Nickel nanoparticle hydroxide catalyst for resisting carbon monoxide poisoning and preparation method thereof
By introducing high-density stacking faults and twin boundary defects on nickel nanoparticles, the hydrogen adsorption energy is improved by using asymmetric convex sites, the problems of low activity of traditional nickel-based catalysts and sensitivity to carbon monoxide poisoning are solved, and high-efficiency Catalytic and anti-CO toxicity properties of hydroxide reaction.
Patent Information
- Application Number
- CN202410871105.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-11-08
AI Technical Summary
Traditional nickel-based catalysts have low catalytic activity in hydrogen fuel cells and are sensitive to carbon monoxide poisoning. It is difficult to introduce high-density stacking faults and twin boundary defects on the nanoscale, limiting their anti-CO toxicity properties.
By combining the salts of two different coordination configurations of Ni in a 1:1 ratio, immersed on a carbon support, and pyrolysis treatment, a high-density stacking fault and twin boundary defects were prepared. Particles, as a hydroxide reaction catalyst, use asymmetric convex sites to increase hydrogen adsorption energy and reduce kinetic barriers.
The high activity of the catalyst and excellent anti-carbon monoxide poisoning performance are achieved, the catalytic activity is close to that of commercial platinum carbon, and the high current density can be maintained for a long time in a high CO concentration environment, which significantly improves the efficiency of the fuel cell.
Smart Images

Figure CN118919745A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of hydrogen oxidation catalysts, and in particular to a nickel nanoparticle hydrogen oxidation catalyst resistant to carbon monoxide poisoning and a preparation method thereof. Background Art
[0002] With the rapid development of human society, the consumption of non-renewable resources such as oil and natural gas has increased dramatically, and there is an urgent need to develop a sustainable energy and efficient energy conversion device. Hydrogen energy, as a renewable secondary energy source, has the characteristics of high energy density and non-polluting products. It has been one of the key research areas in academia and industry in recent years. Fuel cells are important energy conversion devices for hydrogen energy applications. Compared with traditional energy conversion devices such as internal combustion engines and thermal power generation, they are not restricted by the Carnot cycle and have the advantages of high energy conversion efficiency, high power density, and environmental friendliness. However, before the large-scale commercialization of fuel cells, some challenges need to be overcome, among which the cost of hydrogen fuel is a major obstacle. Considering the high cost of obtaining high-purity hydrogen from water electrolysis or complex purification processes, the direct use of low-cost reformed hydrogen is still the most favorable option to reduce the operating cost of fuel cells. However, reformed hydrogen usually contains CO impurities with concentrations ranging from 100ppm to 3%. This makes the advanced platinum group metal (PGM)-based catalysts, which have excellent performance but are sensitive to CO, as the active component of the anode hydrogen oxidation reaction (HOR) of low-temperature hydrogen fuel cells, often lose their activity due to CO poisoning. Recently, the progress of alkaline fuel cells, one of the technical routes for low-temperature hydrogen fuel cells, has made it possible to develop non-PGM-based catalysts with good resistance to CO poisoning. Compared with PGMs with strong CO binding energy, non-PGMs with weak CO adsorption can more easily achieve high resistance to CO poisoning. At the same time, their abundant reserves also make them more suitable for industrial promotion.
[0003] Among the numerous non-PGM materials, nickel-based materials are widely recognized as the most promising candidates for non-PGM-based HOR catalysts. Although their activity is much better than other non-PGM materials, it is still two orders of magnitude lower than that of advanced commercial PGM-based HOR catalysts. This is mainly attributed to the excessively strong hydrogen adsorption energy on the metal Ni surface, which inhibits the further oxidation and desorption of hydrogen intermediates in HOR. In addition, the adsorption of key intermediates such as hydroxyl (*OH) and interfacial water (*H2O) involved in the rate-determining Volmer step of alkaline HOR also affects the kinetics of HOR. Limited by the single atomic configuration on the surface, it is difficult for traditional single metal Ni to achieve simultaneous regulation of the adsorption behavior of multiple intermediates in HOR, including hydrogen, hydroxyl, and interfacial water. A feasible solution is to introduce ordered crystal defects such as stacking faults (SF) and twin boundaries (TB) into single metal Ni to create a geometrically asymmetric surface. Unlike ordinary surfaces, it can provide a variety of atomic configurations to adjust the adsorption and activation of various reaction intermediates in HOR, thereby obtaining high HOR activity. However, the high stacking fault energy (γ SFE =125mJ·m -2 ) makes it extremely difficult to experimentally generate SFs and TBs on metallic Ni, especially at the nanoscale. Therefore, it is necessary to develop a simple and mild synthetic method to introduce SF and TB into Ni nanoparticles to obtain high-performance Ni nanoparticle HOR catalysts that are resistant to CO poisoning.
[0004] The prior art discloses some methods for introducing SF and TB in high stacking fault energy metals. Document 1 (Stacking Fault-Enriched MoNi4 / MoO2 Enables High-Performance Hydrogen Evolution, Adv. Mater. 2024, 2402156.) reports a method combining chemical and thermal reduction. At a medium heating temperature of 500°C, a low-density SF is produced on a molybdenum-nickel array uniformly grown on nickel foam at a conventional cooling rate. Limited by the synthesis conditions, the prepared molybdenum-nickel array is too large (exceeding the micron level). In addition, the method still has many processes and complex processes. Document 2 (Asilver catalyst activated by stacking faults for the hydrogen evolution reaction, Adv. Mater. 2022, 34, 2106973.) reports a method of laser ablation and rapid cooling and quenching in a liquid to obtain dislocation-rich silver nanoparticles under extreme reaction conditions. However, due to the harsh reaction conditions and the intense process, this method of laser ablation and rapid cooling and quenching is difficult to adjust the stacking fault density. In addition, some articles have also tried to introduce SF and TB into some metals through methods such as microwave ultrasound and non-equilibrium high-temperature thermal shock, but these methods often have problems such as harsh conditions, violent reaction processes, time-consuming and energy-consuming, which are not conducive to large-scale promotion and large-scale preparation of high-density SF and TB metal nickel nanoparticles. The inventor's previous patent CN2024108678736 discloses a method for preparing metal nanoparticles with controllable stacking fault and twin boundary density. By using a Ni precursor with two different ligand configurations in a quantitative ratio of 1:1 and a directional controllable pyrolysis strategy, nickel nanoparticles with high SF and TB densities can be obtained. It provides the possibility of providing a high-performance HOR reaction catalyst. Summary of the invention
[0005] In order to overcome the defect of low catalytic activity of prior art nickel-based catalysts in HOR reaction, the present invention provides a carbon monoxide resistant intermediate nickel nanoparticle hydrogenation catalyst and a preparation method thereof, specifically, by using two salts of different coordination configurations of Ni to be compounded in a 1:1 ratio, loaded on a carbon carrier by an impregnation method, and then subjected to pyrolysis treatment to obtain nickel nanoparticles with high density SF and TB defects, which, as a HOR reaction catalyst, have excellent carbon monoxide poisoning resistance and high catalytic activity. The present invention solves the above technical problems through the following technical solutions:
[0006] A carbon monoxide poisoning resistant nickel nanoparticle hydrogenation catalyst has stacking fault (SF) and / or twin boundary (TB) crystal defects, SF and TB defect density is 20-41%, Ni content is 40-50%, particle size is 25-35nm, and there are asymmetric convex sites corresponding to the number of SF and TB at the surface ends of SF and TB defects. The corresponding number means that the number is equal or nearly equal.
[0007] The nickel nanoparticles of the present invention are used as HOR reaction catalysts. Due to the asymmetric convex sites formed by SF and TB on the surface of metal nickel, active hydrogen (*H) can be adsorbed in a bridge configuration with a weaker hydrogen binding energy (HBE), thereby avoiding the overly strong three-point *H adsorption of traditional HBE. Moreover, this asymmetric convex site can also stabilize the interface *H2O through the atomic steps formed, thereby synergistically reducing the kinetic barrier of the rate-determining Volmer step in HOR and obtaining a faster alkaline HOR reaction kinetics. As a result, the catalyst exhibits HOR activity comparable to commercial platinum carbon in electrochemical tests. At the same time, nickel nanoparticles with high-density SF and TB have smaller d-band broadening and a lower matching degree with the CO molecular orbital, and therefore also exhibit excellent anti-CO poisoning performance.
[0008] The defect density of stacking faults (SF) and twin boundaries (TB) is calculated according to the method in the literature (J.Am.Chem.Soc.2022,144,11094-11098). The number of SF and TB appearing per unit length on multiple high-density SF and TB nanoparticles is counted by high-resolution transmission electron microscopy along the metal dense packing direction. The specific calculation is based on the following formula:
[0009] frequency SF+TB (Unit: nm ―1 ) = Number of SF and TB / Length (Formula 1)
[0010] density SF+TB (density; %) = frequency SF+TB ×0.205×100% (Formula 2)
[0011] High-resolution transmission electron microscopy (HRTEM) images show that there are a large number of alternating light and dark stripes in the nanoparticles, and the stripe densities of nanoparticles with different densities of SF and TB are different. SF+TB represents the frequency of SF and TB within a unit range, and 0.205 is the interplanar spacing of the metal close-packed plane. fcc / (001) hcpThe atomic stacking order changes in the close-packed direction. When the atomic stacking order of "ABCAB" appears in the normal atomic stacking order of "ABCABC" or "ABAB", it is marked as SF, and when the atomic stacking order of "ABCBA" appears, it is marked as TB.
[0012] Furthermore, the carbon monoxide poisoning-resistant nickel nanoparticle hydrogen oxidation catalyst includes the following XRD characteristic peaks: 42.2±0.1°, 44.5±0.1°, 47.7±0.1°, 51.8±0.1°, 62.6±0.1°, and 76.4±1°.
[0013] Furthermore, the carbon monoxide poisoning-resistant nickel nanoparticle hydrogen oxidation catalyst also includes the following XRD characteristic peaks: 83.8±0.1, 91.1±0.1, 95.1±0.1, 97.7±0.1, 98.3±0.1, 107.6±0.1, and 112.8±0.1.
[0014] The present invention also provides a method for preparing the above-mentioned nickel nanoparticle hydrogen oxidation catalyst resistant to carbon monoxide poisoning, comprising the following steps:
[0015] (S1) uniformly mixing a nickel salt A solution, a nickel salt B solution, and a carbon support, separating, and drying to obtain carbon-supported Ni precursors with two different coordination structures, wherein the nickel salt A is at least one of a nitrate, a halide, and an ammonia complex salt of Ni(II), and the nickel salt B is a cyano complex salt of Ni(II);
[0016] (S2) The precursor obtained in step (S1) is pyrolyzed under an inert atmosphere, and after cooling, a nickel nanoparticle hydrogen oxidation catalyst resistant to carbon monoxide poisoning is obtained.
[0017] Furthermore, in step (S1), the halide salt is nickel chloride or nickel bromide; the ammine complex salt is tetraamminenickel chloride or tetraamminenickel bromide; the cyano complex salt is potassium tetracyanonickelite or sodium tetracyanonickelite; the molar ratio of Ni in nickel salt A solution to Ni in nickel salt B solution is 1-1.1:1-1.1; further, the concentration of Ni in nickel salt A solution and nickel salt B solution is 10-50 mmol / L.
[0018] Furthermore, in step (S1), the carbon carrier is selected from at least one of graphene, porous carbon, commercial Ketjenblack EC, Vulcan, carbon nanotubes (CNT), and ordered mesoporous carbon (CMK-3); preferably, the amount of the carbon carrier added is 1-5 times the total mass of salt A and salt B, preferably 1-2 times.
[0019] Furthermore, in step (S1), the uniform mixing is performed by stirring at a rotation speed of 600-1000 rpm for 10-60 min, the separation is performed by centrifugal separation, and there is washing after centrifugal separation, the washing is performed by washing with water and ethanol in sequence, and the drying is performed by oven drying or vacuum drying.
[0020] Further, in step (S2), the inert atmosphere is at least one of nitrogen and argon, the pyrolysis temperature is 400-500°C, and the pyrolysis time is 1-5h. The preparation method of the present invention can conveniently regulate SF and TB by regulating the pyrolysis time and the pyrolysis temperature. Considering that as the temperature increases and the pyrolysis time increases, the metal atoms tend to be arranged in a thermodynamically more stable continuous stacking order. Therefore, if high-density SF and TB are to be obtained, within the range of 400-500°C and the pyrolysis time of 1-5h, the lower the temperature, the shorter the pyrolysis time, and the higher the density of SF and TB.
[0021] The preparation method proposed in the present invention overcomes the difficulty in introducing stacking faults (SF) and twin boundaries (TB) at high density on high stacking fault energy metals such as Ni. The present invention uses two different coordination configurations of nickel, namely, tetrahedral coordination configuration and octahedral coordination configuration, to form M in a 1:1 ratio. II X2M' II The Hofmann-type nickel-cyano bridge polymer precursor of (CN)4 is pyrolyzed, and the differences in different coordination configurations will create different local environments for the growth of metal crystals, allowing high dislocation energy metal atoms to stack along different atomic orders (such as "ABAB", "ABCABC"). The original continuous atomic stacking order will be disrupted, and high-density SF and TB will be introduced in the process.
[0022] Figure 1 This is a schematic diagram of the planar tetragonal coordination configuration of nickel coordinated with four carbon atoms and the octahedral coordination configuration coordinated with four nitrogen atoms and two oxygen atoms.
[0023] Compared with other prior arts, the present invention has the following advantages:
[0024] 1. The present invention utilizes the differentiated pyrolysis process of metal M atoms in different coordination environments in the precursor, and successfully introduces high-density SF and TB defects into nickel nanoparticles under relatively mild reaction conditions. By simply changing the pyrolysis temperature and / or pyrolysis time in the pyrolysis process, nickel nanoparticles with different densities of SF and TB are obtained.
[0025] 2. The HOR catalyst obtained by the present invention has high catalytic activity and strong resistance to carbon monoxide. In a hydrogen environment containing 1000ppmCO, it can still maintain 84% of the original HOR current density in a pure H2 environment after running at a constant potential of 50mV relative to the reversible hydrogen electrode for 1600 seconds, while commercial Pt / C shows a sharply decreased current density under the same conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a schematic diagram of the planar tetragonal coordination configuration of nickel coordinated with four carbon atoms and the octahedral coordination configuration coordinated with four nitrogen atoms and two oxygen atoms.
[0027] Figure 2 This is the X-ray powder diffraction spectrum of the Ni metal nanoparticles obtained in Example 1.
[0028] Figure 3 This is a transmission electron microscope image of the Ni metal nanoparticles obtained in Example 1.
[0029] Figure 4 This is the thermogravimetric curve of the Ni metal nanoparticles obtained in Example 1.
[0030] Figure 5 This is a high-resolution transmission electron microscope photograph of the Ni metal nanoparticles obtained in Example 1.
[0031] Figure 6 This is an atomic resolution scanning transmission electron microscope photograph of the Ni metal nanoparticles obtained in Example 1.
[0032] Figure 7 This is an atomic resolution scanning transmission electron microscope photograph of the edge of the Ni metal nanoparticles obtained in Example 1.
[0033] Figure 8 The polarization curves of the hydrogen oxidation experiment of the Ni metal nanoparticles obtained in Example 1 and the commercial Pt / C catalyst are shown.
[0034] Fig. 9 This is the carbon monoxide poisoning resistance test curve of the Ni metal nanoparticles obtained in Example 1 and the commercial Pt / C catalyst. DETAILED DESCRIPTION
[0035] In order to further understand the present invention, the present invention is described below through specific embodiments. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, and the present invention and the limitations of the claims of the present invention are not limited thereto.
[0036] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods; the reagents, materials, etc. used in the following examples, unless otherwise specified, can be obtained from commercial channels.
[0037] Example 1
[0038] (S1) 0.03 mmol nickel nitrate and 0.03 mmol potassium tetracyanonitric acid were added to 10 mL deionized water at room temperature, and stirred at 700 rpm for 30 minutes to obtain clear and transparent solutions A and B; solution A, solution B and 50 mg porous carbon (BET = m 2 g -1 ) were mixed, stirred at 10000 rpm for 10 min, the mixture was collected by centrifugation, washed with deionized water and ethanol in sequence, and dried in an oven at 60°C to obtain a carbon-supported Ni precursor (denoted as Ni-CP@PC);
[0039] (S2) The Ni-CP@PC was transferred to a quartz crucible or a corundum crucible, placed in a tube furnace, purged with argon to exclude air, and then heated to 450°C at a rate of 10°C / min, kept for 2 h, and then naturally cooled to room temperature to obtain Ni metal nanoparticles with SF and TB defects, i.e., HOR catalysts with excellent resistance to carbon monoxide poisoning.
[0040] Figure 2 It is the X-ray powder diffraction spectrum (XRD pattern) of the Ni metal nanoparticles obtained in Example 1. The diffraction peaks of 2θ at 44.5°, 51.8° and 76.4° belong to the fcc phase of Ni, and the diffraction peaks at 42.2, 47.7 and 62.6° belong to an unconventional hcp phase (u-hcp) of Ni. It is calculated that the ratio of the u-hcp to the fcc phase of Ni is about 1:0.8. It can be seen that the Ni metal nanoparticles with SF and TB prepared in Example 1 contain two Ni metal phases, namely, face-centered cubic phase (face-centered cube) and unconventional hexagonal close-packed phase (hexagonal close-packed). In contrast, the Ni metal nanoparticles with low-density SF and TB contain only one face-centered cubic phase. It shows that the formation of SF and TB in the Ni metal nanoparticles prepared in Example 1 is highly correlated with its metal phase composition.
[0041] Figure 3 : is a transmission electron microscope photograph of the Ni metal nanoparticles obtained in Example 1. It can be seen that the high-density SF and TB Ni metal nanoparticles are densely distributed on the carbon substrate, and a large number of alternating light and dark stripes exist in a single particle.
[0042] Figure 4This is the thermogravimetric curve of the Ni metal nanoparticles obtained in Example 1. When the carbon-supported high-density SF and TB Ni metal nanoparticles are calcined to 800°C in an air atmosphere, the mass fraction of the remaining substance is 56.8%, and the remaining substance is nickel oxide. It is known that the mass fraction of nickel in nickel oxide is 78.6%. Through calculation, it can be determined that the mass percentage of metallic nickel in the product is 44.6%.
[0043] Figure 5 : is a high-resolution transmission electron micrograph of the Ni metal nanoparticles obtained in Example 1. It can be seen that there are a large number of wrinkled lattice fringes attributable to SF and mirror-symmetric lattice fringes attributable to TB.
[0044] Figure 6 This is an atomic resolution scanning transmission electron microscope photograph of the Ni metal nanoparticles obtained in Example 1. It can be seen that the obtained high-density SF and TB Ni metal nanoparticles exist, and by counting the number of SF and TB in different regions within a 2.5 nm scale, the average value is 4.2, and the density of SF and TB is calculated to be 34.4%.
[0045] Figure 7 : is an atomic resolution scanning transmission electron micrograph of the edge of the Ni metal nanoparticle obtained in Example 1. It can be seen that there are corresponding numbers of convex sites at the surface ends of SF and TB.
[0046] The specific calculation is as follows:
[0047] frequency SF+TB (nm ―1 )=4.2 / 2.5(nm ―1 )
[0048] The interplanar spacing of the densely packed plane is measured as d = 0.205 nm, and the density of SF and TB is converted through the following calculation process:
[0049] density SF+TB (; %) = 4.2 / 2.5×0.205×100%=34.4%.
[0050] Figure 8The polarization curves of the hydrogen oxidation experiment of the Ni metal nanoparticles obtained in Example 1 and the commercial Pt / C catalyst are shown in Table 1. The specific experimental method is as follows: the hydrogen oxidation polarization curve is measured in a 0.1M KOH solution saturated with H2 using a rotating disk electrode, the rotating speed of the rotating disk electrode is 1600rpm, and the curve scanning rate is 5mV / s. The control platinum carbon catalyst was purchased from Alfa Aesar (Tianjin) Catalyst Co., Ltd. By comparing the two curves, it can be seen that the hydrogen oxidation current density released by the Ni metal nanoparticle catalyst with high-density SF and TB prepared in Example 1 is almost overlapped with that of commercial platinum carbon, indicating that it has hydrogen oxidation performance comparable to that of commercial platinum carbon.
[0051] Fig. 9 The following is the test curve of the Ni metal nanoparticles and the commercial Pt / C catalyst against carbon monoxide poisoning obtained in Example 1. The specific experimental method is: using a rotating disk electrode to measure in a 0.1M KOH solution saturated with 1000ppmCO / H2, the rotating disk electrode speed is 1600rpm, the curve scanning rate is 5mV / s, and the hydrogen oxidation polarization curve under 1000ppmCO / H2 atmosphere is as follows: Fig. 9 The catalyst can still release 87% of the limiting current density under pure H2 atmosphere in 1000ppmCO / H2 atmosphere, while commercial platinum carbon can only release 36% of the limiting current density under pure H2 atmosphere in 1000ppmCO / H2 atmosphere. Further, under constant potential conditions, the chronoamperometric curves of the obtained catalyst and the commercial platinum carbon catalyst in the process of switching the fuel gas from H2 to 1000ppm CO / H2 were tested. The obtained constant potential chronoamperometric curves are shown in Fig. 9 The calculated comparison of the hydrogen oxidation current maintenance of the obtained catalyst and the commercial platinum carbon catalyst in a 1000ppm CO / H2 atmosphere is shown in b. Fig. 9 As shown in c. Fig. 9 As can be seen in figure b, the hydrogen oxidation current released by commercial platinum carbon decays rapidly after switching to 1000ppm CO / H2 fuel gas, and after 1600 seconds it can only maintain 18% of the current before CO treatment. In contrast, the catalyst obtained in Example 1 can maintain 84% of the current before CO treatment, indicating that the obtained catalyst has an ability to resist CO poisoning far exceeding that of commercial platinum carbon.
[0052] Example 2
[0053] The metal nanoparticles with high density SF and TB were prepared in the same manner as in Example 1. The difference was that the heat treatment time was shortened to 1 h, and metal Ni nanoparticles with higher density SF and TB were obtained. The density SF and TB reached 41.0% according to statistical calculation.
[0054] Example 3
[0055] High-density SF and TB metal nanoparticles were prepared in the same manner as in Example 1. The difference was that the pyrolysis time was extended to 3 h. After calculation, the density of the obtained metal Ni nanoparticles SF and TB was 27.1%.
[0056] Example 4
[0057] The high-density SF and TB metal nanoparticles were prepared in substantially the same manner as in Example 1. The difference was that the pyrolysis temperature was 400° C. After calculation, the density of the obtained metal Ni nanoparticles SF and TB was 38.2%.
[0058] Example 5
[0059] High-density SF and TB metal nanoparticles were prepared in substantially the same manner as in Example 1, except that the pyrolysis temperature was 500° C. After calculation, the density of the obtained metal Ni nanoparticles SF and TB was 17.3%.
[0060] Comparative Example 1
[0061] Commercial Pt / C catalyst was used, which was purchased from Alfa Aesar (Tianjin) Catalyst Co., Ltd.
[0062] Comparative Example 2
[0063] The Ni metal nanoparticle catalyst synthesized by a conventional method has a particle size comparable to that of the catalyst obtained in Example 1, but the particle surface is flat and the atomic stacking is continuous.
[0064] The catalysts of the above examples were tested for catalytic activity and carbon monoxide poisoning resistance, and the results are shown in Table 1 below:
[0065] Table 1 Catalytic performance test
[0066]
Claims
1. A nickel nanoparticle hydrogen oxidation catalyst resistant to carbon monoxide poisoning, characterized in that: The invention discloses a crystal defect having stacking faults (SF) and / or twin boundaries (TB), wherein the density of SF and TB defects is 20-41%, the Ni content is 40-50%, the particle size is 25-35 nm, and there are asymmetric convex sites corresponding to the number of SF and TB defects at the surface ends of the SF and TB defects.
2. The carbon monoxide poisoning resistant nickel nanoparticle hydrogen oxidation catalyst according to claim 1, characterized in that: Including the following XRD characteristic peaks: 42.2±0.1°, 44.5±0.1°, 47.7±0.1°, 51.8±0.1°, 62.6±0.1°, and 76.4±1°.
3. The carbon monoxide poisoning resistant nickel nanoparticle hydrogen oxidation catalyst according to claim 2, characterized in that: It also includes the following XRD characteristic peaks: 83.8±0.1, 91.1±0.1, 95.1±0.1, 97.7±0.1, 98.3±0.1, 107.6±0.1, and 112.8±0.
1.
4. The method for preparing the carbon monoxide poisoning resistant nickel nanoparticle hydrogenation catalyst according to any one of claims 1 to 3, characterized in that: The following steps are involved: (S1) uniformly mixing a nickel salt A solution, a nickel salt B solution, and a carbon support, separating, and drying to obtain carbon-supported Ni precursors with two different coordination structures, wherein the nickel salt A is at least one of a nitrate, a halide, and an ammonia complex salt of Ni(II), and the nickel salt B is a cyano complex salt of Ni(II); (S2) The precursor obtained in step (S1) is pyrolyzed under an inert atmosphere, and after cooling, a nickel nanoparticle hydrogen oxidation catalyst resistant to carbon monoxide poisoning is obtained.
5. The preparation method according to claim 4, characterized in that: In step (S1), the halide salt is nickel chloride or nickel bromide; the ammine complex salt is tetraamminenickel chloride or tetraamminenickel bromide; and the cyano complex salt is potassium tetracyanonickelate or sodium tetracyanonickelate.
6. The preparation method according to claim 4, characterized in that: In step (S1), the molar ratio of Ni in nickel salt A solution to Ni in nickel salt B solution is 1-1.1:1-1.
1.
7. The preparation method according to claim 4, characterized in that: In step (S1), the concentration of Ni in the nickel salt A solution and the nickel salt B solution is 10-50 mmol / L.
8. The preparation method according to claim 4, characterized in that: In step (S1), the carbon carrier is selected from at least one of graphene, porous carbon, commercial Ketjenblack EC, Vulcan, carbon nanotubes (CNT), and ordered mesoporous carbon (CMK-3); preferably, the amount of the carbon carrier added is 1-5 times the total mass of salt A and salt B, preferably 1-2 times.
9. The preparation method according to claim 4, characterized in that: In step (S1), the uniform mixing is performed by stirring at a rotation speed of 600-1000 rpm for 10-60 minutes; the separation is performed by centrifugal separation, and after the centrifugal separation, there is washing, which is washing with water and ethanol in sequence; and the drying is oven drying or vacuum drying.
10. The preparation method according to claim 4, characterized in that: In step (S2), the pyrolysis temperature is 400-500°C, and the pyrolysis time is 1-5h.