Preparation method and application of electrolyte containing silane additive for lithium ion battery
By adding additives with specific silane-based structures to the lithium-ion battery electrolyte solution, the problem of insufficient performance of the solid electrolyte membrane is solved, the ratio and circulation performance of the lithium-ion battery are improved, and the lithium-ion transmission efficiency and stability are achieved.
Patent Information
- Application Number
- CN202410971831.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The carbonate-based electrolyte in existing lithium-ion batteries decomposes when the discharge voltage is lower than 1V, resulting in the generated solid electrolyte membrane that cannot meet the homogeneity of the negative electrode, good ion transport characteristics and high mechanical performance requirements, resulting in lithium-ion batteries. Poor performance, especially in high current charge and discharge and cycle stability.
Add additives with a specific silane structure to the electrolyte solution participate in the film formation process of the solid electrolyte membrane, change the composition of the membrane, thereby improving the lithium ion transmission efficiency and membrane stability, and improving the rate performance and cycling performance of the battery.
By using silane-based materials as additives, the rate performance and circulation performance of lithium-ion batteries are significantly improved, the stability of the solid electrolyte membrane is improved, and the capacity retention rate of the battery under high load conditions is significantly improved, and the cycle stability and mechanical properties are also increased. Improved.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The invention relates to a preparation method and application of an electrolyte for a lithium ion battery containing a silane additive, belonging to the technical field of lithium ion batteries. Background Art
[0002] The fact that lithium-ion battery technology won the Nobel Prize in Chemistry in 2019 reflects the society's recognition of lithium-ion batteries, and lithium-ion batteries will play a key role in mobile devices in the foreseeable future. The high reversibility of the negative electrode of lithium-ion batteries is an important basis for the successful development of lithium-ion batteries, and the high reversibility of the negative electrode benefits from the solid electrolyte interface generated by the electrolyte through chemical or electrochemical reactions. The structure of the solid electrolyte interface plays a vital role in determining the performance of the negative electrode of lithium-ion batteries. The solid electrolyte interface has many functions, including limiting further side reactions between the negative electrode and the electrolyte, regulating ion flux and promoting uniform ion conduction. The ideal solid electrolyte interface has the following characteristics: high ion conduction rate and high resistance; stable thickness at the nanoscale; high mechanical strength and toughness, able to withstand volume changes of the negative electrode; insoluble in the electrolyte, etc. A stable solid electrolyte interface is a prerequisite for good battery performance, and the quality of the interface layer greatly affects the performance of the battery.
[0003] The carbonate-based electrolyte widely used in lithium-ion batteries decomposes when the discharge voltage is <1V, producing a solid electrolyte interface film at the negative electrode. The generated solid electrolyte membrane is mainly composed of lithium carbonate, lithium fluoride and lithium alkyl carbonate in different proportions. In this membrane, a small amount of inorganic groups such as lithium carbonate and lithium fluoride are distributed in the organic salt component of lithium, forming the main component of the solid electrolyte membrane. This membrane cannot meet the requirements of homogeneity, good ion transport characteristics and high mechanical properties required by the negative electrode of lithium-ion batteries, resulting in unsatisfactory performance of lithium-ion batteries, mainly manifested in poor charge and discharge capacity under large currents and poor cycle stability.
[0004] In order to improve the performance of the battery, the present invention explores the direction of improving the quality of the solid electrolyte membrane. Adding additives to the electrolyte is a simple and effective method to improve the film-forming quality of the electrolyte.
[0005] The present invention attempts to improve the quality of the solid electrolyte membrane by adding a film-forming additive to the electrolyte, thereby enhancing the rate performance and cycle performance of the lithium-ion battery, which has practical significance for promoting the further development of lithium-ion batteries. Summary of the invention
[0006] The purpose of the present invention is to propose an electrolyte for lithium-ion batteries containing additives to overcome the above-mentioned problems. The additives can participate in the solid electrolyte membrane formation process to change the composition of the solid electrolyte membrane, thereby improving the lithium ion transmission efficiency and the stability of the solid electrolyte membrane, so that the lithium-ion battery has better rate performance and cycle performance.
[0007] In order to achieve the above object, the main technical solutions adopted by the present invention include:
[0008] Provided is an electrolyte containing an additive, which consists of a common electrolyte and an additive, wherein the additive is at least one of silane-based materials having a structure of the following formula (I).
[0009]
[0010] Wherein, R1 to R6 are each independently selected from a hydrogen atom, a halogen atom, a substituted or unsubstituted alkyl group, a substituted or unsubstituted aromatic group, etc.;
[0011] In the embodiment, R1 to R3 are the same group.
[0012] In the embodiment, R4 to R6 are the same group.
[0013] In an embodiment, the organic solvent is a mixed solvent formed by ethylene carbonate, diethyl carbonate and dimethyl carbonate, wherein the volume ratio of ethylene carbonate, dimethyl carbonate and diethyl carbonate is 1:1:1.
[0014] The method is simple to operate, easy to control, has a short process flow, low cost, and is easy to apply to industrial production.
[0015] Another object of the present invention is to provide a method for preparing the above-mentioned electrolyte.
[0016] (1) Ethylene carbonate, diethyl carbonate and dimethyl carbonate are mixed to obtain a mixed solvent, wherein the volume ratio of ethylene carbonate, dimethyl carbonate and diethyl carbonate is 1:1:1.
[0017] (2) The lithium salt and the solvent are mixed evenly to obtain a common electrolyte, wherein the concentration of the lithium salt is 0.1 to 2 mol / L.
[0018] (3) Adding the additive into a common electrolyte and mixing the mixture evenly to obtain the electrolyte.
[0019] Another object of the present invention is to provide an application of the electrolyte for the lithium ion battery, wherein the lithium ion battery comprises a positive electrode sheet, a negative electrode sheet and an electrolyte.
[0020] The negative electrode plate active material is at least one of a lithium plate or graphite or a silicon-carbon composite material.
[0021] The active material of the positive electrode plate is at least one of graphite, silicon-carbon composite material, or lithium iron phosphate, LiCoO2, LiMn2O4, LiNi x Co y Al 1-x-y O2、LiNi x Co y Mn 1-x-y At least one of O2, where 0≤x≤1, 0≤y≤1, 0≤1-xy≤1.
[0022] The electrolyte is the electrolyte obtained by the above preparation method.
[0023] The beneficial effects of the present invention are:
[0024] (1) The present invention uses at least one silane material as a lithium-ion battery electrolyte additive. The additive can participate in the solid electrolyte membrane formation process during the battery charging and discharging process, change the solid electrolyte membrane components, thereby promoting the lithium ion transmission rate, while improving the stability of the solid electrolyte membrane, and improving the rate performance and cycle performance of the lithium-ion battery.
[0025] (2) The additive provided by the present invention does not contain expensive raw materials and meets the low cost requirement of the electrolyte.
[0026] (3) The electrolyte provided by the present invention enables the lithium ion half-cell to have a higher capacity retention rate. Relative to the capacity at 0.5C, the retention rate at 1.5C is 84.7%, and the retention rate at 3C is 54.3%; after 1000 cycles at 1.5C, the capacity retention rate is 63.2%.
[0027] (4) The electrolyte provided by the present invention enables the lithium-ion full battery to have a higher capacity retention rate. Relative to the capacity at 0.2C, the retention rate at 0.5C is 94.1%, and the retention rate at 1C is 93.7%.
[0028] (5) The present invention provides a method for preparing an electrolyte for lithium ions. The method is simple to operate, easy to control, has a short process flow, low cost, and is easy to use for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 The figure shows the rate performance and cycle performance of Comparative Example 1 and Example 1.
[0030] Figure 2 The AC impedance test results of Comparative Example 1 and Example 1 are shown.
[0031] Figure 3 The results of rate performance tests of Comparative Example 2 and Example 2 are shown.
[0032] Figure 4 The figures are the capacity retention results of the rate tests of the comparative examples and embodiments. DETAILED DESCRIPTION
[0033] The following non-limiting embodiments may enable a person skilled in the art to more fully understand the present invention, but are not intended to limit the present invention in any way.
[0034] The test methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.
[0035] Example 1
[0036] A method for preparing an electrolyte for a lithium ion battery, the specific steps are as follows:
[0037] (1) In a glove box filled with argon, ethylene carbonate, dimethyl carbonate, and diethyl carbonate were taken respectively and mixed in a volume ratio of 1:1:1.
[0038] (2) Weigh a certain amount of lithium hexafluorophosphate and dissolve it in the solvent described in step (1) so that the concentration of lithium hexafluorophosphate in the solution is 0.1 to 2 mol / L.
[0039] (3) Add 1% to 20% by weight of an additive to the solution in step (2) and mix well.
[0040] (4) Using lithium sheets as negative electrode active materials, at least one of graphite and silicon-carbon composite materials as positive electrode active materials, and polypropylene diaphragms as diaphragms, adding the electrolyte prepared in step (3), and assembling a half-cell.
[0041] Example 2
[0042] A method for preparing an electrolyte for a lithium ion battery, the specific steps are as follows:
[0043] (1) In a glove box filled with argon, ethylene carbonate, dimethyl carbonate, and diethyl carbonate were taken respectively and mixed in a volume ratio of 1:1:1.
[0044] (2) Weigh a certain amount of lithium hexafluorophosphate and dissolve it in the solvent described in step (1) so that the concentration of lithium hexafluorophosphate in the solution is 0.1 to 2 mol / L.
[0045] (3) Add 1% to 20% by weight of an additive to the solution in step (2) and mix well.
[0046] (4) Using at least one of graphite or silicon-carbon composite materials as the negative electrode active material, polypropylene diaphragm as the diaphragm, lithium iron phosphate, LiCoO2, LiMn2O4, LiNix Co y Al 1-x-y O2、LiNi x Co y Mn 1-x-y At least one of O2 is used as a positive electrode active material, wherein 0≤x≤1, 0≤y≤1, 0≤1-xy≤1, and is added to the electrolyte prepared in step (3) to assemble a full battery.
[0047] Comparative Example 1
[0048] A method for preparing a basic electrolyte for a lithium ion battery, the specific steps are as follows:
[0049] (1) In a glove box filled with argon, ethylene carbonate, dimethyl carbonate, and diethyl carbonate were taken respectively and mixed in a volume ratio of 1:1:1.
[0050] (2) Weigh a certain amount of lithium hexafluorophosphate and dissolve it in the solvent described in step (1) so that the concentration of lithium hexafluorophosphate in the solution is 0.1 to 2 mol / L.
[0051] (3) Using lithium sheets as negative electrode active materials, at least one of graphite and silicon-carbon composite materials as positive electrode active materials, and polypropylene diaphragms as diaphragms, adding the electrolyte prepared in step (2), and assembling a half-cell.
[0052] Comparative Example 2
[0053] A method for preparing a basic electrolyte for a lithium ion battery, the specific steps are as follows:
[0054] (1) In a glove box filled with argon, ethylene carbonate, dimethyl carbonate, and diethyl carbonate were taken respectively and mixed in a volume ratio of 1:1:1.
[0055] (2) Weigh a certain amount of lithium hexafluorophosphate and dissolve it in the solvent described in step (1) so that the concentration of lithium hexafluorophosphate in the solution is 0.1 to 2 mol / L.
[0056] (3) Use at least one of graphite or silicon-carbon composite materials as the negative electrode active material, polypropylene diaphragm as the diaphragm, lithium iron phosphate, LiCoO2, LiMn2O4, LiNi x Co y Al 1-x-y O2、LiNi x Co y Mn 1-x-y At least one of O2 is used as a positive electrode active material, wherein 0≤x≤1, 0≤y≤1, 0≤1-xy≤1, and is added to the electrolyte prepared in step (2) to assemble a full battery.
[0057] Effect Example 1
[0058] The lithium ion batteries prepared in Example 1 and Comparative Example 1 were tested for charge and discharge performance. The test results are as follows: Figure 1 shown.
[0059] In the rate test, Example 1 has a higher capacity retention rate at the same current density and has better rate performance. The specific results are as follows: Figure 4 shown.
[0060] In the cycle test, Example 1 exhibited a higher capacity retention rate at the same current density and had better cycle stability. Specifically, the capacity retention rate was 63.2% after 1000 cycles at 1.5C.
[0061] The lithium ion batteries prepared in Example 1 and Comparative Example 1 were subjected to AC impedance tests. The test results are as follows: Figure 2 The solid electrolyte membrane in Example 1 has higher quality and exhibits smaller impedance.
[0062] Effect Example 2
[0063] The lithium ion batteries prepared in Example 2 and Comparative Example 2 were subjected to rate charge and discharge tests. The test results are as follows: Figure 3 As shown. Example 2 has a higher capacity retention rate and shows better rate performance. The specific results are shown in Figure 4 shown.
Claims
1. An electrolyte, characterized in that: including organic solvents, lithium salts and additives; The additive is one of the compounds shown in formula (I) Wherein, R1 to R6 are each independently selected from a hydrogen atom, a halogen atom, a substituted or unsubstituted alkyl group, or a substituted or unsubstituted aromatic group; The mass percentage of the additive in the electrolyte is 1% to 20%; The organic solvent is a mixed solvent formed by ethylene carbonate, diethyl carbonate and dimethyl carbonate.
2. The electrolyte according to claim 1, wherein: R1 to R3 are the same group.
3. The electrolyte according to claim 1, wherein: R4 to R6 are the same group.
4. The electrolyte according to claim 1, wherein: The concentration of the lithium salt in the electrolyte is 0.1 to 2 mol / L.
5. A method for preparing a lithium-ion battery electrolyte, characterized in that: Mixing the lithium salt and the organic solvent to obtain a common electrolyte; The additive is added into the common electrolyte and mixed evenly to obtain the electrolyte.
6. The preparation method according to claim 5, characterized in that: The lithium salt used in the electrolyte is lithium hexafluorophosphate.
7. The preparation method according to claim 5, characterized in that: The volume ratio of ethylene carbonate, dimethyl carbonate and diethyl carbonate in the organic solvent of the electrolyte is 1:1:
1.
8. The preparation method according to claim 5, characterized in that: The mass ratio of the electrolyte additive in the electrolyte is 1% to 20%.
9. A lithium-ion battery, characterized in that: The invention comprises a positive electrode sheet, a negative electrode sheet and the electrolyte according to any one of claims 1 to 4 or the electrolyte prepared by the preparation method according to claim 5.
10. The lithium-ion battery according to claim 9, wherein: The negative electrode plate is a lithium plate; the positive electrode material is at least one of graphite and silicon-carbon composite material.
11. The lithium-ion battery according to claim 9, wherein: The active material of the negative electrode is graphite; the positive electrode material is lithium iron phosphate, LiCoO2, LiMn2O4, LiNi x Co y Al 1-x-y O2、LiNi x Co y Mn 1-x-y At least one of O2, where 0≤x≤1, 0≤y≤1, 0≤1-xy≤1.
Citation Information
Patent Citations
A lithium battery electrolyte and a battery containing the electrolyte
CN109088102A
Silicon-based negative electrode lithium ion battery electrolyte and preparation method thereof
CN110718716A
Lithium ion battery electrolyte, preparation method and lithium ion battery
CN111540954A
Lithium ion electrolyte containing grafted polysilane additive
CN112886057A