Preparation method of composite solid electrolyte membrane and solid-state battery
By using the combination of mesogenic anatase titanium dioxide powder with polymer solid electrolyte and sulfide solid electrolyte, a composite solid electrolyte membrane is formed, which solves the problems of conductivity and interface stability in solid lithium-ion batteries and significantly improves the circulation of the battery Stability and energy density.
Patent Information
- Application Number
- CN202411178591.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-08
AI Technical Summary
During the industrialization of solid electrolytes in solid-state lithium-ion batteries, the problems of low conductivity at room temperature and unstable interfaces of positive and negative electrodes are faced with problems such as, which affect the safety, energy density and cycle life of the battery.
The mesogenic anatase titanium dioxide powder and polymer solid electrolyte, sulfide solid electrolyte and lithium salt are stirred in a polar solvent at a molar ratio to form a composite solid electrolyte membrane and coated on polymer foil to dry it. A composite solid electrolyte membrane with a highly ordered structure was prepared to improve ion conductivity and mechanical properties and improve interface stability.
It significantly improves ionic conductivity and mechanical properties, reduces interface resistance, enhances charge separation efficiency, improves the cycle stability and energy density of the battery, and improves the overall performance of all-solid-state batteries.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a method for preparing a composite solid electrolyte membrane and a solid-state battery. Background Art
[0002] Lithium-ion batteries are currently the mainstream products in the battery market, and liquid electrolytes are usually used. The energy density and safety performance of lithium-ion batteries using liquid electrolytes have been difficult to be greatly improved. Compared with conventional liquid electrolytes, solid electrolytes have many technical advantages, including high safety, high electrochemical stability, good thermal stability and high mechanical stability to inhibit lithium dendrites and electrolyte leakage. Therefore, solid electrolytes, as the core components of solid-state lithium-ion batteries, play a key role in improving the safety, energy density and cycle life of batteries. However, the industrialization process of solid electrolytes still faces many problems, such as low conductivity of solid electrolytes at room temperature, and unstable interfaces between solid electrolytes and positive and negative electrodes. Therefore, in order to overcome the challenges faced by solid electrolytes, the research on composite solid electrolytes is developing in the direction of improving ionic conductivity, enhancing mechanical strength, improving interface stability and widening electrochemical windows to meet the commercialization needs of all-solid-state batteries. In response to the above technical requirements, this application proposes a method for preparing a composite solid electrolyte membrane and a solid-state battery, which can effectively improve ionic conductivity, enhance mechanical properties and improve interface stability. Summary of the invention
[0003] The object of the present invention is to provide a method for preparing a composite solid electrolyte membrane and a solid-state battery, which can effectively improve ion conductivity, enhance mechanical properties and improve interface stability.
[0004] The technical solution adopted by the present invention to solve the above technical problems is:
[0005] A method for preparing a composite solid electrolyte membrane comprises the following steps:
[0006] S1, preparing mesocrystalline anatase titanium dioxide powder;
[0007] S2. Preparation of composite solid electrolyte membrane using mesocrystalline anatase titanium dioxide powder:
[0008] Add mesocrystalline anatase titanium dioxide powder, polymer solid electrolyte, sulfide solid electrolyte and lithium salt into a polar solvent in a molar ratio of 1-2:2-5:3-7:0.2-1, and continue stirring at room temperature for 12h-25h to obtain a mixed slurry; apply the mixed slurry on a polymer foil, dry it at 40℃-80℃ in a vacuum environment for 8h-16h, and peel off the polymer foil to obtain a composite solid electrolyte membrane.
[0009] Preferably, the mesogenic anatase titanium dioxide powder prepared in step S1 includes pure titanium dioxide and its doped and modified derivatives, and the doped and modified derivatives include at least one of nitrogen doping, carbon doping, sulfur doping, metal and oxide modification.
[0010] Preferably, the lithium salt is one or more of lithium bis(oxalate borate) LiBOB, lithium hexafluorophosphate LiPF6, lithium bis(fluorosulfonyl)imide LiFSI, and lithium bis(trifluoromethanesulfonyl)imide LITFSI.
[0011] Preferably, the mass ratio of the sulfide solid electrolyte to the polar solvent is 10-20:30-45.
[0012] Preferably, the polymer solid electrolyte in step S2 is at least one of polyethylene oxide (PEO), polyvinyl alcohol (PEG), polypropylene (PP), polyacrylate (PBA), polycarbonate (PCE), polypropylene (PAN), polytrimethylene carbonate (PTMC), polyvinyl chloride (PVC), polyamide (PA), and polyvinylidene fluoride (PVDF).
[0013] Preferably, the sulfide solid electrolyte in step S2 is a binary sulfide electrolyte and / or a ternary sulfide solid electrolyte.
[0014] Preferably, the polar solvent in step S2 is one of acetonitrile, formamide, trifluoroacetic acid, DMSO, DMF, hexamethylphosphoramide, methanol, acetic acid, ethanol, isopropanol, pyridine, tetramethylethylenediamine, acetone, triethylamine, n-butanol, dioxane, tetrahydrofuran, and methyl formate.
[0015] Preferably, the composite solid electrolyte membrane prepared in step S2 has a thickness of 50 μm-400 μm.
[0016] Preferably, the specific steps for preparing mesocrystalline anatase titanium dioxide powder are: dissolving a titanium source in a 1 mol / L-3 mol / L hydrochloric acid solution, wherein the volume ratio of the titanium source to the hydrochloric acid is 1-3:4-10, stirring at 40°C-100°C for 40h-60h, centrifuging to obtain a white product, washing the white product with deionized water to remove residual inorganic ions, and then vacuum drying the white product at 80°C-120°C for 12h-36h, and finally calcining in air at 400°C-500°C for 12h-24h to obtain the mesocrystalline anatase titanium dioxide powder.
[0017] A solid-state battery, characterized in that it comprises a composite negative electrode sheet, a composite positive electrode sheet and a composite solid electrolyte membrane prepared by the above method, wherein the composite solid electrolyte membrane is located between the composite positive electrode sheet and the composite negative electrode sheet.
[0018] Compared with the prior art, the advantages of the present invention are:
[0019] Mesocrystalline anatase titanium dioxide is composed of tiny subunits gathered together in the same direction, thus forming a highly ordered structure that is conducive to rapid electron transport, and has a higher specific surface area and more defect sites at the atomic level. Compared with ordinary structure anatase titanium dioxide, after the first cycle, the lattice spacing of mesocrystalline anatase titanium dioxide is widened, providing a more effective ion channel and significantly improving the ion conductivity. At the same time, since the mesocrystalline structure has a large number of pores, it increases the contact area with the electrolyte and reduces the interface resistance, which is beneficial to improve the charge separation efficiency and improve the overall battery performance. In terms of lithium ion transport mechanism, mesocrystalline anatase titanium dioxide is based on a highly reversible crystallization-amorphous-recrystallization process. The synergistic effect of the amorphous phase and the inherent intergranular rapid diffusion network inside the mesocrystal makes the lithium ion diffusion rate inside the structure much higher than that of conventional anatase titanium dioxide, and because the final product after delithiation is Li with good chemical / mechanical stability 0.16 TiO2, the material stability has been significantly improved, and the stability of the solid electrolyte and the positive and negative electrode interfaces has been further improved. DETAILED DESCRIPTION
[0020] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments.
[0021] Example:
[0022] A solid-state battery comprises a composite positive electrode sheet, a composite solid electrolyte membrane and a composite negative electrode sheet of micron-sized silicon particles, wherein the composite solid electrolyte membrane is located between the composite positive electrode sheet and the composite negative electrode sheet.
[0023] Preparation of micron-sized silicon particle composite negative electrode sheet:
[0024] Mesocrystalline anatase titanium dioxide powder, polymer solid electrolyte, sulfide solid electrolyte, micron-sized silicon particles and aqueous binder are added to a polar solvent in a molar ratio of 1.5-3:1-4:0.5-2:20-35:0.01-0.2, and the mass ratio of micron-sized silicon particles to polar solvent is 20-30:45-55, and stirred at room temperature for 10h-30h to obtain a mixed slurry; at room temperature, the mixed slurry is coated on the negative electrode current collector by a doctor blade method or a transfer coating method, and the coating thickness is 50μm-500μm to obtain a composite negative electrode with a certain thickness, and the composite negative electrode is rolled under a pressure of 5MPa-30MPa, and then punched according to requirements to obtain a dense micron-sized silicon particle composite negative electrode sheet. Among them, the particle size of the micron-sized silicon particles is 0.5μm-15μm, and the shape of the silicon particles is not limited.
[0025] The water-based binder is one of styrene-butadiene rubber (SBR) emulsion, carboxymethyl cellulose (CMC), polyacrylic acid (PAA), polyacrylonitrile (PAN) and polyacrylate.
[0026] The negative electrode current collector adopts an elastic composite current collector, and the elastic composite current collector is prepared by a preparation method of a current collector for an all-solid-state battery disclosed in application number 202111044090.0, as in Example 1 in the above application document, MF is mixed in a ratio of 4:3 and heated to 85°C, and melamine is continued to be added to the mixture while keeping the temperature constant, so that the mass ratio of melamine to water is 11:12, and stirring is continued until the mixed solution is clear, and the pH of the mixed solution is adjusted with hexamethylenetetramine to make the pH of the mixed solution 8-9, EG is added, and the mass ratio of EG to water is 1:12, and the reaction is carried out for 2min-3min. After the reaction is completed, sodium borate decahydrate is added to make the pH value of the mixed solution 10-10.5, and the mixed solution is cooled to 28°C, and the temperature is kept constant for 3min to obtain a viscous EG / MF prepolymer; EG / MF prepolymer, n-hexane, dimethyl silicone oil, hydrochloric acid and CF are added into a container in a mass ratio of 55:3:1:0.15:0.4, stirred at room temperature for 15 minutes to obtain a foaming liquid; the foaming liquid is quickly introduced into a mold, foamed at 100°C for 35 minutes, and then cured at 125°C for 5 minutes to obtain CF / MF; the CF / MF is carbonized in nitrogen at 850°C for 2 minutes, cooled to room temperature, and then rinsed with water and ethanol to remove residual impurities therein to obtain carbonized CF / MF; the obtained carbonized CF / MF is used as a cathode, copper foil is used as an anode, and 1.0 mol / L copper sulfate solution is used as an electrolyte, a pulse current of 10 mA / cm2 is applied for electrodeposition, and the electrodeposition lasts for 15 minutes to obtain an elastic composite current collector of CF / MF / Cu.
[0027] The negative electrode current collector may also be one of copper foil, porous copper foil, carbon-coated copper foil, composite copper foil and high molecular polymer foil.
[0028] Preparation of composite solid electrolyte membrane:
[0029] Mesomorphous anatase titanium dioxide powder, polymer solid electrolyte, sulfide solid electrolyte, and lithium salt are added to a polar solvent in a molar ratio of 1-2:2-5:3-7:0.2-1, and the mass ratio of sulfide solid electrolyte to polar solvent is 10-20:30-45. Stirring is continued at room temperature for 12h-25h to obtain a mixed slurry. At room temperature, the mixed slurry is coated on a polymer foil by a doctor blade method or a transfer coating method, and dried at 40℃-80℃ in a vacuum environment for 8h-16h. After peeling off the polymer foil, a composite solid electrolyte membrane is obtained, and the thickness of the composite solid electrolyte membrane is 50μm-400μm. Among them, the polymer foil is made of polyethylene terephthalate.
[0030] The polymer solid electrolyte used in the above-mentioned preparation of the negative electrode sheet and the composite solid electrolyte is at least one or more of polyethylene oxide (PEO), polyvinyl alcohol (PEG), polypropylene (PP), polyacrylate (PBA), polycarbonate (PCE), polypropylene (PAN), polytrimethylene carbonate (PTMC), polyvinyl chloride (PVC), polyamide (PA), and polyvinylidene fluoride (PVDF).
[0031] Preparation of composite positive electrode sheet:
[0032] High nickel ternary positive electrode material, sulfide solid electrolyte, mesomorphous anatase titanium dioxide, lithium salt and binder are added to the solvent in a molar ratio of 30-50:3-8:1.5-5:0.5-2.5:0.5-1.5, and the mass ratio of high nickel ternary positive electrode material to solvent is 11-20:12-25, and the mixture is stirred for 12h-24h at room temperature to obtain a mixed solution; at room temperature, the mixed solution is coated on the positive electrode current collector by a scraper method or a transfer coating method, and the coating thickness is 150μm-500μm to obtain a composite positive electrode with a certain thickness, and then the composite positive electrode is rolled under a pressure of 20MPa-50MPa and punched according to requirements to obtain a dense composite positive electrode sheet. Among them, the binder is one of polyacrylonitrile PAN, polyimide PI, polyvinyl alcohol PVA, polyvinylidene fluoride PVDF, and polyacrylamide PAM. The positive electrode current collector used is one of conventional aluminum foil, perforated aluminum foil, carbon-coated aluminum foil, composite aluminum foil, high molecular polymer foil (such as polyethylene terephthalate), etc.
[0033] The lithium salt used in the preparation of the composite positive electrode sheet and the composite solid electrolyte is one or more of lithium bis(oxalate borate) LiBOB, lithium hexafluorophosphate LiPF6, lithium bis(fluorosulfonyl)imide LiFSI, and lithium bis(trifluoromethanesulfonyl)imide LITFSI.
[0034] Preparation of the aforementioned mesocrystalline anatase titanium dioxide powder: dissolve the titanium source in 1mol / L-3mol / L hydrochloric acid solution, the volume ratio of the titanium source to the hydrochloric acid solution is 1-3:4-10, stir at 40℃-100℃ for 40h-60h, centrifuge to obtain a white product, wash with deionized water 3-6 times to remove the residual inorganic ions in the white product, and then vacuum dry the white product at 80℃-120℃ for 12h-36h, and finally calcine in air at 400℃-500℃ for 12h-24h to obtain mesocrystalline anatase titanium dioxide powder.
[0035] The titanium source includes at least one of dichlorotitacenes, tetraisopropoxytitanium, tetrabutyl titanate, titanium citrate, and titanium tetrachloride. The prepared mesocrystalline anatase titanium dioxide powder includes pure titanium dioxide and its doped and modified derivatives, and the doped and modified derivatives include at least one of nitrogen doping, carbon doping, sulfur doping, metal and oxide modification.
[0036] The sulfide solid electrolyte used in the preparation of the composite negative electrode sheet, composite positive electrode sheet and composite solid electrolyte membrane is a binary sulfide electrolyte and / or a ternary sulfide solid electrolyte. The binary sulfide electrolyte is Li3PS4 and Li7P3S 11 , the ternary sulfide solid electrolyte is Li 10 GeP2S 12 and Li6PS5X, where X = Cl, Br and I.
[0037] The polar solvent used in the preparation of the composite negative electrode sheet, the composite positive electrode sheet and the composite solid electrolyte membrane is one of acetonitrile, formamide, trifluoroacetic acid, DMSO, DMF, hexamethylphosphoramide, methanol, acetic acid, ethanol, isopropanol, pyridine, tetramethylethylenediamine, acetone, triethylamine, n-butanol, dioxane, tetrahydrofuran and methyl formate.
[0038] Embodiment 1,
[0039] A solid-state battery is prepared by the following method:
[0040] Preparation of mesocrystalline anatase titanium dioxide powder: First, a certain amount of isopropoxy titanium was dripped into 1.5 mol / L hydrochloric acid, where the volume ratio of isopropoxy titanium to hydrochloric acid was 2:7. Then, stirring was continued at 80°C for 48 hours, and a white product was obtained after centrifugation. The product was washed with deionized water 4 times to remove the residual non-polar ions. The white product was dried at 110°C for 2 hours, and then sintered in nitrogen at 450°C for 16 hours to obtain nitrogen-doped mesocrystalline anatase titanium dioxide powder.
[0041] Preparation of micron-sized silicon particle composite negative electrode sheet:
[0042] The prepared mesomorphous anatase titanium dioxide powder was mixed with polyethylene oxide (PEO) and ternary sulfide solid electrolyte Li 10 GeP2S 12 , micron-sized silicon particles and a small amount of polyacrylic acid (PAA) as a binder are added to an acetonitrile solvent in a molar ratio of 1.7:3.0:1.8:23:0.11, and the mass ratio of micron-sized silicon particles to acetonitrile is 25:49. After continuous stirring for 18 hours at room temperature, the mixed slurry is coated on the negative electrode current collector by a scraper method or a transfer coating method to obtain a composite negative electrode with a certain thickness. The micron-sized silicon particles used in the present invention have an average size of 3.5 microns, and the negative electrode current collector used is an elastic composite current collector. The coating thickness of the composite negative electrode is 250 microns. The coated composite negative electrode is rolled under a pressure of 25MPa to obtain a dense composite silicon-based negative electrode, and the rolled negative electrode is punched according to demand to obtain a micron-sized silicon particle composite negative electrode sheet.
[0043] Preparation of composite solid electrolytes:
[0044] The prepared mesomorphous anastase titanium dioxide powder, polypropylene (PAN), ternary sulfide solid electrolyte Li6PS5Cl, and lithium salt LITFSI are added to acetonitrile solvent in a molar ratio of 1.3:3.4:5:0.7, with a mass ratio of Li6PS5Cl to acetonitrile of 17:42. The mixture is stirred for 23 hours at room temperature, and the mixed liquid is coated on a polymer foil (polyethylene terephthalate) using a scraper method, and dried at 70°C under vacuum for 15 hours. A composite solid electrolyte membrane is obtained after peeling, and the thickness of the composite solid electrolyte membrane is 50-400 μm.
[0045] Preparation of composite positive electrode sheet:
[0046] The high nickel ternary cathode material and ternary sulfide solid electrolyte Li 10 GeP2S 12 , mesomorphous anatase titanium dioxide, lithium bis(trifluoromethanesulfonic acid imide) LITFSI and polyacrylonitrile PAN are added to dimethyl sulfoxide in a molar ratio of 42:7:3.4:2.2:1.1, and the mass ratio of high nickel ternary material to dimethyl sulfoxide is 17:23. Stir for 22 hours at room temperature to mix evenly to obtain a mixed slurry. The mixed slurry is coated on a carbon-coated aluminum foil at room temperature by transfer coating to obtain a composite positive electrode with a certain thickness, and the coating thickness is 420 microns. Finally, the coated composite positive electrode is rolled at a pressure of 45MPa to obtain a dense composite positive electrode, and the rolled positive electrode is punched according to the requirements to obtain a composite positive electrode sheet.
[0047] The composite positive electrode sheet and composite negative electrode sheet prepared above were pressed on both sides of the composite solid electrolyte membrane at 70 standard atmospheres to prepare a button-type all-solid battery. The assembled battery was cycled at room temperature in the voltage range of 2.5V-4.3V at a rate of 0.5C. The internal resistance of the battery was tested by electrochemical impedance spectroscopy, with a frequency range of 0.1HZ to 1MHZ and an applied voltage amplitude of 5mV.
[0048] Embodiment 2,
[0049] Compared with Example 1, mesomorphous anatase titanium dioxide is sintered at 450°C in air and does not contain nitrogen doping. Preparation conditions of composite negative electrode sheet: the molar ratio of mesomorphous anatase titanium dioxide powder, polymer solid electrolyte, sulfide solid electrolyte, micron-sized silicon particles and binder is 3:1:2.0:20:0.2. Preparation conditions of composite positive electrode sheet: high nickel ternary positive electrode material and sulfide solid electrolyte, mesomorphous anatase titanium dioxide, lithium salt and binder are added to isopropanol in a molar ratio of 30:8:1.5:2.5:1.5, stirred at room temperature for 12 hours to mix evenly, and the mass ratio of high nickel ternary material to isopropanol is 11:25. The other conditions are the same as in Example 1.
[0050] Embodiment 3,
[0051] Compared with Example 1, the preparation conditions of the composite negative electrode sheet are as follows: the molar ratio of mesomorphic anatase titanium dioxide powder, polymer solid electrolyte, sulfide solid electrolyte, micron-sized silicon particles and binder is 1.5:4:0.5:35:0.01. The preparation conditions of the composite positive electrode sheet are as follows: the high nickel ternary positive electrode material and the sulfide solid electrolyte, mesomorphic anatase titanium dioxide, lithium salt and binder are added to dimethyl sulfoxide in a molar ratio of 50:3:5.0:0.5:0.5, stirred at room temperature for 24 hours to mix evenly, and the mass ratio of high nickel ternary material to dimethyl sulfoxide is 20:12. The other conditions are the same as those in Example 1.
[0052] Embodiment 4,
[0053] Compared with Example 1, the preparation conditions of the composite electrolyte membrane are as follows: mesomorphous anatase titanium dioxide powder and polymer solid electrolyte, sulfide solid electrolyte Li3PS4, and lithium salt LITFSI are added to acetonitrile solvent in a molar ratio of 2.0:5:3:0.2, and stirred continuously at room temperature for 25 hours. The mixed liquid is coated on a polymer foil (polyethylene terephthalate) by a doctor blade method, etc., and dried at 65°C under vacuum for 12 hours. After peeling, a composite solid electrolyte membrane is obtained. The mass ratio of Li3PS4 to acetonitrile is 20:45. The positive electrode current collector is conventional aluminum foil, and the negative electrode current collector is conventional copper foil. The remaining conditions are the same as in Example 1.
[0054] Embodiment 5,
[0055] Compared with Example 1, the coating thickness of the composite positive electrode sheet is 500 microns. The composite positive electrode sheet is rolled at a pressure of 50 MPa to obtain a dense composite positive electrode, and the rolled composite positive electrode is punched out as required.
[0056] The composite positive electrode sheet and the composite negative electrode sheet were respectively pressed on both sides of the composite solid electrolyte membrane at 50 standard atmospheres to prepare a button-type all-solid battery. The other conditions were the same as those in Example 1.
[0057] Embodiment 6,
[0058] Compared with Example 1, the preparation conditions of the mesocrystalline anatase titanium dioxide powder are as follows: calcination in air at 450° C. for 12 hours; the lithium salt in the composite solid electrolyte is lithium hexafluorophosphate LiPF6. The other conditions are the same as those in Example 1.
[0059] Comparative Example 1
[0060] Compared with Example 1, the mesogenic titanium dioxide was sintered in air at 650° C. to obtain rutile mesogenic titanium dioxide powder. The other conditions were the same as those in Example 1.
[0061] Comparative Example 2
[0062] Compared with Example 1, commercial titanium dioxide powder (LOMON R 996) was used, and the other conditions were the same as those in Example 1.
[0063] Comparative Example 3
[0064] Compared with Example 1, no mesomorphous anatase titanium dioxide is added to the solid electrolyte membrane, and other conditions are the same as those in Example 1.
[0065] Comparative Example 4
[0066] Compared with Example 1, no mesocrystal anatase titanium dioxide is added to the composite positive electrode sheet, and the other conditions are the same as those in Example 1.
[0067] Comparative Example 5
[0068] Compared with Example 1, no mesocrystal anatase titanium dioxide is added to the composite negative electrode sheet, the composite positive electrode sheet and the solid electrolyte membrane, and the other conditions are the same as those in Example 1.
[0069] Comparative Example 6
[0070] Compared with Example 1, the mesomorphous anatase titanium dioxide in the composite negative electrode sheet is replaced by an equal amount of conductive carbon black, and the other conditions are the same as those in Example 1.
[0071] Comparative Example 7
[0072] Compared with Example 1, the composite negative electrode sheet uses nano-scale silicon powder, and the other conditions are the same as those of Example 1.
[0073] Table 1. Comparison of test results of different all-solid-state batteries
[0074] sample Internal resistance(Ω) Capacity retention rate after 100 cycles (%) Example 1 23.3 89.8 Example 2 30.6 86.2 Example 3 27.7 87.6 Example 4 27.1 88.5 Example 5 26.8 88.7 Example 6 25.5 88.1 Comparative Example 1 44.6 70.8 Comparative Example 2 50.3 66.3 Comparative Example 3 33.7 80.9 Comparative Example 4 39.2 75.1 Comparative Example 5 58.4 64.8 Comparative Example 6 42.8 71.4 Comparative Example 7 35.4 79.2
[0075] The specific test results are shown in Table 1. Combined with Examples 1-6, it can be seen that within the technical requirements of the present invention, the internal resistance and cycle life of the all-solid-state battery have been significantly improved, and Example 1 has the best technical effect. Combined with Example 1 and Comparative Examples 1-6, it is found that the mesogenic anatase titanium dioxide powder prepared by the present invention can significantly reduce the internal resistance of the battery and increase the cycle life of the battery. Compared with conventional commercial titanium dioxide powder and rutile titanium dioxide, the mesogenic anatase titanium dioxide prepared by the present invention is composed of tiny grains of several nanometers, which reduces structural defects such as twins or dislocations in the crystal structure, and is conducive to the appearance of amorphous Li during the lithiation process. 0.5 TiO2 phase rather than orthorhombic phase Li 0.5 TiO2, thus improving the lithium storage capacity and lithium ion conductivity of titanium dioxide materials, while the chemical / mechanical properties of the amorphous phase improve the cycle stability of the battery. The composite silicon negative electrode used in the present invention is micron-sized, has a lower specific surface area than nanoparticles, and has low side reactions with solid electrolytes, which reduces material costs. In addition, the elastic current collector provides a strong support force to buffer the volume changes of the silicon negative electrode during charging and discharging, and fills a small amount of solid electrolyte and mesocrystal rutile titanium dioxide particles to maintain the mechanical stability of the interface between silicon micron particles and the lithium ion transmission channel, so the cycle life and internal resistance of the all-solid-state battery are significantly improved. The above results show that the method proposed in the present invention can significantly improve the internal resistance and cycle stability of silicon-based all-solid-state batteries, providing important technical support for the development of high-performance lithium-ion power batteries.
[0076] By adding mesomorphous anatase titanium dioxide powder to the composite positive electrode sheet, the mesomorphous structure of TiO2 has a high specific surface area and abundant pores, which helps to form a more effective ion conduction path and reduce the ion diffusion resistance inside the battery. In lithium-ion batteries, the unique crystal structure of TiO2 helps to accelerate the insertion and extraction of lithium ions and improve the rate performance of the overall battery. Compared with the ordinary structure anatase titanium dioxide, after the first cycle, the mesomorphous anatase titanium dioxide and the lattice spacing are widened, providing a more effective ion channel and significantly improving the ion conductivity. Since the mesomorphous structure has a large number of pores, it increases the contact area with the electrolyte and reduces the interface resistance, which is conducive to improving the charge separation efficiency and improving the overall battery performance. In terms of lithium ion transport mechanism, mesomorphous anatase titanium dioxide is based on a highly reversible crystallization-amorphous-recrystallization process. The synergistic effect of the amorphous phase and the inherent intergranular rapid diffusion network inside the mesomorphism makes the lithium ion diffusion rate inside the structure much higher than that of conventional anatase titanium dioxide, and because the final product after delithiation is Li with good chemical / mechanical stability 0.16 TiO2, the material stability has been significantly improved, and the interface stability of the high-nickel positive electrode has been further improved.
[0077] Micron-sized pure silicon particles are used in the negative electrode, with a particle size range of 0.5 μm-15 μm. The shape of silicon particles is not restricted, and the silicon material itself has a certain electronic conductivity (about 3×10 -5 S / cm), in order to avoid unnecessary interface side reactions and improve the battery energy density, the negative electrode sheet prepared by the present invention does not add any inactive carbon conductive agent, and adds electrochemically active mesocrystal rutile titanium dioxide to improve the electrode specific capacity and interface conductivity. Compared with nano silicon particles, the negative electrode prepared by micron-sized silicon particles has high conductivity and high volume energy density. However, silicon particles will undergo a maximum volume change of about 300% during the lithium ion deintercalation process. The volume shrinkage of silicon particles during the delithiation process leads to pores inside the negative electrode, causing the internal resistance of the negative electrode sheet to increase and reduce battery performance. To solve this problem, the present invention adds an elastic composite solid electrolyte with electrochemical activity to the above-mentioned silicon particles, fills the pores generated when the silicon particles shrink in volume during lithium deintercalation, always ensures contact with the silicon particles, and has lithium storage capacity, which can significantly improve the transmission speed of lithium ions between silicon particles. The negative electrode current collector adopts an elastic composite current collector, which can provide sufficient elasticity to mitigate the volume change of the silicon-based negative electrode system during the charging and discharging process.
[0078] Compared with conventional nano-titanium dioxide and micro-titanium dioxide materials, the synergistic effect of the inherent inter-granular rapid diffusion network within the mesogenic anatase-type titanium dioxide enables its lithium ion diffusion rate to be higher and can significantly improve the material's cycle stability.
[0079] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a composite solid electrolyte membrane, characterized in that: The following steps are involved: S1, preparing mesocrystalline anatase titanium dioxide powder; S2. Preparation of composite solid electrolyte membrane using mesocrystalline anatase titanium dioxide powder: Add mesocrystalline anatase titanium dioxide powder, polymer solid electrolyte, sulfide solid electrolyte and lithium salt into a polar solvent in a molar ratio of 1-2:2-5:3-7:0.2-1, and continue stirring at room temperature for 12h-25h to obtain a mixed slurry; apply the mixed slurry on a polymer foil, dry it at 40℃-80℃ in a vacuum environment for 8h-16h, and peel off the polymer foil to obtain a composite solid electrolyte membrane.
2. The method for preparing a composite solid electrolyte membrane according to claim 1, characterized in that: The mesocrystalline anatase titanium dioxide powder prepared in step S1 includes pure titanium dioxide and its doped and modified derivatives, and the doped and modified derivatives include at least one of nitrogen doping, carbon doping, sulfur doping, metal and oxide modification.
3. The method for preparing a composite solid electrolyte membrane according to claim 1, characterized in that: The lithium salt is one or more of lithium bis(oxalate borate) LiBOB, lithium hexafluorophosphate LiPF6, lithium bis(fluorosulfonyl)imide LiFSI, and lithium bis(trifluoromethanesulfonyl)imide LITFSI.
4. The method for preparing a composite solid electrolyte membrane according to claim 1, characterized in that: The mass ratio of the sulfide solid electrolyte to the polar solvent is 10-20:30-45.
5. The method for preparing a composite solid electrolyte membrane according to claim 1, characterized in that: The polymer solid electrolyte in step S2 is at least one of polyethylene oxide (PEO), polyvinyl alcohol (PEG), polypropylene (PP), polyacrylate (PBA), polycarbonate (PCE), polypropylene (PAN), polytrimethylene carbonate (PTMC), polyvinyl chloride (PVC), polyamide (PA), and polyvinylidene fluoride (PVDF).
6. The method for preparing a composite solid electrolyte membrane according to claim 1, characterized in that: The sulfide solid electrolyte in step S2 is a binary sulfide electrolyte and / or a ternary sulfide solid electrolyte.
7. The method for preparing a composite solid electrolyte membrane according to claim 1, characterized in that: The polar solvent in step S2 is one of acetonitrile, formamide, trifluoroacetic acid, DMSO, DMF, hexamethylphosphoramide, methanol, acetic acid, ethanol, isopropanol, pyridine, tetramethylethylenediamine, acetone, triethylamine, n-butanol, dioxane, tetrahydrofuran, and methyl formate.
8. The method for preparing a composite solid electrolyte membrane according to claim 1, characterized in that: The thickness of the composite solid electrolyte membrane prepared in step S2 is 50 μm-400 μm.
9. The method for preparing a composite solid electrolyte membrane according to claim 1, characterized in that: The specific steps of preparing mesocrystalline anatase titanium dioxide powder are as follows: dissolving a titanium source in a 1mol / L-3mol / L hydrochloric acid solution, wherein the volume ratio of the titanium source to the hydrochloric acid is 1-3:4-10, stirring at 40°C-100°C for 40h-60h, centrifuging to obtain a white product, washing the white product with deionized water to remove residual non-polar ions, and then vacuum drying the white product at 80°C-120°C for 12h-36h, and finally calcining in air at 400°C-500°C for 12h-24h to obtain the mesocrystalline anatase titanium dioxide powder.
10. A solid-state battery, characterized in that: The invention comprises a composite negative electrode sheet, a composite positive electrode sheet and a composite solid electrolyte membrane prepared by the method according to any one of claims 1 to 9, wherein the composite solid electrolyte membrane is located between the composite positive electrode sheet and the composite negative electrode sheet.
Citation Information
Cited By
Wide-temperature high-rate solid-state battery
CN122136436A