Medium-entropy ceramic material as well as preparation method and application thereof
By using raw materials such as WC, TiC, B4C, HfB2 and ZrB2, combined with discharge plasma sintering and two-step sintering technology, the problem of single types of medium-entropy ceramic systems and insufficient densification of traditional sintering technology is solved, and the mechanical properties of ceramic materials are significantly improved. and processing efficiency.
Patent Information
- Application Number
- CN202410930067.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-07-11
AI Technical Summary
The existing medium-entropy ceramic system has a single type, making it difficult to effectively process difficult materials in high-temperature and high-pressure environments. Traditional sintering technology leads to the growth of grains and the presence of oxide impurities during densification, which affects the mechanical properties.
The medium entropy ceramic powder is prepared by ball milling by ball milling, and the discharge plasma sintering (SPS) and two-step sintering (TSSPS) processes are combined with two anions to improve the densification and mechanics of the material. performance.
Medium-entropy ceramic materials that obtain fine grains at low densification temperatures are achieved, which improves their hardness, fracture toughness and bending strength, reduces sintering damage, and significantly improves the mechanical properties of ceramic materials.
Smart Images

Figure CN119019171A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of ceramic technology, and in particular to a medium-entropy ceramic material and a preparation method and application thereof. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Difficult-to-process materials generally have the characteristics of high hardness, high mechanical strength and strong oxidation resistance. For example, difficult-to-process materials including high-performance alloys (tungsten alloy, titanium alloy, etc.), hard and brittle materials (glass ceramics, silicon carbide, aluminum nitride, etc.) and composite materials (particle-reinforced metal matrix composites, fiber-reinforced ceramic matrix composites, etc.) have been widely used in aerospace, military, energy and other fields that require high temperature resistance and strong thermal stability.
[0004] At present, coated carbide tools are mainly used in milling of such materials. However, since the tool materials are used in harsh environments of high temperature and high pressure, tool durability and processing efficiency face great challenges. Ceramic tools have many advantages such as high hardness, good wear resistance, and stable physical and chemical properties at high temperatures. When cutting difficult materials such as nickel-based alloys, their cutting performance is better than that of carbide tools and high-speed steel tools, and they have been widely used in cutting.
[0005] Compared with traditional ceramics, mesentropy ceramics have higher mechanical properties such as hardness, strength and toughness, as well as better corrosion resistance, biocompatibility and electrochemical properties, and have greater development potential in the fields of ultra-high temperature, biomedicine and energy. However, the existing mesentropy ceramic system is relatively single, and it is urgent to expand the types of mesentropy ceramics. Summary of the invention
[0006] In order to overcome the above problems, the present invention provides a medium-entropy ceramic material and a preparation method and application thereof.
[0007] In order to achieve the above technical objectives, the present invention adopts the following technical solutions:
[0008] The first aspect of the present invention provides a medium-entropy ceramic material, the raw materials of which include equal amounts of WC, TiC, B4C, HfB2 and ZrB2.
[0009] The second aspect of the present invention provides a method for preparing the above-mentioned medium entropy ceramic material, comprising:
[0010] (1) WC, TiC, B4C, HfB2 and ZrB2 are placed in a ball mill according to the ratio, a medium solvent is added, and the ball milled suspension is dried and sieved to obtain a medium entropy ceramic powder;
[0011] (2) The medium-entropy ceramic powder is placed in a mold and then compacted. The molded embryo is pressurized and sintered in a spark plasma sintering (SPS) furnace to obtain a medium-entropy ceramic material.
[0012] The third aspect of the present invention provides the use of the above-mentioned medium-entropy ceramic material in the preparation of ceramic cutting tools.
[0013] The beneficial effects of the present invention are:
[0014] (1) Traditional sintering technology usually requires a very high sintering temperature to prepare high-density high-entropy ceramics, and too high a sintering temperature will mainly lead to severe grain growth, thereby worsening the densification process. The spark plasma sintering (SPS) used in the present invention has the characteristics of fast heating rate and low densification temperature compared with the traditional sintering method; and spark plasma sintering can reduce the oxide impurities on the surface of the raw materials to a certain extent, thereby promoting the densification of ceramic materials. The present invention is a two-step sintering (TSSPS) process based on spark plasma sintering, which can ensure the full densification of ceramic materials while reducing sintering damage. The grains of the dense sintered body are small, thereby improving the overall mechanical properties.
[0015] (2) When a second anion is added to the medium-entropy ceramic system, the increase in entropy is equivalent to the increase in entropy caused by adding an additional metal element. Therefore, when the medium-entropy ceramic system transitions from containing only one anion to containing two anions, the configurational entropy will increase significantly, and there will also be more serious lattice distortion, thereby improving the performance of the medium-entropy ceramic. In the present invention, two anions are introduced and a borocarbide ceramic system is selected, so that the material exhibits good mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0017] Figure 1 This is a scanning electron microscope image of the medium-entropy ceramic material prepared in Example 1;
[0018] Figure 2 Element distribution diagram of the medium entropy ceramic material prepared in Example 1 under EDS scanning;
[0019] Figure 3 This is the EDS spectrum of the medium-entropy ceramic material prepared in Example 1. DETAILED DESCRIPTION
[0020] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0021] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0022] A first typical embodiment of the present invention provides a medium-entropy ceramic material, the raw materials of which include equal amounts of WC, TiC, B4C, HfB2 and ZrB2.
[0023] A second typical embodiment of the present invention provides a method for preparing the above-mentioned medium-entropy ceramic material, comprising:
[0024] (1) WC, TiC, B4C, HfB2 and ZrB2 are placed in a ball mill according to the ratio, a medium solvent is added, and the ball milled suspension is dried and sieved to obtain a medium entropy ceramic powder;
[0025] (2) The medium-entropy ceramic powder is placed in a mold and then compacted. The molded embryo is pressurized and sintered in a spark plasma sintering (SPS) furnace to obtain a medium-entropy ceramic material.
[0026] In one or more embodiments, the purity of the TiC, B4C, HfB2 and ZrB2 raw materials is 99.5%, and the particle size thereof is 0.4 to 0.6 μm, preferably 0.5 μm;
[0027] The purity of the WC raw material is 99.9%, and the particle size thereof is 0.4-0.6 μm, preferably 0.5 μm.
[0028] In one or more embodiments, the medium solvent is anhydrous ethanol.
[0029] In one or more embodiments, during ball milling, the ball-to-material ratio is 8 to 12:1, preferably 10:1; and the ball milling time is 24 to 48 hours.
[0030] In one or more embodiments, the ball-milled suspension is dried and then passed through a 150-170 mesh sieve.
[0031] In one or more embodiments, during pressure sintering, the sintering process is: sintering at a temperature of 1900-2000°C under 23-27MPa for 4-6min; then cooling to 1750-1850°C, increasing the pressure to 28-32MPa, and keeping warm for 8-12min; finally cooling to room temperature to obtain a medium-entropy ceramic body.
[0032] Preferably, the rates during heating and cooling are the same, both at 120-130° C. / min.
[0033] In one or more embodiments, the average grain size of the medium-entropy ceramic material prepared by the above preparation method is 0.1 to 0.3 μm.
[0034] In one or more embodiments, the hardness, fracture toughness and flexural strength of the medium-entropy ceramic material prepared by the above preparation method are 20-22 GPa, 9-10 MPa·m 1 / 2 , 580~620Mpa.
[0035] A third typical embodiment of the present invention provides the use of the above-mentioned medium-entropy ceramic material in the preparation of ceramic cutting tools.
[0036] In one or more embodiments, the ceramic tool is used for milling difficult-to-machine materials.
[0037] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.
[0038] Example 1
[0039] WC (powder purity 99.9%, particle size 0.5μm), TiC (powder purity 99.5%, particle size 0.5μm), B4C (powder purity 99.5%, particle size 0.5μm), HfB2 (powder purity 99.5%, particle size 0.5μm), and ZrB2 (powder purity 99.5%, particle size 0.5μm) are used as raw materials, and the above raw materials are weighed in equal amounts.
[0040] Using anhydrous ethanol as solvent, Al2O3 ball milling medium with a ball-to-material ratio of 10:1 was used for ball milling in a planetary ball mill for 36 hours. The milled suspension was placed in a vacuum drying oven for drying for 12 hours. After drying, it was sieved with a 160-mesh sieve to obtain a medium-entropy ceramic powder which was sealed for later use.
[0041] The mixed powder was loaded into the mold and the powder was pre-compacted at 5 MPa. The mold was placed in a spark plasma sintering (SPS) furnace for sintering. The temperature was raised to 1950°C at a rate of 125°C / min, pressurized to 25 MPa, and sintered for 5 min; then the temperature was lowered to 1800°C at a rate of 125°C / min, pressurized to 30 MPa, and kept at this temperature for 10 min, and finally lowered to room temperature at a rate of 125°C / min.
[0042] Figure 1 This is a SEM image of the fracture of the medium-entropy ceramic material obtained in this example.
[0043] Figure 2 Element distribution diagram of the medium entropy ceramic material obtained in this example under EDS scanning.
[0044] Figure 3 : This is the EDS spectrum of the medium-entropy ceramic material obtained in this example.
[0045] Figure 2 This indicates that the elements in the medium-entropy ceramic material obtained in this embodiment are evenly distributed.
[0046] In this embodiment, the medium entropy ceramic material with good mechanical properties obtained after sintering has a hardness of 22GPa and a fracture toughness of 9.8MPa·m 1 / 2 , the flexural strength is 598MPa.
[0047] Comparative Example 1
[0048] Compared with Example 1, the powders in this comparative example are weighed and prepared with equal volumes.
[0049] WC (powder purity 99.9%, particle size 0.5μm), TiC (powder purity 99.5%, particle size 0.5μm), B4C (powder purity 99.5%, particle size 0.5μm), HfB2 (powder purity 99.5%, particle size 0.5μm), and ZrB2 (powder purity 99.5%, particle size 0.5μm) are used as raw materials, and the above raw materials are weighed and powdered in equal volumes.
[0050] Using anhydrous ethanol as solvent, Al2O3 ball milling medium with a ball-to-material ratio of 10:1 was used for ball milling in a planetary ball mill for 36 hours. The milled suspension was placed in a vacuum drying oven for drying for 12 hours. After drying, it was sieved with a 160-mesh sieve to obtain a medium-entropy ceramic powder which was sealed for later use.
[0051] The mixed powder was loaded into the mold and the powder was pre-compacted at 5 MPa. The mold was placed in a spark plasma sintering (SPS) furnace for sintering. The temperature was raised to 1950°C at a rate of 125°C / min, pressurized to 25 MPa, and sintered for 5 min; then the temperature was lowered to 1800°C at a rate of 125°C / min, pressurized to 30 MPa, and kept at this temperature for 10 min, and finally lowered to room temperature at a rate of 125°C / min.
[0052] In this comparative example, the medium entropy ceramic material obtained after sintering has a hardness of 18.22 GPa and a fracture toughness of 9.07 MPa·m 1 / 2 , the flexural strength is 316MPa.
[0053] Comparative Example 2
[0054] Compared with Example 1, this comparative example uses WC, TiC, NbC and VC powders.
[0055] TiC (powder purity 99.5%, particle size 1 μm), WC (powder purity 99.5%, particle size 1 μm), NbC (powder purity 99.5%, particle size 1 μm), VC (powder purity 99.5%, particle size 1 μm) are used as raw materials, and the above raw materials are weighed and powdered in equal molar fraction ratio.
[0056] The powder was loaded into a WC carbide jar and ball-milled in a planetary ball mill with a carbide ball milling medium having a ball-to-material ratio of 10:1 for 24 h.
[0057] The mixed powder was loaded into the mold, and then the mold was placed in a spark plasma sintering (SPS) furnace for sintering. The temperature was raised to 1500°C at a rate of 100°C / min, pressurized to 25MPa, and sintered for 5min; the temperature was lowered to 1400°C at a rate of 100°C / min, kept at that temperature for 10min, and finally lowered to room temperature at a rate of 100°C / min.
[0058] In this comparative example, the medium entropy ceramic material obtained after sintering has a hardness of 23.4 GPa and a fracture toughness of 6.3 MPa·m 1 / 2 .
[0059] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A medium entropy ceramic material, characterized in that: Its raw materials include WC, TiC, B4C, HfB2 and ZrB2 in equal amounts.
2. The method for preparing the medium-entropy ceramic material according to claim 1, characterized in that: include: (1) WC, TiC, B4C, HfB2 and ZrB2 are placed in a ball mill according to the ratio, a medium solvent is added, and the ball milled suspension is dried and sieved to obtain a medium entropy ceramic powder; (2) The medium-entropy ceramic powder is filled into a mold and then compacted. The molded embryo is pressurized and sintered in a spark plasma sintering furnace to obtain a medium-entropy ceramic material.
3. The preparation method according to claim 2, characterized in that: The purity of the TiC, B4C, HfB2 and ZrB2 raw materials is 99.5%, and the particle size is 0.4-0.6 μm, preferably 0.5 μm; The purity of the WC raw material is 99.9%, and the particle size thereof is 0.4-0.6 μm, preferably 0.5 μm.
4. The preparation method according to claim 2, characterized in that: The medium solvent is anhydrous ethanol.
5. The preparation method according to claim 2, characterized in that: When ball milling is performed, the ball-to-material ratio is 8 to 12:1, preferably 10:1; the ball milling time is 24 to 48 hours; Alternatively, the suspension after ball milling is dried and passed through a 150-170 mesh sieve.
6. The preparation method according to claim 2, characterized in that: During pressure sintering, the sintering process is as follows: sintering at a temperature of 1900-2000°C for 4-6 minutes under 23-27 MPa; then cooling to 1750-1850°C, increasing the pressure to 28-32 MPa, and keeping the temperature for 8-12 minutes; finally cooling to room temperature to obtain a medium-entropy ceramic body; Preferably, the rates during heating and cooling are the same, both at 120-130° C. / min.
7. The preparation method according to claim 2, characterized in that: The average grain size of the medium entropy ceramic material is 0.1 to 0.3 μm.
8. The preparation method according to claim 2, characterized in that: The hardness, fracture toughness and flexural strength of medium entropy ceramic materials are 20-22GPa and 9-10MPa·m 1 / 2 , 580~620Mpa.
9. Use of the medium-entropy ceramic material according to claim 1 and / or the medium-entropy ceramic material prepared by the preparation method according to any one of claims 2 to 8 in the preparation of ceramic cutting tools.
10. The use according to claim 9, characterized in that The ceramic tool is used for milling difficult-to-machine materials.
Citation Information
Patent Citations
High-performance friction stir welding tools
CN101415518A
A kind of toughened ceramics materials
CN109824363A
High-entropy low-boride ceramic and preparation method thereof
CN113480315A
Medium-high-entropy ceramic material as well as preparation method and application thereof
CN114560699A
Functionalized non-spherical powder raw material and preparation method thereof
CN114728332A
Cited By
A medium-entropy ceramic material, a preparation method and application thereof
CN119019171B