Multiphase ceramic material with high infrared transmittance and preparation method thereof

By adding LiF to Gd2O3-MgO nanocomplex phase powder, the sintering temperature is reduced and MgO water absorption is reduced, and the problem of infrared transmittance reduction caused by the monoclinic phase of Gd2O3 and MgO moisture absorption is solved, and the complexity of high infrared transmittance is achieved Preparation of phase ceramic materials.

CN119019154APending Publication Date: 2024-11-26HANGZHOU HENGYING TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411160927.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the existing Gd2O3-MgO infrared complex phase ceramics, the phase of Gd2O3 is a monoclinic phase, resulting in a decrease in infrared transmittance, and MgO is prone to moisture absorption and reduces infrared transmittance.

Method used

LiF is added to the Gd2O3-MgO nanocomplex powder. LiF is used as a sintering aid to reduce the sintering temperature, avoid the Gd2O3 phase change, and serve as a cladding layer to reduce the MgO water absorption, forming a LiF-coated Gd2O3-MgO nanocomplex powder. Complex ceramic materials with high infrared transmittance are obtained by molding, sintering and processing.

Benefits of technology

Maintain Gd2O3 as a cubic phase, improve infrared transmittance, reduce hydroxyl absorption, and increase infrared transmittance of composite ceramic materials by more than 80%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019154A_ABST
    Figure CN119019154A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of ceramic materials, in particular to a multiphase ceramic material with high infrared transmittance and a preparation method of the multiphase ceramic material. The preparation method comprises the following steps: preparing Gd2O3-MgO nano composite phase powder; mixing the Gd2O3-MgO nano-composite powder, a LiNO3 solution and a NH4F solution, then stirring, then standing for layering, and removing supernatant liquid to obtain a precipitate; calcining the precipitate for 3 to 5 hours at the temperature of 300 to 500 DEG C under the protection of an inert atmosphere, so as to obtain LiF-coated Gd2O3-MgO nano complex phase powder; the LiF-coated Gd2O3-MgO nano composite phase powder is subjected to forming, sintering and processing in sequence, and the composite phase ceramic material is obtained. According to the invention, LiF is added into the Gd2O3-MgO nano complex-phase powder, the LiF is used as a sintering aid, and the sintering temperature of the complex-phase ceramic material is reduced to be lower than 1250 DEG C, so that the change of the crystal form of Gd2O3 is avoided, and the infrared transmittance of the material is improved. Meanwhile, LiF with stable chemical properties is used as a coating layer, so that the problem that MgO is extremely easy to absorb water after being in contact with air is avoided, the reduction of absorption of hydroxyl in the composite ceramic material is facilitated, and the infrared transmittance of the composite ceramic material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ceramic materials, and in particular to a multiphase ceramic material with high infrared transmittance and a preparation method thereof. Background Art

[0002] Infrared transparent materials refer to materials that can transmit infrared radiation and are mainly used to manufacture windows for infrared detectors, lenses and prisms for infrared instruments, etc. Infrared transparent window materials used in aircraft are required to protect the optical system from the influence of atmosphere, moisture, and dust, and participate in system imaging and correction of phase difference, which requires infrared transparent materials to have high transmittance, mechanical strength, hardness and thermal shock resistance.

[0003] Gd2O3-MgO infrared composite ceramics have the advantages of longer cut-off wavelength, low high-temperature infrared radiation coefficient, and excellent high-temperature mechanical properties. They are a promising infrared window material. However, the phase of Gd2O3 in the currently prepared Gd2O3-MgO infrared composite ceramics is monoclinic, and the powder is cubic before sintering. Due to the higher density of the monoclinic phase, a phase change occurs during the sintering process, and the volume of Gd2O3 will shrink by about 10%. In addition, the monoclinic phase Gd2O3 is optically anisotropic, which will reduce the infrared transmittance of the material. Since MgO is very easy to absorb moisture, the Gd2O3-MgO nanocomposite powder used to prepare Gd2O3-MgO infrared composite ceramics is extremely fine, and a large amount of water vapor is adsorbed in the powder, and hydroxides are formed on the surface of the powder particles. The presence of a large number of hydroxyl groups is bound to increase the infrared absorption at 3μm and reduce the infrared transmittance of the material.

[0004] Therefore, the prior art still needs to be improved and developed. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a composite ceramic material with high infrared transmittance and a preparation method thereof, aiming to solve the problem that the phases of Gd2O3 in the existing Gd2O3-MgO infrared composite ceramics are all monoclinic phases, which leads to a decrease in its infrared transmittance; and the problem that MgO is extremely easy to absorb moisture, which leads to a decrease in the infrared transmittance of the infrared composite ceramics.

[0006] The technical solution of the present invention is as follows:

[0007] A first aspect of the present invention provides a method for preparing a multiphase ceramic material with high infrared transmittance, comprising:

[0008] Step A, preparing Gd2O3-MgO nanocomposite powder;

[0009] Step B, mixing the Gd2O3-MgO nanocomposite powder, LiNO3 solution and NH4F solution, stirring, standing for stratification, removing the supernatant, and obtaining a precipitate;

[0010] Step C, calcining the precipitate at 300-500° C. for 3-5 hours under an inert atmosphere to obtain a LiF-coated Gd2O3-MgO nanocomposite powder;

[0011] Step D: molding, sintering and processing the LiF-coated Gd2O3-MgO nanocomposite powder in sequence to obtain the composite ceramic material.

[0012] Optionally, the step B specifically includes:

[0013] Adding the Gd2O3-MgO nanocomposite powder to a LiNO3 solution to obtain a Gd2O3-MgO nanocomposite powder suspension, and adding an NH4F solution to the Gd2O3-MgO nanocomposite powder suspension;

[0014] The mixture is then stirred at a temperature of 60 to 100° C. for 1 to 2 hours, and then allowed to stand for stratification, and the supernatant is removed to obtain a precipitate.

[0015] Optionally, the NH4F solution is added dropwise to the Gd2O3-MgO nanocomposite powder suspension at a titration rate of 0.3 to 1 mL / min.

[0016] Optionally, the LiNO3 solution is prepared by dissolving LiNO3 in anhydrous ethanol;

[0017] The NH4F solution is prepared by dissolving NH4F in anhydrous ethanol.

[0018] Optionally, in the step C, the mass percentage of LiF in the LiF-coated Gd2O3-MgO nanocomposite powder is 0.35% to 3.5%.

[0019] Optionally, the step C specifically includes:

[0020] The precipitate is washed, filtered and dried in sequence, and the dried precipitate is calcined at 300-500° C. for 3-5 hours under the protection of an inert atmosphere to obtain a LiF-coated Gd2O3-MgO nanocomposite powder.

[0021] Optionally, the step A specifically includes:

[0022] dissolving gadolinium salt and magnesium salt in water to obtain a mixed solution;

[0023] Adding an organic additive to the mixed solution, stirring and heating, and placing the solution in an oven at 180-220° C. for 1-6 hours after the solution becomes thick, to obtain a dry gel;

[0024] The dry gel is kept at 700-900° C. for 2-5 hours in an oxygen-containing atmosphere to obtain Gd2O3-MgO nanocomposite powder.

[0025] Optionally, the step D specifically includes:

[0026] The LiF-coated Gd2O3-MgO nanocomposite powder is successively ball-milled, dried and sieved, and then heated at 500-700° C. for 2-6 hours to obtain a high-activity powder;

[0027] The high-activity powder is subjected to dry pressing and cold isostatic pressing to obtain a ceramic green body;

[0028] The ceramic green body is subjected to air pre-sintering and hot isostatic pressing to obtain a sintered body;

[0029] The sintered body is annealed and processed to obtain the composite ceramic material.

[0030] Optionally, the air pre-sintering temperature is 1200-1240°C, and the hot isostatic pressing sintering temperature is 1200-1240°C.

[0031] A second aspect of the present invention provides a multiphase ceramic material with high infrared transmittance, wherein the multiphase ceramic material is prepared by the method for preparing a multiphase ceramic material with high infrared transmittance described in the present invention.

[0032] Beneficial effects: The present invention adds LiF to the Gd2O3-MgO nanocomposite powder. LiF can be used as a sintering aid to reduce the densification temperature (i.e., sintering temperature) of the composite ceramic material to 1250°C, which is lower than the phase transition temperature of Gd2O3, thereby avoiding the change of the Gd2O3 crystal form, maintaining Gd2O3 in a cubic phase, and improving the infrared transmittance of the composite ceramic material. LiF, which is chemically stable, can also be used as a coating layer to avoid the problem that MgO easily absorbs water after contacting the air, thereby helping to reduce the absorption of hydroxyl groups in the final composite ceramic material (hydroxyl absorption will cause the infrared transmittance in the 2.7-3μm band to decrease), thereby improving the infrared transmittance of the composite ceramic material. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is the XRD pattern of the LiF-coated Gd2O3-MgO nanocomposite powder prepared in Example 1.

[0034] Figure 2 This is the XRD diagram of the Gd2O3-MgO composite ceramic material prepared in Example 1.

[0035] Figure 3 This is the infrared transmittance diagram of the Gd2O3-MgO composite ceramic material prepared in Example 1.

[0036] Figure 4 This is a scanning electron microscope image of the Gd2O3-MgO composite ceramic material prepared in Example 1.

[0037] Figure 5 This is the XRD pattern of the LiF-coated Gd2O3-MgO nanocomposite powder prepared in Example 2.

[0038] Figure 6 This is the XRD diagram of the Gd2O3-MgO composite ceramic material prepared in Example 2.

[0039] Figure 7 This is the infrared transmittance diagram of the Gd2O3-MgO composite ceramic material prepared in Example 2.

[0040] Figure 8 This is a scanning electron microscope image of the Gd2O3-MgO composite ceramic material prepared in Example 2. DETAILED DESCRIPTION

[0041] The present invention provides a composite ceramic material with high infrared transmittance and a preparation method thereof. To make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0042] The phase of Gd2O3 in the currently prepared Gd2O3-MgO infrared composite ceramics is monoclinic, and the powder is cubic before sintering. Due to the higher density of the monoclinic phase, a phase change occurs during the sintering process, and the volume of Gd2O3 will be reduced by about 10%. In addition, the monoclinic phase Gd2O3 is optically anisotropic, which reduces the infrared transmittance of the material. Therefore, in order to make the phase of Gd2O3 in the prepared Gd2O3-MgO infrared composite ceramics cubic, the phase transition temperature of Gd2O3 is 1250℃, and the sintering temperature of the composite ceramic material can be reduced to avoid the change of the Gd2O3 crystal form.

[0043] Based on this, an embodiment of the present invention provides a method for preparing a multiphase ceramic material with high infrared transmittance, which comprises:

[0044] Step A, preparing Gd2O3-MgO nanocomposite powder;

[0045] Step B, mixing the Gd2O3-MgO nanocomposite powder, LiNO3 solution and NH4F solution, stirring, standing for stratification, removing the supernatant, and obtaining a precipitate;

[0046] Step C, calcining the precipitate at 300-500° C. for 3-5 hours under an inert atmosphere to obtain a LiF-coated Gd2O3-MgO nanocomposite powder;

[0047] Step D: molding, sintering and processing the LiF-coated Gd2O3-MgO nanocomposite powder in sequence to obtain the composite ceramic material.

[0048] The main reason for affecting the density of composite ceramic materials is that the densification temperature (i.e., sintering temperature) of MgO is too high. Above 1400°C, after adding LiF to the Gd2O3-MgO nanocomposite powder, LiF can be used as a sintering aid to promote sintering densification, reduce the sintering temperature of the composite ceramic material to below 1250°C, avoid the change of the Gd2O3 crystal form, maintain Gd2O3 in a cubic phase, and improve the infrared transmittance of the composite ceramic material. LiF, which has stable chemical properties, can also be used as a coating layer to avoid the problem of MgO easily absorbing water after contacting with air, thereby helping to reduce the absorption of hydroxyl groups in the final composite ceramic material (hydroxyl absorption will cause a decrease in infrared transmittance in the 2.7-3μm band), and improve the infrared transmittance of the composite ceramic material.

[0049] The composite ceramic material prepared by the preparation method contains cubic gadolinium oxide and cubic magnesium oxide without other impurities. The infrared transmittance of the composite ceramic material exceeds 80%. The grain size distribution in the composite ceramic material is uniform, and the grain size is less than 200nm.

[0050] In one embodiment, the step A specifically comprises:

[0051] dissolving gadolinium salt and magnesium salt in water to obtain a mixed solution;

[0052] Adding an organic additive (such as citric acid monohydrate and ethylene glycol) to the mixed solution, stirring and heating, and placing the solution in an oven at 180-220° C. for 1-6 hours after the solution becomes thick, to obtain a dry gel;

[0053] The dry gel is kept at 700-900° C. for 2-5 hours in an oxygen-containing atmosphere to obtain Gd2O3-MgO nanocomposite powder.

[0054] In a specific embodiment, the step A specifically comprises:

[0055] dissolving gadolinium nitrate hexahydrate and magnesium nitrate hexahydrate in water to obtain a nitrate mixed solution;

[0056] Adding citric acid monohydrate and ethylene glycol to the nitrate mixed solution, stirring and heating, the stirring rate is 160-180r / min, the heating temperature is 60-75°C, and after the solution becomes thick, it is placed in an oven at 180-200°C and kept warm for 5-6 hours to obtain a dry gel;

[0057] The dry gel is placed in a muffle furnace preheated to 200-220°C, oxygen is introduced, and the temperature is raised to 800-900°C at a heating rate of 1-1.5°C / min, and kept warm for 4-5 hours, and then cooled naturally to obtain Gd2O3-MgO nanocomposite powder.

[0058] In one embodiment, the step B specifically comprises:

[0059] Adding the Gd2O3-MgO nanocomposite powder to a LiNO3 solution to obtain a Gd2O3-MgO nanocomposite powder suspension, and adding an NH4F solution to the Gd2O3-MgO nanocomposite powder suspension;

[0060] The mixture is then stirred at a temperature of 60 to 100° C. for 1 to 2 hours, and then allowed to stand for stratification, and the supernatant is removed to obtain a precipitate.

[0061] Furthermore, the NH4F solution is slowly added to the Gd2O3-MgO nanocomposite powder suspension in a dropwise manner, and the titration rate is 0.3-1 mL / min, such as 0.3 mL / min, 0.5 mL / min, 0.8 mL / min, 1 mL / min, etc.

[0062] Furthermore, the LiNO3 solution is prepared by dissolving LiNO3 in anhydrous ethanol.

[0063] Furthermore, the NH4F solution is prepared by dissolving NH4F in anhydrous ethanol.

[0064] In one embodiment, the step C specifically comprises:

[0065] The precipitate is washed (repeatedly washed with anhydrous ethanol), filtered and dried in sequence, and the dried precipitate is calcined at 300-500° C. for 3-5 hours under an inert atmosphere (such as nitrogen) to obtain LiF-coated Gd2O3-MgO nanocomposite powder.

[0066] In one embodiment, in step C, the mass percentage of LiF in the LiF-coated Gd2O3-MgO nanocomposite powder is 0.35% to 3.5%. Within this range, it can be effectively ensured that LiF plays the role of sintering aid and coating layer, and will not affect the performance of the composite ceramic material.

[0067] Preferably, the mass percentage of LiF in the LiF-coated Gd2O3-MgO nanocomposite powder is 0.7% to 3.5%. Increasing the amount of LiF coating is conducive to further reducing the water absorption of the composite ceramic material and weakening the absorption of hydroxyl groups, thereby further improving the infrared transmittance of the composite ceramic material.

[0068] In one embodiment, the step D specifically comprises:

[0069] The LiF-coated Gd2O3-MgO nanocomposite powder is ball-milled for 36-48 hours, dried and sieved, and then heated at 500-700° C. for 2-6 hours to obtain a high-activity powder;

[0070] The high-activity powder is subjected to dry pressing and cold isostatic pressing (the pressure may be 200-220 MPa) to obtain a ceramic green body;

[0071] The ceramic green body is subjected to air pre-sintering (preferably, keeping the temperature at 1200-1240° C. for 2-3 hours in an air atmosphere) and hot isostatic pressing sintering (preferably, pressurizing to 200 MPa and keeping the temperature at 1200-1240° C. for 1.5-3 hours) to obtain a sintered body;

[0072] The sintered body is annealed (preferably annealed at 900-1050° C. for 20-24 hours) and processed to obtain the composite ceramic material.

[0073] An embodiment of the present invention provides a multiphase ceramic material with high infrared transmittance, wherein the multiphase ceramic material is prepared by the method for preparing the multiphase ceramic material with high infrared transmittance described in the embodiment of the present invention.

[0074] The composite ceramic material prepared by the preparation method contains cubic gadolinium oxide and cubic magnesium oxide without other impurities. The infrared transmittance of the composite ceramic material exceeds 80%. The grain size distribution in the composite ceramic material is uniform, and the grain size is less than 200nm.

[0075] The present invention is described in detail below through several specific embodiments.

[0076] Example 1

[0077] Take the preparation of 100g Gd2O3-MgO nanocomposite powder as an example. Weigh 135.4g of gadolinium nitrate hexahydrate with a purity of not less than 99% and 256.4g of magnesium nitrate hexahydrate into a quartz beaker, and add 200mL of deionized water to dissolve to form a nitrate mixed solution. Add citric acid monohydrate and ethylene glycol to the nitrate mixed solution in sequence, stir and heat on a magnetic stirrer, the stirring rate is 160r / min, the heating temperature is 60℃, and after the solution becomes thick, put it in a 200℃ oven for 5h to obtain a dry gel. Put the obtained dry gel into a muffle furnace preheated to 200℃, pass oxygen, and heat it to 800℃ at a heating rate of 1℃ / min, keep it warm for 4h, and then cool it naturally to obtain a Gd2O3-MgO nanocomposite powder.

[0078] Dissolve 0.07g of LiNO3 in anhydrous ethanol to obtain a LiNO3 solution. Take 20g of Gd2O3-MgO nanocomposite powder and add it to the LiNO3 solution to obtain a Gd2O3-MgO nanocomposite powder suspension. Dissolve 0.03g of NH4F in anhydrous ethanol, slowly add the obtained NH4F solution to the Gd2O3-MgO nanocomposite powder suspension at a titration rate of 0.3mL / min, and finally stir at 70°C for 2h, let it stand until the solution is stratified, remove the upper clear liquid, and then wash and filter it with anhydrous ethanol. Then place it in an oven at 100°C for 10h. The dried precipitate is calcined at 400°C for 5h under nitrogen protection to obtain LiF-coated Gd2O3-MgO nanocomposite powder.

[0079] The LiF-coated Gd2O3-MgO nanocomposite powder was ball-milled with anhydrous ethanol as the ball-milling medium. After ball-milling for 36 hours, it was put into an oven for drying and sieved with a 200-mesh screen. The obtained powder was placed in a muffle furnace and heated at 500℃ for 5 hours to obtain a high-activity powder. 3g of high-activity powder was weighed and poured into a mold and dry-pressed into a small disc by a hydraulic press, and then cold isostatic pressing at 210MPa was performed to obtain a ceramic blank. The ceramic blank was placed in a muffle furnace and kept at 1240℃ for 2 hours under air atmosphere. After cooling, a pre-sintered ceramic blank was obtained. The pre-sintered ceramic blank was placed in a hot isostatic pressing furnace and pressurized to 200MPa under argon atmosphere and kept at 1240℃ for 1.5 hours. After cooling, a sintered body was obtained. The sintered body was annealed at 900℃ for 20 hours. Finally, double-sided high-precision mirror polishing was performed to obtain an infrared transparent Gd2O3-MgO composite ceramic material.

[0080] Figure 1 This is the XRD pattern of the LiF-coated Gd2O3-MgO nanocomposite powder prepared in Example 1. Figure 2This is the XRD diagram of the Gd2O3-MgO composite ceramic material prepared in Example 1. It can be seen from the figure that the prepared Gd2O3-MgO composite ceramic material is cubic gadolinium oxide and cubic magnesium oxide, without other impurity phases. Figure 3 The infrared transmittance of the Gd2O3-MgO composite ceramic material prepared in Example 1 is more than 80% in the range of 3-6 μm, but there is still slight hydroxyl absorption; Figure 4 This is a scanning electron microscope image of the Gd2O3-MgO composite ceramic material prepared in Example 1. It can be seen from the image that the grain size distribution in the composite ceramic material is uniform, and the grain size is about 190nm.

[0081] Example 2

[0082] Take the preparation of 100g Gd2O3-MgO nanocomposite powder as an example. Weigh 135.4g of gadolinium nitrate hexahydrate with a purity of not less than 99% and 256.4g of magnesium nitrate hexahydrate into a quartz beaker, and add 200mL of deionized water to dissolve to form a nitrate mixed solution. Add citric acid monohydrate and ethylene glycol to the nitrate mixed solution in sequence, stir and heat on a magnetic stirrer, the stirring rate is 170r / min, the heating temperature is 70℃, and after the solution becomes thick, put it in an oven at 180℃ and keep it warm for 5.5h to obtain a dry gel. Put the obtained dry gel into a muffle furnace preheated to 210℃, pass oxygen, and heat it to 850℃ at a heating rate of 1.2℃ / min, keep it warm for 4.5h, and then cool it naturally to obtain a Gd2O3-MgO nanocomposite powder.

[0083] Dissolve 0.14g of LiNO3 in anhydrous ethanol to obtain a LiNO3 solution. Take 20g of Gd2O3-MgO nanocomposite powder and add it to the LiNO3 solution to obtain a Gd2O3-MgO nanocomposite powder suspension. Dissolve 0.06g of NH4F in anhydrous ethanol, slowly drop the obtained NH4F solution into the Gd2O3-MgO nanocomposite powder suspension at a titration rate of 0.5mL / min, and finally stir at 75°C for 2.5h, let it stand until the solution is stratified, pour off the upper clear liquid, and then wash and filter with anhydrous ethanol. Then place it in an oven at 110°C for drying for 10.5h. The dried precipitate is calcined at 450°C for 5.5h under nitrogen protection to obtain LiF-coated Gd2O3-MgO nanocomposite powder.

[0084] The LiF-coated Gd2O3-MgO nanocomposite powder was ball-milled with anhydrous ethanol as the ball-milling medium. After 48 hours of ball-milling, it was placed in an oven for drying and sieved with a 200-mesh screen. The obtained powder was placed in a muffle furnace and heated at 600°C for 5 hours to obtain a high-activity powder. 3g of the high-activity powder was weighed and poured into a mold and dry-pressed into a small disc using an oil press, and then subjected to 210MPa cold isostatic pressing to obtain a ceramic blank. The ceramic green body is placed in a muffle furnace and kept at 1220°C for 2.5 hours in an air atmosphere. After cooling, a pre-sintered ceramic body is obtained. The pre-sintered ceramic body is then placed in a hot isostatic pressing furnace and pressurized to 200 MPa in an argon atmosphere and kept at 1220°C for 2.5 hours. After cooling, a sintered body is obtained. The sintered body is annealed at 1000°C for 24 hours and finally double-sided high-precision mirror polishing is performed to obtain an infrared transparent Gd2O3-MgO composite ceramic material.

[0085] Figure 5 The XRD pattern of the LiF-coated Gd2O3-MgO nanocomposite powder prepared in Example 2; Figure 6 This is an XRD diagram of the Gd2O3-MgO composite ceramic material prepared in Example 2. It can be seen from the figure that the prepared Gd2O3-MgO composite ceramic material is cubic gadolinium oxide and cubic magnesium oxide, without other impurities; Figure 7 The infrared transmittance of the Gd2O3-MgO composite ceramic material prepared in Example 2 shows that the infrared transmittance of the composite ceramic material is still maintained at more than 80%, and the absorption of hydroxyl is significantly weakened. This is because the amount of LiF coating increases, making the composite ceramic material absorb less water, so the absorption of hydroxyl is significantly weakened; Figure 8 This is a scanning electron microscope image of the Gd2O3-MgO composite ceramic material prepared in Example 2, and the grain size is less than 200nm.

[0086] Example 3

[0087] Take the preparation of 100g Gd2O3-MgO nanocomposite powder as an example. Weigh 135.4g of gadolinium nitrate hexahydrate with a purity of not less than 99% and 256.4g of magnesium nitrate hexahydrate into a quartz beaker, and add 200mL of deionized water to dissolve to form a nitrate mixed solution. Add citric acid monohydrate and ethylene glycol to the nitrate mixed solution in sequence, stir and heat on a magnetic stirrer, the stirring rate is 180r / min, the heating temperature is 75℃, and after the solution becomes thick, put it in an oven at 180℃ and keep it warm for 6h to obtain a dry gel. Put the obtained dry gel into a muffle furnace preheated to 220℃, pass oxygen, and heat it to 900℃ at a heating rate of 1.5℃ / min, keep it warm for 5h, and then cool it naturally to obtain a Gd2O3-MgO nanocomposite powder.

[0088] Dissolve 0.7g of LiNO3 in anhydrous ethanol to obtain a LiNO3 solution. Take 20g of Gd2O3-MgO nanocomposite powder and add it to the LiNO3 solution to obtain a Gd2O3-MgO nanocomposite powder suspension. Dissolve 0.3g of NH4F in anhydrous ethanol, slowly add the obtained NH4F solution to the Gd2O3-MgO nanocomposite powder suspension at a titration rate of 1mL / min, and finally place it in an 80°C anhydrous ethanol solution and stir for 3.5h, let it stand until the solution is separated, remove the upper clear liquid, and then wash and filter it with anhydrous ethanol. Then place it in an oven at 120°C for 12h. The dried precipitate is calcined at 500°C for 6h under nitrogen protection to obtain LiF-coated Gd2O3-MgO nanocomposite powder.

[0089] The LiF-coated Gd2O3-MgO nanocomposite powder was ball-milled with anhydrous ethanol as the ball-milling medium. After 48 hours of ball-milling, it was placed in an oven for drying and sieved with a 200-mesh screen. The obtained powder was placed in a muffle furnace and heated at 600°C for 5 hours to obtain a high-activity powder. 3g of high-activity powder was weighed and poured into a mold and dry-pressed into a small disc by a hydraulic press, and then subjected to 210MPa cold isostatic pressing to obtain a ceramic blank. The ceramic blank was placed in a muffle furnace and kept at 1200°C for 3 hours under air atmosphere. After cooling, a pre-sintered ceramic blank was obtained. The pre-sintered ceramic blank was then placed in a hot isostatic pressing furnace and pressurized to 200MPa under argon atmosphere and kept at 1200°C for 3 hours. After cooling, a sintered body was obtained. The sintered body was annealed at 1050°C for 24 hours, and finally double-sided high-precision mirror polishing was performed to obtain an infrared transparent Gd2O3-MgO composite ceramic material.

[0090] In summary, the present invention provides a composite ceramic material with high infrared transmittance and a preparation method thereof, wherein LiF is added to the Gd2O3-MgO nanocomposite powder, and LiF is used as a sintering aid. LiF forms a liquid phase during the sintering process, and the densification temperature of the composite ceramic material is reduced to below 1250°C, thereby avoiding the change of the Gd2O3 crystal form, maintaining Gd2O3 in a cubic phase, and improving the infrared transmittance of the composite ceramic material. LiF, which is chemically stable, is also used as a coating layer to avoid the problem that MgO is very easy to absorb water after contacting with air, thereby helping to reduce the absorption of hydroxyl groups in the final composite ceramic material and improving the infrared transmittance of the composite ceramic material.

[0091] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.

Claims

1. A method for preparing a composite ceramic material with high infrared transmittance, characterized in that: include: Step A, preparing Gd2O3-MgO nanocomposite powder; Step B, mixing the Gd2O3-MgO nanocomposite powder, LiNO3 solution and NH4F solution, stirring, standing for stratification, removing the supernatant, and obtaining a precipitate; Step C, calcining the precipitate at 300-500° C. for 3-5 hours under an inert atmosphere to obtain a LiF-coated Gd2O3-MgO nanocomposite powder; Step D: molding, sintering and processing the LiF-coated Gd2O3-MgO nanocomposite powder in sequence to obtain the composite ceramic material.

2. The method for preparing a composite ceramic material with high infrared transmittance according to claim 1, characterized in that: The step B specifically comprises: Adding the Gd2O3-MgO nanocomposite powder to a LiNO3 solution to obtain a Gd2O3-MgO nanocomposite powder suspension, and adding an NH4F solution to the Gd2O3-MgO nanocomposite powder suspension; The mixture is then stirred at a temperature of 60 to 100° C. for 1 to 2 hours, and then allowed to stand for stratification, and the supernatant is removed to obtain a precipitate.

3. The method for preparing a composite ceramic material with high infrared transmittance according to claim 2, characterized in that: The NH4F solution is added dropwise to the Gd2O3-MgO nanocomposite powder suspension at a titration rate of 0.3-1 mL / min.

4. The method for preparing a composite ceramic material with high infrared transmittance according to claim 1 or 2, characterized in that: The LiNO3 solution is prepared by dissolving LiNO3 in anhydrous ethanol; The NH4F solution is prepared by dissolving NH4F in anhydrous ethanol.

5. The method for preparing a composite ceramic material with high infrared transmittance according to claim 1, characterized in that: In the step C, the mass percentage of LiF in the LiF-coated Gd2O3-MgO nanocomposite powder is 0.35% to 3.5%.

6. The method for preparing a composite ceramic material with high infrared transmittance according to claim 1, characterized in that: The step C specifically comprises: The precipitate is washed, filtered and dried in sequence, and the dried precipitate is calcined at 300-500° C. for 3-5 hours under the protection of an inert atmosphere to obtain a LiF-coated Gd2O3-MgO nanocomposite powder.

7. The method for preparing a composite ceramic material with high infrared transmittance according to claim 1, characterized in that: The step A specifically comprises: dissolving gadolinium salt and magnesium salt in water to obtain a mixed solution; Adding an organic additive to the mixed solution, stirring and heating, and placing the solution in an oven at 180-220° C. for 1-6 hours after the solution becomes thick, to obtain a dry gel; The dry gel is kept at 700-900° C. for 2-5 hours in an oxygen-containing atmosphere to obtain Gd2O3-MgO nanocomposite powder.

8. The method for preparing a composite ceramic material with high infrared transmittance according to claim 1, characterized in that: The step D specifically comprises: The LiF-coated Gd2O3-MgO nanocomposite powder is successively ball-milled, dried and sieved, and then heated at 500-700° C. for 2-6 hours to obtain a high-activity powder; The high-activity powder is subjected to dry pressing and cold isostatic pressing to obtain a ceramic green body; The ceramic green body is subjected to air pre-sintering and hot isostatic pressing to obtain a sintered body; The sintered body is annealed and processed to obtain the composite ceramic material.

9. The method for preparing a composite ceramic material with high infrared transmittance according to claim 8, characterized in that: The temperature of the air pre-sintering is 1200-1240°C, and the temperature of the hot isostatic pressing sintering is 1200-1240°C.

10. A composite ceramic material with high infrared transmittance, characterized in that: The composite ceramic material is prepared by the method for preparing a composite ceramic material with high infrared transmittance as described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Y2O3-MgO nano-composite ceramic and preparation method thereof

    CN103922742A

  • Gadolinium oxide-magnesium oxide nano composite ceramic and preparation method thereof

    CN109650890A

  • Infrared transparent ceramic material and preparation method thereof

    CN115745607A