Composite material, solid electrolyte and preparation method thereof, and lithium metal battery
Through the composite material of garnet-type solid electrolyte and zeolite imidazole ester framework, the problems of high density, low conductivity and insufficient mechanical strength in solid lithium metal batteries were solved, and high density, high conductivity and high mechanical strength were prepared. The solid electrolyte improves the performance and life of lithium metal batteries.
Patent Information
- Application Number
- CN202411320872.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-09-20
AI Technical Summary
The solid electrolytes of existing solid-state lithium metal batteries have problems such as high densification temperature, unsatisfactory ionic conductivity and insufficient mechanical strength, which is difficult to meet the high energy density and safety performance requirements of the battery.
Using garnet solid electrolyte and zeolite imidazole ester skeleton composite material, a solid electrolyte with high density, high ionic conductivity and high mechanical strength is prepared by high temperature sintering. The specific steps include obtaining the solid electrolyte precursor and performing it under an inert atmosphere. High temperature sintering, control the sintering temperature and heating speed to reduce the density temperature.
Densification at lower temperatures is achieved, the density, ionic conductivity and mechanical strength of solid electrolytes are improved, the cycle life of lithium metal batteries is extended, and the safety and energy density of batteries are enhanced.
Smart Images

Figure CN118919831A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of lithium-ion batteries, and in particular to a composite material for preparing a solid electrolyte, a solid electrolyte and a preparation method, and a lithium metal battery. Background Art
[0002] At present, lithium-ion batteries have become one of the most important energy storage devices in people's daily lives due to their advantages such as long cycle life and high energy density. In recent years, with the rapid development of electric vehicles, higher requirements have been placed on the energy density and safety performance of batteries. All-solid-state lithium metal batteries replace flammable liquid electrolytes with solid electrolytes, and use metallic lithium with a higher theoretical specific capacity as the negative electrode. They have the advantages of high safety and high energy density, so it is of great significance to study all-solid-state lithium metal batteries.
[0003] Solid-state electrolytes are the core components of all-solid-state lithium metal batteries. They need to meet the requirements of low preparation temperature, high density, high ionic conductivity and high mechanical strength. They must also ensure that lithium ions can migrate quickly between the positive and negative electrodes while suppressing lithium dendrites to maintain long-term stable battery cycles.
[0004] Therefore, there is an urgent need in the art to provide a solid electrolyte with low preparation temperature, high density, high ionic conductivity and high mechanical strength. Summary of the invention
[0005] In view of this, the present application provides a composite material for preparing a solid electrolyte, wherein the composite material can be densified at a relatively low temperature, and the prepared solid electrolyte has high density, high ionic conductivity and high mechanical strength.
[0006] In a first aspect, an embodiment of the present application provides a composite material for preparing a solid electrolyte, wherein the composite material comprises a garnet-type solid electrolyte and a zeolite imidazolate framework, and calculated by mass percentage, the solid electrolyte: zeolite imidazolate framework = 100: (0.01-6);
[0007] The chemical formula of the solid electrolyte is Li 7-x Ln3Z 2-x Ta x O 12 , 0≤x≤1.
[0008] In some embodiments of the present application, the solid electrolyte: zeolite imidazolate framework = 100: (1-5).
[0009] In some embodiments of the present application, the solid electrolyte: zeolite imidazolate framework = 100: (2-4).
[0010] In some embodiments of the present application, the zeolite imidazolate framework includes at least one of the zeolite imidazolate framework 8 and the zeolite imidazolate framework 67 .
[0011] In some embodiments of the present application, the particle size of the zeolite imidazolate framework is 100 nm to 300 nm.
[0012] In some embodiments of the present application, 0.2≤x≤0.8.
[0013] A second aspect of the present application provides a method for preparing a solid electrolyte, the preparation method comprising:
[0014] Obtain a solid electrolyte precursor; wherein the solid electrolyte precursor includes a solid electrolyte and a zeolite imidazolate framework, and the chemical formula of the solid electrolyte is Li 7-x Ln3Z 2-x Ta x O 12 , 0≤x≤1, calculated by mass percentage, the solid electrolyte: zeolite imidazolate framework = 100: (0.01-6);
[0015] The solid electrolyte is obtained by sintering the solid electrolyte precursor at high temperature.
[0016] In some embodiments of the present application, the sintering temperature is 900° C. to 1300° C.; and / or
[0017] The high temperature sintering includes high temperature sintering in an inert atmosphere; and / or
[0018] The heating rate during the high temperature sintering process is 5°C / min to 20°C / min.
[0019] In some embodiments of the present application, the sintering temperature is 1000° C. to 1100° C.; and / or
[0020] The step of obtaining a solid electrolyte precursor comprises:
[0021] Mixing the solid electrolyte powder and the zeolite imidazolate framework according to a preset ratio to obtain a first mixture;
[0022] A certain pressure is applied to the first mixture to obtain a solid electrolyte precursor.
[0023] A third aspect of the present application provides a solid electrolyte, which includes the composite material or is prepared by the preparation method.
[0024] In some embodiments of the present application, the density of the solid electrolyte is 94% to 99%;
[0025] The ionic conductivity of the solid electrolyte is 0.7 mS / cm to 1.3 mS / cm;
[0026] The elastic modulus of the solid electrolyte is 84 GPa to 175 GPa;
[0027] The hardness of the solid electrolyte is 7 GPa to 13 GPa.
[0028] A fourth aspect of the present application provides a lithium metal battery, the lithium metal battery comprising the solid electrolyte, wherein the solid electrolyte is disposed between the positive electrode and the negative electrode.
[0029] Beneficial effects:
[0030] In the present application, a certain amount of zeolite imidazolate skeleton is added to the composite material for preparing the solid electrolyte, so that a solid electrolyte with low densification temperature, high density, high ionic conductivity and high mechanical strength can be prepared from the composite material in the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative work.
[0032] Figure 1 Schematic diagram of the parameters during nanoindentation.
[0033] Figure 2 Load-depth curve of nanoindentation testing.
[0034] Figure 3 It is the diffraction pattern of ZIF-8 prepared in the examples of the present application.
[0035] Figure 4 This is a cycle test diagram of the battery prepared by Application Example 1 of the present application.
[0036] Figure 5 This is a cycle test diagram of the battery prepared by comparative example 1 of the present application.
[0037] Figure 6 It is a process flow chart of the preparation of the solid electrolyte of the present application. DETAILED DESCRIPTION
[0038] The technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative work belong to the scope of protection of the present application. In addition, it should be understood that the specific implementation methods described herein are only used to illustrate and explain the present application, and are not used to limit the present application.
[0039] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0040] In this application, unless otherwise stated, directional words such as "upper" and "lower" generally refer to the upper and lower parts of the device in actual use or working state, specifically the drawing direction in the accompanying drawings; while "inner" and "outer" refer to the outline of the device. In addition, in the description of this application, the term "including" means "including but not limited to". The terms first, second, third, etc. are used only as labels and do not impose numerical requirements or establish an order.
[0041] In this application, "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural.
[0042] In the present application, "at least one" means one or more, and "plurality" means two or more. "One or more", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.
[0043] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0044] At present, lithium-ion batteries have become one of the most important energy storage devices in people's daily lives due to their advantages such as long cycle life and high energy density. In recent years, with the rapid development of electric vehicles, higher requirements have been placed on the energy density and safety performance of batteries. All-solid-state lithium metal batteries replace flammable liquid electrolytes with solid electrolytes, and use metallic lithium with a higher theoretical specific capacity as the negative electrode. They have the advantages of high safety and high energy density, so it is of great significance to study all-solid-state lithium metal batteries.
[0045] Solid-state electrolytes are the core components of all-solid-state lithium metal batteries. They need to meet the requirements of low preparation temperature, high ionic conductivity and high mechanical strength, and while ensuring that lithium ions can migrate quickly between the positive and negative electrodes, they must also inhibit lithium dendrites and maintain long-term stable battery cycles.
[0046] At present, common solid electrolytes include oxide solid electrolytes, sulfide solid electrolytes, composite solid electrolytes and emerging halide solid electrolytes. Oxide solid electrolytes are widely studied as a material with high ionic conductivity, stable structure, simple synthesis process, non-toxic and pollution-free. Among the many solid electrolytes, garnet-type Li7La3Zr2O 12 (LLZO) has attracted much attention due to its advantages such as high conductivity and good electrochemical stability. However, LLZO still has problems such as unsatisfactory ionic conductivity, low mechanical strength and high densification temperature.
[0047] In view of this, a first aspect of an embodiment of the present application provides a composite material for preparing a solid electrolyte, wherein the composite material has the advantages of a low densification temperature, and high ionic conductivity and mechanical strength.
[0048] Specifically, the composite material provided in the embodiment of the present application includes a garnet-type solid electrolyte and a zeolite imidazolate framework, and by mass, the solid electrolyte: the zeolite imidazolate framework = 100: (0.01-6) (i.e., any value between 0.01 and 6), wherein the chemical formula of the solid electrolyte is Li7-x Ln3Z 2-x Ta x O 12 , 0≤x≤1.
[0049] In the present application, by adding a certain amount of zeolite imidazolate framework into the composite material for preparing the solid electrolyte, a solid electrolyte with low densification temperature, high ionic conductivity and high mechanical strength can be prepared from the composite material in the present application.
[0050] Exemplarily, calculated by mass percentage, the zeolite imidazolate framework: solid electrolyte is approximately 0.01%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6% and any value between the foregoing two points.
[0051] Exemplarily, x is about 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, and any value between the two aforementioned point values. It should be noted that "about" in this application means a value that differs from the actual number by a margin of ±10%. Taking the actual number as 1 as an example, correspondingly, about 1 refers to any value between 0.9 and 1.1.
[0052] In some embodiments of the present application, calculated by mass percentage, solid electrolyte: zeolite imidazolate skeleton = 100: (1-5). Further, solid electrolyte: zeolite imidazolate skeleton = 100: (1-3), and further, solid electrolyte: zeolite imidazolate skeleton = 100: (1.5-2.5). In this embodiment, controlling the zeolite imidazolate skeleton within this range can further reduce the densification temperature and improve the ionic conductivity and mechanical strength of the solid electrolyte.
[0053] In some embodiments of the present application, X is greater than 0. That is, the solid electrolyte is LLZTO formed by doping LLZO with Ta element. In this embodiment, doping with Ta element is beneficial to further improve the ionic conductivity of the solid electrolyte.
[0054] It should be noted that, compared with LLZO, although the lithium ion conductivity of LLZTO is greatly improved, its lithium ion conductivity is still not ideal, and LLZTO also has the problems of low density and high densification temperature. In this embodiment, by compounding the zeolite imidazolate framework with LLZTO, the density of LLZTO can be improved, and its densification temperature (referring to the heat treatment temperature when densification is completed) can be reduced, and the ionic conductivity and mechanical strength of the solid electrolyte can be improved.
[0055] In some embodiments of the present application, 0.1≤x≤0.9. Further, 0.4≤x≤0.8. Still further, 0.5≤x≤0.7. In this embodiment, by controlling the content of Ta element doping, it is beneficial to further improve the ionic conductivity and mechanical strength of the solid electrolyte.
[0056] In some embodiments of the present application, the zeolite imidazolate framework includes at least one of zeolite imidazolate framework 8 (also known as ZIF-8) and zeolite imidazolate framework 67 (ZIF-67).
[0057] A second aspect of an embodiment of the present application provides a method for preparing a solid electrolyte, the preparation method comprising the following steps:
[0058] S10 obtains a solid electrolyte precursor; wherein the solid electrolyte precursor includes a solid electrolyte and a zeolite imidazolate framework, and the chemical formula of the solid electrolyte is Li 7-x LqCy 2-x Ta x O 12 , 0≤x≤1, calculated by mass percentage, the solid electrolyte: zeolite imidazolate framework = 100: (0.01-6).
[0059] S20: sintering the solid electrolyte precursor at high temperature to obtain a solid electrolyte.
[0060] In the present application, by adding a certain amount of zeolite imidazolate skeleton into the solid electrolyte, a solid electrolyte with low densification temperature, high ion conductivity and high mechanical strength can be prepared from the composite material in the present application.
[0061] Exemplarily, calculated by mass percentage, the zeolite imidazolate framework: solid electrolyte is approximately 0.01%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6% and any value between the foregoing two points.
[0062] Exemplarily, x is about 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, and any value between the two aforementioned point values. It should be noted that "about" in this application means a value that differs from the actual number by a margin of ±10%. Taking the actual number as 1 as an example, correspondingly, about 1 refers to any value between 0.9 and 1.1.
[0063] In some embodiments of the present application, calculated by mass percentage, solid electrolyte: zeolite imidazolate skeleton = 100: (1-5). Further, solid electrolyte: zeolite imidazolate skeleton = 100: (1-3), and further, solid electrolyte: zeolite imidazolate skeleton = 100: (1.5-2.5). In this embodiment, controlling the zeolite imidazolate skeleton within this range can further reduce the densification temperature and improve the ionic conductivity and mechanical strength of the solid electrolyte.
[0064] In some embodiments of the present application, X is greater than 0. That is, the solid electrolyte is LLZTO formed by adding Ta to LLZO. In this embodiment, Ta doping is beneficial to further improve the ionic conductivity of the solid electrolyte.
[0065] It should be noted that, compared with LLZO, although the lithium ion conductivity of LLZTO is greatly improved, its lithium ion conductivity is still not ideal, and LLZTO also has the problems of low density and high densification temperature. In this embodiment, by compounding the zeolite imidazolate framework with LLZTO, the density of LLZTO can be improved, and its densification temperature (referring to the heat treatment temperature when densification is completed) can be reduced, and the ionic conductivity and mechanical strength of the solid electrolyte can be improved.
[0066] In some embodiments of the present application, 0.1≤x≤0.9. Further, 0.4≤x≤0.8. Still further, 0.5≤x≤0.7. In this embodiment, by controlling the content of Ta element doping, it is beneficial to further improve the ionic conductivity and mechanical strength of the solid electrolyte.
[0067] In some embodiments of the present application, the sintering temperature is 900° C. to 1300° C. For example, the sintering temperature is about 900° C., 950° C., 1000° C., 1050° C., 1100° C., 1150° C., 1200° C., 1250° C., 1300° C. and any value between the foregoing two values.
[0068] Furthermore, the sintering temperature is 1000° C. to 1100° C. Within this sintering temperature range, the electrolyte in the present application can be densified, which is beneficial to reducing costs.
[0069] In some embodiments of the present application, the high temperature sintering includes high temperature sintering in an inert atmosphere. For example, the inert atmosphere includes argon. Of course, in other embodiments of the present application, the inert atmosphere may also include other inert gases, which are not limited here.
[0070] In some embodiments of the present application, the heating rate during the high temperature sintering process is 5°C / min to 20°C / min. For example, the heating rate is about 5°C / min, 10°C / min, 15°C / min, 20°C / min, and any value between the above two values.
[0071] In some embodiments of the present application, the step of obtaining a solid electrolyte precursor includes: mixing a solid electrolyte and a zeolite imidazolate framework according to a preset ratio to obtain a first mixture; and applying a certain pressure to the first mixture to obtain a solid electrolyte precursor.
[0072] It should be noted that the solid electrolyte and zeolite imidazolate framework in the embodiments of the present application can be prepared by oneself or obtained from the market, which is not limited here.
[0073] In some embodiments of the present application, the zeolite imidazolate framework includes at least one of the zeolite imidazolate framework 8 and the zeolite imidazolate framework 67 .
[0074] Exemplarily, the process of preparing ZIF-8 includes: dissolving 1.835g of zinc nitrate hexahydrate in 125ml of methanol under stirring (e.g., mechanical stirring or magnetic stirring) at room temperature, stirring and dissolving to form solution A. Then 4.058g of dimethylimidazole is dissolved in 125ml of methanol, stirring and dissolving to form solution B. Then solution A is slowly added to solution B, the solution becomes a milky white liquid, the beaker is sealed with a sealing film and stirred for 20h, and then centrifuged (7000rpm, 10min) to obtain a solid substance. The solid substance obtained by centrifugation is washed three times with methanol, then placed in a vacuum drying oven and dried for 12h, and finally the dried solid (ZIF-8) is ground for standby use.
[0075] Exemplarily, the solid electrolyte preparation includes (with Li 6.4 Ln3Z 1.4 Ta 0.6 O 12For example): LiOH·H2O, La2O3, ZrO2 and Ta2O5 are weighed according to the stoichiometric ratio of 7.0:1.5:1.4:0.6 (the lithium source content needs to be added in 10% excess compared to the theoretical content). After fully mixing the configured raw materials, place them in a ball mill, add an appropriate amount of isopropanol, and ball mill them at a speed of 300rpm for 12 hours to obtain the first mixture after ball milling. After drying the first mixture after ball milling, a dry second mixture is obtained, and the second mixture is placed in a tubular furnace for high-temperature sintering. The high-temperature sintering conditions are 900℃ for 12 hours and a heating rate of 10℃ / min. After the reaction is completed, the sample is placed in a tubular furnace and cooled naturally to take out the product. The product is placed in a zirconia ball mill, and an appropriate amount of ethanol is added and ball milled at a speed of 300rpm for 12 hours for powder refinement. After the powder is dried, it is screened to obtain LLZTO (Li 6.4 LqCy 1.4 Ta 0.6 O 12 )powder.
[0076] Exemplarily, the preparation of the solid electrolyte includes: mixing the prepared solid electrolyte powder and the zeolite imidazolate skeleton in a preset ratio to obtain a composite material, and then placing the composite material into a mold for uniaxial tableting to obtain a solid electrolyte precursor (i.e., a solid electrolyte ceramic sheet). The obtained solid electrolyte precursor is sintered at high temperature under argon, and heat treated in an argon environment at 1100°C for 12 hours at a heating rate of 10°C / min; after the heat treatment, the sample is placed in a tube furnace for natural cooling to obtain a test sample (i.e., a solid electrolyte).
[0077] In some embodiments of the present application, the density of the solid electrolyte is 94% to 99%; the ionic conductivity of the solid electrolyte is 0.7 mS / cm to 1.3 mS / cm; the elastic modulus of the solid electrolyte is 84 GPa to 175 GPa; and the Vickers hardness of the solid electrolyte is 7 GPa to 13 GPa.
[0078] The fourth aspect of the embodiment of the present application provides a lithium metal battery, wherein the lithium metal battery comprises the solid electrolyte. It is understandable that since the lithium metal battery in the present application comprises the solid electrolyte, it also has the beneficial effects of the solid electrolyte and has a good cycle life.
[0079] Specifically, the lithium metal battery includes a positive electrode, a negative electrode and a solid electrolyte, wherein the solid electrolyte is disposed between the positive electrode and the negative electrode. Exemplarily, the negative electrode includes lithium metal or a lithium alloy.
[0080] The electrolyte and lithium ion electrons in the present application are further described below in conjunction with specific embodiments.
[0081] Electrolyte Example 1
[0082] Preparation of ZIF-8: Using mechanical stirring at room temperature, 1.835g zinc nitrate hexahydrate was dissolved in 125ml methanol to prepare solution A, and 4.058g dimethylimidazole was dissolved in 125ml methanol to prepare solution B. Solution A was slowly added to solution B, and the solution became a milky white liquid. The beaker was sealed with a sealing film and stirred for 20 hours, then centrifuged (7000rpm, 10min) and washed three times with methanol, placed in a vacuum drying oven to dry for 12 hours, and finally the dried ZIF-8 solid was ground for use. The particle size of ZIF-8 is about 200nm. Its diffraction spectrum is as follows Figure 3 As shown. Figure 3 It can be seen that the characteristic peaks on the diffraction pattern of the prepared product match the characteristic peaks of the standard ZIF-8 spectrum, indicating that ZIF-8 was successfully prepared.
[0083] Solid electrolyte (LLZTO) preparation: LiOH·H2O, La2O3, ZrO2 and Ta2O5 were weighed according to the stoichiometric ratio of 7.0:1.5:1.4:0.6 to prepare Li 6.4 Ln3Z 1.4 Ta 0.6 O 12 , where the lithium source content needs to be added in excess of 10% compared to the theoretical content. After fully mixing the configured raw materials, place them in a ball mill, add an appropriate amount of isopropanol, and ball mill at 300rpm for 12 hours. After drying, place the mixed sample raw materials in a tubular furnace for high-temperature sintering. The high-temperature sintering conditions are 900℃ for 12 hours, and the heating rate is 10℃ / min. After the reaction is completed, place the sample in a tubular furnace and cool it naturally to take out the product. Place the product in a zirconia ball mill, add an appropriate amount of ethanol and ball mill at 300rpm for 12 hours for powder refinement. After the powder is dried, it is screened to obtain LLZTO (Li 6.4 Ln3Z 1.4 Ta 0.6 O 12 )powder.
[0084] Preparation of solid electrolyte: The prepared LLZTO powder was mixed with ZIF-8 in a mass ratio of 100:2, and placed in a mold for uniaxial tableting. The obtained solid electrolyte ceramic sheet was sintered at high temperature under argon and heat treated in an argon environment at 1100°C for 12 hours with a heating rate of 10°C / min. After the heat treatment, the sample was placed in a tubular furnace for natural cooling to obtain a test sample.
[0085] Electrolyte Example 2
[0086] The difference between this embodiment and embodiment 1 is that during the preparation of the solid electrolyte, the heat treatment temperature is 1050°C.
[0087] Electrolyte Example 3
[0088] The difference between this embodiment and embodiment 1 is that during the preparation of the solid electrolyte, the heat treatment temperature is 1150°C.
[0089] Electrolyte Example 4
[0090] The difference between this embodiment and Example 1 is that during the preparation of the solid electrolyte, the heat treatment temperature is 1200°C.
[0091] Electrolyte Example 5
[0092] The difference between this embodiment and embodiment 1 is that during the preparation of the solid electrolyte, the heat treatment temperature is 1250°C.
[0093] Electrolyte Example 6
[0094] The difference between this embodiment and Example 1 is that during the preparation of the solid electrolyte, the heat treatment temperature is 1300°C.
[0095] Electrolyte Example 7
[0096] The difference from Example 1 is that LLZTO powder and ZIF-8 are mixed in a mass ratio of 100:1.
[0097] Electrolyte Example 8
[0098] The difference from Example 1 is that LLZTO powder and ZIF-8 are mixed in a mass ratio of 100:3.
[0099] Electrolyte Example 9
[0100] The difference from Example 1 is that LLZTO powder and ZIF-8 are mixed in a mass ratio of 100:4.
[0101] Electrolyte Example 10
[0102] The difference from Example 1 is that LLZTO powder and ZIF-8 are mixed in a mass ratio of 100:5.
[0103] Electrolyte Example 11
[0104] The difference between this embodiment and Example 1 is that the prepared solid electrolyte is Li 6.8 Ln3Z 1.8 Ta 0.2 O 12 .
[0105] Electrolyte Example 12
[0106] The difference between this embodiment and Example 1 is that the prepared solid electrolyte is Li 6.6 LqCy 1.6 Ta 0.4 O 12 .
[0107] Electrolyte Example 13
[0108] The difference between this embodiment and Example 1 is that the prepared solid electrolyte is Li 6.2 LqCy 1.2 Ta 0.8 O 12 .
[0109] Electrolyte Example 14
[0110] The difference between this embodiment and Example 1 is that the prepared solid electrolyte is Li6La3ZrTaO 12 .
[0111] Electrolyte Example 15
[0112] The difference between this embodiment and Example 1 is that the prepared solid electrolyte is LLZO (Li7La3Zr2O 12 ).
[0113] Electrolyte Example 16
[0114] The difference from Example 1 is that LLZTO powder and ZIF-67 are mixed in a mass ratio of 100:2.
[0115] Electrolyte Comparative Example 1
[0116] Solid electrolyte (LLZTO) preparation: LiOH·H2O, La2O3, ZrO2 and Ta2O5 were weighed according to the stoichiometric ratio of 7.0:1.5:1.4:0.6 to prepare Li 6.4 LqCy 1.4 Ta 0.6 O 12, where the lithium source content needs to be added in excess of 10% compared to the theoretical content. After fully mixing the configured raw materials, place them in a ball mill, add an appropriate amount of isopropanol, and ball mill at 300rpm for 12 hours. After drying, place the mixed sample raw materials in a tubular furnace for high-temperature sintering. The high-temperature sintering conditions are 900℃ for 12 hours, and the heating rate is 10℃ / min. After the reaction is completed, place the sample in a tubular furnace and cool it naturally to take out the product. Place the product in a zirconia ball mill, add an appropriate amount of ethanol and ball mill at 300rpm for 12 hours for powder refinement. After the powder is dried, it is screened to obtain LLZTO (Li 6.4 LqCy 1.4 Ta 0.6 O 12 )powder.
[0117] Preparation of solid electrolyte: The prepared LLZTO powder is placed in a mold for uniaxial tableting. The obtained solid electrolyte ceramic sheet is sintered at high temperature under argon and heat treated in an argon environment at 1100°C for 12 hours with a heating rate of 10°C / min. After the heat treatment, the sample is placed in a tubular furnace for natural cooling to obtain a test sample.
[0118] The difference between this embodiment and Example 1 is that no ZIF-8 is added to the solid electrolyte.
[0119] Electrolyte Comparative Example 2
[0120] The difference between this embodiment and Example 2 is that ZIF-8 is not added to the solid electrolyte.
[0121] Electrolyte Comparative Example 3
[0122] The difference between this embodiment and Example 3 is that no ZIF-8 is added to the solid electrolyte.
[0123] Electrolyte Comparative Example 4
[0124] The difference between this embodiment and Example 4 is that no ZIF-8 is added to the solid electrolyte.
[0125] Electrolyte Comparative Example 5
[0126] The difference between this embodiment and Example 5 is that no ZIF-8 is added to the solid electrolyte.
[0127] Electrolyte Comparative Example 6
[0128] The difference between this embodiment and Example 6 is that no ZIF-8 is added to the solid electrolyte.
[0129] Electrolyte Comparative Example 7
[0130] The difference between this embodiment and Example 15 is that no ZIF-8 is added to the solid electrolyte.
[0131] Experimental testing
[0132] Density test:
[0133] Density = actual density / theoretical density. The theoretical density of LLZTO is 5.5g / cm 3 The actual density is measured by Archimedes displacement method. The buoyancy of an object immersed in a liquid can be calculated by the difference between its actual weight m1 and its apparent weight m2 ("apparent weight" refers to the gravity measured when the object is immersed in a liquid). The volume of the object is calculated by Archimedes principle, V = (m1-m2) / (ρg), and the density of the object is: ρobject = m1*ρliquid / (m1-m2).
[0134] Ionic conductivity test:
[0135] The sintered solid electrolyte ceramic sheet was polished and cleaned, then soaked in glacial acetic acid for 30 seconds to remove impurities such as Li2CO3 and LiOH on the surface, and then placed in a glove box for standby use. A layer of Ag was evaporated on both sides of the solid electrolyte sheet using a thermal evaporation coating instrument to form an Ag / LLZTO / Ag blocking system, using lithium sheets as electrodes and button batteries for packaging.
[0136] An electrochemical workstation was used to apply a small-amplitude sine wave to the button battery, with an AC amplitude of 0.01V and a test temperature of room temperature. The frequency of the applied small-amplitude sine wave was changed within the test frequency range of 1Hz to 1MHz to obtain a series of impedances at different frequencies. The real part of the impedance was used as the horizontal axis, the imaginary part was used as the vertical axis, and each point represented a different frequency to obtain the Nyquist diagram. The left side of the diagram has a high frequency, which is called the high-frequency zone, and the high-frequency zone is semicircular; the right side has a low frequency, which is called the low-frequency zone, and the low-frequency zone is linear. According to the equivalent circuit analysis, the intersection of the semicircle with the real axis at low frequency corresponds to the ionic resistance R of the solid electrolyte ceramic sheet. The conductivity is calculated according to the following formula.
[0137] σ=1 / ρ=L / (A×R)
[0138] Wherein, σ represents the conductivity, the unit is S / m; L represents the length of the solid electrolyte ceramic sheet, the unit is m; A represents the cross-sectional area of the solid electrolyte ceramic sheet, the unit is m 2 ; R represents the ionic resistance of the solid electrolyte ceramic sheet.
[0139] Mechanical properties test:
[0140] See also Figure 1 and Figure 2Nanoindentation technology is a commonly used method for testing the mechanical properties of materials. Since this technology is based on high-precision displacement testing, it is sometimes referred to as depth-sensitive indentation technology (DSI) in the literature; and since this technology requires the use of high-precision displacement and load testing devices, it is sometimes referred to as instrumented indentation technology (IIT) in the literature. It controls the indenter to press into the material to be tested through a computer, records the continuous change of the load in real time, and monitors the indentation depth online to obtain the load-depth curve. By studying the change law of the indenter load with the indentation depth, the ability of the material's microstructure to resist external force deformation can be understood, and the corresponding mechanical performance parameters can be calculated. The entire indentation process includes two stages: loading and unloading. During the loading process, the load P exerted by the indenter on the material will increase with the increase of the indentation depth h. After unloading, the indenter returns to the initial position, and there will be residual indentation marks on the surface of the sample. This is caused by the plastic deformation of the sample.
[0141] The most commonly used method for nanoindentation measurement is Oliver-Pharr (O&P). Based on the load-depth curve measured experimentally, the elastic modulus can be calculated based on the load-depth curve, and the hardness (E) can be calculated from the maximum load (P max ) and the residual deformation area of the indentation.
[0142] In the parameter diagram of the nanoindentation process, h c Indicates the contact depth of the indenter when it is pressed into the sample, A c Indicates the radius of contact between the tested sample and the indenter, h s It indicates the displacement of the sample surface when the indenter is pressed into the sample. By recording the load (P) during the nanoindentation process, as the depth (h) of the indenter pressing into the substrate changes, the load-depth curve is obtained (see the following figure). Figure 2 ), where P max is the maximum load, h max is the maximum displacement, h f is the residual displacement after complete unloading, and S is the elastic contact stiffness.
[0143] Load-Depth Curve
[0144] Cycle life test:
[0145] The prepared solid electrolyte was polished to make its surface flat, and the surface was treated with glacial acetic acid to remove impurities such as Li2CO3. Nanosilver (thickness 300nm) was evaporated on both sides of the positive and negative electrodes of LLZTO, and the evaporation conditions were 50A and 50s. The evaporated LLZTO and lithium foil (20um) were placed in an atmosphere furnace (Ar) for hot pressing at a temperature of 200°C and a pressure of 10MPa for 10 minutes to ensure that the lithium foil and LLZTO fit tightly. LLZTO with double-sided silver plating and lithium foil is used in lithium symmetric batteries to test the cycle life of lithium.
[0146] Table 1
[0147]
[0148]
[0149] The prepared electrolyte was tested for density, ionic conductivity and mechanical properties, and the test results are shown in Table 1. It can be seen from Examples 1 to 16 that the density of the electrolyte in the present application can reach up to 98.7%, and the densification temperature is about 1100°C. In combination with Comparative Examples 1 to 7, it can be seen that the electrolyte without the addition of the zeolite imidazolate skeleton has a density of up to 95.9%, and the densification temperature is about 1200°C. It can be seen that adding a certain amount of zeolite imidazolate skeleton to LLZO or LLZTO can improve the density of the electrolyte and reduce the densification temperature. At the same time, in combination with the electrolyte embodiment and the corresponding electrolyte comparative example, it can be seen that adding a certain amount of zeolite imidazolate skeleton to LLZO or LLZTO can improve the ionic conductivity and mechanical strength of the electrolyte.
[0150] It can be seen from the electrolyte examples 1, 7 and 10 that when the mass ratio of the zeolite imidazolate framework to the solid electrolyte in the electrolyte is about 2% to 4%, it is beneficial to further improve the density, ionic conductivity and mechanical strength of the electrolyte.
[0151] Combined with Electrolyte Example 1, Example 11 to Example 15, Comparative Example 1 and Comparative Example 7, it can be seen that Ta element doping can significantly improve the ionic conductivity of LLZO, but the improvement of density and mechanical properties is not obvious. However, LLZTO still has the problem of poor mechanical properties and less than ideal ionic conductivity. When the Ta element is doped at about 0.2 to 0.8, and the mass ratio of the zeolite imidazolate skeleton to the solid electrolyte in the electrolyte is about 2% to 4%, the density, mechanical properties and ionic conductivity of LLZTO can be further improved.
[0152] Preparation of Application Examples and Comparative Examples
[0153] The prepared lithium metal battery was subjected to a cycle life test, and the test results are as follows: Figures 4 to 5 And as shown in Table 2.
[0154] Table 2
[0155]
[0156]
[0157] Depend on Figure 4 , Figure 5 As can be seen from Table 2, adding a certain amount of ZIF-8 to the electrolyte is beneficial to improving the cycle life of lithium metal batteries. The possible reason is that adding a certain amount of zeolite imidazolate framework to the electrolyte improves the density and mechanical strength of the electrolyte, thereby enhancing the ability to block lithium dendrites, thereby improving the cycle life of lithium metal batteries.
[0158] The technical solutions provided by the embodiments of the present application are introduced in detail above. Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea. At the same time, for technical personnel in this field, according to the idea of the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.
Claims
1. A composite material for preparing a solid electrolyte, comprising a garnet-type solid electrolyte and a zeolite imidazolate framework, wherein by mass, the solid electrolyte: zeolite imidazolate framework = 100: (0.01-6); in, The chemical formula of the solid electrolyte is Li 7-x Ln3Z 2-x Ta x O 12 , 0≤x≤1.
2. The composite material according to claim 1, characterized in that By mass, the solid electrolyte: zeolite imidazolate framework = 100: (1-5); and / or The zeolite imidazolate framework comprises at least one of the zeolite imidazolate framework 8 and the zeolite imidazolate framework 67; and / or The particle size of the zeolite imidazolate framework is 100 nm to 300 nm.
3. The composite material according to claim 2, characterized in that By mass, the solid electrolyte: zeolite imidazolate framework = 100: (2-4).
4. The composite material according to any one of claims 1 to 3, characterized in that 0.2≤x≤0.8。 5. A method for preparing a solid electrolyte, characterized in that: The preparation method comprises: Obtain a solid electrolyte precursor; wherein the solid electrolyte precursor comprises a solid electrolyte and a zeolite imidazolate framework, and the chemical formula of the solid electrolyte is Li 7-x Ln3Z 2-x Ta x O 12 , 0≤x≤1, calculated by mass, the solid electrolyte: zeolite imidazolate framework = 100: (0.01-6); The solid electrolyte is obtained by sintering the solid electrolyte precursor at high temperature.
6. The preparation method according to claim 5, characterized in that: The sintering temperature is 900°C to 1300°C; and / or Sintering includes high temperature sintering in an inert atmosphere; and / or The heating rate during sintering is 5°C / min to 20°C / min; and / or The zeolite imidazolate framework includes at least one of a zeolite imidazolate framework 8 and a zeolite imidazolate framework 67 .
7. The preparation method according to claim 5, characterized in that: The sintering temperature is 1000°C to 1100°C; and / or The step of obtaining a solid electrolyte precursor comprises: Mixing the solid electrolyte powder and the zeolite imidazolate framework according to a preset ratio to obtain a first mixture; Applying pressure to the first mixture obtains a solid electrolyte precursor.
8. A solid electrolyte, characterized in that The solid electrolyte comprises the composite material according to any one of claims 1 to 4, or is prepared by the preparation method according to any one of claims 5 to 7.
9. The solid electrolyte according to claim 8, characterized in that The density of the solid electrolyte is 94% to 99%; the ionic conductivity of the solid electrolyte is 0.7 mS / cm to 1.3 mS / cm; the elastic modulus of the solid electrolyte is 84 GPa to 175 GPa; and the hardness of the solid electrolyte is 7 GPa to 13 GPa.
10. A lithium metal battery, characterized in that: The lithium metal battery comprises a positive electrode, a negative electrode and the solid electrolyte according to claim 8 or 9, wherein the solid electrolyte is arranged between the positive electrode and the negative electrode.
Citation Information
Patent Citations
Organic-inorganic composite solid electrolyte membrane and preparation method and application thereof
CN113991174A
Polymer / inorganic composite solid electrolyte membrane and preparation method and application thereof
CN116487681A
Preparation method of solid electrolyte containing oxygen vacancies and solid-state battery
CN117976969A
Co-doped asymmetric composite solid electrolyte, battery and preparation method of co-doped asymmetric composite solid electrolyte
CN118213612A
Composite inorganic solid electrolyte based on ceramic particles and zeolite particles and preparation method thereof
CN118367207A