Sodium ion battery and preparation method and application thereof

By using a combination of specific positive electrode active substances and electrolytes in sodium ion batteries, the CO2 production rate and quantity are regulated, and combined with explosion-proof valves, the safety risks of sodium ion batteries are solved when the capacity is reduced, and the battery is timely disconnected or failed. , reducing safety risks and combustible gas accumulation.

CN118919823APending Publication Date: 2024-11-08SO-FUN TECH CORP LTD

Patent Information

Application Number
CN202410416167.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-04-08
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing sodium ion batteries are prone to combustible gases during charging and discharging, resulting in capacity decay and safety risks, especially when the battery cell capacity is reduced to 60%, which increases the safety risks of use.

Method used

Use specific combinations of positive electrode active substances and electrolytes, including layered oxide materials, sodium carbonate, sodium citrate or sodium oxalate, and vinyl carbonate as electrolyte solvents to regulate the rate and amount of CO2 production, and combine the explosion-proof on the battery shell. Valve ensures that the internal pressure of the battery cell reaches the upper limit of the explosion-proof valve, and reduces safety risks.

Benefits of technology

Effectively reduce the safety risks of sodium ion batteries during use, ensure that the battery is disconnected or failed in time when the capacity is reduced to 60%~80%, avoids sharp drop in capacity and accumulation of combustible gases, and improves the safety and circulation performance of the battery. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919823A_ABST
    Figure CN118919823A_ABST
Patent Text Reader

Abstract

The invention discloses a sodium ion battery as well as a preparation method and application thereof. The sodium ion battery comprises a battery shell containing an anti-explosion valve and a battery cell, a positive active substance in a positive plate of the battery cell is a mixture of a positive active substance I and a positive active substance II (with the mass fraction of 5-45%), the positive active substance I is at least one of a polyanion material or a Prussian material, and the positive active substance II is at least one of a polyanion material and a Prussian material. The positive active substance II is at least one of a layered oxide material, sodium carbonate, sodium citrate or sodium oxalate; the electrolyte solvent contains ethylene carbonate with the mass fraction of 5%-70%. By regulating and controlling the mass fraction of the layered oxide material, the sodium carbonate, the sodium citrate or the sodium oxalate in the positive electrode active material and the mass fraction of the ethylene carbonate in the electrolyte solvent, the sodium-ion battery can generate the gas which takes CO2 as a main component and is controllable in gas production rate in the charge-discharge cycle, so that the use safety of the sodium-ion battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of methods or devices for directly converting chemical energy into electrical energy, and more specifically, to a sodium ion battery and a preparation method and application thereof. Background Art

[0002] At present, the energy storage batteries in new energy vehicles are mainly lithium-ion batteries, but due to the limited lithium resources and extremely uneven distribution, it is difficult to meet the rapid development of the electric vehicle field; sodium-ion batteries have advantages such as abundant sodium resources, low cost, and good safety performance, and have broader application prospects in the field of energy storage. The working principle of sodium-ion batteries is similar to that of lithium-ion batteries. Both use the reversible embedding / release of metal ions (lithium or sodium ions) between the positive and negative electrodes to achieve energy storage and release. Therefore, the positive and negative electrode materials are the key factors affecting the performance of sodium-ion batteries. At present, the positive electrode materials suitable for sodium-ion batteries are mainly layered oxides, Prussian materials, and polyanion materials, etc., and are used in combination with hard carbon (negative electrode materials).

[0003] However, due to its strong alkalinity, layered oxide materials are prone to react with ester electrolytes during the charge and discharge process, resulting in capacity decay of the sodium-ion battery cell; while the alkalinity of Prussian materials and polyanions is relatively low, their water content is high, which will also cause the sodium-ion battery to produce more flammable gases during use, which will also cause the capacity decay of the battery cell. Moreover, the SEI film formed on the hard carbon surface, which is mainly composed of organic and inorganic compounds of sodium, will continue to dissolve and repair during the cycle, thereby reacting with carbonate electrolytes to continuously generate alkane or olefin flammable gases.

[0004] Whether it is the capacity decay of the battery cell or the generated alkane or olefin combustible gases, they will bring great safety risks. Especially for automotive batteries, when the capacity of the battery cell decays to 80% of its initial capacity, it is generally recommended to replace it; when the capacity of the battery cell decays to 60% of its initial capacity, it needs to be replaced in time to reduce safety risks. However, the current sodium-ion batteries are difficult to disconnect or fail in time even if their battery capacity is reduced to less than 60% of their initial capacity, resulting in a greater safety risk in the use of sodium-ion batteries. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects and shortcomings of existing sodium ion batteries, which have high safety risks during use, and to provide a sodium ion battery.

[0006] Another object of the present invention is to provide a method for preparing a sodium ion battery.

[0007] Another object of the present invention is to provide an application of a sodium ion battery in a battery module or a battery pack.

[0008] The above-mentioned purpose of the present invention is achieved through the following technical solutions: The present invention protects a sodium ion battery, which comprises a battery shell and a battery core, wherein the battery core comprises a positive electrode sheet, a diaphragm, a negative electrode sheet and an electrolyte, and the battery shell comprises an explosion-proof valve; The positive electrode active material in the positive electrode sheet is a mixture of positive electrode active material I and positive electrode active material II, wherein the positive electrode active material I is at least one of a polyanion material or a Prussian material, and the positive electrode active material II is at least one of a layered oxide material, sodium carbonate, sodium citrate or sodium oxalate; The mass fraction of the positive electrode active material II in the positive electrode active material is 5% to 45%; The electrolyte includes sodium salt and a solvent, wherein the solvent is a mixture of ethylene carbonate and propylene carbonate, and the mass fraction of ethylene carbonate in the solvent is 5% to 70%.

[0009] The present invention combines a specific positive electrode active material with an electrolyte containing ethylene carbonate, and is equipped with an explosion-proof valve on a battery shell. By adjusting the mass fraction of layered oxide material, sodium carbonate, sodium citrate or sodium oxalate in the positive electrode active material, and the mass fraction of ethylene carbonate in the electrolyte solvent, the sodium ion battery generates a gas mainly composed of CO2 and with a controllable gas production rate during the charge and discharge cycle. The gas is used to regulate the pressure inside the battery cell, so that when the capacity of the sodium ion battery is reduced to between 60% and 80% of its initial capacity, the internal pressure just reaches the upper limit of the pressure that the explosion-proof valve can withstand, thereby triggering the explosion-proof valve to cause the sodium ion battery to self-disconnect or fail in time, thereby effectively reducing the safety risk of the sodium ion battery during use.

[0010] Compared with other alkaline substances, the layered oxide materials, sodium carbonate, sodium citrate or sodium oxalate in the above-mentioned positive electrode active materials basically do not produce gas during the storage process of the battery, but react with the electrolyte solvent only during the charge and discharge cycle process, and mainly produce CO2, which not only has excellent storage stability, but also can effectively reduce the proportion of combustible gases (alkane or olefin gases) in the generated gas, thereby effectively reducing the risk of flammability. However, when its mass fraction is too large, CO2 will be produced faster and more, which will not only cause the capacity of the sodium ion battery to drop sharply and the cycle performance to deteriorate, but also cause the pressure inside the sodium ion battery to increase rapidly to reach the upper limit of the pressure that the explosion-proof valve can withstand, causing the sodium ion battery to be short-circuited or fail; and when the mass fraction is too small, that is, it is equivalent to a large proportion of polyanionic materials and / or Prussian materials with a high water content in the positive electrode active material, at this time, more combustible gases will be generated and accumulated, and combustion and explosion are prone to occur, thereby significantly increasing the safety risk of sodium ion batteries.

[0011] The combination of ethylene carbonate in the electrolyte solvent and the layered oxide material, sodium carbonate, sodium citrate or sodium oxalate in the positive electrode active material can regulate the rate and amount of CO2 produced by the sodium ion battery during the cycle, thereby making the pressure increase rate inside the sodium ion battery compatible with the capacity decrease rate of the sodium ion battery, so that when the capacity of the sodium ion battery is reduced to between 60% and 80% of its initial capacity, its internal pressure just reaches the upper limit of the pressure that the explosion-proof valve can withstand and automatically breaks the circuit or fails. In addition, when the mass fraction of ethylene carbonate in the above electrolyte solvent is too large, the electrolyte will be solid at room temperature; when the mass fraction is too small, too little CO2 is produced, making it difficult to trigger the explosion-proof valve of the sodium ion battery in time.

[0012] It should also be noted that the positive electrode sheet of the above-mentioned sodium ion battery is composed of an aluminum foil and a positive electrode active material, a conductive agent and a binder coated on the surface of the aluminum foil. The mass ratio between the positive electrode active material, the conductive agent and the binder is conventionally selected in the art, for example, the mass ratio of the positive electrode active material, the conductive agent and the binder is (80%~98%): (1%~10%): (1%~10%); the negative electrode active material in the above-mentioned negative electrode sheet can be at least one of hard carbon, soft carbon, sieved carbon or alloys (Bi, P, Sn, etc.).

[0013] Preferably, the mass fraction of the positive electrode active material II in the positive electrode active material is 5% to 25%, specifically 10%, 15% or 20%; the mass fraction of the ethylene carbonate in the solvent is 20% to 50%, specifically 25%, 30%, 35%, 40% or 45%.

[0014] Optionally, the explosion-proof valve on the battery shell can be conventionally selected according to actual needs, and the model of the sodium ion battery is related to its shell. The shell can be a steel shell or an aluminum shell, generally cylindrical or square shell, wherein the cylindrical top cover is provided with an explosion-proof valve (for example, CN109148747A, CN105977407A, etc.), and the square shell top cover is also provided with an explosion-proof valve (for example, CN218039483U, CN217086730U, etc.). When the battery shell is cylindrical, the corresponding explosion-proof valve pressure resistance value is generally ≤1.5MPa, specifically 0.5~1.5MPa; when the battery shell is square shell, the corresponding explosion-proof valve pressure resistance value is generally ≤1.2MPa, specifically 0.1~1.2MPa.

[0015] Optionally, the layered oxide material is a layered oxide material well known in the art for use as a positive electrode material, and its crystal structure is composed of alkali metals (Na +) layer and a transition metal (MO2) layer in an orderly stacked form, and the chemical formula can be expressed as NaMO2, wherein M is at least one of Fe, Ni, Mn, Cu, Co, Ru, Ir, Sn, Cr, Nb or Mo, preferably Ni, Fe and Mn, or Cu, Ni, Ti and Mn. Specifically, the layered oxide material is NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2、NaCu 1 / 9 Ni 2 / 9 Ti 1 / 3Mn 1 / 3 O2.

[0016] Optionally, the Prussian material includes a Prussian blue material and a Prussian white material, and the chemical formula of the Prussian blue material is Na x P[R(CN)6]y; wherein P and R are independently at least one of Mn, Fe, Ni, Co, Cu, Ce, Cr, Ti, Zn or V; the values ​​of x and y satisfy the charge balance of the chemical formula.

[0017] Optionally, the chemical formula of the polyanion material is Na4Fe m M n (PO4)2P2O7 / C、Na4Fe m M n PO4P2O7F3 / C、Na3Fe m M n PO4F / C, Na3Mn m M n (PO4)3 / C or Na2Fe m M m P2O7 / C; wherein " / C" in the above chemical formula represents carbon coating, M is at least one of Ni, Mn, Co, Cu, Zn, Mg, Al, Ca, Sr, Ce, Ti, Zr, Sn, V, Nb, Sb or Mo, and the values ​​of m and n satisfy the charge balance of the chemical formula. Specifically, the polyanion material is Na3V2(PO4)3, Na 1.5 Fe[Fe(CN)6].

[0018] The present invention also protects a method for preparing the above-mentioned sodium ion battery, comprising the following steps: firstly winding the positive electrode sheet, the separator, and the negative electrode sheet to obtain a bare cell, then placing the bare cell into the inner cavity of the battery shell, and then injecting electrolyte into the bare cell to obtain a sodium ion battery. Specifically, the above-mentioned bare cell occupies 95% to 99% of the total volume of the inner cavity of the battery shell, which can be selected according to actual needs.

[0019] The application of the above-mentioned sodium ion battery in a battery module or a battery pack is also within the protection scope of the present invention.

[0020] Compared with the prior art, the present invention has the following technical effects: The present invention combines a specific positive electrode active material with an electrolyte containing ethylene carbonate, and is equipped with an explosion-proof valve on a battery shell. By adjusting the mass fraction of layered oxide material, sodium carbonate, sodium citrate or sodium oxalate in the positive electrode active material and the mass fraction of ethylene carbonate in the electrolyte solvent, the sodium ion battery generates a gas mainly composed of CO2 and with a controllable gas production rate during the charge and discharge cycle. The gas is used to adjust the pressure inside the battery cell, so that when the capacity of the sodium ion battery is reduced to between 60% and 80% of its initial capacity, the internal pressure just reaches the upper limit of the pressure that the explosion-proof valve can withstand, and then the explosion-proof valve is triggered to make the sodium ion battery self-circuited or fail in time, thereby ensuring that the sodium ion battery has high safety during use. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 1 is a cycle diagram of the sodium ion battery in Example 1 and Comparative Example 1.

[0022] Figure 2 2 is a cycle diagram of the sodium ion battery in Example 6 and Comparative Example 2. DETAILED DESCRIPTION

[0023] The present invention is further described below in conjunction with specific embodiments, but the embodiments do not limit the present invention in any form. Unless otherwise specified, the raw materials and reagents used in the embodiments of the present invention are conventionally purchased raw materials and reagents.

[0024] Example 1 A sodium ion battery comprises a battery shell containing an explosion-proof valve and a battery core, wherein the battery core comprises a positive electrode sheet, a diaphragm, a negative electrode sheet and an electrolyte.

[0025] The positive electrode sheet is composed of aluminum foil and positive electrode active material, conductive carbon SP and binder PVDF coated on the surface of the aluminum foil (the mass ratio of positive electrode active material, conductive carbon SP and binder PVDF is 90:5:5); the positive electrode active material is NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2 and Na3V2(PO4)3 (polyanion material) are composed in a mass ratio of 5%:95%.

[0026] The negative electrode sheet is composed of aluminum foil and hard carbon, conductive carbon SP and binder PVDF coated on the surface of the aluminum foil (the mass ratio of hard carbon, conductive carbon SP and binder PVDF is 90:5:5).

[0027] The electrolyte was an EC / PC solution of 1 mol / L NaPF6, with the mass ratio of EC to PC being 50%:50%.

[0028] The above sodium ion battery can be prepared by the following preparation method: The positive electrode sheet, the separator and the negative electrode sheet are wound to obtain a bare cell; the bare cell is placed in a 32700 cylindrical steel shell, with the bare cell occupying 98% of the inner volume of the 32700 cylindrical shell; the electrolyte is injected and the cap is covered to obtain a sodium ion battery; an explosion-proof valve is provided on the cap, which can withstand a maximum pressure of 1.5MPa.

[0029] Example 2 A sodium ion battery, which is substantially the same as that of Example 1, except that the positive electrode active material is NaNi 1 / 3 Fe 1 / 3Mn 1 / 3 O2 and Na3V2(PO4)3 are composed in a mass ratio of 45%:55%.

[0030] The preparation method of the above sodium ion battery is the same as that of Example 1.

[0031] Example 3 A sodium ion battery, which is substantially the same as that of Example 1, except that the positive electrode active material is NaNi 1 / 3 Fe 1 / 3Mn 1 / 3 O2 and Na3V2(PO4)3 are composed in a mass ratio of 25%:75%.

[0032] The preparation method of the above sodium ion battery is the same as that of Example 1.

[0033] Example 4 A sodium ion battery is substantially the same as that of Example 1, except that the electrolyte is an EC / PC solution of 1 mol / L NaPF6, and the mass ratio of EC to PC is 5%:95%.

[0034] The preparation method of the above sodium ion battery is the same as that of Example 1.

[0035] Example 5 A sodium ion battery is substantially the same as that of Example 1, except that the electrolyte is an EC / PC solution of 1 mol / L NaPF6, and the mass ratio of EC to PC is 70%:30%.

[0036] The preparation method of the above sodium ion battery is the same as that of Example 1.

[0037] Example 6 A sodium ion battery, which is basically the same as Example 1, except that the positive electrode active material is composed of Na2C2O4 (sodium oxalate) and Na 1.5 Fe[Fe(CN)6] is composed of 5%:95% by mass.

[0038] The preparation method of the above sodium ion battery is the same as that of Example 1.

[0039] Example 7 A sodium ion battery, which is substantially the same as that of Example 1, except that the positive electrode active material is NaCu 1 / 9 Ni 2 / 9Ti 1 / 3 Mn 1 / 3 O2 (layered oxide) and Na 1.5 Fe[Fe(CN)6] is composed of 5%:95% by mass.

[0040] The preparation method of the above sodium ion battery is the same as that of Example 1.

[0041] Comparative Example 1 A sodium ion battery is basically the same as Example 1, except that the positive electrode active material is Na3V2(PO4)3.

[0042] The preparation method of the above sodium ion battery is the same as that of Example 1.

[0043] Comparative Example 2 A sodium ion battery, which is substantially the same as Example 6, except that the positive electrode active material is Na 1.5 Fe[Fe(CN)6].

[0044] The preparation method of the above sodium ion battery is the same as that of Example 1.

[0045] Comparative Example 3 A sodium ion battery, which is substantially the same as that of Example 1, except that: 1 / 3 Fe 1 / 3 Mn 1 / 3 O2 and Na3V2(PO4)3 are composed in a mass ratio of 60%:40%.

[0046] The preparation method of the above sodium ion battery is the same as that of Example 1.

[0047] Comparative Example 4 A sodium ion battery is basically the same as Example 1, except that the electrolyte is a 1 mol / L NaPF6 PC solution.

[0048] The preparation method of the above sodium ion battery is the same as that of Example 1.

[0049] Comparative Example 5 A sodium ion battery is substantially the same as that of Example 1, except that the electrolyte is an EMC (ethyl methyl carbonate) / PC solution of 1 mol / L NaPF6, and the mass ratio of EMC to PC is 50%:50%.

[0050] The preparation method of the above sodium ion battery is the same as that of Example 1.

[0051] Comparative Example 6 A sodium ion battery is substantially the same as that of Example 1, except that the electrolyte is a DEC / PC solution of 1 mol / L NaPF6, and the mass ratio of DEC to PC is 50%:50%.

[0052] The preparation method of the above sodium ion battery is the same as that of Example 1.

[0053] Table 1 Composition of positive electrode active materials and electrolyte solvents of sodium ion batteries in various embodiments and comparative examples

[0054] Performance Testing (1) Sodium ion battery cell attenuation test: The sodium ion batteries in Examples 1 to 7 and Comparative Examples 1 to 6 were subjected to charge and discharge tests at a current density of 100 mA / g (1C) and a voltage range of 1.5 to 3.6 V. The charge and discharge cycles were performed under 1C conditions. When performing the open circuit / failure test, 5 batteries were taken from each Example or Comparative Example for testing, and the average ratio of the capacity at the time of open circuit / failure to the initial capacity was used for evaluation.

[0055] (2) Thermal abuse safety test: The sodium ion batteries in Examples 1 to 7 and Comparative Examples 1 to 6 were charged until their voltage reached 3.6 V. After standing for 1 hour, they were placed in a closed oven and heated to 180° C. at a heating rate of 10° C. / min. The temperature was then kept at this temperature for 30 minutes to observe whether the battery cells would catch fire or explode.

[0056] Table 2 Performance of sodium ion batteries in various embodiments and comparative examples

[0057] According to the data in Table 2, when the capacity of the sodium ion batteries in Examples 1 to 7 is reduced to between 60% and 80% of its initial capacity, the circuit will be broken or fail, indicating that the sodium ion batteries of the present invention can effectively reduce the safety risks brought about by the attenuation of the battery cell capacity. At the same time, during the thermal abuse process of the sodium ion batteries in Examples 1 to 7, the battery cells did not catch fire or explode, indicating that the sodium ion batteries of the present invention have good safety and reliability. It should also be noted that the number of cycles corresponding to the capacity of the above-mentioned sodium ion battery being reduced to 80% of its initial capacity is used to illustrate the impact of different experimental variables, and different cycle performance can meet the needs of different application scenarios.

[0058] According to Example 1 and Comparative Example 1, Example 6 and Comparative Example 2, when the positive active material of the sodium ion battery is a simple polyanion material or a Prussian material, it is impossible to open the circuit or fail when its capacity is reduced to 60% to 80% of the initial capacity; the sodium ion battery in Comparative Example 3 short-circuit when its capacity is reduced to 87% of the initial capacity, and cannot meet the application requirements; at the same time, it can be found from Comparative Examples 4 to 6 that the type and content of the organic solvent in the electrolyte also have a certain influence on the capacity decay of the sodium ion battery. In addition, according to Figure 1~Figure 2 It can be seen that the sodium ion battery of the present invention can maintain good cycle performance before the explosion-proof valve is triggered and the battery breaks down or fails.

[0059] (3) Analysis of battery cell gas composition: The gases in the battery cells of the sodium ion batteries in Example 1, Example 6 and Comparative Examples 1, 2, 4 and 5 after thermal abuse at 180° C. were collected, and the gas composition was analyzed by gas chromatography (GC). The test results are shown in Table 3.

[0060] Table 3 Gas composition of the sodium ion battery after thermal abuse at 180°C in Examples 1, 6 and Comparative Examples 1, 2, 4 and 5

[0061] According to the data in Table 3, the gas component in the battery cell of Example 1 or 6 is mainly CO2, which can effectively reduce the risk of combustion or explosion of the sodium ion battery due to thermal abuse; the data of Comparative Examples 1 and 2 show that when the positive electrode active material of the sodium ion battery is a simple polyanion material or a Prussian material, the gas component in the battery cell is mainly combustible gases such as C2H4, C3H6, C3H8, H2, CH4 and CO, which has a greater risk of combustion or explosion; the data of Comparative Examples 4 and 5 show that when the type and content of the organic solvent in the electrolyte are inappropriate, the risk of combustion or explosion of the battery cell will also increase.

[0062] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A sodium ion battery, comprising a battery shell and a battery core, wherein the battery core comprises a positive electrode sheet, a separator, a negative electrode sheet and an electrolyte, characterized in that: The battery case contains an explosion-proof valve; The positive electrode active material in the positive electrode sheet is a mixture of positive electrode active material I and positive electrode active material II, wherein the positive electrode active material I is at least one of a polyanion material or a Prussian material, and the positive electrode active material II is at least one of a layered oxide material, sodium carbonate, sodium citrate or sodium oxalate; The mass fraction of the positive electrode active material II in the positive electrode active material is 5% to 45%; The electrolyte includes sodium salt and a solvent, wherein the solvent is a mixture of ethylene carbonate and propylene carbonate, and the mass fraction of ethylene carbonate in the solvent is 5% to 70%.

2. The sodium ion battery according to claim 1, characterized in that: The mass fraction of the positive electrode active material II in the positive electrode active material is 5% to 25%.

3. The sodium ion battery according to claim 1, characterized in that: The mass fraction of the ethylene carbonate in the solvent is 20% to 50%.

4. The sodium ion battery according to any one of claims 1 to 3, characterized in that: The sodium ion battery is cylindrical, and the pressure resistance value of its explosion-proof valve is ≤1.5MPa.

5. The sodium ion battery according to any one of claims 1 to 3, characterized in that: The sodium ion battery is of square shell type, and the pressure resistance value of its explosion-proof valve is ≤1.2MPa.

6. The sodium ion battery according to claim 1, characterized in that: The chemical formula of the layered oxide material is NaMO2, wherein M is at least one of Fe, Ni, Mn, Cu, Co, Ru, Ir, Sn, Cr, Nb or Mo.

7. The sodium ion battery according to claim 1, characterized in that: The Prussian material includes a Prussian blue material or a Prussian white material; The chemical formula of the Prussian blue material is Na x P[R(CN)6] y , wherein P and R are independently at least one of Mn, Fe, Ni, Co, Cu, Ce, Cr, Ti, Zn or V; and the values ​​of x and y satisfy the charge balance of the chemical formula.

8. The sodium ion battery according to claim 1, characterized in that: The chemical formula of the polyanion material is Na4Fe m M n (PO4)2P2O7 / C、Na4Fe m M n PO4P2O7F3 / C、Na3Fe m M n PO4F / C, Na3Mn m M n (PO4)3 / C or Na2Fe m M n P2O7 / C; Wherein, M is at least one of Ni, Mn, Co, Cu, Zn, Mg, Al, Ca, Sr, Ce, Ti, Zr, Sn, V, Nb, Sb or Mo; and the values ​​of m and n satisfy the charge balance of the chemical formula.

9. A method for preparing a sodium ion battery according to any one of claims 1 to 8, further characterized in that it comprises the following steps: First, the positive electrode sheet, the separator, and the negative electrode sheet are wound to obtain a bare cell, and then the bare cell is placed in the inner cavity of the battery shell, and then the electrolyte is injected into the bare cell to obtain a sodium ion battery.

10. Use of the sodium ion battery according to any one of claims 1 to 8 in a battery module or a battery pack.

Citation Information

Patent Citations

  • Explosion-proof housing of battery

    CN105977407A

  • A cylindrical lithium battery cap

    CN109148747A

  • Square aluminum shell lithium ion battery and battery cover plate thereof

    CN217086730U

  • Square aluminum shell battery top cover

    CN218039483U

Cited By

  • Sodium ion battery and application thereof

    CN120413677A