Solid electrolyte film, preparation method and solid-state battery

Through the composite binder modified by polyacrylonitrile and polydopamine, a solid electrolyte film with high flexibility and high ionic conductivity was prepared, which solved the problems of poor flexibility and unclear ion conduction mechanism in the inorganic solid electrolyte, and improved the solid battery Performance and production convenience.

CN118919837AActive Publication Date: 2024-11-08JILIN UNIVERSITY

Patent Information

Application Number
CN202411134599.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-08
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

The high mechanical strength of inorganic solid electrolytes in existing solid-state batteries leads to poor flexibility, making it difficult to measure high ion conductivity through simple processes, and the ion conduction mechanism is unclear, affecting conductivity and large-scale production.

Method used

The inorganic solid electrolyte modified by polyacrylonitrile and polydopamine modified polytetrafluoroethylene composite adhesive is prepared through high-energy ball milling and rotary defoaming mechanism to improve flexibility and bonding to form a continuous Ion channel.

Benefits of technology

Li+ transmission is achieved without sintering or external pressure, improving the ion transmission performance, redox reversibility and cycling performance of solid-state batteries, and simplifying the preparation process, reducing costs, and suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919837A_ABST
    Figure CN118919837A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of solid electrolyte, in particular to a solid electrolyte film, a preparation method and a solid-state battery. The solid electrolyte film provided by the invention is prepared from an organic polymer polyacrylonitrile modified inorganic solid electrolyte and a polydopamine modified polytetrafluoroethylene composite binder. On one hand, by introducing the organic flexible polymer polyacrylonitrile, the flexibility and machinability of the inorganic solid electrolyte are improved, and the problem of poor interface compatibility of an inorganic electrolyte / inorganic electrode is improved; on the other hand, by introducing the polydopamine containing amido and hydroxyl polar groups, the cohesiveness of the polytetrafluoroethylene binder with the low friction coefficient is improved, the solid electrolyte is more compact, and an ion channel is more continuous. When the solid electrolyte film provided by the invention is applied to the solid-state battery, the ion transmission performance, the redox reversibility and the cycle performance of the solid-state battery can be effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of solid electrolyte technology, and in particular to a solid electrolyte film, a preparation method and a solid-state battery. Background Art

[0002] In recent years, people have an increasing demand for 3C electronic devices (computers, communications, consumer electronics), electric vehicles, aircraft, etc., and the performance requirements for new energy power supply devices represented by lithium batteries are also getting higher and higher, which must provide higher safety and energy density.

[0003] Solid-state batteries can provide higher energy and higher safety. Inorganic solid electrolytes have low cost, high lithium ion conductivity, high electrochemical stability and good compatibility with metallic lithium. Inorganic solid electrolytes have high hardness, and filling solid electrolyte particles into a lithium ion conductive polymer matrix to prepare a composite electrolyte can improve its ductility and flexibility. However, the mechanism of ion conduction in the current composite electrolyte is still unclear. If the particles do not form a continuous conductive network in the polymer, the contribution of lithium ion transport between solid electrolyte particles to the total conductivity may be limited. In addition, due to the high mechanical strength of inorganic solid electrolytes, their high ionic conductivity cannot be measured by simple cold pressing. High-temperature sintering processes can achieve their high ionic conductivity, but the flexibility of the membrane will be lost, which faces great challenges in large-scale production. Summary of the invention

[0004] Based on this, the present invention provides a solid electrolyte film, a preparation method thereof, and an application in a solid-state battery. The solid electrolyte film provided by the present invention is prepared by using an inorganic solid electrolyte modified by an organic polymer polyacrylonitrile and a polydopamine-modified polytetrafluoroethylene composite binder. On the one hand, by introducing the organic flexible polymer polyacrylonitrile, the flexibility and processability of the inorganic solid electrolyte are improved, and the problem of poor compatibility of the inorganic electrolyte / inorganic electrode interface is improved. On the other hand, by introducing polydopamine containing polar groups such as amino groups and hydroxyl groups, the adhesion of the polytetrafluoroethylene binder with a low friction coefficient is improved, making the solid electrolyte denser and the ion channel more continuous.

[0005] The objective of the present invention is achieved through the following technical solutions:

[0006] In a first aspect, the present invention provides a method for preparing a solid electrolyte film, characterized in that it comprises the following steps:

[0007] A. Preparation of polyacrylonitrile modified solid electrolyte particles:

[0008] A1, dissolving polyacrylonitrile in dimethyl sulfoxide and performing high-energy ball milling process;

[0009] A2, placing an inorganic solid electrolyte and a lithium salt in the above-mentioned ball-milled material and performing a high-energy ball milling process again;

[0010] A3, adding 1-propanol as a precipitant to the material obtained in step A2, performing a final ball milling, and then centrifuging and drying the ball milled product to obtain polyacrylonitrile-modified solid electrolyte particles;

[0011] B. Preparation of polydopamine-modified polytetrafluoroethylene composite binder:

[0012] B1. Pre-treating polytetrafluoroethylene with a potassium permanganate / nitric acid mixed solution to form hydrophilic manganese oxide or manganese hydroxide covering polytetrafluoroethylene particles;

[0013] B2, adding dopamine monomer and potassium permanganate in proportion to an alkaline solution with a pH of 8.5, and then slowly adding the polytetrafluoroethylene pretreated in step B1 to carry out a polymerization reaction. After the reaction is completed, ultrasonic washing with deionized water and vacuum drying are performed to obtain a polydopamine-coated polytetrafluoroethylene binder;

[0014] C. Preparation into solid electrolyte film:

[0015] C1. The solid electrolyte modified with polyacrylonitrile and the polytetrafluoroethylene composite binder modified with polydopamine are uniformly mixed according to a mass ratio in a protective gas atmosphere by a rotary defoamer, wherein the protective gas is one of argon, nitrogen and helium;

[0016] C2. Grinding the obtained mixture powder in a special ball mill for 3 minutes under a protective gas atmosphere to obtain a microfibrillated mixture, wherein the protective gas is one of argon, nitrogen and helium;

[0017] C3. The microfibrillated mixture powder is rolled using a double-roll roller press under set parameters to fully fiberize the binder to obtain a solid electrolyte film.

[0018] Furthermore, in step A2, the inorganic solid electrolyte is one of a sulfide solid electrolyte, an oxide solid electrolyte and a halide solid electrolyte; the lithium salt is one of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), lithium perchlorate (LiClO4), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6) and lithium hexafluorophosphate (LiPF6).

[0019] Furthermore, in said step A, the mass ratio of polyacrylonitrile to solid electrolyte is (1-3):100.

[0020] Furthermore, in the step C1, based on the total mass of the solid electrolyte film, the mass proportion of the solid electrolyte modified by polyacrylonitrile is 97-99%, and the mass proportion of the polytetrafluoroethylene modified by polydopamine is 1-3%.

[0021] Furthermore, in the step C3, the set parameters involve temperature, rolling times, rolling direction and film thickness, the temperature is 25°C to 80°C, the rolling times are 5 to 20 times, the rolling direction is unidirectional or bidirectional, and the film thickness is 50 to 150 μm.

[0022] In a second aspect, the present invention provides a solid electrolyte film, which is prepared by the method described in the above technical solution.

[0023] In a third aspect, the present invention provides a solid-state battery, comprising an electrode sheet and the above-mentioned solid electrolyte film; the electrode sheet comprises a current collector and an active layer on the current collector, and the active layer comprises an electrode active material, conductive carbon and a polydopamine-modified polytetrafluoroethylene composite binder.

[0024] Furthermore, in the active layer on the current collector, the polydopamine-modified polytetrafluoroethylene composite binder accounts for 1 to 10% of the mass of the active layer.

[0025] Furthermore, the electrode active material includes a positive electrode active material or a negative electrode active material. Positive electrode active materials include but are not limited to lithium iron phosphate (LiFePO4), lithium cobalt oxide (LiCoO2), lithium manganese oxide (LiMn2O4), lithium nickel cobalt manganese oxide (LiNi 0.5 Co 0.2 Mn 0.3 O2、LiNi 0.8 Co 0.1 Mn 0.1 O2、LiNi 0.6 Co 0.2 Mn 0.2 O2) at least one; the negative electrode active material includes but is not limited to at least one of lithium metal, carbon-based, and silicon-based negative electrode active materials.

[0026] Furthermore, the silicon-based negative electrode active material includes a silicon-oxygen negative electrode material: the molecular formula is SiOx, and x is any value from 0 to 2. Non-limiting examples include: silicon dioxide and silicon dioxide.

[0027] Furthermore, the carbon-based negative electrode active material can adopt the carbon negative electrode material commonly used in the art, including but not limited to: at least one of mesophase carbon microbeads, natural graphite, artificial graphite, graphene, glassy carbon, carbon nanotubes, carbon fiber, hard carbon, and soft carbon.

[0028] Furthermore, the active layer also includes conductive carbon, and the conductive carbon includes but is not limited to at least one of graphite, carbon nanotubes, nanofibers, carbon black and graphene.

[0029] Furthermore, the thickness of the active layer is 50 μm to 200 μm, for example, 50 μm, 100 μm, 150 μm or 200 μm.

[0030] Furthermore, the current collector adopts a current collector commonly used in the art, such as copper foil, aluminum foil, etc.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] 1. The present invention uses polyacrylonitrile with high ionic conductivity and high elastic modulus to modify the solid electrolyte, giving it excellent flexibility and processability. The solid electrolyte membrane can effectively achieve Li+ between particles without sintering or applying external pressure. + transmission;

[0033] 2. In the present invention, the potassium permanganate / nitric acid mixed solution is used to pretreat polytetrafluoroethylene to increase the subsequent coating area of ​​polydopamine. Polydopamine contains polar groups such as amine groups and hydroxyl groups, which improve the adhesion of polytetrafluoroethylene with a low friction coefficient, making the solid electrolyte denser and the ion channel more continuous.

[0034] 3. The ion transport performance, redox reversibility and cycle performance of the solid-state battery provided by the present invention are effectively improved. In addition, the technical solution of the present invention involves a dry process, that is, preparing electrolytes and electrode sheets without using solvents, which can greatly simplify the preparation process, reduce preparation costs, and facilitate large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0036] Figure 1 Schematic diagram of the preparation process of polyacrylonitrile-modified lithium lanthanum zirconium oxide particles in Example 1 of the present invention;

[0037] Figure 2 1 is a SEM image of lithium lanthanum zirconium oxide particles modified with polyacrylonitrile at different sizes in Example 1 of the present invention;

[0038] Figure 3 FT-IR images of polyacrylonitrile, lithium lanthanum zirconium oxide and lithium lanthanum zirconium oxide modified with polyacrylonitrile in Example 1 of the present invention;

[0039] Figure 4 is a schematic diagram of a solid electrolyte film preparation process in Example 1 of the present invention;

[0040] Figure 5 This is a physical picture of the solid electrolyte film in Example 1 of the present invention;

[0041] Figure 6 is a schematic diagram of the microscopic morphology (SEM) of the solid electrolyte film in Example 1 of the present invention;

[0042] Figure 7 is an impedance comparison diagram of the battery of Example 6 of the present invention and Comparative Example 1;

[0043] Figure 8 It is a comparison chart of the coulombic efficiency of the batteries of Example 6 of the present invention and Comparative Example 2 in the first three cycles. DETAILED DESCRIPTION

[0044] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively below. Preferred embodiments of the present invention are given in the specific embodiments. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. It should be understood that the attached claims summarize the scope of the present invention. Under the guidance of the inventive concept, those skilled in the art should be aware that certain changes made to the various embodiments of the present invention will be covered by the spirit and scope of the claims of the present invention.

[0045] Embodiment 1

[0046] This embodiment provides a method for preparing a solid electrolyte film, comprising the following steps:

[0047] Step 1: Preparation of polyacrylonitrile (PAN) modified lithium lanthanum zirconium oxide (LLZTO) particles. The specific reaction route is as follows: Figure 1 As shown. The specific operation is: first, weigh 0.15g PAN and dissolve it in 20mL dimethyl sulfoxide and perform high-energy ball milling until the liquid turns light yellow. Secondly, weigh the lithium salt bistrifluoromethanesulfonyl imide, and the mass ratio of PAN to lithium salt is 1:1. At the same time, weigh 5.0g LLZTO nanoparticles, the mass ratio of LLZTO to PAN is 100:3, and perform high-energy ball milling again until the turbid liquid turns brown. Finally, add 2.0mL of precipitant 1-propanol and mix it by ball milling for the last time. After that, centrifuge the supernatant, transfer the mixture precipitate to a vacuum oven, keep it in a vacuum drying oven at 60°C overnight to remove the solvent, and store it in a glove box filled with argon.

[0048] Step 2: Polymerize dopamine on the surface of polytetrafluoroethylene (PTFE). The specific operation is: add buffer salt tris(hydroxymethyl)aminomethane to the dopamine salt solution and adjust the pH to 8.5 to accelerate the polymerization of dopamine. KMnO4 is used as an oxidant, and 0.04 mol of KMnO4 solid and 0.018 mol of dopamine monomer are added to the above alkaline solvent. Then 30.00 g of PTFE pretreated in step 1 is slowly added. At 0°C, high-speed stirring is carried out for polymerization for 24 hours. After the reaction is completed, the obtained solid is washed with water several times until the filtrate is clear and transparent, and then dried under vacuum conditions at 100°C for 12 hours to obtain a polydopamine (PDA)-modified PTFE composite adhesive.

[0049] Step 3: Preparation of solid electrolyte film. The preparation process is as follows: Figure 4 As shown. The specific operation is: the PAN-modified LLZTO electrolyte and the PDA-modified PTFE composite binder are uniformly mixed in a mass ratio of 97:3 by a rotary defoamer. Subsequently, the obtained mixture powder is ground in a special ball mill for 3 minutes to obtain a microfibrillated mixture powder. Finally, the obtained microfibrillated mixture powder is set at 80°C with a double roller distance of 50μm, and the roller press is used in a bidirectional manner for 15 times to reach 50μm to obtain a solid electrolyte film.

[0050] Embodiment 2

[0051] This embodiment provides a method for preparing a solid electrolyte film, comprising the following steps:

[0052] Step 1: Preparation of PAN-modified Li 6.4 Ln3Z 1.4 Nb 0.6 O 12 (LLZNO) particles. The specific operation is: first, weigh 0.15g PAN and dissolve it in 20mL dimethyl sulfoxide and perform high-energy ball milling until the liquid turns light yellow. Secondly, weigh the lithium salt bistrifluoromethanesulfonyl imide, and the mass ratio of PAN to lithium salt is 1:1. At the same time, weigh 5.0g LLZNO nanoparticles, the mass ratio of LLZNO to PAN is 100:3, and perform high-energy ball milling again until the turbid liquid turns brown. Finally, add 2.0mL of precipitant 1-propanol and mix it by ball milling for the last time. After that, centrifuge the supernatant, transfer the mixture precipitate to a vacuum oven, keep it in a vacuum drying oven at 60°C overnight to remove the solvent, and store it in a glove box filled with argon.

[0053] Step 2: Polymerize dopamine on the PTFE surface. The specific operation is: add buffer salt tris(hydroxymethyl)aminomethane to the dopamine salt solution and adjust the pH to 8.5 to accelerate the polymerization of dopamine. KMnO4 is used as an oxidant, and 0.04 mol of KMnO4 solid and 0.018 mol of dopamine monomer are added to the above alkaline solvent. Then slowly add 30.00 g of PTFE pretreated in step 1. At 0°C, stir at high speed for 24 hours. After the reaction is completed, wash the obtained solid with water several times until the filtrate is clear and transparent, and then dry it under vacuum conditions at 100°C for 12 hours to obtain a PDA-modified PTFE composite adhesive.

[0054] Step 3: Preparation of solid electrolyte film. The specific operation is: the PAN-modified LLZNO electrolyte and the PDA-modified PTFE composite binder are uniformly mixed in a mass ratio of 97:3 by a rotary defoamer. Subsequently, the obtained mixture powder is ground in a special ball mill for 3 minutes to obtain a microfibrillated mixture powder. Finally, the obtained microfibrillated mixture powder is set at 80°C with a double roller distance of 50μm on the roller press, and the roller press is rolled 10 times in both directions to reach 50μm to obtain a solid electrolyte film.

[0055] Embodiment 3

[0056] This embodiment provides a method for preparing a solid electrolyte film, comprising the following steps:

[0057] Step 1: Preparation of PAN-modified LLZTO particles. The specific reaction route is as follows: Figure 1 As shown. The specific operation is: first, weigh 0.15g PAN and dissolve it in 20mL dimethyl sulfoxide and perform high-energy ball milling until the liquid turns light yellow. Secondly, weigh the lithium salt bistrifluoromethanesulfonyl imide, and the mass ratio of PAN to lithium salt is 1:1. At the same time, weigh 15.0g LLZTO nanoparticles, the mass ratio of LLZTO to PAN is 100:1, and perform high-energy ball milling again until the turbid liquid turns brown. Finally, add 2.0mL of precipitant 1-propanol and mix it by ball milling for the last time. After that, centrifuge the supernatant, transfer the mixture precipitate to a vacuum oven, keep it in a vacuum drying oven at 60°C overnight to remove the solvent, and store it in a glove box filled with argon.

[0058] Step 2: Polymerize dopamine on the PTFE surface. The specific operation is: add buffer salt tris(hydroxymethyl)aminomethane to the dopamine salt solution and adjust the pH to 8.5 to accelerate the polymerization of dopamine. KMnO4 is used as an oxidant, and 0.04 mol of KMnO4 solid and 0.018 mol of dopamine monomer are added to the above alkaline solvent. Then slowly add 30.00 g of PTFE pretreated in step 1. At 0°C, stir at high speed for 24 hours. After the reaction is completed, wash the obtained solid with water several times until the filtrate is clear and transparent, and then dry it under vacuum conditions at 100°C for 12 hours to obtain a PDA-modified PTFE composite adhesive.

[0059] Step 3: Preparation of solid electrolyte film. The specific operation is: the PAN-modified LLZTO electrolyte and the PDA-modified PTFE composite binder are uniformly mixed in a mass ratio of 99:1 by a rotary defoamer. Subsequently, the obtained mixture powder is ground in a special ball mill for 3 minutes to obtain a microfibrillated mixture powder. Finally, the obtained microfibrillated mixture powder is set at 80°C with a double roller distance of 50μm on the roller press, and the roller press is calendered 20 times in a unidirectional manner to reach 50μm to obtain a solid electrolyte film.

[0060] Embodiment 4

[0061] This embodiment provides a method for preparing a solid electrolyte film, comprising the following steps:

[0062] Step 1: Preparation of polyacrylonitrile (PAN) modified lithium lanthanum zirconium oxide (LLZTO) particles. The specific reaction route is as follows: Figure 1 As shown. The specific operation is: First, weigh 0.15g PAN and dissolve it in 20mL dimethyl sulfoxide and perform high-energy ball milling until the liquid turns light yellow. Secondly, weigh the lithium salt bistrifluoromethanesulfonyl imide, and the mass ratio of PAN to lithium salt is 1:1. At the same time, weigh 5.0g LLZTO nanoparticles, and the mass ratio of LLZTO to PAN is 100:3, and perform high-energy ball milling again until the turbid liquid turns brown. Finally, add 2.0mL of precipitant 1-propanol and mix by ball milling for the last time. After that, centrifuge the supernatant, transfer the mixture precipitate to a vacuum oven, keep it in a vacuum drying oven at 60°C overnight to remove the solvent, and store it in an argon-filled glove box. The SEM of the electrolyte powder is as follows Figure 2 The FT-IR of PAN, LLZTO and PAN-modified LLZTO is shown in 3.

[0063] Step 2: Polymerize dopamine on the PTFE surface. The specific operation is: add buffer salt tris(hydroxymethyl)aminomethane to the dopamine salt solution and adjust the pH to 8.5 to accelerate the polymerization of dopamine. KMnO4 is used as an oxidant, and 0.04 mol of KMnO4 solid and 0.018 mol of dopamine monomer are added to the above alkaline solvent. Then slowly add 30.00 g of PTFE pretreated in step 1. At 0°C, stir at high speed for 24 hours. After the reaction is completed, wash the obtained solid with water several times until the filtrate is clear and transparent, and then dry it under vacuum conditions at 100°C for 12 hours to obtain a PDA-modified PTFE composite adhesive.

[0064] Step 3: Preparation of solid electrolyte film. The specific operation is: the PAN-modified LLZTO electrolyte and the PDA-modified PTFE composite binder are uniformly mixed in a mass ratio of 97:3 by a rotary defoamer. Subsequently, the obtained mixture powder is ground in a special ball mill for 1 minute to obtain a microfibrillated mixture powder. Finally, the obtained microfibrillated mixture powder is set at 80°C with a double roller distance of 100μm on the roller press, and the roller press is rolled 15 times in both directions to reach 100μm to obtain a solid electrolyte film.

[0065] Embodiment 5

[0066] This embodiment provides a method for preparing a solid electrolyte film, comprising the following steps:

[0067] Step 1: Preparation of polyacrylonitrile (PAN) modified lithium lanthanum zirconium oxide (LLZTO) particles. The specific reaction route is as follows: Figure 1 As shown. The specific operation is: First, weigh 0.15g PAN and dissolve it in 20mL dimethyl sulfoxide and perform high-energy ball milling until the liquid turns light yellow. Secondly, weigh the lithium salt bistrifluoromethanesulfonyl imide, and the mass ratio of PAN to lithium salt is 1:1. At the same time, weigh 5.0g LLZTO nanoparticles, and the mass ratio of LLZTO to PAN is 100:3, and perform high-energy ball milling again until the turbid liquid turns brown. Finally, add 2.0mL of precipitant 1-propanol and mix by ball milling for the last time. After that, centrifuge the supernatant, transfer the mixture precipitate to a vacuum oven, keep it in a vacuum drying oven at 60°C overnight to remove the solvent, and store it in an argon-filled glove box. The SEM of the electrolyte powder is as follows Figure 2 The FT-IR of PAN, LLZTO and PAN-modified LLZTO is shown in 3.

[0068] Step 2: Polymerize dopamine on the PTFE surface. The specific operation is: add buffer salt tris(hydroxymethyl)aminomethane to the dopamine salt solution and adjust the pH to 8.5 to accelerate the polymerization of dopamine. KMnO4 is used as an oxidant, and 0.04 mol of KMnO4 solid and 0.018 mol of dopamine monomer are added to the above alkaline solvent. Then slowly add 30.00 g of PTFE pretreated in step 1. At 0°C, stir at high speed for 24 hours. After the reaction is completed, wash the obtained solid with water several times until the filtrate is clear and transparent, and then dry it under vacuum conditions at 100°C for 12 hours to obtain a PDA-modified PTFE composite adhesive.

[0069] Step 3: Preparation of solid electrolyte film. The specific operation is: the PAN-modified LLZTO electrolyte and the PDA-modified PTFE composite binder are uniformly mixed in a mass ratio of 97:3 by a rotary defoamer. Subsequently, the obtained mixture powder is ground in a special ball mill for 1 minute to obtain a microfibrillated mixture powder. Finally, the obtained microfibrillated mixture powder is set at 25°C with a double roller distance of 50μm on the roller press, and the roller press is rolled 15 times in both directions to reach 50μm to obtain a solid electrolyte film.

[0070] Embodiment 6

[0071] This embodiment provides a method for preparing a solid electrolyte battery

[0072] Step 1: Preparation of positive electrode battery cells. The specific operation is: lithium iron phosphate (LiFePO4), conductive carbon (Super P) and PDA-modified PTFE composite binder are mixed at 87:10:3 at 25°C for 2 hours to make an active mixture, and then mixed at 25°C for 20 minutes to make a powdered mixture; the powdered mixture is hot-rolled at 120°C into an active layer with a thickness of 80μm and placed on the current collector to obtain a positive electrode sheet.

[0073] Step 2: Assembly of solid-state battery. The specific operation is: use the solid electrolyte film prepared by LLZTO electrolyte modified by PAN and PTFE modified by PDA in Example 1 as the solid electrolyte of the battery, use the electrode sheet prepared in step 1 as the positive electrode of the battery, and the metal Li sheet as the negative electrode of the battery. Use a CR2032 button battery shell to assemble the solid-state battery in the order of positive electrode-solid electrolyte-negative electrode.

[0074] Embodiment 7

[0075] This embodiment provides a method for preparing a solid electrolyte battery:

[0076] Step 1: Preparation of positive electrode battery cells. The specific operation is: lithium iron phosphate (LiFePO4), conductive carbon (Super P) and PDA-modified PTFE composite binder are mixed at 80:10:10 at 25°C for 2 hours to make an active mixture, and mixed at 25°C for 20 minutes to make a powder mixture; the powder mixture is hot-rolled at 120°C into an active layer with a thickness of 80μm and placed on the current collector to obtain a positive electrode sheet.

[0077] Step 2: Assembly of solid-state battery. The specific operation is: use the solid electrolyte film prepared by LLZTO electrolyte modified by PAN and PTFE modified by PDA in Example 1 as the solid electrolyte of the battery, use the electrode sheet prepared in step 1 as the positive electrode of the battery, and the metal Li sheet as the negative electrode of the battery. Use a CR2032 button battery shell to assemble the solid-state battery in the order of positive electrode-solid electrolyte-negative electrode.

[0078] Comparative Example 1

[0079] Comparative Example 1 is basically the same as Example 6, except that in step 2 of Comparative Example 1, the PAN-modified LLZTO in step 2 of Example 6 is replaced by untreated LLZTO. The coulombic efficiency of the battery in the first three cycles of Comparative Example 1 and Example 6 is as follows: Figure 7 For specific test conditions, see Table 1.

[0080] Comparative Example 2

[0081] Comparative Example 2 is basically the same as Example 6, except that the PDA-modified PTFE composite binder in Example 6 is replaced with untreated PTFE. Figure 8 For specific test conditions, see Table 1.

[0082] The preparation conditions and proportions of representative embodiments and comparative examples are shown in Table 1.

[0083] Table 1

[0084]

[0085] like Figure 2 As shown in the SEM image of the electrolyte powder, the PAN@LLZTO particles are irregular, with no agglomeration and uniform distribution.

[0086] like Figure 3 As shown in the figure, compared with PAN, PAN@LLZTO has a -1 The CH bond and 2242cm -1 The -CN stretching vibration peak intensities at all locations decreased, indicating the successful preparation of PAN@LLZTO.

[0087] Figure 5 This is a physical picture of the solid electrolyte film. The film is smooth as a whole and is brown-yellow in color. Compared with the illustration, it can be seen that the film is very flexible, indicating that it can be mass-produced without sintering or applying external pressure.

[0088] Figure 6 Microscopic diagram of solid electrolyte film.

[0089] Depend on Figure 7 It can be seen that the impedance value of the solid-state battery prepared by PDA@PTFE is 4.9*10 3 Ω, the impedance value of solid-state battery made of PTFE is 9*10 3 Ω, indicating that PDA@PTFE has stronger ionic conductivity than PTFE, which helps to improve the performance of solid-state batteries.

[0090] Depend on Figure 8 It can be seen that the coulombic efficiency of the solid-state battery prepared by PDA@LLZTO in the first three cycles is 98%, 99% and 99%, respectively, which is significantly higher than that of the solid-state battery prepared by LLZTO (85%, 97%, 98%), indicating that the solid-state battery prepared by PDA@LLZTO has better cycle reversibility.

[0091] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0092] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a solid electrolyte film, characterized in that: The steps include: A. Preparation of polyacrylonitrile modified solid electrolyte particles: A1, dissolving polyacrylonitrile in dimethyl sulfoxide and performing high-energy ball milling process; A2, placing an inorganic solid electrolyte and a lithium salt in the above-mentioned ball-milled material and performing a high-energy ball milling process again; A3, adding 1-propanol as a precipitant to the material obtained in step A2, performing a final ball milling, and then centrifuging and drying the ball milled product to obtain polyacrylonitrile-modified solid electrolyte particles; Preparation of polydopamine-modified polytetrafluoroethylene composite binder: B1. Pre-treating polytetrafluoroethylene with a potassium permanganate / nitric acid mixed solution to form hydrophilic manganese oxide or manganese hydroxide covering polytetrafluoroethylene particles; B2, adding dopamine monomer and potassium permanganate in proportion to an alkaline solution with a pH of 8.5, and then slowly adding the polytetrafluoroethylene pretreated in step B1 to carry out a polymerization reaction. After the reaction is completed, ultrasonic washing with deionized water and vacuum drying are performed to obtain a polydopamine-coated polytetrafluoroethylene binder; Prepared into solid electrolyte film: C1. Using a rotary defoamer, the solid electrolyte modified with polyacrylonitrile and the polytetrafluoroethylene composite binder modified with polydopamine are uniformly mixed according to the mass ratio in a protective gas atmosphere; C2. Grinding the obtained mixture powder in a special ball mill for 3 minutes under a protective gas atmosphere to obtain a microfibrillated mixture; C3, rolling the microfibrillated mixture powder using a double-roll roller press under set parameters to fully fiberize the binder to obtain a solid electrolyte film; The protective gas in step C is one of argon, nitrogen and helium.

2. The method for preparing a solid electrolyte film according to claim 1, characterized in that: In step A2, the inorganic solid electrolyte is one of a sulfide solid electrolyte, an oxide solid electrolyte and a halide solid electrolyte; the lithium salt is one of lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium perchlorate, lithium tetrafluoroborate, lithium hexafluoroarsenate and lithium hexafluorophosphate.

3. The method for preparing a solid electrolyte film according to claim 1, characterized in that: In the step A, the mass ratio of polyacrylonitrile to the solid electrolyte is (1-3):

100.

4. The method for preparing a solid electrolyte film according to claim 1, characterized in that: In the step C1, based on the total mass of the solid electrolyte film, the mass of the solid electrolyte modified by polyacrylonitrile accounts for 97-99%, and the mass of the polytetrafluoroethylene modified by polydopamine accounts for 1-3%.

5. The method for preparing a solid electrolyte film according to claim 1, characterized in that: In the step C3, the set parameters involve temperature, rolling times, rolling direction and film thickness, the temperature is 25-80°C, the rolling times are 5-20 times, the rolling direction is unidirectional or bidirectional, and the film thickness is 50-150 μm.

6. A solid electrolyte film, characterized in that: The solid electrolyte film is obtained by the preparation method according to any one of claims 1 to 5.

7. A solid-state battery, characterized in that: The solid-state battery comprises an electrode sheet and the solid electrolyte film according to claim 6.

8. A solid-state battery according to claim 7, characterized in that: The electrode sheet comprises a current collector and an active layer on the current collector, wherein the active layer comprises an electrode active material, conductive carbon and a polytetrafluoroethylene composite binder modified by polydopamine.

9. A solid-state battery according to claim 8, characterized in that: In the active layer on the current collector, the polydopamine-modified polytetrafluoroethylene composite binder accounts for 1-10% of the mass of the active layer.

Citation Information

Patent Citations

  • Organic in-situ interface modified solid electrolyte and preparation method thereof

    CN113363560A

  • Oxide solid electrolyte sheet and preparation method and application thereof

    CN115117440A

  • Composite binder, electrode plate, preparation method of electrode plate, battery and electric device

    CN118398817A

  • Hot-Melt Pressure Sensitive Adhesive Composition and Uses Thereof

    US20210115238A1

  • Method for manufacturing solid secondary battery including composite electrolyte film

    US20220131181A1

Cited By

  • LLZO-based composite solid electrolyte prepared by solvent-free method as well as preparation method and application of LLZO-based composite solid electrolyte

    CN119852503A