, V, Ti, Fe, Ni, Mn, Cr, Cu, and Zn, 1≤n1≤3, 1≤m1≤3, 1≤n2≤3, and 1≤m2≤3. It can be understood that the transition metal element in the metal oxide and the metal sulfide is the same.
[0065] Moreover, at least part of the metal oxide and the metal sulfide are connected and form a heterojunction. It should be explained that the metal oxide and the metal sulfide are connected, and a heterojunction is formed at the connection. The metal oxide and the metal sulfide share the transition metal ions in the heterojunction, and the transition metal ions are respectively connected to the oxygen ions and sulfur ions in the metal oxide and the metal sulfide. Therefore, the transition metal ions in the heterojunction are used to form the crystal structure of the metal oxide and the metal sulfide. It can be understood that in the present invention, the heterojunction is similar to a "double-sided adhesive" with a two-way connection function. The heterojunction is connected to the metal oxide on one side and the metal sulfide on the other side, so that the two are tightly connected.
[0066] The heterojunction catalyst 30 can improve its own catalytic performance and conductivity, thereby improving the electron transfer efficiency and catalytic activity of the lithium-rich material 10; by connecting the heterojunction catalyst 30 to the lithium-rich material 10, on the one hand, the conductivity of the lithium-rich material 10 can be improved, and on the other hand, the decomposition voltage of the lithium-rich material 10 can be effectively reduced, so that it can be decomposed at a smaller voltage to release capacity, thereby achieving a high lithium replenishment capacity.
[0067] In a specific embodiment, the metal oxide can be grown in situ on the one-dimensional carbon material 21, or the metal oxide can be physically mixed and bonded to the one-dimensional carbon material 21. The metal sulfide is obtained by sulfiding the metal oxide. Therefore, it can be understood that during the sulfidation of the metal oxide, as the degree of sulfidation deepens, the degree of conversion of the metal oxide to the metal sulfide also deepens. When only a part of the metal oxide is converted into the metal sulfide, a heterojunction of the metal oxide and the metal sulfide is obtained.
[0068] In other specific embodiments, the catalyst 30 in the lithium supplement material includes metal oxide and metal nitride, and at least part of the metal oxide and the metal nitride are connected to form a heterojunction. It can be understood that the transition metal element in the metal oxide and the metal nitride is the same.
[0069] In other specific embodiments, the catalyst 30 in the lithium supplement material includes metal oxide and metal carbide, and at least part of the metal oxide and the metal carbide are connected to form a heterojunction. It can be understood that the transition metal element in the metal oxide and the metal carbide is the same.
[0070] In other specific embodiments, the catalyst 30 in the lithium supplement material includes metal oxide and metal phosphide, and at least part of the metal oxide and the metal phosphide are connected to form a heterojunction. It can be understood that the transition metal element in the metal oxide and the metal phosphide is the same.
[0071] In other specific embodiments, the catalyst 30 in the lithium supplement material includes metal sulfide and metal carbide, and at least part of the metal sulfide and the metal carbide are connected to form a heterojunction. It can be understood that the transition metal element in the metal sulfide and the metal carbide is the same.
[0072] In one embodiment, the metal oxide and metal sulfide forming the heterojunction are metal heterojunction compounds, and the content of the metal heterojunction compound is greater than the content of the metal oxide or the content of the metal sulfide.
[0073] Specifically, based on the above embodiments, the catalyst 30 in the lithium supplement material can be of three types, namely metal oxide, metal sulfide and metal heterojunction compound. Among them, the metal heterojunction compound includes the heterojunction catalyst 30 provided in the above embodiments.
[0074] It should be explained that, in the present embodiment, particles of the above three types of catalysts 30 (metal oxide, metal sulfide and metal heterojunction compound) are bonded to the one-dimensional carbon material 21, and particles of different types of catalysts 30 can be independent of each other.
[0075] It is understandable that the performance of the metal heterojunction compound is better than that of the metal oxide and the metal sulfide, so in order to fully exert the metal heterojunction compound, it is necessary to control the content of the metal heterojunction compound to be greater than the content of the metal oxide or the content of the metal sulfide. Optionally, the content of the metal heterojunction compound is greater than the sum of the content of the metal oxide and the content of the metal sulfide.
[0076] In one embodiment, the specific surface area of the one-dimensional carbon material 21 is 90 m 2 / g~200m 2 / g. Optionally, the specific surface area of the one-dimensional carbon material 21 can be 90m 2 / g、100m 2 / g, 120m 2 / g, 140m 2 / g, 160m 2 / g, 180m 2 / g, 200m 2 / g.
[0077] The present invention interweaves the one-dimensional carbon material 21 into a three-dimensional network structure, thereby forming a large number of meshes (holes) on the one-dimensional carbon material 21. In addition, the formed meshes can maximize the surface area of the one-dimensional carbon material 21, thereby obtaining a one-dimensional carbon material 21 with a high specific surface area. When the specific surface area of the one-dimensional carbon material 21 is within the above range, the loading amount of the lithium-rich material 10 and the catalyst 30 can be increased, and the active sites of the two on the one-dimensional carbon material 21 can be increased, thereby improving the lithium replenishment capacity and electrochemical performance of the lithium replenishment material. When the specific surface area of the one-dimensional carbon material 21 is less than the above range, the loading amount of the lithium-rich material 10 and the catalyst 30 is small, not only the capacity improvement is limited, but also the effect of the catalyst 30 is weak. When the specific surface area of the porous carbon carrier is greater than the above range, it is difficult for the porous carbon carrier to suppress the lattice volume expansion of the lithium-rich material 10.
[0078] In one embodiment, the particle size D50 of the lithium-rich material 10 is 1 μm to 5 μm. Optionally, the particle size D50 of the lithium-rich material 10 may be 1 μm, 2 μm, 3 μm, 4 μm, or 5 μm.
[0079] In one embodiment, the particle size D99 of the lithium-rich material 10 is less than or equal to 10 μm. Optionally, the particle size D99 of the lithium-rich material 10 may be 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, or 10 μm.
[0080] In one embodiment, the particle size D10 of the lithium-rich material 10 is 0.2 μm to 0.6 μm. Optionally, the particle size D10 of the lithium-rich material 10 may be 0.2 μm, 0.3 μm, 0.4 μm, 0.5 μm, or 0.6 μm.
[0081] The particle size of the lithium-rich material 10 is within the above range, so that the lithium-rich material 10 can achieve good contact with the catalyst 30, and is conducive to improving the conductivity of the lithium-rich material 10, reducing the decomposition voltage, and avoiding the agglomeration of the lithium-rich material 10. When the particle size of the lithium-rich material 10 is smaller than the above range, the difficulty of preparing the lithium-rich material 10 increases, and the lithium-rich material 10 is easy to agglomerate and difficult to disperse, and is easy to form agglomerated large particles; when the particle size of the lithium-rich material 10 is larger than the above range, the lithium-rich material 10 is difficult to connect with the lithium-rich material 10, and the conductivity of the lithium-rich material 10 is too poor, which will also lead to an increase in the decomposition voltage of the lithium-rich material 10.
[0082] In one embodiment, the particle sizes of the metal oxide, metal sulfide and metal heterojunction compound are all smaller than the particle size of the lithium-rich material 10 .
[0083] In one embodiment, the particle size of the metal oxide, metal sulfide and metal heterojunction compound is 10nm to 100nm. Optionally, the particle size of the metal oxide, metal sulfide and metal heterojunction compound can be 10nm, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm.
[0084] It can be understood that both metal sulfides and metal heterojunction compounds are obtained by sulfiding metal oxides, and the sulfidation process has little effect on the particle size of the product, so the particle size of metal sulfides and metal heterojunction compounds is similar to that of metal oxides.
[0085] When the particle size of the metal oxide, metal sulfide and metal heterojunction compound is within the above range, the catalytic performance of the catalyst 30 can be released as much as possible, the catalytic efficiency can be improved, and the difficulty of preparing the catalyst 30 can be reduced to avoid the agglomeration of the catalyst 30. When the particle size of the catalyst 30 is smaller than the above, the difficulty of preparing the catalyst 30 increases, and the agglomeration of the catalyst 30 is serious, which affects the performance of its catalytic performance; when the particle size of the catalyst 30 is larger than the above, the catalytic effect of the catalyst 30 on the lithium-rich material 10 decreases, and the distribution density of the catalyst 30 on the one-dimensional carbon material 21 becomes smaller.
[0086] In one embodiment, the mass ratio of the lithium-rich material 10, the one-dimensional carbon material 21 and the catalyst 30 is 100:(4-15):(1-5). Optionally, the mass ratio of the lithium-rich material 10, the one-dimensional carbon material 21 and the catalyst 30 can be 100:(4-15):1, 100:(4-15):2, 100:(4-15):3, 100:(4-15):4, 100:(4-15):5, 100:4:(1-5), 100:6:(1-5), 100:8:(1-5), 100:10:(1-5), 100:12:(1-5), 100:15:(1-5).
[0087] When the mass proportion of the three materials is within the above range, the lithium replenishing capacity of the lithium replenishing material can be ensured, and the catalytic effect of the catalyst 30 can be fully exerted, and the conductivity of the material can be ensured, and the delithiation potential of the lithium-rich material 10 can be reduced. When the mass proportion of the one-dimensional carbon material 21 is less than the above range, the one-dimensional carbon material 21 has limited improvement in the conductivity of the lithium-rich material 10, and the one-dimensional carbon material 21 has limited carrying capacity for the lithium-rich material 10 and the catalyst 30, so it can carry more lithium-rich materials 10 and catalysts 30. When the mass proportion of the catalyst 30 is less than the above range, the catalytic effect and conductivity of the catalyst 30 are poor. When the mass proportion of the above two materials is greater than the above range, the proportion of the lithium-rich material 10 will be further reduced, and the lithium-rich material 10 will find it difficult to exert more battery capacity, resulting in a decrease in the energy density of the battery.
[0088] In one embodiment, the present invention provides a method for preparing a lithium supplement material, please refer to Figure 3 , specifically used to prepare the lithium supplement material provided in the first aspect, comprising the following steps:
[0089] Step S10: mixing a catalyst raw material with a one-dimensional carbon material to react, so that at least a portion of the catalyst is loaded on the one-dimensional carbon material.
[0090] Step S20, mixing the lithium-rich material with the one-dimensional carbon material carrying the catalyst, so that at least a portion of the lithium-rich material is carried on the one-dimensional carbon material, to obtain a lithium-supplementing material.
[0091] Optional, please refer to Figure 3 , before step S10, it also includes step S00: preparing a one-dimensional carbon material.
[0092] In step S00, one-dimensional carbon material is prepared, specifically including: making carbon nanotubes (CNTs). The preparation method of carbon nanotubes mainly includes any one of arc discharge method, laser evaporation method and chemical vapor deposition method, which is not specifically limited.
[0093] Optionally, in step S10, the catalyst raw material and the one-dimensional carbon material are mixed for reaction, specifically comprising: dissolving the catalyst raw material in deionized water, and then adding the one-dimensional carbon material to the deionized water; then continuing to add an appropriate amount of ammonia water to the deionized water, filtering and drying after sufficient stirring to obtain a mixture of the catalyst precursor and the one-dimensional carbon material.
[0094] Optionally, in step S10, the catalyst raw material includes a transition metal salt, specifically including but not limited to chloride, nitrate, organic acid salt, etc. The catalyst precursor obtained by the reaction is a hydroxide (transition metal).
[0095] Optionally, in step S10, the drying temperature is 60°C to 80°C, and the drying time is 4h to 8h.
[0096] Optionally, in step S10, after the catalyst raw material and the one-dimensional carbon material are mixed and reacted, the obtained catalyst precursor needs to be converted into a catalyst, specifically including: heat treating the mixture of the catalyst precursor and the one-dimensional carbon material to obtain a one-dimensional carbon material combined with the catalyst.
[0097] Optionally, in step S10, the atmosphere of the heat treatment is an inert atmosphere, the temperature of the heat treatment is 300° C. to 500° C., and the time of the heat treatment is 3 h to 6 h.
[0098] Optionally, in step S20, the lithium-rich material is mixed with the one-dimensional carbon material loaded with a catalyst, specifically comprising: dissolving the lithium-rich material in deionized water, then dispersing the one-dimensional carbon material loaded with the catalyst in ethanol, mixing the deionized water (containing the lithium-rich material) and ethanol (containing the one-dimensional carbon material loaded with the catalyst), and obtaining the lithium-supplementing material after filtering and drying.
[0099] Optionally, in step S20, deionized water (containing the lithium-rich material) can be added dropwise to ethanol (containing the one-dimensional carbon material loaded with the catalyst) by a peristaltic pump.
[0100] In one embodiment, based on the above step S10, the present invention further provides a method for preparing a heterojunction, please refer to Figure 4 , specifically used for preparing a heterojunction of metal oxide and metal sulfide, comprising the following steps:
[0101] Step S11, mixing the catalyst raw material with the one-dimensional carbon material to react, to obtain the one-dimensional carbon material loaded with metal oxides.
[0102] Step S12, mixing and reacting the one-dimensional carbon material loaded with metal oxides with a sulfur source to obtain a one-dimensional carbon material loaded with a catalyst.
[0103] The catalyst in step S12 includes metal oxides, metal sulfides and metal heterojunction compounds, and the metal heterojunction compound is a heterojunction formed by metal oxides and metal sulfides.
[0104] Optionally, in step S11, the catalyst raw material is mixed with the one-dimensional carbon material for reaction, which can refer to step S10 in the above embodiment and will not be described in detail here.
[0105] Optionally, in step S12, the one-dimensional carbon material loaded with metal oxides is mixed and reacted with a sulfur source, specifically comprising: dispersing the one-dimensional carbon material loaded with metal oxides in deionized water, then adding an appropriate amount of sulfur source to the deionized water, transferring it to a reactor, and obtaining the one-dimensional carbon material loaded with a catalyst through a hydrothermal reaction.
[0106] Optionally, in step S12, the sulfur source may be thioacetamide, and the hydrothermal reaction is carried out at 120°C for 1 to 2 hours.
[0107] The lithium-supplementing material preparation method provided by the present invention can be used to prepare a composite lithium-supplementing material, which includes a one-dimensional carbon material, a heterojunction catalyst and a lithium-rich material. The preparation method first grows a metal oxide catalyst in situ on a conductive carbon composed of a one-dimensional carbon material, and then sulfurizes part of the metal oxide catalyst into a metal sulfide through a sulfurization reaction, and a heterojunction is formed at the connection between the sulfurized metal sulfide and the metal oxide.
[0108] Under the influence of the one-dimensional carbon material, it can provide active sites for the growth of the catalyst. The metal oxide catalyst grown in situ has the characteristics of small particle size, and the catalyst can still maintain the original particle size after sulfurization, so that the catalyst particle size is small in the lithium-supplementing material provided by the present invention, so that the catalyst can fully exert the catalytic effect and reduce the decomposition voltage of the lithium-rich material. At the same time, the preparation method provided by the present invention also grows lithium-rich materials in situ, and the lithium-rich materials also have a small particle size, so that the lithium-rich material and the catalyst can be evenly mixed to form a good contact. Under the synergistic effect of the small particle sizes of the two, the conductivity of the lithium-rich material can be effectively improved and the decomposition voltage of the lithium-rich material can be reduced. In addition, the heterojunction of the metal sulfide and the metal oxide obtained after sulfurization can effectively improve the electron transfer efficiency and catalytic activity of the catalyst.
[0109] In a second aspect, the present invention provides a lithium supplement material, please refer to Figure 2 , including a one-dimensional carbon material 21, a lithium-rich material 10 and a catalyst 30, at least part of the lithium-rich material 10 and at least part of the catalyst 30 are loaded on the one-dimensional carbon material 21.
[0110] Specifically, in this aspect, the effects of the one-dimensional carbon material 21, the lithium-rich material 10 and the catalyst 30 and the effect of the combination of the three can all refer to the description of the first aspect. In a specific embodiment, the type of lithium-rich material 10 can refer to the one provided in the embodiment of the first aspect above, and will not be repeated here.
[0111] In one implementation, please refer to Figure 2 The lithium supplement material also includes a two-dimensional carbon material 22 , and part of the lithium-rich material 10 and part of the catalyst 30 are combined on the surface of the two-dimensional carbon material 22 .
[0112] Specifically, in this aspect, the one-dimensional carbon material 21 includes one or more of carbon nanotubes, carbon nanorods, and carbon nanofibers. In a specific embodiment, the one-dimensional carbon material 21 may be carbon nanotubes (CNTs), and the two-dimensional carbon material 22 may be carbon nanosheets (NPs).
[0113] In a specific embodiment, the one-dimensional carbon material 21 and the two-dimensional carbon material 22 can be mixed and combined together irregularly. Since the one-dimensional carbon material 21 and the two-dimensional carbon material 22 have different shapes and in the case of intermolecular forces, the one-dimensional carbon material 21 and the two-dimensional carbon material 22 can form a three-dimensional structure together; and since the one-dimensional carbon material 21 and the two-dimensional carbon material 22 do not form a tight connection, more gaps will be formed between the one-dimensional carbon material 21 and the two-dimensional carbon material 22, so that the one-dimensional carbon material 21 and the two-dimensional carbon material 22 together form the above-mentioned conductive network structure.
[0114] In one implementation, please refer to Figure 2 The lithium-rich material 10 and the catalyst 30 are both connected to the one-dimensional carbon material 21 and the two-dimensional carbon material 22, and at least part of the lithium-rich material 10 and the catalyst 30 are contained in the gap.
[0115] In one embodiment, in the second aspect, the catalyst 30 and the lithium-rich material 10 are both in-situ grown on the one-dimensional carbon material 21 and the two-dimensional carbon material 22 .
[0116] In one implementation, please refer to Figure 2 The number of the two-dimensional carbon material 22 is multiple, and the multiple two-dimensional carbon materials 22 are stacked; and / or at least one one-dimensional carbon material 21 is inserted in the gap between two adjacent two-dimensional carbon materials 22.
[0117] Specifically, Figure 2 As shown, multiple sheets of two-dimensional carbon material 22 are stacked together, and one-dimensional carbon material 21 is interspersed in the gap between two adjacent two-dimensional carbon materials 22. Optionally, in a specific embodiment, the number of one-dimensional carbon materials 21 interspersed in the gap is multiple, and the multiple one-dimensional carbon materials 21 are woven into a mesh. Therefore, the one-dimensional carbon material 21 and the two-dimensional carbon material 22 together form a multilayer structure, respectively including a two-dimensional carbon material layer and a one-dimensional carbon material mesh layer, and the one-dimensional carbon material mesh layer is between two adjacent two-dimensional carbon material layers.
[0118] By inserting the one-dimensional carbon material 21 between the two-dimensional carbon materials 22, it is possible to prevent multiple pieces of two-dimensional carbon materials 22 from stacking and agglomerating. The intercalation effect of the one-dimensional carbon material 21 supports the stacked two-dimensional carbon material 22, which can prevent the stacking collapse in the subsequent reaction; and under the intercalation effect of the one-dimensional carbon material 21, the two-dimensional carbon material 22 can expose a larger specific surface area and more active sites, which is conducive to the growth of more catalysts 30 and lithium-rich materials 10. The lithium-rich material 10 is more likely to recrystallize on the surface of the catalyst 30, which can prevent the contact between the catalyst 30 and the electrolyte to a certain extent and reduce the occurrence of side reactions; moreover, the lithium-rich material 10 can be in close contact with the catalyst 30 to achieve a good catalytic effect. The combination of the two-dimensional carbon material 22 and the one-dimensional carbon material 21 creates a large number of pore structures, which is conducive to the overflow of the gas generated during the lithium-rich material delithiation process and protects the integrity of the material structure. In addition, a certain interlayer spacing between adjacent two-dimensional carbon materials 22 can effectively alleviate the expansion problem of the lithium-rich material 10 during the charging and discharging process. The electronic structure and stability of the active sites are effectively regulated by the one-dimensional carbon material 21 and the two-dimensional carbon material 22, thereby enhancing the charge transfer at the interface and accelerating the delithiation reaction kinetics of the lithium-rich material 10.
[0119] In one embodiment, at least part of the one-dimensional carbon material 21 has a gap so that the inside of the one-dimensional carbon material 21 is connected to the external space. Specifically, a gap left by etching is formed on the one-dimensional carbon material 21. In a specific embodiment, the gap is formed on the outer surface of the one-dimensional carbon material 21 and extends to the inside of the one-dimensional carbon material 21, and the gap also extends in the axial direction of the one-dimensional carbon material 21.
[0120] In a specific embodiment, since the one-dimensional carbon material 21 is fibrous or tubular, the gaps on its surface are similar to the cuts in the material (e.g., cutting bamboo), so that the inside of the one-dimensional carbon material 21 is connected to the external space. Optionally, the catalyst 30 can be grown at the gaps of the one-dimensional carbon material 21 to be accommodated in the gaps.
[0121] By opening a gap on the one-dimensional carbon material 21, the interior of the one-dimensional carbon material 21 is connected with the external space, and the one-dimensional carbon material 21 can expose a larger specific surface area and more active sites, which is conducive to the growth of more catalysts 30 and lithium-rich materials 10. In addition, the gap on the one-dimensional carbon material 21 can also serve as a guide channel for the gas generated by the lithium-rich material 10, which can guide the gas generated by the lithium-rich material 10 after discharge, and avoid the gas generated by the lithium-rich material 10 from accumulating in the material, thereby reducing the impact of gas production on the battery, and ultimately achieving the purpose of improving battery performance.
[0122] In one embodiment, the two-dimensional carbon material 22 has holes, and at least part of the one-dimensional carbon material 21 is interspersed in the holes. Specifically, the surface of the two-dimensional carbon material 22 has holes, and the holes penetrate the two opposite sides of the two-dimensional carbon material 22. In a specific embodiment, since the one-dimensional carbon material 21 is contained in the interlayer gap of the two-dimensional carbon material 22, part of the one-dimensional carbon material 21 will extend into the holes. In this way, the one-dimensional carbon material 21 is interspersed in the two-dimensional carbon material 22, and the one-dimensional carbon material 21 and the two-dimensional carbon material 22 form an interwoven three-dimensional network structure.
[0123] By opening holes in the two-dimensional carbon material 22, the two-dimensional carbon material 22 can expose a larger specific surface area and more active sites, which is conducive to the growth of more catalysts 30 and lithium-rich materials 10. In addition, the holes in the two-dimensional carbon material 22 can also serve as a flow channel for the gas generated by the lithium-rich material 10, which can guide the gas generated by the lithium-rich material 10 after discharge, and avoid the gas generated by the lithium-rich material 10 from accumulating in the material, thereby reducing the impact of gas production on the battery, and ultimately achieving the purpose of improving battery performance.
[0124] In one embodiment, the one-dimensional carbon material 21 and / or the two-dimensional carbon material 22 is doped with non-metallic elements, and the non-metallic elements include at least one of O, N, and S. Specifically, in the second aspect, the one-dimensional carbon material 21 is doped with O elements, and the two-dimensional carbon material 22 is doped with N elements and S elements.
[0125] In a specific embodiment, the O element is mainly doped in the gaps of the one-dimensional carbon material 21 , and the N element and the S element are doped on the large surface of the two-dimensional carbon material 22 .
[0126] By doping the one-dimensional carbon material 21 with O element and the two-dimensional carbon material 22 with N element and S element, more defect sites can be formed on the one-dimensional carbon material 21 and the two-dimensional carbon material 22. The electronic structure and stability of the active sites can be effectively regulated through the defect sites, thereby enhancing the charge transfer at the interface and accelerating the delithiation reaction kinetics of the material.
[0127] In one embodiment, the catalyst 30 comprises a metal oxide having a general chemical formula of D2 n3 O m3 , wherein D2 is a transition metal element, D2 includes at least one of Co, Mo, W, V, Ti, Fe, Ni, Mn, Cr, Cu, and Zn, 1≤n3≤3, 1≤m3≤3. In a specific embodiment, the metal oxide grown on the one-dimensional carbon material 21 and the two-dimensional carbon material 22 includes manganese oxide, cobalt oxide, nickel oxide, titanium oxide, and the like.
[0128] In one embodiment, at least part of the lithium-rich material 10 and at least part of the catalyst 30 are in contact with each other, and part of the lithium-rich material 10 is coated on the outer surface of the catalyst 30. Specifically, in the preparation process of the lithium-supplementing material, the catalyst 30 can be first grown on the one-dimensional carbon material 21 and the two-dimensional carbon material 22, and then the lithium-rich material 10 is grown on the one-dimensional carbon material 21 and the two-dimensional carbon material 22. Therefore, during the growth process of the lithium-rich material 10, the catalyst 30 will be directly coated.
[0129] In one embodiment, the thickness of the lithium-rich material 10 coated on the surface of the catalyst 30 is 2 nm to 1 μm. Optionally, the thickness of the lithium-rich material 10 coated on the surface of the conductive carbon and the catalyst 30 may be 2 nm, 5 nm, 10 nm, 20 nm, 50 nm, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, or 1 μm.
[0130] When the coating thickness of the lithium-rich material 10 is within the above range, it can ensure that the lithium-rich material 10 is in full contact with the catalyst 30, thereby improving the catalytic effect. When the coating thickness is less than the above range, it means that the content of the lithium-rich material 10 is relatively small, which is not conducive to improving the lithium replenishment capacity of the lithium replenishment material. When the coating thickness is greater than the above range, part of the lithium-rich material 10 will not be in contact with the catalyst 30, thereby affecting the catalytic effect of the catalyst 30.
[0131] In one embodiment, the length of the one-dimensional carbon material 21 is 5 μm to 20 μm. Optionally, the length of the one-dimensional carbon material 21 may be 5 μm, 6 μm, 8 μm, 10 μm, 12 μm, 14 μm, 16 μm, 18 μm, or 20 μm.
[0132] When the length of the one-dimensional carbon material 21 is within the above range, it can ensure that the one-dimensional carbon material 21 has a larger specific surface area, thereby providing higher conductivity and better bearing capacity for the lithium-rich material 10. When the length of the one-dimensional carbon material 21 is less than the above range, the one-dimensional carbon material 21 is shorter, resulting in fewer attachment points provided by the one-dimensional carbon material 21 to the lithium-rich material 10, making the bonding between the lithium-rich material 10 and the one-dimensional carbon material 21 poor. When the length of the one-dimensional carbon material 21 is greater than the above range, the biomass carbon carrier is longer, resulting in a decrease in the specific surface area of the one-dimensional carbon material 21, which is not conducive to improving conductivity.
[0133] In one embodiment, the diameter of the one-dimensional carbon material 21 is 2 nm to 5 nm. Optionally, the diameter of the one-dimensional carbon material 21 can be 2 nm, 3 nm, 4 nm, or 5 nm.
[0134] When the diameter of the one-dimensional carbon material 21 is within the above range, it can ensure that the one-dimensional carbon material 21 has a larger specific surface area, thereby providing higher conductivity, and the one-dimensional carbon material 21 has higher strength. When the diameter of the one-dimensional carbon material 21 is smaller than the above range, the one-dimensional carbon material 21 is thinner, resulting in the deterioration of the strength of the one-dimensional carbon material 21, and it is easy to break and fall off. When the diameter of the one-dimensional carbon material 21 is larger than the above range, the biomass carbon carrier is coarser, resulting in a decrease in the specific surface area of the one-dimensional carbon material 21, which is not conducive to improving conductivity.
[0135] In one embodiment, the thickness of the two-dimensional carbon material 22 is 1 nm to 10 nm. Optionally, the thickness of the two-dimensional carbon material 22 can be 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, or 10 nm.
[0136] When the thickness of the lithium-rich material 10 is within the above range, it can ensure that the material has a high self-strength and a high curlability. When the thickness of the lithium-rich material 10 is less than the above range, the lithium-rich material 10 is thinner, resulting in a decrease in the strength of the lithium-rich material 10 and a tendency to break and fall off. When the thickness of the lithium-rich material 10 is greater than the above range, the lithium-rich material 10 is thicker, resulting in an increased difficulty in curling the lithium-rich material 10 and difficulty in firmly bonding to the surface of the one-dimensional carbon material 21.
[0137] In one embodiment, the pore size of the two-dimensional carbon material 22 is 1 nm to 5 nm. Optionally, the pore size of the two-dimensional carbon material 22 can be 1 nm, 1.5 nm, 2 nm, 2.5 nm, 3 nm, 3.5 nm, 4 nm, 4.5 nm, or 5 nm.
[0138] When the pore size of the two-dimensional carbon material 22 is within the above range, it can ensure that the two-dimensional carbon material 22 has a larger surface area and more active sites, and can also ensure the structural stability of the two-dimensional carbon material 22. When the pore size of the two-dimensional carbon material 22 is smaller than the above range, the specific surface area of the two-dimensional carbon material 22 is limited, which is not conducive to improving the combination of the catalyst 30 and the lithium-rich material 10 with the two-dimensional carbon material 22; when the pore size of the two-dimensional carbon material 22 is larger than the above range, the structural stability of the two-dimensional carbon material 22 is poor.
[0139] In one embodiment, the porosity of the two-dimensional carbon material 22 is 30% to 70%. Optionally, the porosity of the two-dimensional carbon material 22 may be 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, or 70%.
[0140] When the porosity of the two-dimensional carbon material 22 is within the above range, the two-dimensional carbon material 22 can have a larger specific surface area to combine with the catalyst 30 and the lithium-rich material 10, and ensure the structural stability of the two-dimensional carbon material 22. When the porosity of the two-dimensional carbon material 22 is less than the above range, the specific surface area of the two-dimensional carbon material 22 is limited, which is not conducive to improving the combination of the catalyst 30 and the lithium-rich material 10 with the two-dimensional carbon material 22. When the porosity of the two-dimensional carbon material 22 is greater than the above range, the structural stability of the two-dimensional carbon material 22 deteriorates, and the overall strength of the lithium-supplementing material deteriorates.
[0141] In one embodiment, the mass ratio of the one-dimensional carbon material 21 to the two-dimensional carbon material 22 is 1:(1-10). Optionally, the mass ratio of the one-dimensional carbon material 21 to the two-dimensional carbon material 22 can be 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10.
[0142] Meeting the mass ratio of the one-dimensional carbon material 21 and the two-dimensional carbon material 22 within the above range can ensure that the one-dimensional carbon material 21 and the two-dimensional carbon material 22 cooperate with each other to increase the specific surface area and active sites for a better effect. When the mass ratio of the one-dimensional carbon material 21 is relatively small, the content of the one-dimensional carbon material 21 in the interlayer gap of the two-dimensional carbon material 22 is relatively small, and the two-dimensional carbon material 22 cannot be effectively supported, resulting in the two-dimensional carbon material 22 being easily stacked and collapsed during subsequent processing. When the mass ratio of the one-dimensional carbon material 21 is relatively large, the surface of the two-dimensional carbon material 22 is covered by the one-dimensional carbon material 21, resulting in the catalyst 30 and the lithium-rich material 10 being difficult to combine with the two-dimensional carbon material 22, and the two-dimensional carbon material 22 is difficult to exert its effect.
[0143] In one embodiment, the specific surface area of the one-dimensional carbon material 21 and the two-dimensional carbon material 22 is 200 m 2 / g~800m 2 / g. Specifically, it can be the common specific surface area of the one-dimensional carbon material 21 and the two-dimensional carbon material 22 in the second aspect. Optionally, the specific surface area of the one-dimensional carbon material 21 and the two-dimensional carbon material 22 can be 200m 2 / g、300m 2 / g, 400m 2 / g、500m 2 / g, 600m 2 / g、700m 2 / g、800m 2 / g.
[0144] The present invention forms a multi-layer conductive network structure by mixing the one-dimensional carbon material 21 and the two-dimensional carbon material 22. In addition, the stacked two-dimensional carbon material 22 is supported by the one-dimensional carbon material 21 interspersed in the interlayer gap of the two-dimensional carbon material 22 to prevent the stacking collapse in the subsequent reaction and expose a larger active surface area and active sites for the growth of the catalyst 30 and the lithium-rich material 10.
[0145] When the specific surface areas of the one-dimensional carbon material 21 and the two-dimensional carbon material 22 are within the above range, the loading amount of the lithium-rich material 10 and the catalyst 30 can be increased, and the active sites of the two on the one-dimensional carbon material 21 and the two-dimensional carbon material 22 can be increased, thereby improving the lithium replenishment capacity and electrochemical performance of the lithium replenishment material, and inhibiting the lattice volume expansion of the lithium-rich material 10. When the specific surface areas of the one-dimensional carbon material 21 and the two-dimensional carbon material 22 are less than the above range, the loading amount of the lithium-rich material 10 and the catalyst 30 is small, not only the capacity improvement is limited, but also the effect of the catalyst 30 is weak. When the specific surface area of the porous carbon carrier is greater than the above range, it is difficult for the porous carbon carrier to inhibit the lattice volume expansion of the lithium-rich material 10.
[0146] In one embodiment, the particle size of the lithium-rich material 10 is 10 nm to 1 μm. Optionally, in this aspect, the particle size of the lithium-rich material 10 can be 10 nm, 20 nm, 50 nm, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm, or 1 μm.
[0147] When the particle size of the lithium-rich material 10 is within the above range, it can be ensured that the lithium-rich material 10 can be loaded onto the one-dimensional carbon material 21 and the two-dimensional carbon material 22 as much as possible, and the connection sites with the catalyst 30 are increased, and the material has a higher conductivity and avoids material agglomeration. When the particle size of the lithium-rich material 10 is smaller than the above range, the difficulty of preparing the lithium-rich material 10 increases, and the lithium-rich material 10 is easy to agglomerate and difficult to disperse; when the particle size of the lithium-rich material 10 is larger than the above range, the conductivity of the lithium-rich material 10 is too poor, and the connection density between the conductive agent and the catalyst 30 is reduced, and the catalyst 30 is difficult to effectively catalyze the lithium-rich material 10.
[0148] In one embodiment, the particle size of the catalyst 30 is 2 nm to 10 nm. Optionally, in this aspect, the particle size of the catalyst 30 can be 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, or 10 nm.
[0149] When the particle size of the catalyst 30 is within the above range, it can ensure that the catalyst 30 has a high catalytic performance, and can also reduce the difficulty of preparing the catalyst 30 and avoid agglomeration of the catalyst 30. When the particle size of the catalyst 30 is smaller than the above range, the difficulty of preparing the catalyst 30 increases, and the agglomeration of the catalyst 30 is serious, which affects the performance of its catalytic performance; when the particle size of the catalyst 30 is larger than the above range, the catalytic performance of the catalyst 30 decreases.
[0150] In one embodiment, the mass ratio of the lithium-rich material 10, the catalyst 30 and the conductive carbon support (including the one-dimensional carbon material 21 and the two-dimensional carbon material 22) is 100:(1-10):(5-40). Optionally, the mass ratio of the lithium-rich material 10, the catalyst 30 and the conductive carbon carrier can be 100:(1-10):5, 100:(1-10):10, 100:(1-10):15, 100:(1-10):20, 100:(1-10):25, 100:(1-10):30, 100:(1-10):35, 100:(1-10):40, 100:1:(5-40), 100:2:(5-40), 100:4:(5-40), 100:6:(5-40), 100:8:(5-40), 100:10:(5-40).
[0151] When the mass proportion of the three materials is within the above range, the lithium replenishing capacity of the lithium replenishing material can be ensured, and the catalytic effect of the catalyst 30 can be fully exerted, and the conductivity of the material can be ensured, and the delithiation potential of the lithium-rich material 10 can be reduced. When the mass proportion of the one-dimensional carbon material 21 and the two-dimensional carbon material 22 is less than the above range, the one-dimensional carbon material 21 and the two-dimensional carbon material 22 have limited improvement in the conductivity of the lithium-rich material 10, and the one-dimensional carbon material 21 and the two-dimensional carbon material 22 have limited carrying capacity for the lithium-rich material 10 and the catalyst 30, so they can carry more lithium-rich materials 10 and catalysts 30. When the mass proportion of the catalyst 30 is less than the above range, the catalytic effect and conductivity of the catalyst 30 are poor. When the mass proportion of the above two materials is greater than the above range, the proportion of the lithium-rich material 10 will be further reduced, and the lithium-rich material 10 will find it difficult to exert more battery capacity, resulting in a decrease in the energy density of the battery.
[0152] In one embodiment, the present invention provides a method for preparing a lithium supplement material, please refer to Figure 5 , specifically used to prepare the lithium supplement material provided in the second aspect, comprising the following steps:
[0153] Step SS10: mixing the catalyst raw material with the one-dimensional carbon material to react, so that at least part of the catalyst is loaded on the one-dimensional carbon material.
[0154] Step SS20, mixing the lithium-rich material with the one-dimensional carbon material carrying the catalyst, so that at least a portion of the lithium-rich material is loaded on the one-dimensional carbon material, to obtain a lithium-supplementing material.
[0155] In one embodiment, the lithium supplement material prepared by the method for preparing the lithium supplement material provided by the present invention also includes a two-dimensional carbon material. Figure 5 , before step SS10, it also includes step SS00: preparing a mixture of a one-dimensional carbon material and a two-dimensional carbon material to obtain a conductive carbon support.
[0156] Therefore, based on the above step SS00, step SS10 includes: mixing the catalyst raw material with the conductive carbon carrier to react, so that at least part of the catalyst is loaded on the one-dimensional carbon material.
[0157] Therefore, based on the above step SS00, step SS20 includes: mixing the lithium-rich material with the conductive carbon carrier carrying the catalyst, so that at least part of the lithium-rich material is loaded on the one-dimensional carbon material to obtain a lithium-supplementing material.
[0158] In one embodiment, based on the above step SS00, the present invention also provides a method for preparing a conductive carbon carrier, please refer to Figure 6 , specifically for a conductive carbon carrier composed of a one-dimensional carbon material and a two-dimensional carbon material, comprising the following steps:
[0159] Step SS01, forming gaps on the one-dimensional carbon material raw material, and doping heteroatoms on the one-dimensional carbon material raw material to obtain a one-dimensional carbon material.
[0160] Step SS02, mixing the two-dimensional carbon material raw material, the driving agent, the template agent and the activating agent, placing them in a freezing environment for freeze drying after sufficient reaction, and then heat treating the freeze-dried mixture, and obtaining the two-dimensional carbon material after washing and drying.
[0161] Step SS03, mixing the one-dimensional carbon material and the two-dimensional carbon material to obtain a conductive carbon carrier.
[0162] Optionally, in step SS01, gaps are formed on the one-dimensional carbon material raw material, and heteroatoms are doped on the one-dimensional carbon material raw material, specifically comprising: placing the one-dimensional carbon material raw material and nitrate in an acid solution, stirring them fully in an ice bath environment, and then adding potassium permanganate thereto, continuing to stir the reaction in an environment higher than the ice bath temperature, and then adding hydrogen peroxide thereto, filtering after centrifugal washing, and obtaining an oxygen-doped one-dimensional carbon material with gaps after drying.
[0163] Optionally, in step SS01, the one-dimensional carbon material raw material may be multi-walled carbon nanotubes (MWCNTs), the acid solution may be concentrated sulfuric acid with a concentration of 98%, and the mass fraction of hydrogen peroxide may be 30%.
[0164] Optionally, in step SS01, the environment temperature higher than the ice bath temperature is 40° C. and above.
[0165] Optionally, in step SS01, the specific washing process includes washing with ethanol and deionized water for several times until the pH value of the centrifuged suspension is close to 7.
[0166] Optionally, in step SS02, the two-dimensional carbon material raw material, the driver, the template and the activator are mixed, specifically comprising: placing the two-dimensional carbon material raw material, the driver, the template and the activator in deionized water and stirring until dissolved.
[0167] Optionally, in the above steps, the raw material of the two-dimensional carbon material is n-allylthiourea, the driving agent and the template agent are both potassium sulfate, and the activator is potassium nitrate. The advantage of using n-allylthiourea as a raw material is that n-allylthiourea itself is rich in S and N elements. After the carbonization of n-allylthiourea, the rich S and N elements are retained, thereby forming rich heteroatom doping. Potassium nitrate is used as a combustion activator, and potassium sulfate is used as a sulfur source / salt template and synergistic activator to form pores and defects on the surface of the carbon material.
[0168] Optionally, in step SS02, freeze drying is performed in a freezing environment, specifically comprising: freezing the solution (including the two-dimensional carbon material raw material, the driver, the template and the activator) at -20°C for 24 hours, and then continuing to freeze drying at -45°C.
[0169] Optionally, in step SS02, the freeze-dried mixed material is heat treated at a temperature of 600°C to 800°C.
[0170] In one embodiment, based on the above step SS20, the catalyst raw material and the conductive carbon carrier are mixed for reaction, specifically comprising: dispersing the one-dimensional carbon material and the two-dimensional carbon material in a dispersion, then adding the catalyst raw material to the dispersion, adding urea to the dispersion after stirring and dispersing, placing the dispersion in a hydrothermal reactor to react, centrifugally washing and then drying to obtain a conductive carbon carrier loaded with the catalyst.
[0171] Optionally, in step SS10, the catalyst raw material includes a transition metal salt, specifically including but not limited to sulfates, chlorides, nitrates, organic acid salts, and the like.
[0172] Optionally, in step SS20, the lithium-rich material and the conductive carbon carrier loaded with the catalyst are mixed for reaction, specifically comprising: dissolving the lithium-rich material in deionized water, then dispersing the conductive carbon carrier loaded with the catalyst in ethanol, mixing the deionized water (containing the lithium-rich material) and ethanol (containing the conductive carbon carrier loaded with the catalyst), and obtaining the lithium-supplementing material after filtering and drying.
[0173] The lithium-supplementing material preparation method provided by the present invention can be used to prepare a composite lithium-supplementing material, which includes a one-dimensional carbon material, a two-dimensional carbon material, a catalyst and a lithium-rich material. The preparation method first opens a gap on the one-dimensional carbon material and performs doping, then prepares a two-dimensional carbon material doped with heteroatoms, then inserts the one-dimensional carbon material into the interlayer gap of the two-dimensional carbon material through a hydrothermal reaction, and grows a catalyst on the surface of a conductive carbon carrier through a hydrothermal reaction and recrystallizes a lithium-rich material.
[0174] In a third aspect, the present invention further provides a positive electrode material, the positive electrode material comprising a positive electrode active material and a lithium supplement material. The lithium supplement material is the lithium supplement material provided in the above-mentioned embodiment. Optionally, the positive electrode active material can be a phosphate positive electrode active material and a ternary positive electrode active material, and in a specific embodiment, includes one or more of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, lithium manganese iron phosphate, lithium vanadium phosphate, lithium vanadium oxyphosphate, lithium fluorinated vanadium phosphate, lithium titanate, lithium nickel cobalt manganese oxide, and lithium nickel cobalt aluminum oxide.
[0175] In one embodiment, the content of lithium-supplementing material in the positive electrode material can be controlled at 1% to 6% of the mass of the positive electrode active material. This ratio can just make up for the loss of active lithium in the battery during the first charging process. If the amount of lithium-supplementing material added to the positive electrode material is too low, the active lithium lost in the positive electrode active material cannot be fully replenished, which is not conducive to improving the energy density and capacity retention rate of the battery. If the amount of lithium-supplementing material added to the positive electrode active material is too high, the original reversible capacity will be occupied and the cost will be increased. In some specific embodiments, in the positive electrode material, the mass percentage of the lithium-supplementing material can be 1%, 2%, 4%, 6%, etc.
[0176] In a fourth aspect, the present invention further provides a positive electrode sheet, the positive electrode sheet comprising a current collector and an active material layer disposed on the current collector, the active material layer comprising the lithium supplement material of any one of the above embodiments, or the active material layer comprising the lithium supplement material obtained by the preparation method of the lithium supplement material of the above embodiments.
[0177] In one embodiment, the positive electrode sheet includes a positive electrode current collector, and the positive electrode current collector has a positive electrode active layer, and the positive electrode active layer includes components such as positive electrode active materials, lithium supplement materials, conductive agents, and binders. The present invention does not specifically limit these materials, and suitable materials can be selected according to actual application requirements. The positive electrode current collector includes but is not limited to any one of copper foil and aluminum foil. The conductive agent includes one or more of graphite, carbon black, acetylene black, graphene, carbon fiber, C60 and carbon nanotubes, and the content of the conductive agent in the positive electrode active layer is 3wt% to 5wt%. The types of binders include polyvinylidene chloride, soluble polytetrafluoroethylene, styrene-butadiene rubber, hydroxypropyl methylcellulose, methylcellulose, carboxymethyl cellulose, polyvinyl alcohol, acrylonitrile copolymer, sodium alginate, chitosan and chitosan derivatives, and the content of the binder in the positive electrode active layer is 2wt% to 4wt%.
[0178] In a fifth aspect, the present invention further provides a secondary battery, comprising a negative electrode, a separator and the positive electrode described above. The positive electrode comprises the composite positive electrode material described above.
[0179] The technical solution of the present invention is described in detail below through specific embodiments.
[0180] Example 1
[0181] This embodiment provides a lithium supplement material, which includes a one-dimensional carbon material (CNTs), a lithium-rich material (Li 2 C 2 O 4 ) and catalyst (CoO / CoS 2 ), wherein the lithium-rich material and the catalyst are distributed on the one-dimensional carbon material, and a heterojunction is formed at the junction of CoS and CoO in the catalyst.
[0182] The length of CNTs is 25 μm, the diameter of CNTs is about 10 nm, and the specific surface area of CNTs is 140 m 2 / g.Li 2 C 2 O 4 The D50 of CoO / CoS is 3μm. 2 The particle size is about 50 nm. The mass ratio of lithium-rich material, catalyst and one-dimensional carbon material is 100:10:5.
[0183] The preparation method of the lithium supplement material comprises the following steps:
[0184] 1) Take 3 mmol of cobalt nitrate and dissolve it in 30 ml of deionized water, then add 0.5 g of CNTs and 20 ml of ethanol, stir for 5 ml, and ultrasonicate for 30 min.
[0185] 2) Add 2 ml of ammonia water to the solution in 1), stir thoroughly and ultrasonicate for 15 min, then react at 70 °C for 6 h, wash and dry the precipitate to obtain catalyst precursor A (Co(OH) 2 @CNTs).
[0186] 3) The catalyst precursor A was placed in an Ar atmosphere and sintered at 400° C. for 5 h to obtain the precursor B (CoO@CNTs).
[0187] 4) Take 0.5g of precursor B and disperse it in 40ml of deionized water, add 0.06g of TAA (thioacetamide), stir thoroughly and transfer it into a reactor, react at 120 degrees for 2h, wash and dry the precipitate to obtain catalyst C (CoO / CoS 2 @CNTs).
[0188] 5) Prepare a saturated lithium oxalate solution with deionized water, disperse the catalyst C in ethanol, and use a peristaltic pump to drop the saturated lithium oxalate solution into the ethanol solution of the catalyst C at a dropping rate of 5 ml / min. The two solutions are stirred throughout the process at a speed of 400 rpm.
[0189] 6) The solution obtained in 5) is filtered to obtain an intermediate product, which is placed in a vacuum drying oven and dried at 60 degrees for 12 hours to remove the solvent to obtain a lithium supplement material.
[0190] Example 2
[0191] This embodiment provides a lithium supplement material. The difference between this embodiment 2 and embodiment 1 is that the length of CNTs is about 10 μm, the diameter of CNTs is about 8 nm, and the specific surface area of CNTs is 200 m 2 / g.
[0192] Example 3
[0193] This embodiment provides a lithium supplement material. The difference between this embodiment 3 and embodiment 1 is that the length of CNTs is about 50 μm, the diameter of CNTs is about 15 nm, and the specific surface area of CNTs is 90 m 2 / g.
[0194] Example 4
[0195] This embodiment provides a lithium supplement material. The difference between this embodiment 4 and embodiment 1 is that: Li 2 C 2 O 4 The D50 is 1μm.
[0196] Example 5
[0197] This embodiment provides a lithium supplement material. The difference between this embodiment 5 and embodiment 1 is that the catalyst only includes CoO.
[0198] Example 6
[0199] This embodiment provides a lithium supplement material. The difference between this embodiment 6 and embodiment 1 is that the catalyst only includes CoS 2 .
[0200] Example 7
[0201] This embodiment provides a lithium supplement material. The difference between this embodiment 7 and embodiment 1 is that: CoO / CoS 2 The particle size is about 10nm.
[0202] Example 8
[0203] This embodiment provides a lithium supplement material. The difference between this embodiment 8 and embodiment 1 is that: CoO / CoS 2 The particle size is about 100nm.
[0204] Example 9
[0205] This embodiment provides a lithium supplement material. The difference between this embodiment 9 and embodiment 1 is that the mass ratio of the lithium-rich material, the catalyst and the one-dimensional carbon material is 100:4:1.
[0206] Example 10
[0207] This embodiment provides a lithium supplement material. The difference between this embodiment 10 and embodiment 1 is that the mass ratio of the lithium-rich material, the catalyst and the one-dimensional carbon material is 100:15:5.
[0208] Embodiment 11
[0209] This embodiment provides a lithium supplement material. The difference between this embodiment 11 and embodiment 1 is that the catalyst is NiO / NiS2 .
[0210] Example 12
[0211] This embodiment provides a lithium-supplementing material. The difference between this embodiment 12 and embodiment 1 is that the lithium-rich material is lithium quartz (Li 2 C 4 O 4 ).
[0212] Example 13
[0213] This embodiment provides a lithium supplement material, which includes a conductive carbon carrier (CNTs and NPs), a lithium-rich material (Li 2 C 2 O 4 ) and catalyst (MnO), wherein the lithium-rich material and the catalyst are distributed on the conductive carbon support, CNTs are interspersed in the interlayer gaps of NPs, CNTs are doped with O element, and NPs are doped with N element and S element.
[0214] The length of CNTs is 5 μm to 15 μm, the diameter of CNTs is 2 nm to 5 nm, the thickness of NPs is 3 nm, the pore diameter of NPs is 3 nm, the mass ratio of CNTs to NPs is 1:3, the porosity of NPs is 60%, and the specific surface area of CNTs and NPs is 700 m 2 / g.
[0215] Li 2 C 2 O 4 The particle size range is 10nm~100nm, Li 2 C 2 O 4 The coating thickness is 500nm, the particle size of MnO is 5nm to 30nm, and the mass ratio of the lithium-rich material, the catalyst and the conductive carbon carrier is 100:10:30.
[0216] The preparation method of the lithium supplement material comprises the following steps:
[0217] 1) Disperse 1g MWCNTs and 0.5g sodium nitrate in a round-bottom flask filled with 46mL concentrated sulfuric acid (98%), then stir the mixture in ice for half an hour, and then slowly add 5g potassium permanganate under strong stirring. After the addition is complete, remove the ice bath and then react at 40°C for 2h. After the reaction is completed, slowly add 100mL water under strong stirring. After the solution cools to room temperature, add 5mL H 2 O 2(mass fraction 30%). The obtained solution was centrifuged and washed with ethanol and deionized water several times until the pH of the centrifuged suspension was close to 7. Finally, the obtained product was transferred to a vacuum drying oven and dried at 60°C overnight to obtain CNTs.
[0218] 2) n-allylthiourea was used as a self-doping precursor, potassium sulfate was used as a sulfur source driver and salt template. Then a certain amount of potassium nitrate was added as an activator. The above materials were stirred and dissolved in 100 mL of deionized water solution for 4 h, frozen at -20 ° C for 24 h, freeze-dried at -45 ° C, and then calcined at 700 ° C for 2 h at 5 ° C / min. The resulting product was washed with hydrochloric acid and deionized water, and dried at 80 ° C for 24 h to obtain NPs.
[0219] 3) Weigh NPs and dissolve them in deionized water, sonicate for 1 h, then mix the obtained NPs dispersion with CNTs, continue sonicating for 1 h, and weigh MnSO 4 Add urea to the above dispersion, stir for 30 minutes, then add urea, and after it is completely dissolved, transfer all the solution to a polytetrafluoroethylene hydrothermal reactor for reaction, centrifuge and wash, and the product obtained after drying is MnO@CNTs / NPs.
[0220] 4) MnO@CNTs / NPs are fully dispersed in an ethanol solution. Then, a saturated lithium oxalate aqueous solution is added dropwise to the dispersed solution of MnO@CNTs / NPs for recrystallization, so that the lithium oxalate recrystallization covers the catalyst surface. The obtained recrystallized composite sample is placed in a tube furnace for high-temperature drying to obtain a lithium supplement material.
[0221] Embodiment 14
[0222] This embodiment provides a lithium supplement material. The difference between this embodiment 16 and embodiment 13 is that the thickness of NPs is about 1 nm, and the specific surface area of CNTs and NPs is 670 m 2 / g.
[0223] Embodiment 15
[0224] This embodiment provides a lithium supplement material. The difference between this embodiment 17 and embodiment 13 is that the thickness of NPs is about 10nm, and the specific surface area of CNTs and NPs is 352m 2 / g.
[0225] Example 16
[0226] This embodiment provides a lithium supplement material. The difference between this embodiment 18 and embodiment 13 is that the pore diameter of the NPs is about 1 nm, and the specific surface area of CNTs and NPs is 460 m 2 / g.
[0227] Embodiment 17
[0228] This embodiment provides a lithium supplement material. The difference between this embodiment 19 and embodiment 13 is that the pore diameter of the NPs is about 5 nm, and the specific surface area of CNTs and NPs is 720 m 2 / g.
[0229] Embodiment 18
[0230] This embodiment provides a lithium supplement material. The difference between this embodiment 20 and embodiment 13 is that the mass ratio of CNTs to NPs is 1:10.
[0231] Embodiment 19
[0232] This embodiment provides a lithium supplement material. The difference between this embodiment 21 and embodiment 13 is that the mass ratio of CNTs to NPs is 1:1.
[0233] Embodiment 20
[0234] This embodiment provides a lithium supplement material. The difference between this embodiment 22 and embodiment 13 is that: Li 2 C 2 O 4 The particle size is 500nm~1μm, Li 2 C 2 O 4 The coating thickness is about 1 μm.
[0235] Embodiment 21
[0236] This embodiment provides a lithium supplement material. The difference between this embodiment 27 and embodiment 13 is that the mass ratio of the lithium-rich material, the catalyst and the conductive carbon carrier is 100:1:10.
[0237] Embodiment 22
[0238] This embodiment provides a lithium supplement material. The difference between this embodiment 28 and embodiment 13 is that the mass ratio of the lithium-rich material, the catalyst and the conductive carbon carrier is 100:5:40.
[0239] Embodiment 23
[0240] This embodiment provides a lithium supplement material. The difference between this embodiment 29 and embodiment 13 is that the catalyst is MnO / MnS.
[0241] Comparative Example 1
[0242] This comparative example provides a lithium-rich material (Li 2 C 2 O 4 ).
[0243] Comparative Example 2
[0244] This comparative example provides a lithium supplement material, including Li 2 C 2 O 4 and CNTs, the two are simply mixed.
[0245] Comparative Example 3
[0246] This comparative example provides a lithium supplement material, including Li 2 C 2 O 4 , CNTs, CoS and CoO, the four are simply mixed.
[0247] Comparative Example 4
[0248] This comparative example provides a lithium supplement material, including Li 2 C 2 O 4 , CNTs, NPs and MnO, the four are simply mixed.
[0249] The lithium supplement materials provided in the above examples 1-23 and the lithium supplement materials provided in comparative examples 1-4 are respectively assembled into positive electrode sheets and lithium ion batteries according to the following methods:
[0250] Positive electrode sheet: The lithium supplement material, SP and PVDF are mixed in a mass ratio of 90:4:6 to prepare a positive electrode slurry, the positive electrode slurry is coated on the surface of aluminum foil, vacuum dried at 110°C overnight, and rolled to obtain a positive electrode sheet;
[0251] Negative electrode: lithium sheet;
[0252] Electrolyte: Ethylene carbonate and ethyl methyl carbonate were mixed in a volume ratio of 3:7, and LiPF was added 6 , forming an electrolyte, LiPF 6 The concentration is 1 mol / L;
[0253] Diaphragm: Polypropylene microporous separator;
[0254] Lithium-ion battery assembly: Assemble button-type lithium-ion full batteries in an inert atmosphere glove box in the order of negative electrode sheet - separator - electrolyte - positive electrode sheet.
[0255] The electrochemical performance of each lithium-ion battery assembled in the above lithium-ion battery embodiment was tested under the following test conditions:
[0256] The battery was charged at a rate of 0.1C with a cut-off voltage of 4.7V. The battery was charged at a constant voltage of 4.7V. After the charging process was completed, the battery was allowed to stand for 10 minutes and then discharged at a rate of 0.1C with a cut-off voltage of 2.5V. The charging platform was observed during the charging process to obtain the delithiation potential of the lithium supplement material.
[0257] The test results of the above lithium supplement materials and lithium batteries are shown in Tables 1 and 2 below:
[0258] Table 1. Test results of Example 1-Example 12 and Comparative Example 1-Comparative Example 3
[0259]
[0260] Table 2. Test results of Example 13-Example 23 and Comparative Example 4
[0261]
[0262]
[0263] From the test results of Examples 1 to 10 and Comparative Examples 1 to 3 in Table 1 and Table 2, it can be seen that the battery charging specific capacity and lithium replenishment capacity provided by Examples 1 to 10 are greater than those of Comparative Examples 1 to 3, and the delithiation potentials of Examples 1 to 10 are less than those of Comparative Examples 1 to 3, indicating that the lithium oxalate preparation method provided in the present application has a positive effect on reducing the delithiation potential of lithium oxalate and increasing the lithium replenishment capacity of lithium oxalate.
[0264] Furthermore, it can be seen from the test results of Example 1 and Comparative Example 3 that, compared with simple mixing, the lithium replenishment capacity of lithium oxalate can be further improved and the delithiation potential of lithium oxalate can be reduced through recrystallization integration, because recrystallization integration can make lithium oxalate fully contact with the catalyst and the conductive network, thereby improving the catalytic efficiency and reducing the delithiation potential of the material.
[0265] From the test results of Examples 1 to 3 in Table 1, it can be seen that the use of CNTs with a high specific surface area has a positive effect on reducing the delithiation potential of the material and increasing the lithium replenishment capacity. The reason is that a larger specific surface area can provide more active sites and improve the reaction efficiency.
[0266] From the test results of Example 1 and Example 4 in Table 1, it can be seen that lithium oxalate with a smaller particle size has a higher lithium replenishment capacity and a lower lithium desorption potential, because the reduction in the particle size of lithium oxalate can effectively increase the contact area with CNT and catalyst, and effectively reduce the lithium desorption potential.
[0267] It can be seen from the test results of Example 1, Example 5 and Example 6 in Table 1 that, compared with a single catalyst, forming a heterojunction catalyst has a positive effect on reducing the material decomposition voltage and increasing the lithium replenishment capacity, because the heterojunction structure can effectively improve the electron transfer efficiency and catalytic activity of the catalyst.
[0268] It can be seen from the test results of Example 1, Example 7 and Example 8 in Table 1 that, compared with catalysts with larger particle sizes, catalysts with smaller particle sizes have a positive effect on reducing the delithiation potential and increasing the lithium replenishment capacity, because reducing the particle size of the catalyst can effectively improve the catalytic efficiency and activity of the catalyst.
[0269] It can be seen from the test results of Example 1, Example 9 and Example 10 in Table 1 that the performance of the material will be affected by regulating the ratio of lithium oxalate, catalyst and CNT. When the ratio of catalyst to CNT is too high, the performance of the material decreases, because the low ratio of lithium oxalate leads to a decrease in the gram capacity of lithium supplementation. When the ratio of catalyst to CNT is too low, the performance of the material will also decrease, because the low ratio of catalyst affects the catalytic activity and thus reduces the gram capacity of lithium supplementation. However, the catalyst can effectively reduce the delithiation potential of the material, so that the solution provided in this application can be suitable for low-voltage usage scenarios.
[0270] It can be seen from the test results of Example 1 and Example 11 in Table 1 that the use of different heterojunction catalysts has a positive effect on reducing the lithium delithiation potential of lithium oxalate and increasing the lithium replenishment capacity.
[0271] It can be seen from the test results of Example 1 and Example 12 in Table 1 that the heterojunction catalyst has an effect on different materials. The reason why the lithium replenishment capacity and lithium desorption potential of Example 12 are lower is because the theoretical capacity and lithium desorption potential of lithium oxalate are lower than those of lithium oxalate.
[0272] From the data of Examples 13 to 23 and Comparative Example 4 in Table 2, it can be seen that the lithium supplement material and battery performance prepared by the scheme provided by the present application are relatively excellent, specifically manifested in the first-cycle lithium supplement specific capacity, the lithium supplement gram capacity below 4.2V is higher than the comparative material, and the lithium desorption potential and powder resistivity are significantly lower than the comparative example. The lithium supplement material lithium oxalate provided by the present application is compounded with a new carbon material to have better conductivity and ion transport properties, thereby improving the conductivity of the lithium supplement material and the problem of high lithium desorption potential, and achieving the effect of catalytic lithium desorption.
[0273] From Example 13 in Table 2 and Comparative Examples 1, 2 and 4, it can be seen that the catalyst grown in the intercalation structure by in-situ growth has a better catalytic effect. In the comparative example, the original lithium oxalate has a large powder resistivity and poor conductivity, which leads to that it can only start to delithiate after reaching the 4.7V platform, and the delithiation is incomplete, and the lithium replenishment effect is poor. In Comparative Example 2, the simple mixing of lithium oxalate and carbon tubes can only slightly improve its conductivity, which is not enough for practical application. In Comparative Example 4, Li 2 C 2 O 4After the simple mixing of CNTs, NPs and MnO, the delithiation potential did not drop sufficiently due to the addition of the catalyst. The reason is that NPs and CNTs cannot form an intercalation structure, which is not conducive to the full contact between the catalyst, lithium oxalate and carbon materials. On the other hand, direct mixing may cause mutual coating on the surface of the materials, and the increase in coating thickness may lead to the problem of difficulty in delithiation.
[0274] It can be seen from Examples 13, 14 and 15 in Table 2 that the thickness of the nanosheet has an impact on the performance of the lithium supplement material. The reason is that the thickness of the nanosheet synthesized in Example 14 is 1nm, which is too thin. It has been broken during the reaction, resulting in the stacking of carbon materials without sufficient interlayer distance. The nanosheet in Example 15 is too thick, resulting in a small specific surface area exposed, and the amount of grown catalyst is reduced, so that its catalytic effect cannot be fully exerted.
[0275] From the comparison of Example 13, Example 16 and Example 17 in Table 2, it can be seen that the appropriate pore size on the nanosheet is more conducive to the lithium supplementation effect. In Example 16, the pore diameter is about 1nm, and the gap is small, which is not conducive to adapting to the volume change of the material during the lithium removal process. In Example 17, the pore diameter is too large, and the growth process and deposition process of the catalyst may block the gap and affect the gas overflow.
[0276] From the comparison of Example 13, Example 18 and Example 19 in Table 2, it can be seen that the mass ratio of nanosheets to nanotubes also has an impact on the performance of lithium supplement materials. The amount of CNT added in Example 18 is too small, resulting in insufficient intercalation effect, resulting in fewer gaps between its nanosheets, and the nanosheets are prone to stacking, affecting conductivity and specific surface area. The amount of CNT added in Example 19 is too large, and agglomeration and entanglement have occurred, affecting conductivity.
[0277] From the comparison between Example 13 and Example 20 in Table 2, it can be seen that lithium oxalate with a small particle size has more catalytic advantages. The reason is that lithium oxalate with a large particle size has very poor conductivity and it is difficult to release lithium ions to achieve the lithium replenishment effect.
[0278] From the comparison of Example 13, Example 21 and Example 22 in Table 1, it can be seen that the ratio of lithium-rich material, catalyst and conductive carbon carrier needs to be controlled within an appropriate range. In Example 21, the catalyst content is about 1% of lithium oxalate, and too little content is not conducive to the catalysis of the material. In Example 22, the content of catalyst and conductive carrier in the material accounts for too much, resulting in too little actual active components in the material.
[0279] From the comparison between Example 13 and Example 23 in Table 1, it can be seen that Example 13 has a greater catalytic advantage. Although the use of heterojunction catalysts can reduce its overpotential to a certain extent, the effect is not perfect. The reason may be that the catalytic effect of the in-situ grown MnO particles in the system is better.
[0280] In the description of the embodiments of the present application, it should be noted that the orientation or positional relationship of terms such as "center", "up", "down", "left", "right", "vertical", "horizontal", "inside" and "outside" are based on the orientation or positional relationship described in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application.
[0281] What is disclosed above is only a preferred embodiment of the present application, and it certainly cannot be used to limit the scope of rights of the present application. Ordinary technicians in this field can understand that all or part of the processes of implementing the above embodiment and equivalent changes made according to the claims of the present application are still within the scope covered by the present application.
Claims
1. A lithium supplement material, characterized in that: It comprises a one-dimensional carbon material, a lithium-rich material and a catalyst, wherein at least part of the lithium-rich material and at least part of the catalyst are loaded on the one-dimensional carbon material.
2. The lithium supplement material according to claim 1, characterized in that: There are multiple one-dimensional carbon materials, and the multiple one-dimensional carbon materials are stacked to form a conductive wire bundle structure; and / or the multiple one-dimensional carbon materials are interwoven to form a conductive network structure.
3. The lithium supplement material according to claim 1, characterized in that: The lithium-supplementing material further includes a two-dimensional carbon material, and part of the lithium-rich material and part of the catalyst are combined on the surface of the two-dimensional carbon material.
4. The lithium supplement material according to claim 3, characterized in that: The number of the two-dimensional carbon material is multiple, and the multiple two-dimensional carbon material sheets are stacked; and / or, At least one of the one-dimensional carbon materials is inserted into the gap between two adjacent two-dimensional carbon materials; and / or The two-dimensional carbon material has holes, and at least part of the one-dimensional carbon material is interspersed in the holes; and / or The one-dimensional carbon material and / or the two-dimensional carbon material is doped with a non-metallic element, wherein the non-metallic element comprises at least one of O, N, and S; and / or The catalyst is in-situ grown on the one-dimensional carbon material and / or on the two-dimensional carbon material.
5. The lithium supplement material according to claim 3, characterized in that: The two-dimensional carbon material comprises carbon nanosheets; and / or The porosity of the two-dimensional carbon material is 30% to 70%; and / or The mass ratio of the one-dimensional carbon material to the two-dimensional carbon material is 1:(1-10); and / or The specific surface area of the one-dimensional carbon material and the two-dimensional carbon material is 200 m 2 / g~800m 2 / g.
6. The lithium supplement material according to any one of claims 1 to 5, characterized in that: The catalyst comprises at least two different metal compounds, and the two metal compounds are interconnected to form a heterojunction; and / or At least a portion of the lithium-rich material and at least a portion of the catalyst are in contact with each other; and / or Part of the lithium-rich material is coated on the outer surface of the catalyst; and / or At least part of the one-dimensional carbon material has gaps, so that the inside of the one-dimensional carbon material is connected with the external space.
7. The lithium supplement material according to any one of claims 1 to 5, characterized in that: The one-dimensional carbon material comprises carbon nanotubes; and / or The particle size of the lithium-rich material is 10 nm to 3 μm; and / or The particle size of the catalyst is 2nm to 100nm; and / or The mass ratio of the lithium-rich material to the catalyst is 100:(1-15); and / or The chemical formula of the lithium-rich material is Li x1 C y1 O z1 , where 0<x1≤2,y1> 0,z1>0.
8. A method for preparing a lithium supplement material, characterized in that: include: Mixing a catalyst raw material with a one-dimensional carbon material to react so that at least a portion of the catalyst is supported on the one-dimensional carbon material; The lithium-rich material is mixed with the one-dimensional carbon material supporting the catalyst, so that at least a portion of the lithium-rich material is supported on the one-dimensional carbon material, thereby obtaining a lithium-supplementing material.
9. A positive electrode material, characterized in that: The positive electrode material includes an active material and a lithium supplement material, and the lithium supplement material includes the lithium supplement material according to any one of claims 1 to 7, or includes the lithium supplement material obtained by the preparation method of the lithium supplement material according to claim 8.
10. A secondary battery, characterized in that: The invention comprises a positive electrode, a negative electrode and a separator arranged between the positive electrode and the negative electrode, wherein the positive electrode comprises the positive electrode material as claimed in claim 9.