Method for producing a coated object comprising a coating with tunable properties

By identifying the characteristic groups of different areas of the car body and applying a matching coating composition, the conflict between coatings in improving stone impact resistance and chemical resistance is solved, achieving a more efficient coating method, reducing costs and Material consumption improves the overall characteristics of coated objects.

CN118922255APending Publication Date: 2024-11-08BASF COATINGS GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028840.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-23
Filing Date
2023-03-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the existing automotive coating technology, there is a conflict between high stone impact resistance and high chemical resistance, which leads to the coating that will inevitably reduce the other when improving one characteristic, increase the cost of coating, and it is difficult to improve at different times. The overall mechanical and chemical properties of the coated object.

Method used

By identifying the characteristic groups of different areas of the car body and applying a coating composition with adjustable characteristics for each area, ensuring that the characteristics of the coating match the target area, including the use of different adhesives and hardener components to prepare the coating with Coatings with high stone impact resistance, chemical resistance, scratch resistance and light resistance.

Benefits of technology

It is achieved without increasing the total cost, improving the overall mechanical and chemical characteristics of the coated object, reducing material consumption and volatile organic matter generation, and improving the adaptability and performance of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922255A_ABST
    Figure CN118922255A_ABST
Patent Text Reader

Abstract

The invention relates to a method for producing a coated object comprising a plurality of target regions, wherein at least parts of the plurality of target regions are coated with a coating having adjustable properties. The coatings are produced by applying a coating composition to the target areas such that the properties of the resulting coatings match the respective sets of properties of the target areas, i.e. The coatings are produced in such a way that the same coating is not present on the target areas having different sets of properties. The method according to the invention allows the properties of the coating, such as flexibility, hardness, scratch resistance, light resistance, to be matched to the set of properties required for the corresponding target area. Since the properties of these coatings can match the set of properties required for the corresponding target area, this results in higher overall mechanical and / or chemical properties of the coated object. Furthermore, the invention relates to the use of the method according to the invention for producing a coated object comprising a target region requiring a coating having different properties. Finally, the invention relates to a system for applying, with an application device, at least two coating compositions producing a coating having adjustable properties to an object comprising a plurality of target regions, at least portions of which have different sets of properties.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a method for producing a coated object including a plurality of target areas, wherein at least a portion of the plurality of target areas is coated with a coating having adjustable properties. These coatings are produced by applying a coating composition to the target areas so that the properties of the resulting coatings match the property groups of the corresponding target areas, i.e., the coatings are produced in such a way that the same coating does not exist on target areas having different property groups. The method of the present invention allows the properties of the coatings, such as flexibility, hardness, scratch resistance, and light resistance, to match the property groups required for the corresponding target areas. Since the properties of these coatings can match the property groups required for the corresponding target areas, this allows the coated object to have higher overall mechanical and / or chemical properties. In addition, the present invention relates to the use of the method of the present invention for preparing a coated object including a target area that requires a coating having different properties. Finally, the present invention relates to a system for applying at least two coating compositions that produce a coating having adjustable properties to an object including a plurality of target areas using an application device, wherein at least a portion of the plurality of target areas have different property groups. Prior art

[0002] In the painting of high-quality goods, such as automobiles, the paint is usually applied in multiple layers. In such a multi-layer paint system for automobile chassis, a primer is first applied, which is intended to improve the adhesion between the substrate and the subsequent layers and, if the substrate is prone to corrosion, is also used to protect the substrate from corrosion. In addition, the primer ensures the improvement of the surface characteristics by covering any rough places and structures present in the substrate. Especially in the case of metal substrates, a primer-surfacer is usually applied to the primer, the task of which is to further improve the surface characteristics and improve the stone chip resistance. Typically, one or more coloring layers and / or effect layers are applied to the primer-surfacer, which is called a color paint. Finally, a clearcoat is usually applied to the color paint, which ensures the desired shiny appearance and protects the paint system from environmental influences. The combination of a color paint and a clearcoat is also called a color-plus-clear composite coating.

[0003] When the exterior coating must have the best visual appearance as well as superior durability and weatherability, a color plus clear system is usually selected. Therefore, the automotive industry has been widely using color plus clear composite coatings, especially for automotive body panels. The clearcoat for the color plus clear system is usually applied at a film thickness significantly higher than the film thickness (film build) when the colored paint is applied. Such higher clearcoat film thickness is a feature of the system, which helps to achieve the desired appearance and / or durability of the entire color plus clear system. For example, an automotive OEM (OEM) plant typically applies a clearcoat composition at a wet film thickness of 20.3 to 152.4 μm (0.8 to 6.0 mils) to provide a cured clearcoat film thickness of 12.7 to 88.9 μm (0.5 to 3.5 mils). In contrast, pigmented paint compositions are typically applied at a wet film thickness of 5.1 to 101.6 μm (0.2 to 4.0 mils) to provide a cured paint film thickness of 2.5 to 50.8 μm (0.1 to 2.0 mils).

[0004] Minimum performance requirements for clearcoat coating compositions intended for use on automotive body panels include high adhesion levels, scratch and abrasion resistance, chip resistance, moisture resistance, and weatherability as measured by QUV, etc. Clearcoat compositions must also be able to provide a visual appearance characterized by high gloss, distinctness of image (DOI), and smoothness. Finally, such coatings must also be easy to apply in a manufacturing environment and be resistant to application defects.

[0005] However, varnish layers with a higher stone chip resistance traditionally show reduced chemical resistance due to the higher flexibility required for their higher stone chip resistance. For scratch resistance or light resistance, the same conflicting requirements also occur, because varnish layers with a higher scratch resistance and / or light resistance are usually more expensive to produce than varnish layers with a lower scratch resistance and / or light resistance. Therefore, in terms of efficiency, it is desirable to produce a varnish layer with high scratch resistance and / or high light resistance only on the target areas where high scratch resistance and / or light resistance is required, while leaving other target areas covered by a less expensive varnish layer with a lower scratch resistance and / or light resistance.

[0006] Obviously, high stone resistance and high chemical resistance are conflicting requirements. The same is true for achieving good scratch resistance and / or good light resistance without significantly increasing the overall cost of the coating. A method of obtaining sufficient overall properties is to carefully control the properties of the coating obtained by applying the coating material to the object to ensure that the coating shows a proper balance between stone resistance and chemical resistance or a proper balance between scratch resistance and / or light resistance and the overall cost of the coated object. This method is currently used in the automotive manufacturing industry (hereinafter also referred to as OEM), where only one varnish quality has a good balance between stone resistance and chemical resistance or between scratch resistance and / or light resistance and the overall cost of coating. Although the use of the varnish quality produces sufficient mechanical and chemical properties, it is impossible to increase stone resistance without simultaneously reducing chemical resistance, and vice versa. The same applies to increasing scratch resistance and / or light resistance without simultaneously increasing the overall cost of coating, and vice versa.

[0007] Applying different coating materials that produce coatings with properties that are tailored to the properties of the area of ​​the object to be coated is advantageous, since in this way the properties of the coatings can be optimized independently of one another to obtain a higher quality in terms of mechanical and / or chemical properties of the resulting coated object. Coatings with tailorable properties should be easy to produce from a limited number of coating compositions, and these coating compositions should be suitable for use in combination with conventional application equipment. Furthermore, the adjusted properties of the coatings should allow a more efficient use of the relevant coating composition in terms of material consumption, since their properties are adjusted to the properties of the respective target area, and unadjusted coatings that produce a higher film thickness to achieve the same result are superfluous.

[0008] Purpose

[0009] The object of the present invention is therefore to provide a method which allows the properties of a coating to be matched to the set of properties of a corresponding target area of ​​an object on which it is present, such as stone chip resistance, chemical resistance, scratch resistance, light resistance, in order to improve the overall mechanical and chemical properties of the coated object. The production of a coating with properties adjusted to the properties of the corresponding target area of ​​an object should allow a lower consumption of the coating composition used for its production, thus making the method more efficient and reducing the generation of volatile organics during the curing of the applied coating material. Finally, the method should be carried out with commonly used application equipment.

[0010] Technical Solutions

[0011] This problem is solved by the subject matter claimed in the claims and also by preferred embodiments of the subject matter as described below.

[0012] Thus, a first subject of the invention is a method for producing an object comprising a plurality of target areas, at least some of which have different sets of properties and are coated with at least two coatings having adjustable properties, the method comprising

[0013] (a) identifying at least two target regions and a set of characteristics associated with each identified target region, wherein at least two of the target regions have different sets of characteristics,

[0014] (b) providing at least two different coating compositions (C i ) i=1,…,n , wherein each coating composition (C 1 , …, C n ) produces a coating (CL) having properties matching the different property groups identified in step (a) 1 , …, CL n ),as well as

[0015] (c) each coating composition (C) provided in step (b) 1 , …, C n ) is applied to the target area associated with the matching feature set.

[0016] The method described above is also referred to below as the method of the invention and is therefore the subject matter of the present invention. Preferred embodiments of the method of the invention are evident from the following description and also from the dependent claims.

[0017] The inventive method allows the characteristics of the coating to be matched with the characteristic group of the corresponding target area of ​​the object. For example, a coating with high flexibility is produced on the target area of ​​the object that needs high stone resistance, such as the front of the car, and a coating with low flexibility but high chemical resistance is produced on the target area that needs low stone resistance, but high chemical resistance, such as the roof of the car. In another example, only a coating with high scratch resistance or high light resistance is produced on the target area that needs high scratch resistance, such as the side of the car or the target area that needs high light resistance, such as the roof of the car. This allows to reduce the total cost associated with the inventive method because it avoids producing a coating with the optimized characteristics and related to higher costs on the target area that does not need the optimized characteristics. Compared with the coating with balanced characteristics, the production of a coating with characteristics that match the characteristic group of the target area allows to reduce the overall film thickness. This allows to reduce the emissions generated during the drying of the coating composition and obtain a more effective coating method. In addition, matching the characteristics of the coating with different characteristic groups of the target area of ​​the object produces higher quality in terms of the mechanical and / or chemical characteristics of the resulting coated object.

[0018] A further subject of the invention is the use of the method according to the invention for producing coated objects comprising target areas for which a coating with different properties is desired.

[0019] Another subject of the invention is a system for applying at least two coating compositions producing a coating with adjustable properties to an object comprising a plurality of target areas, at least some of which have different sets of properties, by means of an application device, the system comprising:

[0020] - an application device comprising a nozzle;

[0021] - a storage device for storing application instructions and optionally mixing ratio instructions;

[0022] - one or more data processors configured to execute the application instructions and optionally the mixing ratio instructions to control the application device; and

[0023] - at least two reservoirs, which are in fluid communication with the application device and are configured to contain at least two components (A i ) i=1,…,n and optionally at least one hardener component B, each component A i or each A i A mixture of A and B produces a coating CL with properties that match the property set of the target area. i , or is configured to contain at least two types of coatings (CL i ) i=1,…,n The coating composition (C i ) i=1,…,n , CL for each coating i has characteristics that match the characteristic set of the target region,

[0024] wherein the application device is configured

[0025] o Receive the components from the reservoir (A i ) i=1,…,n and optionally the hardener component B and mixing the components in the nozzle based on the mixing ratio instructions (A i ) i=1,…,n , optionally mixed with the hardener component B, and

[0026] ○ Based on the application instruction, the obtained coating composition (C i ) i=1,…,n Discharging to a target area having a matching set of properties to form at least two coatings; or

[0027] wherein the applicator is configured to

[0028] o receiving the at least two coating compositions (Ci ) i=1,…,n ,as well as

[0029] ○ Based on the application instruction, the coating composition (C i ) i=1,…,n Discharged to at least two target areas having matching sets of properties to form at least two coatings.

[0030] Another subject of the invention is a system for applying at least two varnish coating compositions producing a varnish coating with adjustable properties to an object comprising a plurality of target areas, at least some of which have different sets of properties, using an application device, wherein each applied coating composition produces a varnish coating with properties matching the sets of properties of at least two target areas, the system comprising:

[0031] - an application device comprising a nozzle;

[0032] - a storage device for storing application instructions and related mixing ratio instructions;

[0033] - one or more data processors configured to execute the application instructions and the mixing ratio instructions to control the application device; and

[0034] - at least three reservoirs, which are in fluid communication with the application device and are configured to contain at least two components (A i ) i=1,…,n and at least one hardener component B,

[0035] wherein the application device is configured

[0036] o Receive the components from the reservoir (A i ) i=1,…,n and the hardener component B and based on these mixing ratio instructions one or more components (A i ) i=1,…,n Mixed with the hardener component B to prepare a clear coating composition (C 1 , …, C n ),and

[0037] ○ Based on these for preparing the corresponding varnish composition C i These application instructions are associated with the mixing instructions to pass the resulting coating composition (C i ) i=1,…,n Discharged to a varnish having a composition C corresponding to i The properties of the corresponding varnish layers produced match the property sets of the target areas to form at least two varnish coatings.

[0038] Another subject of the invention is a system for coating an object comprising a plurality of target areas, at least some of which have different sets of properties, with at least two varnish coatings, each varnish coating having properties matching a different set of properties of these target areas, said system comprising:

[0039] a) a computing unit configured to determine control data for controlling the application device by:

[0040] obtaining data relating to the object to be coated and determining target area position data for at least some of the plurality of target areas and target area characteristic data for each of the target areas based on the obtained data relating to the object,

[0041] obtaining data relating to the components for preparing the clearcoat coating composition to be applied and determining mixing ratio data based on the determined target area property data,

[0042] generating control data (including the determined target area location data and the associated mixing ratio data) and providing the generated control data to one or more data processors configured to control the application device,

[0043] b) one or more data processors configured to execute the provided control data to control the application device,

[0044] c) an application device comprising a nozzle and at least three reservoirs in fluid communication with the application device and configured to contain at least two components (A i ) i=1,…,n and at least one hardener component B, the application device being configured to:

[0045] - receiving the one or more components and the at least one hardener component B from the reservoir and mixing the received one or more components and the at least one hardener component B in the nozzle based on the mixing ratio data to prepare a clearcoat coating composition (C 1 , …, C n ),as well as

[0046] - Each prepared clear coating composition (C i ) i=1,…,n Discharging to the target area associated with the target area position data associated with the mixing ratio data for preparing the corresponding varnish composition to form a varnish coating having properties matching the properties of the target area. DETAILED DESCRIPTION

[0047] definition:

[0048] First, some terms used in the context of the present invention will be explained.

[0049] As used herein, unless otherwise indicated, the grammatical articles "a", "an", and "the" are intended to include "at least one" or "one or more", even though "at least one" or "one or more" are explicitly used in certain instances. Thus, these articles are used in this specification to refer to one or more than one (i.e., "at least one") of the grammatical objects of the article. By way of example and not limitation, "a component" means one or more components, and thus, potentially, more than one component is contemplated and may be employed or used in the implementation of the described embodiments. Further, use of a singular noun includes the plural, and use of a plural noun includes the singular, unless the context of the usage requires otherwise.

[0050] In this description of the invention, for convenience, "polymer" and "resin" are used interchangeably to encompass resins, oligomers and polymers.

[0051] The term "poly(meth)acrylate" stands for both polyacrylates and polymethacrylates. Thus, poly(meth)acrylates may consist of acrylates and / or methacrylates and may contain further ethylenically unsaturated monomers such as, for example, styrene or acrylic acid. The term "(meth)acryloyl" includes within the meaning of the present invention methacryloyl compounds, acryl compounds and mixtures thereof, respectively.

[0052] The term "multiple target areas" refers to at least two target areas present on an object to be coated. A target area is a defined area on an object, i.e., an area with a defined size. The term "at least some of the multiple target areas have different sets of properties" means within the meaning of the present invention that at least two of the multiple target areas have different sets of properties. Thus, all target areas present on an object have different sets of properties, i.e., the properties of each target area are different from the properties of each other target area, or some target areas have the same set of properties, while other target areas have different sets of properties. The term "set of properties" refers to a single property or multiple properties associated with the target area. These properties can be selected from the orientation of the target area relative to other target areas, the position of the target area on the object, or a combination thereof. The term "different sets of properties" means within the meaning of the present invention that at least one property or multiple properties associated with the corresponding target area are different from the properties contained in the set of properties associated with another target area. Therefore, the term "different sets of properties" does not necessarily mean that all properties included in the set of properties are different from the properties contained in another set of properties.

[0053] The term "object coated with at least two coatings having adjustable properties" refers to an object coated with at least two coatings and wherein the properties of these coatings have been adjusted to match the property set of the target area on which each coating is present. This can be achieved, for example, by using defined coating materials that, after being applied to the respective target areas, produce coatings having properties that match the property set of the target area on which the coating has been produced. For example, a coating material containing a plasticizer to produce a flexible coating is produced on a target area where a coating with high flexibility is required, such as a vertically oriented target area, while a coating material that does not contain or contains a lower amount of plasticizer is applied to a target area where a coating with high hardness is required, such as a horizontally oriented target area to produce high chemical resistance. In another example, a coating material containing a high amount of UV filters and / or UV stabilizers to produce a coating with high UV stability is produced on a target area where a coating with high UV stability is required, such as a horizontally oriented target area, while a coating material containing a lower amount of UV filters and / or UV stabilizers and therefore having a lower price is applied to the remaining target area, such as a vertically oriented target area. In yet another example, a coating material that produces a coating having high hardness and UV resistance is applied to a target area requiring a coating having high scratch resistance and UV resistance, such as an exterior target area of ​​a vehicle, while a coating material that has a lower price and produces a coating having lower scratch resistance and UV resistance is applied to an interior target area of ​​the vehicle.

[0054] The term “(C i ) i=1,…,n " represents a series of coating compositions C, such as C 1 , C 2 , C 3 , …, C n , where n is the last member of the series. The same applies to the term "(CL i ) i=1,…,n ”, which represents a series of coating CLs.

[0055] The term "each coating has properties matching a different set of properties" means within the meaning of the present invention that the properties of each coating completely match one set of properties of the target area. For example, if an object is to be coated with 2 coatings and the object comprises a target area with two different sets of properties, the properties of the first coating match the first set of properties and the properties of the second coating match the second set of properties, and vice versa.

[0056] The term "applying each coating composition to a target area associated with a matching set of properties" refers to an application process in which each coating composition is applied to a target area having a set of properties that matches the properties of one or more coatings produced from the corresponding coating composition. Thus, for example, if coating composition C 1 Generate a 1 , A 3 and A 5 Feature Group SP 1 Matching characteristics SP 1 Coating CL 1 , then in one step or in multiple steps, in the target area A 1 , A 3 and A 5 Apply the coating composition C 1 To produce coating CL 1 However, applying a coating composition to one or more than one defined target area does not exclude that parts of adjacent target areas having a different set of properties may be inadvertently coated with the coating composition due to an overspray effect. However, it is not intentional to apply the same coating composition to target areas having different sets of properties.

[0057] In the context of the present invention, a "hardener component" is a material comprising at least one cross-linking component that is capable of reacting with chemical functional groups present in at least one compound, such as at least one binder, contained in at least one component provided in step (a) of the method of the present invention. The cross-linking component is reacted with the binder present in at least one component provided in step (a) so that a network structure is formed when the applied coating composition is cured.

[0058] In the context of the present invention and according to DIN EN ISO 4618:2007-03, "binders" are non-volatile components of coating compositions that are free of pigments and fillers. However, in the following, this expression is mainly used with respect to specific physically and / or chemically curable polymers, examples being polyurethanes, polyesters, polyethers, polyureas, polyacrylates, polysiloxanes and / or copolymers of said polymers. The non-volatile fraction can be determined according to DIN EN ISO 3251:2018-07 using a starting weight of 1.0 g at 130° C. for 60 min.

[0059] As used herein, the term "water-based coating composition" refers to a coating composition comprising a water fraction of at least 20 wt.%, preferably at least 25 wt.%, very preferably at least 50 wt.%, based in each case on the total weight of the coating composition. The water fraction is preferably 40 to 60 wt.%, more particularly 45 to 70 wt.%, very preferably 50 to 80 wt.%, based in each case on the total weight of the coating composition. In contrast, the term "solvent-based coating composition" refers to a coating composition comprising an organic solvent fraction of at least 20 wt.%, preferably at least 25 wt.%, very preferably at least 45 wt.%, based in each case on the total weight of the coating composition. The organic solvent fraction is preferably 40 to 70 wt.%, more particularly 45 to 65 wt.%, very preferably 50 to 60 wt.%, based in each case on the total weight of the coating composition.

[0060] As used herein, the term "drying" the applied coating composition refers to evaporating the solvent from the applied coating composition. Drying can be carried out at ambient temperature or by using high temperature. However, drying does not produce a ready-to-use coating film, i.e., a cured coating film as described below, because the coating film is still soft or sticky after drying. Accordingly, "curing" the applied coating composition or the coating film obtained by drying the applied coating composition refers to converting such a composition or film into a ready-to-use state, i.e., a state in which the object provided with the corresponding coating can be transported, stored and used as expected. More particularly, the cured coating is no longer soft or sticky, but has been adjusted to a solid coating, and even if further exposed to curing conditions, its characteristics, such as hardness or adhesion to the object do not undergo any further significant changes. Curing can be carried out at a higher temperature than that used for drying the applied coating composition and / or for a longer time.

[0061] The measurement methods to be used in the context of the present invention for determining certain characteristic variables can be found in the Examples section. Unless otherwise explicitly indicated, these measurement methods are to be used to determine the corresponding characteristic variables. In the context of the present invention, when an official standard is cited without any indication of the official effective date, it is implied that the standard version in force on the date of submission is cited, or the latest effective version is cited at that point in time when no effective version exists.

[0062] All film thicknesses reported in the context of the present invention are to be understood as dry film thicknesses. It is therefore in each case the cured film thickness. Thus, where it is reported that a coating material is applied at a certain film thickness, this means that the coating material is applied in such a way that after curing the stated film thickness is obtained.

[0063] All temperatures stated in the context of the present invention are to be understood as the temperature of the room in which the object or coated object is located. Therefore, this does not mean that it is required that the object itself has the temperature in question.

[0064] The method of the present invention:

[0065] The method of the invention allows the preparation of a coated object comprising at least two coatings with adjustable properties by matching the properties of the coatings with different sets of properties of target areas of the object, so that a coating with defined properties, like high stone chip resistance, high chemical resistance, high scratch resistance and / or high light resistance, is present on those target areas of the object where said defined properties are required. For example, a coating producing high stone chip resistance, i.e. a flexible coating with low chemical resistance, is present on target areas where high stone chip resistance is required (such as the front or sides of a car), while a coating with high chemical resistance, i.e. a coating with high hardness and therefore low flexibility, is present on target areas where high chemical resistance is required (such as the roof of a car). Matching the set of properties of the target area with the properties of the coating allows obtaining improved mechanical and / or chemical properties of the resulting coated object and reduced material consumption during the production of the corresponding coating.

[0066] According to a preferred embodiment of the method, the adjustable properties of the coating include the hardness, scratch resistance, light resistance, appearance and / or adhesion of the coating. The hardness of the coating can be adjusted, for example, by using a commonly known plasticizer or by using an adhesive, so as to provide a cured coating with higher flexibility, such as a flexible polyester resin. Scratch resistance can be improved by using a silanized adhesive (which provides additional crosslinking during the hardener so that the crosslinking density and thus the total hardness are improved) or by using any of the nano-scale inorganic materials, organic materials, or inorganic / organic hybrid materials known in the art. The light resistance of the coating can be improved, for example, by adding a larger amount or a specific type of UV stabilizer or UV filter to the coating material for preparing the corresponding coating. The term "appearance" refers to the appearance of the varnish layer and includes gloss, haze, distinctness of image (DOI), orange peel, mottling, transparency or a combination thereof.

[0067] Step (a):

[0068] Step (a) of the method of the present invention comprises identifying at least two target regions and a set of characteristics associated with each identified target region, wherein at least two of the identified target regions have different sets of characteristics. In one example, the object comprises at least two target regions, each target region having a different set of characteristics. In another example, the object comprises a plurality of target regions, wherein a portion of the plurality of target regions have the same set of characteristics, and a remaining portion of the plurality of target regions have different sets of characteristics.

[0069] The identification of the target area and the associated set of characteristics may be performed according to several methods, some of which are presented below in a non-limiting manner. According to an embodiment of step (a), step (a) comprises on a computing device having a display and one or more user input devices adapted to detect user input:

[0070] (a-1) displaying a user interface including the object on the display,

[0071] (a-2) detecting user input indicating identification of at least two target regions and a set of characteristics associated with each target region on the object,

[0072] (a-3) determining the target regions and each set of characteristics associated with each identified target region based on the detected user input, and

[0073] (a-4) providing the data determined in step (a-3) to the application device and / or displaying the data determined in step (a-3) within the user interface.

[0074] The computing device includes a processor and a memory in addition to a display and at least one user input device. The term "memory" may refer to physical and other computer-readable media for carrying or storing computer-executable instructions and / or data structures. Such a computer-readable medium may be any available medium that can be accessed by a general or special computer system. The computer-readable medium may include a physical storage medium that stores computer-executable instructions and / or data structures. The physical storage medium includes computer hardware, such as RAM, ROM, EEPROM, solid-state drive ("SSD"), flash memory, phase change memory ("PCM"), optical disk storage, disk storage or other magnetic storage devices, or any other (multiple) hardware storage devices that can be used to store program codes in the form of computer-executable instructions or data structures, which (these) hardware storage devices can be accessed and executed by a general or special computer system to implement the functions disclosed in the present invention. The computer-executable instructions allow the computing device to detect user inputs to determine the target area and each characteristic group associated with each identified target area based on the detected user inputs and provide the identified data to the application device or display.

[0075] The term "processor" refers to any logic circuit configured to perform the basic operations of a computer or system, and / or generally refers to a device configured to perform calculations or logical operations. In particular, a processing device or a computer processor may be configured to process basic instructions that drive a computer or system. As an example, a processing device or a computer processor may include at least one arithmetic logic unit ("ALU"), at least one floating point unit ("FPU") (such as a math coprocessor or a digital coprocessor), a plurality of registers (specifically registers configured to supply operands to the ALU and store the results of the operations) and a memory (such as L1 and L2 cache memory). In particular, a processing device or a computer processor may be a multi-core processor. In particular, a processing device or a computer processor may be or may include a central processing unit ("CPU"). A processing device or a computer processor may be a ("GPU") graphics processing unit, a ("TPU") tensor processing unit, a ("CISC") complex instruction set computing microprocessor, a reduced instruction set computing ("RISC") microprocessor, a very long instruction word ("VLIW") microprocessor, or a processor implementing other instruction sets or a processor implementing a combination of instruction sets. The processing means may also be one or more special-purpose processing devices, such as an application-specific integrated circuit ("ASIC"), a field-programmable gate array ("FPGA"), a complex programmable logic device ("CPLD"), a digital signal processor ("DSP"), a network processor, etc. The methods, systems, and devices described herein may be implemented as software in a DSP, a microcontroller, or any other auxiliary processor, or as hardware circuits within an ASIC, CPLD, or FPGA. It should be understood that, unless otherwise specified, the term processing means or processor may also refer to one or more processing devices, such as a distributed system of processing devices located on multiple computer systems (e.g., cloud computing), and is not limited to a single device. Terminology

[0076] "Processor" and "computer processor" are used synonymously herein. A processor is configured to execute computer-executable instructions stored in a memory.

[0077] The display may be any display device generally known in the prior art, such as a mobile or portable display device. The display device may also include a user input device, such as a touch screen. In this case, the display detects user input and provides the detected user input to the computing device.

[0078] In step (a-1), a user interface including an object is displayed on a display. The object may be any virtual 2D or 3D object, such as a car or a part thereof. Preferably, the virtual object is similar to the actual object to be coated to improve user comfort during identification of target areas and associated characteristic groups. The user interface may further include a toolbar that allows the user to mark the identified target areas and assign labels indicating associated characteristic groups to the identified target areas.

[0079] In step (a-2), the computing device detects user input indicating identification of at least two target areas and a characteristic group associated with each target area on the object. The user input can be detected by a processor of the computing device or by a processor of the display. In the latter case, the detected input is provided to the computing device via a communication interface. The user input is performed using an input device such as a touch screen, a mouse, a keyboard, a touch pad or a combination thereof. The user input may include drawing a border around each target area or may include marking points on the border of each target area. The user input further includes a characteristic group associated with each identified target area. This can be accomplished, for example, by adding a label associated with the corresponding characteristic group to the corresponding target area or by entering the characteristic group in a field associated with the corresponding target area.

[0080] In step (a-3), the processor of the computing device determines the target areas and each characteristic group associated with each identified target area based on the detected user input. The determination of the target areas can be performed by determining the boundaries of each target area based on the user input and assigning a number to each target area. The determination of the characteristic group associated with each target area can be performed by determining the type of label or by determining the data input by the user in the previous step. The identified target areas are preferably associated with the associated characteristic groups, for example by storing a unique number indicating the corresponding target area with data about the characteristic group on a data storage medium, such as an internal memory of the computing device.

[0081] In step (a-4), the data determined in step (a-3) are provided to the application device and / or displayed in the user interface. In the first case, the computing device is connected to the application device via a communication interface, and the application device uses the data to automatically apply the coating composition to the corresponding target area, as described later. Displaying the determined target area and each related characteristic group in the user interface allows the user to check whether the target area is correctly marked and whether the correct characteristic group is assigned. The user can change the displayed data and the processor can detect the change and determine the target area and the related characteristic group based on the user input of the correction. The processor can be configured to automatically update the user interface after determining a new target area and / or a new characteristic group based on the detected correction. After the determined data is associated with a unique ID, the data can be stored on a data storage medium to facilitate retrieval when the data is used again.

[0082] In an alternative embodiment of step (a), step (a) includes providing a user interface containing an object, the object including at least two marked target areas and an indication of a set of characteristics associated with the marked target areas. The user interface can be generated using data of a virtual 2D or 3D object, data about target areas present on the object and sets of characteristics assigned to the target areas. In one example, the user interface is generated by loading previously stored data about the virtual object, the assigned target areas and the associated characteristics and displaying the data within the user interface. Such data can be generated using steps (a-1) to (a-3) described previously.

[0083] In yet another alternative embodiment, step (a) includes visually determining at least two target regions and a set of characteristics associated with each identified target region, wherein at least two target regions have different sets of characteristics. "Visually determining the target region" refers to determining the region without using a computing device, such as by drawing the target region on an object printed on paper or by marking the target region on a real pre-existing object.

[0084] Step (b):

[0085] In step (b) of the method of the present invention, at least two different coating compositions (C i ) i=1,…,n Each coating composition (C 1 , …, C n ) produces, after application to the object, a coating (CL) having properties matching the different sets of properties identified in step (a) 1 , …, CL n ). Therefore, each coating composition (C) provided in step (b) 1, …, C n ) produces a coating having properties matching the property set identified in step (a). In addition, each coating composition (C 1 , …, C n ) is preferably not applied to a target area having a set of properties that do not match the properties of the coating obtained from each applied coating composition. 1 , …, C n ) is preferably applied only to target areas having the same set of properties, wherein said set of properties matches the properties of the resulting corresponding coating. This allows obtaining a coating having properties that match the properties of the corresponding target area, resulting in higher overall mechanical and / or chemical properties of the coated object. Furthermore, since the optimized coating can be produced with a reduced film thickness compared to a coating that is not optimized in terms of its properties, material consumption is reduced.

[0086] The coating composition (C) provided in step (a) i ) i=1,…,n :

[0087] The coating composition (C) provided in step (b) i ) i=1,…,n The coating composition may be a liquid solvent-based or water-based coating composition. Preferably, the coating composition C provided in step (a) 1 and each additional coating composition C provided when step (a) is repeated at least once x The coating composition C provided in step (b) is a liquid solvent-based coating composition. 1 It is a coating composition based on liquid solvent.

[0088] The coating composition (C) provided in step (b) i ) i=1,…,nCan be transparent, translucent or opaque.Opaque coating compositions are colored coating compositions, which have a light transmittance less than 4% when applied to an object as measured according to ASTM D 1003-00 (Procedure A) using CIE standard light source D65 at a film thickness of 15 to 18 microns.Suitable opaque coating compositions include paint compositions comprising one or more coloring pigments and / or effect pigments with a concentration high enough to achieve the above-mentioned light transmittance.By contrast, translucent coating compositions have a light transmittance of at least 4% when applied to an object.Therefore, translucent coating compositions are neither completely transparent nor opaque.Compared with transparent coating compositions, translucent coating compositions contain coloring pigments and / or effect pigments and / or matting agents, so that they are not completely transparent.Translucent coating compositions can be colored translucent coating compositions, such as colored varnish compositions.Transparent coating compositions preferably include varnish compositions.

[0089] According to a preferred embodiment, at least one coating composition provided produces a coating with high stone chip resistance and at least one further coating composition provided produces a coating with high chemical resistance, and / or wherein at least one coating composition provided produces a coating with high scratch resistance and at least one further coating composition provided produces a coating with lower scratch resistance, and / or wherein at least one coating composition provided produces a coating with high light resistance and at least one further coating composition provided produces a coating with lower light resistance. This allows the properties of the resulting coating to be matched to the location of the target area on the substrate, resulting in higher overall mechanical and / or chemical properties of the coated object.

[0090] Adhesives:

[0091] In the examples, each coating composition (C 1 , …, C n ) comprises at least one binder. Each of the coating compositions (C 1 , …, C n The at least one binder present in the coating composition (C) may be the same as the at least one binder present in the other provided coating compositions, or each provided coating composition (C) may be the same as the at least one binder present in the other provided coating compositions. 1 , …, C n ) may be different from one or more binders present in the other provided coating compositions. It may be advantageous if each coating composition comprises at least one identical binder, i.e., each provided coating composition contains at least one binder that is the same as one or more binders present in the other provided coating compositions. This allows for the composition to be prepared from components (A) as described later. 1 , …, A n) to prepare a coating composition without causing the application of the resulting coating composition or the resulting coating CL i The properties of the components have undesirable incompatibilities that have a negative impact.

[0092] Suitable binders include (i) poly(meth)acrylates, more particularly hydroxy-functional and / or carboxylate-functional and / or amine-functional poly(meth)acrylates, (ii) polyurethanes, more particularly hydroxy-functional and / or carboxylate-functional and / or amine-functional polyurethanes, (iii) polyesters, more particularly polyester polyols, (iv) polyethers, more particularly polyether polyols, (v) copolymers of the aforementioned polymers, and (vi) mixtures thereof. Particularly preferably, at least one binder is selected from hydroxy-functional poly(meth)acrylates and / or polyesters.

[0093] The one or more hydroxy-functional (meth)acrylates may contain, in polymerized form, at least one unsaturated monomer M1 containing at least one acid group, at least one unsaturated aliphatic and / or alicyclic monomer M2, at least one unsaturated aromatic monomer M3 and at least one unsaturated hydroxyl-containing monomer M4. In the context of the present invention, it is said that in the case where the one or more hydroxy-functional (meth)acrylates contain the components M1 to M4 in polymerized form, this means that these specific components are used as starting compounds for the preparation of the one or more hydroxy-functional (meth)acrylates in question. Since the monomers M1 to M4 can be polymerized via their unsaturated moieties, the one or more hydroxy-functional (meth)acrylates preferably contain unsaturated moieties previously present in the monomers M1 to M4 in the form of CC single bonds (in other words in their correspondingly reacted form).

[0094] Suitable unsaturated monomers comprising at least one acid group M1 include (meth)acrylic acid.

[0095] The at least one unsaturated aliphatic monomer M2 may be selected from alkyl (meth)acrylates, more preferably alkyl (meth)acrylates. 1 -C 22 Alkyl esters, even more preferably (meth)acrylic acid C 1 -C 14 Alkyl esters such as (meth) acrylic acid C 3 Alkyl esters, (meth) acrylic acid C 4 Alkyl esters, (meth) acrylic acid C 5 Alkyl esters, (meth) acrylic acid C 6 Alkyl esters, (meth) acrylic acid C 7 Alkyl esters and (meth) acrylic acid C 13 Alkyl esters, very preferably butyl (meth)acrylate and / or esters of (meth)acrylic acid 13.0.

[0096] Suitable unsaturated alicyclic monomers M2 include cycloalkyl (meth)acrylates, such as cycloalkyl (meth)acrylates. 5 -C 7 - Alkyl esters, in particular cyclohexyl (meth)acrylate.

[0097] The at least one unsaturated aromatic monomer M3 may be chosen from styrene.

[0098] Suitable unsaturated hydroxyl-containing monomers M4 include hydroxyl-containing (meth)acrylates, more preferably hydroxyl-containing C 1 -C 12 Alkyl (meth)acrylates, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxyisopropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, hydroxyisobutyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate, in particular 2-hydroxyethyl (meth)acrylate and 3-hydroxypropyl (meth)acrylate.

[0099] Hydroxy-functional (meth)acrylates can be prepared in an organic solvent by polymerizing the above-mentioned unsaturated monomers M1 to M4 in the presence of a free radical initiator. The free radical initiator can be selected from tert-amyl peroxide compounds such as 1,1-di(tert-amylperoxy)cyclohexane, tert-amyl peroxyesters such as tert-amyl peroxy, ethyl-3,3-di(tert-amylperoxy)butyrate and tert-amyl peroxyacetate, other peroxides such as di-tert-butyl peroxide, dicumyl peroxide, cumene hydroperoxide and tert-butyl perbenzoate, and azo compounds such as 2,2'-azobis(2-methylbutyronitrile). The amount of free radical initiator used will vary within an amount of about 0.5 to 10 wt.-%, preferably 1 to 4 wt.-%, based on the total weight of the monomers M1 to M4.

[0100] In some embodiments, at least one adhesive is a polyester. Suitable polyesters can be prepared by reacting a polyfunctional acid or anhydride compound or a mixture of monofunctional and polyfunctional acid or anhydride compounds with a polyfunctional alcohol. Typical acid compounds include alkyl, alkylene, aryl alkylene, and aromatic monocarboxylic acids, dicarboxylic acids, and anhydrides; however, acids or anhydrides with higher functionality can also be used. If trifunctional compounds or higher functionality compounds are used, these can be used in mixtures with monofunctional carboxylic acids or anhydrides of monocarboxylic acids (such as versatic acid, fatty acids, or neodecanoic acid). Illustrative examples of acid- or anhydride-functional compounds, or anhydrides of such compounds, suitable for forming polyester groups include phthalic acid, phthalic anhydride, isophthalic acid, terephthalic acid, hexahydrophthalic acid, tetrachlorophthalic anhydride, hexahydrophthalic anhydride, pyromellitic anhydride, succinic acid, azelaic acid, adipic acid, 1,4-cyclohexanedicarboxylic acid, citric acid, and trimellitic anhydride.

[0101] The polyol component for making polyester has a hydroxyl functionality of at least 2. The polyol component can contain mono-, di- and tri-functional alcohols, as well as alcohols with higher functionality. Diols are typical polyol components. When some branching of polyester is required, alcohols with higher functionality can be used, and mixtures of diols and triols can be used as polyol components. However, in some cases, highly branched polyesters are undesirable due to the influence on coating (such as reduced flow) and the undesirable influence on cured film (such as reduced anti-chip property and smoothness). Examples of useful polyols include but are not limited to ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, butanediol, glycerol, trimethylolpropane, trimethylolethane, pentaerythritol, neopentyl glycol, 2,2,4-trimethyl-1,3-pentanediol, 1,6-hexanediol, 1,4-cyclohexanedimethanol, hydrogenated bisphenol A and ethoxylated bisphenol. The method for making polyester is well known. Polyesters are typically formed by heating the polyol and polyfunctional acid components together, with or without catalysis, while removing byproduct water to drive the reaction to completion. A small amount of solvent, such as toluene, may be added to azeotropically remove the water.

[0102] At least one binder is preferably present in each of the provided coating compositions (C ) in a total amount of 10 to 70 wt.-%, preferably 20 to 65 wt.-%, more preferably 30 to 60 wt.-%, very preferably 40 to 50 wt.-%. 1 , …, C n ), in each case based on the coating composition C provided i If more than one binder is present, for example a mixture of a hydroxy-functional poly(meth)acrylate and a polyester, the above amounts refer to the total amount of binder present in the respective coating composition provided and therefore to the sum of the amounts of the hydroxy-functional poly(meth)acrylate and the one or more polyesters.

[0103] Crosslinking agent:

[0104] Each coating composition (C 1 , …, C n ) may contain at least one crosslinking agent. The presence of at least one crosslinking agent is generally optional and is only necessary if the coating composition contains one or more binders having functional groups that are not self-reactive. In the case where the coating compositions are formulated as 2K coating compositions, they are prepared by mixing a base component (usually comprising a resin, additives and optionally a crosslinking agent that is not reactive with the binder component at storage temperature) and at least one hardener component containing a crosslinking agent prior to application. In one example, a coating composition C is provided iThe at least one crosslinking agent present in the at least one crosslinking agent present in the other provided coating compositions is the same. This may be preferred to avoid the possibility of crosslinking by mixing at least two components (A i ) i=1,…,n Incompatibility occurs when preparing a coating composition, as described below. In another example, each coating composition (C 1 , …, C n ) comprises at least one cross-linking agent that is different from one or more cross-linking agents present in other provided coating compositions.

[0105] At least one crosslinking agent is preferably capable of reacting with the coating composition C i Preferably, the at least one crosslinking agent is capable of reacting with functional groups of at least one compound present in the at least one binder.

[0106] In the case where the functional groups of the adhesive are active hydrogen, especially OH, the curing agent can be an aminoplast or a polyisocyanate, wherein polyisocyanates are preferred. Suitable polyisocyanates include organic polyisocyanates containing aliphatic, alicyclic, araliphatic and / or aromatically bonded free isocyanate groups. Polyisocyanates having 2 to 5 isocyanate groups per molecule and having a viscosity of 100 to 10,000 mPa*s, preferably 100 to 5,000 mPa*s and especially 100 to 2,000 mPa*s (at 23°C) are preferably used. Where appropriate, a small amount, preferably 1 to 25 wt.-% of an organic solvent based on the linear polyisocyanate, can be added to the polyisocyanate in order to improve the ease of incorporation of the polyisocyanate and, where appropriate, reduce the viscosity of the polyisocyanate to a level within the above range. Examples of suitable solvent additives for polyisocyanates include ethoxyethyl propionate, amyl methyl ketone, and butyl acetate. In addition, the polyisocyanates may have been conventionally hydrophilic or hydrophobic modified. Other examples of suitable polyisocyanates are polyisocyanates containing isocyanurate, biuret, allophanate, iminooxadiazinedione, carbamate, urea and / or uretdione groups. For example, polyisocyanates containing carbamate groups are obtained by reacting some isocyanate groups with polyols, such as trimethylolpropane and glycerol. Preference is given to using aliphatic or cycloaliphatic polyisocyanates, in particular hexamethylene diisocyanate, dimer and trimer hexamethylene diisocyanate, isophorone diisocyanate, 2-isocyanatopropylcyclohexyl isocyanate, dicyclohexylmethane 2,4′-diisocyanate, dicyclohexylmethane 4,4′-diisocyanate or 1,3-bis(isocyanatomethyl)cyclohexane, such as the diisocyanates derived from dimer fatty acids sold under the trade name DDI 1410 by Henkel, i.e. 1,8-diisocyanato-4-isocyanatomethyloctane, 1,7-diisocyanato-4-isocyanatomethylheptane or 1-isocyanato-2-(3-isocyanatopropyl)cyclohexane, or mixtures of these polyisocyanates.

[0107] When the functional group is an amine, the curing agent may be a polyisocyanate, a polyepoxide or a polyanhydride; when the functional group is a carboxylic acid, the curing agent may be a polyepoxide or a polyanhydride; when the functional group is an epoxy, the curing agent may be a polyacid or a polyamine.

[0108] Suitable crosslinkers include aminoplast resins and / or polyisocyanates, preferably aminoplast resins and aliphatic or cycloaliphatic polyisocyanates, very preferably aminoplast resins and hexamethylene diisocyanate and / or dimer and / or trimer hexamethylene diisocyanate.

[0109] Sag Control Agent (SCA):

[0110] The coating composition C provided in step (b) i At least one of the coating compositions may further contain at least one sag control agent (SCA) to adjust the thixotropic rheological behavior of the coating composition. SCA affects the sag-leveling properties of the coating composition because the SCA particles tend to form a loose percolation network under low shear stress by controlled flocculation. Under high shear stress (e.g., during spraying of the coating composition), the SCA network is damaged and the effect of SCA addition on high shear viscosity is almost zero because SCA is typically used in low concentrations. After application, the wet coating composition is subjected to low (gravity) shear stress. Under these low shear conditions, the SCA network gradually forms, resulting in an increase in viscosity. This shear-thinning behavior of the SCA-modified coating composition is advantageous because it improves the sag resistance of the paint. Due to the relatively slow formation rate of the SCA network, the SCA-modified coating composition is generally thixotropic. Thus, one or more provided coating compositions containing a higher amount of SCA have better sag resistance than one or more provided coating compositions containing a lower amount of SCA or no SCA (i.e. containing a total amount of SCA of less than 1 wt.-%, preferably 0 wt.-%, based on the total weight of the coating composition). However, one or more provided coating compositions containing a lower amount of SCA or no SCA have better leveling properties. Thus, the addition of SCA can be used to adjust the sag resistance and / or leveling properties of each provided coating composition so that these properties match the orientation of the target area. For example, a coating composition applied on a horizontally oriented target area contains a small amount of or no SCA to improve the leveling properties, while a coating composition applied on a vertically oriented target area contains a higher amount of SCA to improve sag resistance and avoid sag of the applied coating composition. "Vertically oriented" as used herein refers to a surface that is substantially parallel to the direction of gravity, i.e. at an angle of 90°±45° relative to the earth's surface, more preferably at an angle of 90°±30° relative to the earth's surface. "Horizontally oriented" refers to a surface that is substantially perpendicular to the direction of gravity, ie at an angle of 180°±45° relative to the earth's surface, more preferably at an angle of 180°±30° relative to the earth's surface.

[0111] SCA is generally anisotropic colloidal particles formed by crystallizing urea molecules. Urea molecules can be obtained by reacting isocyanate compounds with primary or secondary amines, optionally in the presence of a resin, such as a (meth) acrylate resin. Isocyanate compounds are isocyanate functional polymers, such as isocyanate functional (meth) acrylic polymers, or can be generally known polyisocyanates. The reaction between isocyanate compounds and primary or secondary amines can be generally carried out in any arbitrarily selected manner by combining reaction components, optionally in the presence of a resin. The reaction can be carried out at a temperature in the range of 20°C to 120°C, more particularly in the range of 25°C to 95°C. Typically, primary or secondary amines are directly added to isocyanate compounds, optionally in the presence of a catalyst, such as a tin compound, at a desired reaction temperature. The reaction continues until the isocyanate is completely consumed. In the case of reacting in the presence of a resin, the isocyanate compound and the primary or secondary amine are added to the resin together or in sequence.

[0112] It is preferred within the present invention that the sag control agent (SCA) is selected from polymeric sag control agents. The term "polymeric sag control agent" refers to an SCA obtained by reacting an isocyanate functional polymer with a primary or secondary amine or by reacting a polyisocyanate with a primary or secondary amine in the presence of at least one resin. Thus, SCA prepared by reacting a polyisocyanate with an amine is not covered by the term "polymeric sag control agent".

[0113] The polymeric sag control agent (SCA) can be obtained by reacting a primary or secondary amine with an isocyanate compound in the presence of a hydroxyl-functional poly(meth)acrylate. Suitable polyisocyanates that can be used to form SCA include blocked or unblocked aliphatic, alicyclic, heterocyclic, aromatic di-, tri-, polyisocyanates or combinations thereof. Examples of suitable polyisocyanates may include 1,6-hexamethylene diisocyanate, 2,2,4-trimethylhexane-1,6-diisocyanate, 2,4,4-trimethylhexane-1,6-diisocyanate, cyclohexyl-1,4-diisocyanate, isophorone diisocyanate, an adduct of 1 molecule of 1,4-butanediol and 2 molecules of isophorone diisocyanate, an adduct of 1 molecule of 1,4-butanediol and 2 molecules of hexamethylene diisocyanate, dicyclohexylmethane-4,4′-diisocyanate, xylene diisocyanate, 1,3,5-trimethyl-2,4-bis(isocyanatomethyl)benzene, toluene diisocyanate, diphenylmethane-4,4′-diisocyanate, an adduct of hexamethylene diisocyanate, an adduct of isophorone diisocyanate, and an adduct of toluene diisocyanate. Isocyanurate trimers of diisocyanates may also be suitable.In some embodiments, aliphatic polyisocyanates are used, such as hexamethylene diisocyanate.

[0114] Examples of primary amines include benzylamine, ethylamine, n-propylamine, sec-propylamine, n-butylamine, sec-butylamine, tert-butylamine, n-pentylamine, α-methylbutylamine, α-ethylpropylamine, β-ethylbutylamine, hexylamine, octylamine, decylamine, stearylamine, cyclohexylamine, aniline and hexamethylenediamine. Examples of suitable secondary amines include dibutylamine, diethylamine, diisopropylamine, diethanolamine and diisopropanolamine. These amines generally contain no more than 30 carbon atoms and preferably 1 to 18 carbon atoms. Amines containing one or more primary or secondary amino groups and one or more ether groups and / or hydroxyls are also suitable. For example, ethanolamine, 6-aminohexanol, p-methoxybenzylamine, methoxypropylamine, 3,4-dimethoxyphenyl-ethylamine, 2,5-dimethoxyaniline, furfurylamine, tetrahydrofurfurylamine can be used. A mixture of the amines mentioned above can also be used. In certain embodiments, aromatic primary amines are used, such as benzylamine.

[0115] Suitable hydroxy-functional poly(meth)acrylates contain, in polymerized form, at least one unsaturated monomer M1 comprising at least one acid group, at least one unsaturated aliphatic monomer M2, at least one unsaturated aromatic monomer M3 and at least one unsaturated hydroxyl-containing monomer M4.

[0116] Suitable unsaturated monomers comprising at least one acid group M1 include (meth)acrylic acid.

[0117] The at least one unsaturated aliphatic monomer M2 may be selected from alkyl (meth)acrylates, more preferably alkyl (meth)acrylates. 1 -C 22 Alkyl esters, even more preferably (meth)acrylic acid C 1 -C 14 Alkyl esters such as (meth) acrylic acid C 3 Alkyl esters, (meth) acrylic acid C 4 Alkyl esters, (meth) acrylic acid C 5 Alkyl esters, (meth) acrylic acid C 6 Alkyl esters, (meth) acrylic acid C 7 Alkyl esters and (meth) acrylic acid C 13 Alkyl esters.

[0118] The at least one unsaturated aromatic monomer M3 may be chosen from styrene.

[0119] Suitable unsaturated hydroxyl-containing monomers M4 include hydroxyl-containing (meth)acrylates, such as hydroxyl-containing (meth)acrylate 2-hydroxyethyl (meth)acrylate, 2-hydroxyisopropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, hydroxyisobutyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate. 1 -C 12 Alkyl (meth)acrylate.

[0120] The hydroxy-functional poly(meth)acrylate particularly preferably contains (meth)acrylic acid, butyl (meth)acrylate and / or (meth)acrylic acid ester 13.0, styrene and 2-hydroxyethyl (meth)acrylate in polymeric form.

[0121] Suitable weight ratios of monomers M1:M2:M3:M4 include 1:50:50:30 to 1:30:20:10.

[0122] The hydroxy-functional poly(meth)acrylates can be prepared as described previously for the hydroxy-functional poly(meth)acrylate binders by free-radical polymerization of the monomers M1 to M4.

[0123] The polymeric sag control agent (SCA) may have an average molecular weight M of 3,000 to 50,000 g / mol, preferably 4,000 to 30,000 g / mol, very preferably 5,000 to 15,000 g / mol, as determined by GPC using polystyrene as an internal standard. w .

[0124] The viscosity of the sag control agent may be in the range of 500 to 4,000 mPa*s, preferably 700 to 3,000 mPa*s, very preferably 1,000 to 2,500 mPa*s (25° C., 10 / s, Z3) (DIN ISO 2884-1:2006-09).

[0125] The provided coating compositions that do not contain a polymeric sag control agent or contain a lower amount of a polymeric sag control agent preferably also contain a hydroxyl-functional poly(meth)acrylate used to prepare the polymeric sag control agent compared to the provided coating compositions that contain a higher amount of a polymeric sag control agent. This allows the composition to be prepared from components (A) as described later. 1 , …, A n ) to prepare the provided coating compositions without the occurrence of incompatibilities which could result in clogging of application equipment during application of the coating composition or degradation of the optical quality of the resulting coating.

[0126] Preferably, sag control agents (SCA), in particular polymeric sag control agents, are present in a total amount of 0.1 to 40 wt.-%, preferably 2 to 30 wt.-%, more preferably 3 to 20 wt.-%, very preferably 4 to 15 wt.-%, in each case based on the respective provided coating composition C i According to each coating composition C provided i The amount of SCA in each coating composition C i Having good leveling properties (low or no SCA) or good sag resistance (high SCA) as previously described.

[0127] Additional additives besides SCA:

[0128] In addition to SCA, at least one coating composition C is provided i It may further include at least one additive other than the sag control agent (SCA).

[0129] In one embodiment, all coating compositions (C 1 , …, C n ) further comprises at least one additive, in particular a similar additive. This allows the composition (A) to be composed of the components described later. 1 , …, A n ) to prepare the provided coating compositions without incompatibility occurring during the preparation of the provided coating compositions.

[0130] In another example, only part of the provided coating compositions comprises an additional additive, while the other part of the provided coating compositions does not contain said additive (ie contains 0 wt.-% of the additional additive based on the total weight of the respective coating composition).

[0131] Suitable additives other than sag control additives include crosslinkers, light stabilizers, leveling agents, UV absorbers, pigments, free radical scavengers, slip additives, polymerization inhibitors, defoamers, wetting agents, adhesion promoters, flow control agents, film-forming aids such as cellulose derivatives, fillers, rheology control additives, flame retardants, and / or water scavengers, in particular crosslinkers, light stabilizers and leveling agents.

[0132] Suitable leveling agents include silicon-containing leveling agents, such as silicon-containing leveling agents having the following structural formula:

[0133]

[0134] in

[0135] R represents hydrogen, an alkyl residue, an alkylaryl residue, a glycol residue, a hydroxyl group, a hydroxyalkyl group, an amino group or an aminoalkyl residue, and

[0136] n and m are positive integers respectively.

[0137] Representative silicon-containing leveling agents are dimethylpolysiloxane (R=H in the above formula) and modified silicone leveling agents, wherein R in the above formula is an alkyl group such as methyl, ethyl, propyl, etc., an alkyl aryl group such as methyl aryl, ethyl aryl, etc., a diol residue, a hydroxyl group, a hydroxyalkyl group such as hydroxymethyl, hydroxyethyl, and an amino group.

[0138] In a preferred embodiment, each coating composition (C 1 , …, C n) differ only in that the corresponding resulting coating (C 1 , …, C n ) that match the set of properties identified in step (a). At least one solvent can be used to compensate for a lack of ingredients in one coating composition compared to the other coating composition provided. In the case of a solvent-based coating composition, the at least one solvent can be an organic solvent commonly used in solvent-based coating compositions, such as solvent naphtha. This approach avoids incompatibilities during the preparation of the coating in the overspray area and thus reduces the negative impact on the overall appearance of the coated object.

[0139] In one example of this preferred embodiment, only two coating compositions C are provided. 1 and C 2 , wherein one of the two coating compositions provided contains a higher amount of a flexible polyester resin to provide a coating with enhanced flexibility and stone chip resistance but reduced chemical resistance, while the other coating composition provided contains a lower amount of a flexible polyester resin to provide a coating with enhanced hardness and chemical resistance but reduced stone chip resistance.

[0140] The coating composition can be provided in step (b) in a variety of ways. According to a first embodiment of step (b), step (b) comprises

[0141] (b-1) providing at least two components (A) having different characteristics i ) i=1,…,n and optionally at least one hardener component B,

[0142] (b-2) Selecting the components A provided in step (b-1) i to produce a coating CL having properties matching the set of properties identified in step (a) i ,

[0143] (b-3) optionally selecting a mixing ratio for the at least one hardener component B provided in step (b-1), and

[0144] (b-4) mixing component A in the mixing ratio selected in step (b-2) and optionally (b-3) i , optionally mixed with the at least one hardener component B to provide the coating composition C i , the coating composition produces a coating CL having properties matching the set of properties identified in step (a) i .

[0145] The term “(A i ) i=1,...,n " represents a series of components A, such as A1 , A 2 , A 3 , ..., A n , where n is the last member of the series. The term "component" refers to a single ingredient or a mixture of at least two ingredients.

[0146] If the component (A) provided in step (b-1) i ) i=1,…,n If, when applied, does not produce a corresponding coating matching the set of properties identified in step (a), then according to this embodiment at least two coating compositions (C i ) i=1,…,n This may be preferred. This may be the case if the components provided in step (b-1) produce a coating having properties that are too high / low compared to the properties that need to match the set of properties identified in step (a) (e.g. the location of the corresponding target area on the object). In order to produce a coating having properties that match the set of properties identified in step (a), at least some of the components provided in step (b-1) must be mixed.

[0147] The hardener component B preferably contains a i At least one crosslinking agent that reacts the functional groups of the compounds present in step (b-1) with each other. Suitable crosslinking agents include polyisocyanate compounds as described earlier. During the preparation of the coating composition, the use of the hardener component B is generally optional and is only used if the coating composition is composed of a base component (i.e., by mixing the component (A) provided in step (b-1) with the component (A) provided in step (b-2). 1 , …, A n ) and at least one hardener component B. In the 2K coating composition, the component (A) provided in step (b-1) 1 , …, A n ) contains an adhesive having a non-self-reactive functional group, or the provided component (A 1 , …, A n ) is too low / small to achieve sufficient crosslinking during curing of the applied coating composition.

[0148] In step (b-2), the mixing ratio for at least part of the components provided in step (b-1) is selected so that a coating having properties matching the set of properties identified in step (a) can be produced. The properties of the coating may be predefined properties and may depend, for example, on the location of the target area to which the respective coating composition is intended to be applied in step (c).

[0149] Step (b-2) may comprise determining the desired properties of the respective coating and selecting a mixing ratio for at least part of the components provided in step (b-1) such that upon applying the coating composition obtained from step (b-4) on the respective target area of ​​the object, a resulting coating CL is obtained. i The properties of the coating may include determining the orientation and / or position of a target area on the object to be coated with the coating composition in step (c) and selecting a mixing ratio to obtain a coating with properties suitable for the determined orientation and / or position. In one example, the mixing ratio may be the same as component A. i The composition and the characteristic groups associated with the target area are correlated and can be provided to the user performing the method of the present invention in paper form or in electronic form. In another example, the mixing ratio can be related to component A. i The characteristic group associated with the target area is associated with each other and can be stored in a database. A processing device that can access the database can provide the determined characteristic group of the target area and the component A to the processing device. i Instructions (such as formula, the number indicates component A i The appropriate mixing ratio is determined and displayed to the user or provided to the mixing device based on the provided mixing ratio and the information about component A. i The coating composition is automatically mixed based on the data.

[0150] In one example, if a coating with higher flexibility and stone chip resistance is desired, a higher fraction of the component provided in step (b-1) and containing a large amount of flexible polyester is selected in step (b-2). In another example, if a coating with higher hardness and chemical resistance is desired, a lower fraction of the component provided in step (b-1) and containing a large amount of flexible polyester is selected in step (b-2). This allows the properties of the resulting coating to be adjusted according to the corresponding property groups of different target areas, such as the position, by selecting an appropriate mixing ratio between at least two components provided in step (b-1). This allows the properties of the coating to be changed according to the corresponding property groups of the target areas and allows, for example, the flexibility of the coating to be adjusted according to the position of the target area on the object. Changing the mixing ratio to achieve the desired properties of the coating allows a large number of coatings with defined properties to be produced by providing only two components in step (b-1), namely a component containing an adhesive and a component containing a flexible polyester resin and / or a component that increases scratch resistance and / or a component containing a light stabilizer. This allows reducing the amount of coating composition that needs to be stored to obtain comparable results in terms of the overall mechanical and / or chemical properties of the coated object, thereby reducing the need for large storage capacity.

[0151] At least one component A provided in step (b-1) iAt least one binder as described above may be included. Particularly preferably, each component (A 1 , …, A n ) comprises at least one binder, in particular at least one of the previously described binders. Each component A provided i The at least one binder present in the n-i At least one binder present in the same or each component A provided i The at least one binder present in the n-i The binders present in the i Contains at least one identical binder, namely each component A provided i Containing other coating compositions provided by A n-i It may be advantageous if at least one binder is the same as the binder present in the mixture. This is done by mixing the components (A) provided in step (b-4). 1 , …, A n ) increases compatibility and thus reduces the occurrence of unwanted incompatibilities that have a negative impact on the resulting properties of the coating obtained from step (c). Suitable binders and total amounts of binders are the binders and total amounts previously described.

[0152] The mixing ratios selected in step (b-2) and optionally in step (b-3) are preferably by volume. i A volume:volume mixing ratio of 8:1 to 1:1, preferably 4:1 to 1:1, of a mixture of and at least one hardener component B is selected in step (b-3). In case more than one hardener component B is provided in step (b-1), the above mixing ratio is valid for each hardener component provided in step (b-1). The use of these mixing ratios ensures that the resulting coating composition is sufficiently hardened after application to the corresponding target area, thereby avoiding an adverse effect on the overall optical appearance due to insufficient hardening of the formed coating.

[0153] According to a second alternative embodiment of step (b), at least two coating compositions (C i ) i=1,…,n The method comprises preparing at least two different compositions (C) by mixing at least two coating material components. i ) i=1,…,n , so that the coating obtained from the corresponding coating composition (C i ) i=1,…,nEach has properties that match the different property groups identified in step (a). The term "coating material ingredients" refers to compounds commonly used to prepare coating materials, such as solvents, pigments, binders, additives, etc. The desired properties of the coating that match the property groups identified in step (a) can be obtained by using commonly known flexible resins, modified binders, light stabilizers, etc.

[0154] In one embodiment, the coating material composition comprises

[0155] -Base component BC i ,and

[0156] - At least one hardener component B.

[0157] The base component may be selected so that the properties of the resulting coating match the property set identified in step (a). For example, the base component may contain a high amount of a flexible polyester resin to produce a coating with high flexibility and, therefore, high stone chip resistance. The coating composition may be applied to a target area where high stone chip resistance is desired. In another example, the base component may contain a low amount of a flexible polyester resin or may not contain any flexible polyester to produce a coating with high hardness and, therefore, high chemical resistance (but low stone chip resistance). The coating composition may be applied to a target area where high chemical resistance but low stone chip resistance is desired. In another example, the base component may contain particles, such as SiO 2 Particles and nanoparticles to produce a coating with scratch resistance. The coating composition can be applied to a target area requiring high scratch resistance. In another example, the base component can contain a low amount of the particles or can not contain any of the particles to produce a coating with low scratch resistance. The coating composition can be applied to a target area requiring low scratch resistance. In another example, the hardener component can be selected so that the properties of the resulting coating match the property group identified in step (a). For example, hardener component B can contain at least one compound containing one or more hydrolyzable silane groups to produce a coating with high scratch resistance. The coating composition prepared by the hardener B can be applied to a target area requiring a coating with high scratch resistance. In another example, hardener component B may not contain the compound containing one or more hydrolyzable silane groups to produce a coating with lower scratch resistance. The coating composition prepared by the hardener B can be applied to a target area requiring a coating with low or lower scratch resistance.

[0158] At least one base component BC i It can be mixed with at least one hardener component B in a volume:volume mixing ratio of 8:1 to 1:1, preferably 4:1 to 1:1.

[0159] In step (b-4), component A i Mix, optionally with hardener component B or with base component BC i The mixing with the hardener component B to prepare the at least two coating compositions can be carried out in many ways known in the prior art.

[0160] In one example, each component A is mixed in a selected mixing ratio before supplying the resulting coating composition to the application equipment. i , optionally mixed with a hardener component B. In the coating composition, at least one base component BC i In the case of preparation by mixing with at least one hardener component B, the at least one base component BC is mixed with at least one hardener component B before the resulting coating composition is supplied to the application device. i Mixed with at least one hardener component B. Component (A 1 , …, A n The order of mixing of component A) and optionally hardener component B is not critical and can be varied. For example, component A) can be mixed before mixing the obtained mixture with hardener component B (if appropriate). 1 , …A n ), or the components (A 1 , …A n ) in the second step, and in the second step, component (A 1 , …A n ) is mixed with the hardener component B, or vice versa. Thereafter, the mixtures obtained in steps 1 and 2 are combined. Mixing can be performed manually or using a generally known mixing device. The reservoir for mixing can be directly connected to the application device or the mixed coating composition can be filled into a corresponding reservoir attached to the application device after the mixing operation. Suitable reservoirs include tanks, containers, etc., which are suitable for storing the coating composition or parts thereof and allow attachment to the application device, for example via a pipeline. If steps (b) and (c) are performed sequentially, it may be preferred to prepare these coating compositions before applying them to the target area of ​​the object.

[0161] In another embodiment, the coating compositions are each prepared by mixing component A and component B in a selected mixing ratio in an application apparatus. i The coating composition is obtained by mixing at least one base component BC i In the case of preparation by mixing with at least one hardener component B, the at least one base component BC is applied in an application device. i and at least one hardener component B. Mixing in the application device can be facilitated by placing a mixture containing the provided components (A 1 , …, A n) or at least one base component BC i A corresponding reservoir of component A and optionally a hardener component B is attached to the spray device and the attached components are mixed in the atomizer of the spray device by providing the spray device with the selected mixing ratio and information about the components to be mixed. Mixing can also be done by having component A i or BC i The mixture is preferably mixed with the hardener component B before the application device is supplied with the mixture. In this case, the remaining component A, which is optionally mixed with the hardener component B, is preferably mixed with the hardener component B. n-i , or hardener component B is supplied to the mixing device by additionally attaching a reservoir containing the remaining components to the application device. Suitable spray devices that allow at least two different reservoirs to be attached and the components present in the at least two attached reservoirs to be mixed in the atomizer include, for example, the commercially available EcoBell 3 2X2K from Dürr. The preparation of the coating composition in the application device avoids the use of a separate mixing device and allows the mixing ratio to be automatically controlled to produce a reproducible coating composition. Mixing in the application device reduces the time span necessary for the production and application of the coating composition, because steps (b) and (c) can be carried out immediately after each other with only a minimal time difference between the preparation of the coating composition and the application of the prepared coating composition, thereby significantly reducing the total time required to carry out the method of the present invention. In addition, the time for cleaning the application device is reduced compared to the use of different coating compositions, because the same components are used to produce coatings with different properties, thereby making the cleaning of the application device redundant.

[0162] Step (c):

[0163] In step (c) of the method of the present invention, the coating compositions provided in step (b) are applied to a target area associated with a matching set of characteristics. Thus, in step (c) each coating composition is applied to a target area having a set of characteristics that matches the characteristics of a coating obtained by applying the coating composition to the target area of ​​the object. Preferred characteristics within the set of characteristics include the location of the target area on the object.

[0164] The application of the coating composition in step (c) can be carried out with any type of application equipment, which is known for applying the coating composition to an object and can include, for example, a dip coating device, a rod coating device, a spray coating device, a roller coating device, etc. Particularly preferably, step (b) is carried out using a spray application device. Suitable spray application equipment includes compressed air spray equipment (pneumatic spray equipment), airless spray equipment, high-speed rotary equipment or electrostatic spray application equipment (ESTA), optionally associated with thermal spraying, such as a hot air spray equipment.

[0165] Each coating composition can be applied to all target areas having the same set of matching properties or only to a portion of a target area having the same set of matching properties. Preferably, each coating composition is applied to all target areas having the same set of matching properties. This avoids switching coating compositions during application, thereby reducing cleaning time and material consumption. If a specific coating composition is only applied to a portion of a target area having the same set of properties in step (c), step (c) can be repeated for the coating composition, provided that the coating composition is applied to the remaining target areas having the same set of properties as the target area to which the coating composition was applied in step (c). Repetition of step (c) is generally optional and only needs to be performed when only a portion of the target area having the same set of properties in step (c) is coated with the provided coating composition.

[0166] In one example, a coating composition that produces a coating with high flexibility and thus high stone chip resistance is applied on a target area requiring high stone chip resistance, while another coating composition that produces a coating with high hardness and thus low stone chip resistance, but high chemical resistance, is applied on a target area requiring high chemical resistance but low stone chip resistance. This allows achieving an overall high mechanical, physical and / or chemical quality of the final coating, since the properties of the coating are adjusted according to the set of properties of the coated target area.

[0167] In another example, a coating composition that produces a coating with high scratch resistance is applied to target areas requiring high scratch resistance, while another coating composition that produces lower scratch resistance and is therefore less expensive is applied to target areas requiring lower scratch resistance.

[0168] In yet another example, a coating composition that produces a coating with high lightfastness is applied over target areas requiring high lightfastness, while another coating composition that produces lower lightfastness and is therefore less expensive is applied over target areas requiring lower lightfastness.

[0169] This allows the object to be coated more efficiently in terms of cost and with a higher overall quality in terms of mechanical and / or chemical properties, since the properties of the coating are adjusted to the property set of the target area for coating.

[0170] The coating compositions are applied in such a way that each coating layer, after curing in step (d), has a dry film thickness of, for example, 15 to 80 μm, preferably 20 to 65 μm, particularly preferably 25 to 60 μm.

[0171] The method of the present invention is suitable for coating various metal and non-metal objects in batch or continuous processes. In a batch process (also referred to as a modular process), the object is fixed during each processing step of the process, while in a continuous process, the object is in continuous movement along the coating line in an assembly line manner.

[0172] Suitable objects to be coated according to the method of the present invention include (i) uncoated metal objects or metal objects coated with a cured electrophoretic paint layer and / or a cured filler layer and / or a non-cured color paint layer; (ii) plastic objects optionally coated with a cured primer layer and / or a non-cured color paint layer; and (iii) objects comprising metal parts and plastic parts and optionally coated with a cured electrophoretic paint layer and / or a cured filler layer and / or a cured primer-surfacer layer and / or a cured primer layer and / or a non-cured color paint layer, preferably metal objects coated with a cured electrophoretic paint layer and / or a cured filler layer and / or a non-cured color paint layer, very preferably metal objects coated with a cured electrophoretic paint layer and a non-cured color paint layer. The object preferably contains regions with different orientations relative to each other, such as vertically oriented regions and horizontally oriented regions.

[0173] Suitable metal objects are selected from the group comprising or consisting of steel, iron, aluminium, copper, zinc and magnesium objects and objects made of alloys of steel, iron, aluminium, copper, zinc and magnesium.

[0174] The coated and uncoated metal objects can be pretreated in a manner known per se (i.e., for example, cleaned) and / or provided with a known conversion coating. Cleaning can be performed mechanically, for example by wiping, grinding and / or polishing, and / or chemically by etching methods, such as surface etching in an acid bath or alkaline bath using, for example, hydrochloric acid or sulfuric acid, or by cleaning with organic solvents or aqueous detergents. Pretreatment can likewise be performed by applying a conversion coating, in particular by phosphating and / or chromating, preferably phosphating. Preferably, the metal object is at least phosphated by a conversion coating treatment, in particular preferably by zinc phosphate treatment.

[0175] The metal object coated with the cured electrophoretic paint is produced by electrophoretically applying the electrophoretic paint material to the object and then curing the applied electrophoretic paint material. The electrophoretic paint material can be a cathode or an anode electrophoretic paint material, preferably a cathode electrophoretic paint material. The electrophoretic paint material is an aqueous coating material containing anionic or cationic polymers as a binder. These polymers contain potentially anionic functional groups, i.e., can be converted into anionic groups, such as carboxylic acid groups, or potentially cationic functional groups, i.e., can be converted into cationic groups, such as amino groups. The conversion into charged groups is usually achieved by using suitable neutralizing agents (organic amines (anions), organic carboxylic acids such as formic acid (cations). Electrophoretic coating materials usually include typically corrosion-resistant pigments. Cationic electrophoretic coating materials preferred in the context of the present invention preferably contain cationic polymers as binders, especially hydroxy-functional polyetheramines, which preferably have aromatic structural units. These polymers are used in particular in combination with blocked polyisocyanates known per se. The application of the electrophoretic coating materials is carried out by electrophoresis. For this purpose, the metal workpiece to be coated is first immersed in a dipping tank containing the coating material, and a DC electric field is applied between the metal workpiece and the counterelectrode. The workpiece thus acts as an electrode; Since the polymer used as a binder carries the described charge, the non-volatile components of the electrophoretic paint material migrate to the object through the electric field and are deposited on the object, thereby forming an electrophoretic paint film. For example, in the case of a cathodic electrophoretic paint, the object is thus connected as a cathode, and the hydroxide ions formed there by water electrolysis neutralize the cationic binder, so that the cationic binder is deposited on the object and forms an electrophoretic paint layer. After the electrolytic application of the electrophoretic paint material, the coated object is removed from the tank, optionally rinsed with, for example, a water-based rinsing solution, then optionally flashed and / or immediately dried, and finally cured. The dry film thickness of the cured electrophoretic paint is, for example, 10 to 40 microns, preferably 15 to 25 microns.

[0176] The metal object coated with a cured filler layer is produced by applying a filler coating composition to the object, optionally flashing and / or immediately drying the applied composition and finally curing the composition. Suitable filler coating compositions are known in the prior art. The dry film thickness of the cured filler layer is, for example, 10 to 40 microns, preferably 25 to 30 microns.

[0177] The metal object coated with the non-curing color paint layer is produced by applying at least one color paint composition to an object optionally coated with at least one curing or non-curing coating and optionally flashing and / or immediately drying the applied color paint composition. The dry film thickness of the cured color paint layer is, for example, 5 to 40 microns, preferably 10 to 30 microns.

[0178] Preferred plastic objects are objects which essentially comprise or consist of (i) polar plastics, such as polycarbonate, polyamide, polystyrene, styrene copolymers, polyesters, polyphenylene ethers and blends of these plastics, (ii) synthetic resins such as polyurethane RIM, SMC, BMC and (iii) polyolefin objects of the polyethylene and polypropylene type with a high rubber content, such as PP-EPDM, and surface-activated polyolefin objects. In addition, the plastics may be fiber-reinforced, in particular using carbon fibers and / or metal fibers.

[0179] Preferably, the objects to be coated according to the method of the present invention are used as parts for manufacturing vehicles, preferably automotive vehicles, including but not limited to cars, trucks, and tractors. The objects can have any shape, but are usually in the form of automotive body parts, such as bodies, hoods, doors, fenders, bumpers and / or automotive vehicle trim. The present invention is most suitable for coating automotive bodies and parts thereof that travel in a continuous moving manner along an automotive assembly line.

[0180] Step (d):

[0181] The method of the present invention may further include a step (d) of curing or drying and curing the coating composition applied in step (c) to form at least two coatings with adjustable properties. Curing or drying and curing may be performed after all coating compositions are applied to all target areas or after each coating composition is applied to at least part of the target area. Since the curing operation requiring high temperature is only performed once, it is more efficient to perform step (d) after all coating compositions are applied to all target areas.

[0182] Drying can be carried out at 15° C. to 35° C. for a period of 10 to 30 minutes. Curing is preferably carried out at a temperature of 80° C. to 250° C., preferably 80° C. to 180° C., for a period of 5 to 60 min, preferably 10 to 45 min. Such curing conditions are particularly suitable for the preferred case where the coating composition is based on a thermally curable 2K coating composition, since these conditions are necessary to achieve curing of this type / class of 2K coating compositions.

[0183] The method according to the invention allows the properties of the coating to be matched to the property set of the corresponding target area, for example the location of the target area on the object. This allows higher overall mechanical and / or chemical properties to be achieved compared to producing a coating with balanced properties, since properties like flexibility and hardness are conflicting properties that cannot be adjusted without negatively affecting each other. In principle, a coating with adjustable properties can be made by combining only two components A and B. 1 and A 2For example, a coating composition prepared by mixing a component containing a high amount of a flexible polyester resin and a component containing a low amount or no flexible polyester resin in an appropriate mixing ratio is obtained, thereby allowing a coating with desired properties to be produced from a minimum amount of components. This reduces the amount of coating composition that needs to be stocked or attached to the application equipment, thereby reducing the overall cost associated with the method of the present invention.

[0184] Application of the present invention:

[0185] A further subject of the invention is the use of the method according to the invention for producing coated objects comprising target areas for which a coating with different properties is desired.

[0186] As previously mentioned, use of the method of the present invention results in higher overall mechanical and / or chemical properties of the coated object because the properties of the coating are matched to the set of properties of each target area, such as the location of each target area on the object.

[0187] What has been said about the method according to the invention applies mutatis mutandis to the further preferred embodiments of the use according to the invention.

[0188] The system of the present invention:

[0189] Another subject of the invention is a system for applying at least two coating compositions producing a coating with adjustable properties to an object comprising a plurality of target areas, at least some of which have different sets of properties. Each coating composition is applied to a target area having a set of properties that matches the properties of the corresponding coating composition. Thus, the coating composition is not applied to a target area having a different set of properties.

[0190] The system comprises: an application device including a nozzle, a storage device for storing application instructions and optionally mixing ratio instructions, one or more data processors configured to execute the application instructions and optionally mixing ratio instructions to control the application device, and a liquid crystal display device in fluid communication with the application device and comprising at least two components (A i ) i=1,…,n and optionally at least one hardener component B or at least two coating compositions (C i ) i=1,…,n Each component A i Each mixture of one or more components and B produces a coating CL having properties that match the property set of one or more target areas. i As previously mentioned with respect to step (b) of the process of the present invention, component A i At least part of the adhesive component A may already be mixed with the adhesive component B, so that the reservoir may contain component A. i and adhesive B.

[0191] In one embodiment of the system, the application device is configured to receive one or more components A from the reservoir. i and optionally B and based on the mixing ratio instruction, causing the received one or more components A to be mixed in the nozzle i Mixing, optionally mixing it with B. Mixing can prepare a varnish composition (C 1 , …, C n ). Mixing can prepare at least two varnish compositions (C 1 , …, C n ), thereby producing a coating with different properties. Then, based on the application instructions, the resulting coating composition (C i ) i=1,…,n The coating composition C is discharged through a nozzle to a target coating area having a matching set of characteristics. The application instructions may be used to prepare the corresponding coating composition C i This allows ensuring that the corresponding coating composition C prepared according to the mixing instructions is applied according to the application instructions. i The properties of the coating obtained by discharge are related to the corresponding coating composition C i The property set of the target area onto which it is discharged is matched. This embodiment is preferred if the coating composition to be discharged onto the target area needs to be produced from at least two different components and a separate mixing step outside the application device is to be avoided.

[0192] In an alternative embodiment of the system, the application device is configured to receive at least two coating compositions (C i ) i=1,…,n and applying the coating composition (C i ) i=1,…,n Discharge to a target area having a matching set of properties. This embodiment may be preferred if a coating composition is used that produces a coating having properties that need to match the property set of a corresponding target area.

[0193] In both embodiments, the same coating composition is not discharged onto target areas with different sets of properties, i.e., a coating composition producing a coating with defined properties is only discharged onto target areas with a matching set of properties and is not discharged onto target areas with a mismatching set of properties. This allows the production of a coating with properties that match the set of properties of the target area, such as the location of the target area on the object.

[0194] Suitable application equipment includes the spray application equipment mentioned previously in relation to step (c) of the process of the present invention.

[0195] The storage device stores the application instructions and optionally the mixing ratio instructions. The application instructions may include position data associated with each target area (target area position data). The application instructions may further include characteristic data associated with at least part of the characteristic group in the target area. The mixing ratio instructions may include mixing ratio data associated with component data. The mixing ratio data may include mixing ratios of different components A and optionally hardener B. The mixing ratio data may include characteristic data associated with the characteristics of the resulting coating. The characteristic data may be associated with the mixing ratio of the corresponding components A and B. The component data may include component names and / or component identifiers. The application instructions may be associated with the mixing ratio instructions. This may include associating the target area position data with the corresponding mixing ratio data. The application instructions are associated with the mixing instructions to ensure that the correct coating composition is applied to the correct target area, for example, a coating composition that produces a coating having characteristics that match the characteristic group of the target area is applied to the target area. The instructions are computer executable instructions that allow a computer processor to control the mixing and discharge process performed by the application device. Therefore, the application instructions and optionally the mixing ratio instructions can be regarded as control data for controlling the application device. The control data can be generated by one or more computer processors. The control data may be generated by a further computing unit and may be provided to one or more computer processors to control the application device based on the provided control data.

[0196] One or more computer processors may reside in a computing system as previously described with respect to step (a). The computing system may further include a storage device as previously described. The processor of the computing system is configured to execute the application instructions and optionally the mixing ratio instructions and control the application device when executing the instructions.

[0197] The reservoir may be any container suitable for containing the coating composition or a portion thereof and which may be connected to an application device such that the application device may receive the components present in the respective reservoir. The connection between the reservoir and the application device may be facilitated using tubing.

[0198] In one aspect, the one or more data processors are further configured to generate the apply instruction by:

[0199] - receiving, by the one or more data processors, target image data of the object, the target image data comprising a plurality of target areas,

[0200] - generating these application instructions based on the received image data.

[0201] The target image data of the object can be provided to the data processor from a storage device, such as a database. The retrieval of the data can be performed by inputting data indicating the object, such as a vehicle identification number, a unique ID, etc. and retrieving the data based on the input data. In one example, the target image data can be an image of the object. In another example, the target image data can be CAD data of the object. The application instructions can be generated in the following manner: determining the characteristics of the target area, in particular the characteristics and the position and generating the application instructions based on the determined characteristics, in particular based on the determined characteristics and the position. Determining the characteristics can be based on the instructions present in the provided target image data.

[0202] In one aspect, the one or more data processors are further configured to generate the hybrid instruction by:

[0203] - obtaining application instructions including characteristic data relating to at least part of a set of characteristics in a target area,

[0204] - obtaining data relating to the components used to prepare the coating composition to be applied, and

[0205] The mixing ratio command is determined based on the application command, in particular based on characteristic data contained in the application command and relating to at least part of the characteristic group in the target area.

[0206] The data associated with the component may include mixing ratio data that correlates with the characteristics of the resulting coating. The data associated with the component may further include a component name and / or a component identifier. The mixing instructions may be determined by mapping the characteristics contained in the data associated with the component with a matching set of characteristics contained in the characteristic data included in the application instructions and determining a mixing ratio associated with the mapped characteristics.

[0207] The system of the present invention can be used to carry out the method of the present invention.

[0208] What has been said about the method according to the invention and the use according to the invention applies mutatis mutandis to the further preferred embodiments of the system according to the invention.

[0209] The present invention is described in particular by the following examples:

[0210] 1. A method for preparing an object comprising a plurality of target regions, at least some of which have different sets of properties and are coated with at least two coatings having tunable properties, the method comprising:

[0211] (a) identifying at least two target regions and a set of characteristics associated with each identified target region, wherein at least two of the target regions have different sets of characteristics,

[0212] (b) providing at least two different coating compositions (C i ) i=1,…,n , wherein each coating composition (C 1 , …, C n ) produces a coating (CL) having properties matching the different property groups identified in step (a) 1 , …, CL n ),as well as

[0213] (c) each coating composition (C) provided in step (b) 1 , …, C n ) is applied to the target area associated with the matching feature set.

[0214] 2. The method of embodiment 1, wherein the tunable properties include hardness, scratch resistance, light resistance, appearance and / or adhesion.

[0215] 3. A method according to embodiment 1 or 2, wherein the different sets of characteristics identified in step (a) include different orientations of the corresponding target areas relative to each other and / or different positions of the corresponding target areas on the object.

[0216] 4. The method of any preceding embodiment, wherein step (a) comprises, on a computing device having a display and one or more user input devices adapted to detect user input:

[0217] (a-1) displaying a user interface including the object on the display,

[0218] (a-2) detecting user input indicating identification of at least two target regions and a set of characteristics associated with each target region on the object,

[0219] (a-3) determining the target regions and each set of characteristics associated with each identified target region based on the detected user input, and

[0220] (a-4) providing the data determined in step (a-3) to the application device and / or displaying the data determined in step (a-3) within the user interface.

[0221] 5. The method of embodiment 1, wherein step (a) comprises providing a user interface comprising an object comprising at least two marked target areas and an indication of a set of characteristics associated with the marked target areas.

[0222] 6. The method of embodiment 1, wherein step (a) comprises visually identifying at least two target regions and a set of characteristics associated with each identified target region, wherein at least two target regions have different sets of characteristics.

[0223] 7. The method according to any one of the preceding embodiments, wherein each coating composition (C 1 , …, C n ) is a liquid solvent-based or water-based coating composition, preferably a liquid solvent-based coating composition.

[0224] 8. The method according to any one of the preceding embodiments, wherein each coating composition (C 1 , …, C n ) is transparent, translucent or opaque, especially transparent.

[0225] 9. The method according to any one of the preceding embodiments, wherein at least one coating composition C provided is i Produces a coating CL with high stone chip resistance i And at least one additional coating composition C is provided n-i Produces coatings with high chemical resistance CL n-i , and / or wherein at least one coating composition C provided i Produces a coating with high scratch resistance CL i And at least one additional coating composition C is provided n-i Produces a coating with lower scratch resistance CL n-i , and / or wherein at least one coating composition C provided i Produces coatings with high light resistance CL i And at least one additional coating composition C is provided n-i Produces a coating with lower light resistance CL n-i .

[0226] 10. The method according to any one of the preceding embodiments, wherein each coating composition (C 1 , …, C n ) comprises at least one binder that is the same as at least one binder present in other provided coating compositions, or wherein each provided coating composition comprises at least one binder that is different from the binder present in other provided coating compositions.

[0227] 11. The method according to embodiment 10, wherein the at least one binder is selected from (i) poly(meth)acrylates, more particularly hydroxy-functional and / or carboxylate-functional and / or amine-functional poly(meth)acrylates, (ii) polyurethanes, more particularly hydroxy-functional and / or carboxylate-functional and / or amine-functional polyurethanes, (iii) polyesters, more particularly polyester polyols, (iv) polyethers, more particularly polyether polyols, (v) copolymers of the aforementioned polymers, and (vi) mixtures thereof, in particular selected from hydroxy-functional poly(meth)acrylates and / or polyesters.

[0228] 12. The method according to embodiment 11, wherein the hydroxy-functional (meth)acrylate contains in polymerized form at least one unsaturated monomer M1 comprising at least one acid group, at least one unsaturated aliphatic and / or alicyclic monomer M2, at least one unsaturated aromatic monomer M3 and at least one unsaturated hydroxyl-containing monomer M4.

[0229] 13. The method according to embodiment 12, wherein the at least one unsaturated monomer M1 comprising at least one acid group is selected from (meth)acrylic acid.

[0230] 14. The method according to embodiment 12 or 13, wherein the at least one unsaturated aliphatic monomer M2 is selected from alkyl (meth)acrylates, more preferably C (meth)acrylates. 1 -C 22 Alkyl esters, even more preferably (meth)acrylic acid C 1 -C 14 Alkyl esters such as (meth) acrylic acid C 3 Alkyl esters, (meth) acrylic acid C 4 Alkyl esters, (meth) acrylic acid C 5 Alkyl esters, (meth) acrylic acid C 6 Alkyl esters, (meth) acrylic acid C 7 Alkyl esters and (meth) acrylic acid C 13 Alkyl esters, very preferably butyl (meth)acrylate and / or esters of (meth)acrylic acid 13.0.

[0231] 15. The method according to any one of embodiments 12 to 14, wherein the at least one unsaturated alicyclic monomer M2 is selected from cycloalkyl (meth)acrylates, preferably cycloalkyl (meth)acrylates. 5 -C 7 - Alkyl esters, in particular cyclohexyl (meth)acrylate.

[0232] 16. The method according to any one of embodiments 12 to 15, wherein the at least one unsaturated aromatic monomer M3 is selected from styrene.

[0233] 17. The method according to any one of embodiments 12 to 16, wherein the at least one unsaturated hydroxyl-containing monomer M4 is selected from hydroxyl-containing (meth)acrylates, more preferably from hydroxyl-containing C 1 -C 12 The alkyl (meth)acrylate is even more preferably selected from 2-hydroxyethyl (meth)acrylate, 2-hydroxyisopropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, hydroxyisobutyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate, very preferably from 2-hydroxyethyl (meth)acrylate and 3-hydroxypropyl (meth)acrylate.

[0234] 18. The method according to any one of embodiments 10 to 17, wherein the at least one binder is present in each provided coating composition (C 1 , …, C n ), in each case based on the coating composition C provided i total weight.

[0235] 19. The method according to any one of the preceding embodiments, wherein each coating composition (C 1 , …, C n ) comprises at least one crosslinking agent that is the same as at least one crosslinking agent present in other provided coating compositions, or wherein each provided coating composition (C 1 , …, C n ) comprises at least one cross-linking agent that is different from the cross-linking agent present in other provided coating compositions.

[0236] 20. The method of embodiment 19, wherein the at least one crosslinking agent is capable of reacting with the coating composition C i The functional group of at least one compound present in the reaction.

[0237] 21. The method according to embodiment 19 or 20, wherein the at least one crosslinking agent comprises an aminoplast resin and / or a polyisocyanate, preferably an aminoplast resin and an aliphatic or cycloaliphatic polyisocyanate, very preferably an aminoplast resin and hexamethylene diisocyanate and / or dimer and / or trimer hexamethylene diisocyanate.

[0238] 22. The method according to any one of the preceding embodiments, wherein at least one coating composition C provided in step (b) i Further comprising at least one sag control agent (SCA), in particular at least one polymeric sag control agent.

[0239] 23. The method according to embodiment 22, wherein the polymeric sag control agent (SCA) is obtained by reacting a primary or secondary amine, in particular benzylamine, with an isocyanate compound, in particular a polyisocyanate, in the presence of a hydroxy-functional poly(meth)acrylate.

[0240] 24. The method according to embodiment 23, wherein the hydroxy-functional poly(meth)acrylate contains in polymerized form at least one unsaturated monomer M1 comprising at least one acid group, at least one unsaturated aliphatic monomer M2, at least one unsaturated aromatic monomer M3 and at least one unsaturated hydroxyl-containing monomer M4.

[0241] 25. The method according to any one of embodiments 22 to 24, wherein the polymer sag control agent has an average molecular weight M of 3,000 to 50,000 g / mol, preferably 4,000 to 30,000 g / mol, very preferably 5,000 to 15,000 g / mol, as determined by GPC using polystyrene as an internal standard. w .

[0242] 26. The method of any one of embodiments 22 to 25, wherein the sag control agent (SCA) is present in the coating composition where higher sag resistance is desired.

[0243] 27. The method according to any one of embodiments 22 to 26, wherein the sag control agent (SCA), in particular the polymeric sag control agent, is present in a total amount of 0.1 to 40 wt.-%, preferably 2 to 30 wt.-%, more preferably 3 to 20 wt.-%, very preferably 4 to 15 wt.-%, in each case based on the respective coating composition C provided. i total weight.

[0244] 28. The method of any preceding embodiment, wherein the at least one coating composition provided further comprises at least one additive different from the sag control agent (SCA).

[0245] 29. The method of embodiment 28, wherein the at least one additive different from the sag control additive is selected from light stabilizers, leveling agents, UV absorbers, pigments, free radical scavengers, slip additives, polymerization inhibitors, defoamers, wetting agents, adhesion promoters, flow control agents, film-forming aids such as cellulose derivatives, fillers, rheology control additives, flame retardants, and / or water scavengers, in particular light stabilizers and leveling agents.

[0246] 30. The method according to embodiment 29, wherein the leveling agents are selected from silicon-containing leveling agents.

[0247] 31. The method according to any one of the preceding embodiments, wherein each coating composition (C 1 , …, C n ) differ only in that the corresponding coating (C 1 , …, C n ) that match the set of characteristics identified in step (a).

[0248] 32. The method according to any one of the preceding embodiments, wherein step (b) comprises

[0249] (b-1) providing at least two components (A) having different characteristics i ) i=1,…,n and optionally at least one hardener component B,

[0250] (b-2) Selecting the components A provided in step (b-1) i to produce a coating CL having properties matching the set of properties identified in step (a) i ,

[0251] (b-3) optionally selecting a mixing ratio for the at least one hardener component B provided in step (b-1), and

[0252] (b-4) mixing component A in the mixing ratio selected in step (b-2) and optionally (b-3) i , optionally mixed with the at least one hardener component B to provide the coating composition C i , the coating composition produces a coating CL having properties matching the set of properties identified in step (a) i .

[0253] 33. The method of embodiment 32, wherein step (b-2) comprises determining the coating CL i The desired properties and the mixing ratio for at least part of these components provided in step (b-1) are selected so that the resulting coating CL is obtained i The features of match the feature set identified in step (a).

[0254] 34. The method according to embodiment 32 or 33, wherein the mixing ratios selected in step (b-2) and optionally step (b-3) are by volume, and / or wherein component A i A volume:volume mixing ratio of 8:1 to 1:1, preferably 4:1 to 1:1, of the mixture of and the at least one hardener component B is selected in step (b-3).

[0255] 35. The method of any one of embodiments 1 to 31, wherein step (b) comprises preparing the at least two different compositions (C i ) i=1,…,n , so that the coating obtained from the corresponding coating composition (C i ) i=1,…,n Each has properties that match a different set of properties identified in step (a).

[0256] 36. The method according to embodiment 35, wherein the coating material components include

[0257] -Base component BC i ,and

[0258] - At least one hardener component B.

[0259] 37. The method according to embodiment 36, wherein a volume:volume mixing ratio of 8:1 to 1:1, preferably 4:1 to 1:1, is used to mix the base component BC i With the at least one hardener component B.

[0260] 38. The method according to any one of embodiments 32 to 36, wherein the coating composition C is supplied to the application device. i Before Component A i In a selected mixing ratio, optionally together with the hardener component B, and / or wherein the coating composition C is supplied to the application device i Previously, the at least one base component BC i With the at least one hardener component B is mixed.

[0261] 39. The method of any one of embodiments 32 to 36, wherein each coating composition C i By mixing component A in the selected mixing ratio in the application device i , optionally mixed with the hardener component B, and / or wherein the at least one base component BC i The at least one hardener component B is mixed in the application device.

[0262] 40. The method of any preceding embodiment wherein step (c) is performed using a spray application device.

[0263] 41. The method according to any one of the preceding embodiments, wherein each coating composition (C 1 , …, C n ) is applied to all target areas with the same set of characteristics.

[0264] 42. The method of any preceding embodiment, further comprising the step (d) of curing or drying and curing the applied coating composition.

[0265] 43. Use of the method of any preceding embodiment for preparing a coated object comprising a target area requiring a coating with different properties.

[0266] 44. A system for applying at least two coating compositions producing a coating having tunable properties to an object comprising a plurality of target areas, at least some of the plurality of target areas having different sets of properties, using an application apparatus, the system comprising:

[0267] - an application device comprising a nozzle;

[0268] - a storage device for storing application instructions and optionally mixing ratio instructions;

[0269] - one or more data processors configured to execute the application instructions and optionally the mixing ratio instructions to control the application device; and

[0270] - at least two reservoirs, which are in fluid communication with the application device and are configured to contain at least two components (A i ) i=1,…,n and optionally at least one hardener component B, each component A i or each A i A mixture of A and B produces a coating CL with properties that match the property set of the target area. i , or is configured to contain at least two types of coatings (CL i ) i=1,…,n The coating composition (C i ) i=1,…,n , CL for each coating i has characteristics that match the characteristic set of the target region,

[0271] wherein the application device is configured

[0272] o Receive the components from the reservoir (A i ) i=1,…,n and optionally the hardener component B and mixing the components in the nozzle based on the mixing ratio instructions (A i ) i=1,…,n , optionally mixed with the hardener component B, and

[0273] ○ Based on the application instruction, the obtained coating composition (C i ) i=1,…,n Discharging to a target area having a matching set of properties to form at least two coatings; or

[0274] wherein the applicator is configured to

[0275] o receiving the at least two coating compositions (C i ) i=1,…,n ,as well as

[0276] ○ Based on the application instruction, the coating composition (C i ) i=1,…,n Discharged to a target area having a matching set of properties to form at least two coatings.

[0277] 45. The system of claim 44, wherein the one or more data processors are further configured to generate the apply instructions by:

[0278] - receiving, by the one or more data processors, target image data of the object, the target image data comprising different target areas,

[0279] - generating these application instructions based on the received image data. BRIEF DESCRIPTION OF THE DRAWINGS

[0280] Figure 1 A schematic diagram of a vehicle 100 to be coated with a coating material is shown. In this example, the coating material is a varnish material. In another example, the coating material is a primer coating material, a primer-surfacer coating material, a filler coating material, or a color paint material. The vehicle 100 contains a target area 102 located on the top of the vehicle and a target area 104 located on the side of the vehicle. Using the method of the present invention, a coating with high hardness and chemical resistance (i.e., low flexibility) is produced on the target area 102 located on the top of the vehicle, while a coating with high flexibility and stone chip resistance (i.e., high hardness) is produced on the target area 104 located on the side of the vehicle. For this purpose, a coating material that produces a coating with high flexibility (e.g., by containing a suitable amount of flexible polyester resin) is applied to the target area 104, while a coating material that produces a coating with high hardness (e.g., by containing a lower amount or no flexible polyester resin) is applied to the target area 102. The coating material applied to the target area 102 can be, for example, by using component A containing a high amount of flexible polyester i and component A without flexible polyester i+1 A coating material which produces a coating with lower flexibility can be obtained by mixing these components A in a suitable mixing ratio. i , A i+1 To obtain.

[0281] Examples

[0282] The present invention will now be explained in more detail using working examples, but the present invention is not limited to these working examples. In addition, unless otherwise indicated, the terms "part", "%" and "ratio" in these examples represent "part by mass", "mass %" and "mass ratio" respectively.

[0283] A) Determination method:

[0284] 1. Solid content (solid, non-volatile fraction)

[0285] Unless otherwise indicated, the solids content (also referred to below as solids fraction) was determined in accordance with DIN EN ISO 3251:2008-06 at 130° C. and 60 min, initial mass 1.0 g.

[0286] 2. Determination of chemical resistance (gradient oven method)

[0287] To determine the chemical resistance, multicoat paint systems were produced according to the following general protocol:

[0288] The coating was coated with a cured cathodic electrodeposition paint (from BASF Coatings GmbH) in a single application. Steel panels (10×50 cm) containing a 100% varnish (100% varnish) and a cured commercially available water-based basecoat material (ColorBrite from BASF Coatings) were electrostatically coated with the corresponding clearcoat composition at a target film thickness of 40 μm±5 μm (film thickness of the dried material). After a flash-off time of 10 minutes at room temperature (25° C.), the resulting clearcoat films were cured in a forced-air oven at 125° C. for 20 minutes or at 160° C. for 30 minutes.

[0289] The determination of the chemical resistance is determined by the customary and known gradient oven test. For this purpose, sulfuric acid solution (1 wt.-%), pancreatin, tree resin, and sodium hydroxide solution (1 wt.-%) are applied to the surface of the corresponding multi-coat paint system. The test panels are placed in a preheated gradient oven for 30 minutes. After heating, the test panels are rinsed with water and washing gasoline and the temperature reached before any visible signs of damage to the painted surface are determined in each case.

[0290] 3. Determination of hardness

[0291] The microindentation hardness was determined in accordance with DIN EN ISO 14577-4 on the multicoat paint systems produced as described in relation to point 2. The above with the following deviation: The resulting clearcoat films were cured in a forced-air oven at 140° C. for 20 minutes.

[0292] 4. Determination of stone chip resistance

[0293] To determine the stone chip resistance, a multicoat paint system was produced according to the following general protocol:

[0294] In a single application, the coating was coated with a cured cathodic electrodeposition paint (from BASF Coatings Steel panels (10×20 cm) containing a 100% sintered carbon steel sheet (10×20 cm) of ...

[0295] The resulting multicoat paint system was tested for its stone chip resistance. This was done using the stone chip test of DIN 55966-1:2001-04. The results of the stone chip test were evaluated in accordance with DIN EN ISO 20567-1:2017-07. Lower values ​​indicate better stone chip resistance.

[0296] B) Preparation of different clearcoat compositions

[0297] 1. Basic component BC i Preparation

[0298] Each base component BC 1 and B.C. 2 Prepared by mixing the components given in Table 1. Base Component BC 1 Contains a low amount of flexible polyester resin, while the base component BC 2 Contains a higher amount of flexible polyester resin.

[0299] Table 1: Preparation of base components BC 1 and B.C. 2 Ingredients (all amounts are given in % by weight)

[0300]

[0301] 1) Hydroxy-functional (meth)acrylic resin containing the following monomers: styrene, hydroxyethyl methacrylate, hydroxypropyl methacrylate, butyl methacrylate, cyclohexyl methacrylate and acrylic acid, solid content = 56%,

[0302] 2) According to WO 2008148555A1, page 18, lines 5 to 26, “Herstellung eines SCA Harzes" was prepared by the procedure described,

[0303] 3Saturated polyester having an OH content of 4.4% based on solids, a solids content of 71%-73%, an acid number of 6.5 to 9.8, at 23°C and 100s -1 Viscosity of 4.0 to 5.8 Pas (supplied by Allnex);

[0304] 4) n-Butylated high imino melamine crosslinker, solid content = 68%-72% (supplied by Allnex);

[0305] 5) Highly methylated monomeric melamine crosslinker, solid content = ≥98% (supplied by Allnex);

[0306] 6) Liquid UV absorbers of the hydroxyphenylbenzotriazole type (supplied by BASF Dispersions & Resins);

[0307] 7) Liquid Hindered Amine Light Stabilizer 292) (supplied by BASF Dispersions & Resins);

[0308] 8) Polyether-modified polymethylalkylsiloxane, solid content = 52% (supplied by BYK-Chemie GmbH);

[0309] 9) Polyester modified polymethylalkylsiloxane, solid content = 25% (supplied by BYK Chemical);

[0310] 10) Acrylic polymer / polyvinyl ether, solids content = 77% (supplied by Kyoeisha Chemical)

[0311] 2. Preparation of Hardener Components

[0312] Hardener component B was prepared by mixing the components given in Table 2:

[0313] Table 2: Ingredients for preparing hardener component B

[0314]

[0315] 1) Desmodur Ultra N 3390BA / SN, solid content = 90% (supplied by Covestro AG)

[0316] 3. Preparation of different varnish coating compositions

[0317] The varnish compositions CC1 and CC2 are each prepared by mixing the corresponding base components BC 1 or BC 2 Prepared by mixing with hardener component B in the mixing ratio given in Table 3.

[0318] Table 3: Varnish compositions CC1 and CC1

[0319]

[0320] C) Preparation of coated objects

[0321] Test panels for evaluating chemical resistance, hardness and stone chip resistance were prepared as described above in point A).

[0322] D) Results

[0323] 1. Chemical resistance

[0324] The chemical resistance of the multilayer coating system MC1 comprising the varnish composition CC1 and the multilayer coating system MC2 comprising the varnish composition CC2 was determined as described previously. The results obtained are listed in Table 4 and Table 5. In the upper part of the table, only the differences with regard to the composition of the varnishes CC1 and CC2 are listed. Footnote 1) corresponds to footnote 1) of Table 1.

[0325] Table 4: Results of the chemical resistance of the multilayer coating systems MC1 and MC2 (the clearcoat was cured at 125° C. for 20 minutes, and started to fail after 30 minutes at 125° C.)

[0326]

[0327] Table 5: Results of the chemical resistance of the multilayer coating systems MC1 and MC2 (the clearcoat was cured at 160° C. for 30 minutes and started to deteriorate after 24 hours at 160° C.)

[0328]

[0329] 2. Microindentation hardness

[0330] The hardness of the multilayer coating system MC1 comprising the clearcoat CC1 and the multilayer coating system MC2 comprising the clearcoat composition CC2 was determined as described previously. The results obtained are listed in Table 6. In the upper part of this table, only the differences with regard to the composition of the clearcoats CC1 and CC2 are listed. Footnote 1) corresponds to footnote 1) of Table 1.

[0331] Table 6: Results of hardness measurements of multilayer coating systems MC1 and MC2

[0332]

[0333] 3. Stone chip resistance

[0334] The stone chip resistance of the multilayer coating system MC1 comprising the varnish composition CC1 and the multilayer coating system MC2 comprising the varnish composition CC2 was determined as described previously. The results obtained are listed in Table 7. In the upper part of this table, only the differences with regard to the composition of the varnishes CC1 and CC2 are listed. Footnote 1) corresponds to footnote 1 of Table 1). In addition, the term "without correction" refers to the multilayer coating system prepared as described in point 4, while the term "corrected" refers to the multilayer coating system prepared according to point 4, which was corrected as described in the table before carrying out the stone chip resistance test.

[0335] Table 7: Results for the stone chip resistance of the multilayer coating systems MC1 and MC2 (the substrate temperatures for the stone chip resistance test are given in square brackets)

[0336]

[0337] E) Discussion of Results

[0338] Better chemical resistance was obtained from the coating prepared from the coating composition (CC1) containing a lower amount of flexible polyester. The coating also included a higher hardness. However, the coating produced a reduced stone chip resistance as compared to the more flexible coating prepared from the coating composition (CC2) containing a higher amount of flexible polyester resin (see Table 7). However, the latter coating included a lower chemical resistance due to its higher flexibility.

[0339] These results demonstrate that the production of coatings with tunable properties allows avoiding balancing conflicting properties, such as flexibility and hardness, but allows coating the respective target area with a coating having properties optimized according to the property set of said respective target area to obtain higher overall mechanical and / or chemical properties.

Claims

1. A method for preparing an object comprising a plurality of target regions, at least some of which have different sets of properties and are coated with at least two coatings having tunable properties, the method comprising: (a) identifying at least two target regions and a set of characteristics associated with each identified target region, wherein at least two of the target regions have different sets of characteristics, (b) providing at least two different coating compositions (C i ) i=1,…,n , wherein each coating composition (C1, ..., C n ) produces coatings (CL1, ..., CL2) having properties matching the different sets of properties identified in step (a) n ),as well as (c) each coating composition (C1, ..., C n ) is applied to the target area associated with the matching feature set.

2. The method according to claim 1, wherein: Each of the coating compositions (C1, ..., C n ) is a liquid solvent-based or water-based coating composition, preferably a liquid solvent-based coating composition.

3. The method according to claim 1 or 2, wherein: At least one coating composition C provided i Produces a coating CL with high stone chip resistance i And at least one additional coating composition C is provided n-i Produces coatings with high chemical resistance CL n-i , and / or wherein at least one coating composition C provided i Produces a coating with high scratch resistance CL i And at least one additional coating composition C is provided n-i Produces a coating with lower scratch resistance CL n-i , and / or wherein at least one coating composition C provided i Produces coatings with high light resistance CL i And at least one additional coating composition C is provided n-i Produces a coating with lower light resistance CL n-i .

4. A method according to any one of the preceding claims, wherein: Each of the coating compositions (C1, ..., C n ) comprises at least one binder that is the same as at least one binder present in other provided coating compositions, or wherein each provided coating composition comprises at least one binder that is different from the binder present in other provided coating compositions.

5. A method according to any one of the preceding claims, wherein: Each of the coating compositions (C1, ..., C n ) differ only in that the corresponding coatings (C1, ..., C n ) that match the set of characteristics identified in step (a).

6. A method according to any one of the preceding claims, wherein: Step (b) comprises (b-1) providing at least two components (A) having different characteristics i ) i=1,…,n and optionally at least one hardener component B, (b-2) Selecting the components A provided in step (b-1) i to produce a coating CL having properties matching the set of properties identified in step (a) i , (b-3) optionally selecting a mixing ratio for the at least one hardener component B provided in step (b-1), and (b-4) mixing component A in the mixing ratio selected in step (b-2) and optionally (b-3) i , optionally mixed with the at least one hardener component B to provide the coating composition C i , the coating composition produces a coating CL having properties matching the set of properties identified in step (a) i .

7. The method according to claim 6, wherein: Step (b-2) comprises determining the coating CL i The desired properties and the mixing ratio for at least part of these components provided in step (b-1) are selected so that the resulting coating CL is obtained i The features of match the feature set identified in step (a).

8. The method according to any one of claims 1 to 5, wherein: Step (b) comprises preparing the at least two different compositions (C) by mixing at least two coating material components i ) i=1,…,n , so that the coating obtained from the corresponding coating composition (C i ) i=1,…,n Each has properties that match a different set of properties identified in step (a).

9. The method according to claim 8, wherein: These coating materials include -Base component BC i ,and - At least one hardener component B.

10. The method according to any one of claims 6 to 9, wherein: The coating composition C obtained is supplied to the application device i Before Component A i In a selected mixing ratio, optionally together with the hardener component B, and / or wherein the coating composition C is supplied to the application device i Previously, the at least one base component BC i With the at least one hardener component B is mixed.

11. The method according to any one of claims 6 to 9, wherein: Each coating composition C i By mixing component A in the selected mixing ratio in the application device i , optionally mixed with the hardener component B, and / or wherein the at least one base component BC i The at least one hardener component B is mixed in the application device.

12. A method according to any one of the preceding claims, wherein: Each of the coating compositions (C1, ..., C n ) is applied to all target areas with the same set of characteristics.

13. A method according to any one of the preceding claims, further comprising the step of curing, or drying and curing, the applied coating composition.

14. Use of the method according to any one of the preceding claims for coating target areas of a substrate having different orientations relative to one another.

15. A system for applying at least two coating compositions producing a coating having adjustable properties to an object comprising a plurality of target areas, at least some of the plurality of target areas having different sets of properties, using an application apparatus, the system comprising: - an application device comprising a nozzle; - a storage device for storing application instructions and optionally mixing ratio instructions; - one or more data processors configured to execute the application instructions and optionally the mixing ratio instructions to control the application device; as well as - at least two reservoirs, which are in fluid communication with the application device and are configured to contain at least two components (A i ) i=1,…,n and optionally at least one hardener component B, each component A i or each A i A mixture of A and B produces a coating CL with properties that match the property set of the target area. i , or is configured to contain at least two types of coatings (CL i ) i=1,…,n The coating composition (C i ) i=1,…,n , CL for each coating i has characteristics that match the characteristic set of the target region, wherein the application device is configured o Receive the components from the reservoir (A i ) i=1,…,n and optionally the hardener component B and mixing the components in the nozzle based on the mixing ratio instructions (A i ) i=1,…,n , optionally mixed with the hardener component B, and ○ Based on the application instruction, the obtained coating composition (C i ) i=1,…,n discharging to a target area having a matched set of properties to form at least two coatings; or wherein the applicator is configured to o receiving the at least two coating compositions (C i ) i=1,…,n ,as well as ○ Based on the application instruction, the coating composition (C i ) i=1,…,n Discharged to a target area having a matching set of properties to form at least two coatings.