Ceramic bond superhard abrasive grinding wheel
By controlling the area ratio of coarse ceramic bonding agent particles in the ceramic bonding agent superhard abrasive grinding wheel, a superhard abrasive grinding layer with good dispersion is solved, and the problem of high wear rate of ceramic bonding agent superhard abrasive grinding wheel is achieved lower wear rate and longer service life.
Patent Information
- Application Number
- CN202380027230.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-24
- Filing Date
- 2023-03-20
- Publication Date
- 2024-11-08
AI Technical Summary
The existing ceramic bonding agent ultrahard abrasive grinding wheels have a problem of high wear rate, especially due to the excessive area ratio of coarse ceramic bonding agent particles, which lead to serious wear.
In the ultra-hard abrasive layer of the ceramic bonding agent ultra-hard abrasive grinding wheel, the area ratio of the coarse ceramic bonding agent particles with an area of 30 μm2 or more is less than 10%. By optimizing the ratio of pores, ceramic bonding agent and Al2O3, dispersion is formed to form Good super hard abrasive layer to reduce wear.
It effectively reduces the wear rate, extends the service life of the grinding wheel, and maintains good sharpness during grinding processing, and is suitable for different workpieces and grinding conditions.
Smart Images

Figure CN118922274A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a vitrified bond superabrasive grinding wheel. This application claims priority based on Japanese patent application No. 2022-048144 filed on March 24, 2022. All the contents described in the Japanese patent application are incorporated herein by reference. Background Art
[0002] Conventionally, a vitrified bond superabrasive grinding wheel is disclosed in, for example, Japanese Patent Application Laid-Open No. 2014-61585 (Patent Document 1).
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2014-61585 Summary of the invention
[0006] The ceramic bond super-hard abrasive grinding wheel disclosed in the present invention has a super-hard abrasive grain layer, wherein the super-hard abrasive grain layer comprises super-hard abrasive grains, pores and a ceramic bond, and in the super-hard abrasive grain layer, the area is 30 μm 2 The area ratio of the above coarse ceramic binder particles is 10% or less. BRIEF DESCRIPTION OF THE DRAWINGS
[0007] [ Figure 1 ] Figure 1 This is a diagram showing an enlarged portion of a cut surface of the superabrasive grain layer 6 of the vitrified bond superabrasive grinding wheel according to the present disclosure.
[0008] [ Figure 2 ] Figure 2 This is a schematic diagram of a sintered body obtained in the production process of Examples.
[0009] [ Figure 3 ] Figure 3 This is a photograph of one field of view (80 μm×62 μm) of a sample in which Si constituting a ceramic binder is colored. DETAILED DESCRIPTION
[0010] [Problems to be Solved by the Present Disclosure]
[0011] The previous vitrified bond superabrasive grinding wheels had the problem of easy wear.
[0012] Conventional vitrified bond superabrasive grinding wheels have a problem of high wear rate.
[0013] The inventors have conducted intensive research to reduce the wear rate and found that in the super-hard abrasive layer constituting the vitrified bond super-hard abrasive grinding wheel, the area of 30 μm2 There is a correlation between the area of the above coarse vitrified bond particles and the wear rate of the vitrified bond superabrasive grinding wheel.
[0014] The present disclosure, which was completed based on such findings, is a ceramic bond super-hard abrasive grinding wheel having a super-hard abrasive grain layer, wherein the super-hard abrasive grain layer contains super-hard abrasive grains, pores, and a ceramic bond, which are dispersed in the super-hard abrasive grain layer, and in the super-hard abrasive grain layer, the area of the super-hard abrasive grain layer is 30 μm 2 The area ratio of the above coarse ceramic binder particles is 10% or less.
[0015] In the vitrified bond superabrasive grinding wheel having such a structure, the area of the coarse vitrified bond particles is small, so that wear based on the coarse vitrified bond particles can be prevented and the wear rate can be reduced.
[0016] Figure 1 FIG. 1 is a diagram showing a portion of a cross-section of the super-hard abrasive grain layer 6 of the vitrified bond super-hard abrasive grinding wheel according to the present disclosure in an enlarged manner. Figure 1 As shown, the vitrified bond superabrasive grinding wheel is a vitrified bond superabrasive grinding wheel having a superabrasive grain layer 6 obtained by bonding superabrasive grains 3 with vitrified bond 2, and the superabrasive grain layer 6 includes pores 5, vitrified bond 2, and Al2O3 4 constituting a filler. The pores 5 are preferably 50 to 70% by volume. The vitrified bond 2 is preferably 5 to 20% by volume. The Al2O3 4 constituting a filler is preferably 5 to 30% by volume.
[0017] It should be noted that the super abrasive grain layer 6 more preferably contains 55 to 70 volume % of pores 5, 5 to 15 volume % of vitrified binder 2, and 10 to 30 volume % of Al 2 O 3 4. Al 2 O 3 4 may not be contained.
[0018] Furthermore, the super abrasive grain layer 6 most preferably contains 55 to 70 volume % of pores 5, 5 to 15 volume % of vitrified binder 2, and 10 to 25 volume % of Al2O34.
[0019] Since the volume percentages of the superabrasive grains 3, pores 5, vitrified binder 2, and Al2O3 4 can be varied within a wide range, the specifications of the grinding wheel can be selected to best suit the type of workpiece, grinding conditions, and type of grinding device.
[0020] In particular, when surface grinding of a workpiece is performed using a cup-shaped grinding wheel (e.g., type 6A2 specified in JIS B4131) and a rotary table-type longitudinal axis surface grinding device, a grinding wheel specification can be selected that can maintain good sharpness for a long time even if the contact area between the superhard abrasive layer 6 and the workpiece becomes larger.
[0021] In the present disclosure, a vitrified bond having a known composition can be applied. For example, a vitrified bond having the following composition can be applied.
[0022] SiO2: 30-50 mass%, Al2O3: 2-10 mass%, B2O3: 40-60 mass%, RO (RO is one or more oxides selected from CaO, MgO and BaO): 1-10 mass%, R2O (R2O is one or more oxides selected from Li2O, Na2O and K2O): 2-5 mass%.
[0023] It should be noted that ceramic binders other than those described above can also be applied to the present disclosure.
[0024] Al2O3 4 is, for example, α-Al2O3. By using α-Al2O3, wafers such as silicon, sapphire, single crystal SiC, and GaN can be ground with high precision and high efficiency.
[0025] By adding α-Al2O3 to the super-hard abrasive grain layer 6, the concentration of super-hard abrasive grains can be reduced without reducing the mechanical strength of the super-hard abrasive grain layer 6. As a result, even for wafers made of materials that are difficult to cut, the grinding resistance can be reduced during grinding, and stable sharpness can be maintained for a long time.
[0026] The average grain size of Al 2 O 3 4 is, for example, 200% or less of the average grain size of the super abrasive grains 3 .
[0027] (Example)
[0028] The provided ceramic bond superabrasive grinding wheel has a superabrasive grain layer with good glass dispersibility. In order to manufacture the grinding wheel, first, diamond abrasive grains, a ceramic bond containing glass, a pore-forming material, a filler, a binder, and a ceramic ball are combined in various compositions to obtain a mixed powder. The mixed powder is mixed at a certain rotation speed (15-150rpm) for 10 hours in sample numbers 1 and 2, and for more than 120 hours in sample numbers 3 to 5, and dried and crushed to obtain a predetermined granulated powder. Then, a press is used to form a thin sheet (chip-shaped) formed body, a debinder treatment is carried out in an atmospheric atmosphere, and then it is sintered at a temperature of 750°C in an atmospheric atmosphere. Thus, sintered bodies of superabrasive grain layers of various compositions are obtained. The analysis results of the composition of these sintered bodies are shown below.
[0029] [Table 1]
[0030]
[0031] The method for determining each component is to use a combustion test and ICP emission spectral analysis. The sintered body is crushed into powder and burned at 1000°C. The mass reduction before and after combustion is converted into the reduction of diamond abrasive grains. After the remaining powder is dissolved in an alkaline solution, the concentration of Al, Si, etc. obtained by ICP emission spectral analysis is used as the concentration of Al2O3, SiO2, etc. to calculate the mass. The mass % is obtained from the obtained masses, and the volume % is obtained from the volume calculated using the known density. The composition of the sintered body is determined by the above method.
[0032] The main component of ceramic binder is SiO2.
[0033] Figure 2 Schematic diagram of a sintered body obtained in the manufacturing process of the embodiment. For sample numbers 1 to 5, samples with a size of 7 mm × 5 mm × 3 mm were cut out from the front face 101, the top face 102, and the back face 103 of the sintered body 100, respectively. CP (cross section polishing) processing and carbon coating were performed at one location of each sample. The CP processing device was CROSSSECTION POLISHER IB-19530 manufactured by JEOL Ltd.
[0034] Under the following measurement conditions, the CP-processed surface of each sample was subjected to SEM (Scanning Electron Microscope) measurement and EDX (Energy Dispersive X-ray Spectroscopy) measurement. This is to use EDX to color the Si element and visualize the glass in the tissue. The SEM device is a desktop microscope MiniscopeTM3030 manufactured by Hitachi High-Technologies Corporation. The EDX device is an energy dispersive X-ray analyzer Quantax70 manufactured by BRUKER. The SEM measurement conditions are an acceleration voltage of 15kV and a measurement magnification of 2000 times. The EDX measurement conditions are an acceleration voltage of 15kV and a photography time of 200 seconds.
[0035] Thus, eight images (80 μm×62 μm) in which Si was colored were obtained for each of the three samples, namely, the front surface 101 , the upper surface 102 , and the rear surface 103 .
[0036] The obtained 24 images were imported into image analysis software (MultiImageTool manufactured by SYSTEM IN FRONTIER) and automatically converted into binarization images according to the command in Table 2.
[0037] [Table 2]
[0038]
[0039] Thus, numerical data on the distribution of the region containing Si (glass) and the region not containing Si and the size of each region were obtained.
[0040] There are multiple glasses in the field of view in the form of scattered points. The area mapped by EDX is taken as the glass area. The glass area is the total area of multiple glasses (ceramic binder particles) in the form of scattered points. 2 The glass with the above area is regarded as coarse ceramic binder particles, and their total area is calculated.
[0041] The coarse glass area ratio (area 30 μm) was calculated using the following formula using Microsoft Excel. 2 The proportion of glass above).
[0042] Rough glass area ratio = (A / B) × 100
[0043] A = 30 μm in area in 24 images 2 The sum of the areas of the ceramic binder particles above
[0044] B = the sum of the areas of the ceramic binder particles in the 24 images
[0045] The coarse glass area ratio was calculated for the three samples and the average value was calculated. In addition, the Vickers hardness of each sample was calculated. The results are shown in Table 3.
[0046] [Table 3]
[0047]
[0048] Figure 3 This is a photograph of a field of view (80 μm × 62 μm) of a sample in which Si constituting a vitrified binder is colored. In the field of view of the superabrasive grain layer, region 201 is a 30 μm 2 The above coarse ceramic binder particles. The pores 202 are shown as black in the photograph. One coarse glass was observed in the field of view 200. Figure 3 In the region 201 constituting the coarse ceramic binder particles, except for Figure 1 In addition to the vitrified binder 2 shown, super-hard abrasive grains 3 and Al2O3 4 are also included.
[0049] The thin slice of the sintered body was bonded to a base metal made of an aluminum alloy using an adhesive, and then truing / dressing was performed using an existing grindstone, and a vitrified bond diamond grinding wheel was completed for each of the sample numbers 1 to 5.
[0050] The size of the grinding wheel is a segmented cup grinding wheel (JIS B41316A7S type) having an outer diameter of 250 mm and a super-hard abrasive grain layer width of 3 mm.
[0051] After sharpening the grinding wheel using a vertical axis rotary surface grinder, 8 pieces of 16-sided SiC wafers with a diameter of 4 inches (10.16 cm) were continuously processed as the cutting material. In addition, the grinding resistance (load current and normal resistance) and the wear rate of the abrasive layer during processing were measured and evaluated using the transition or average value during continuous processing.
[0052] Grinding machine: HRG300 manufactured by Tokyo Seimitsu
[0053] Workpiece: 4-inch SiC (grind the (0001) surface of the crystal plane orientation and then grind the (000-1) surface)
[0054] Spindle speed (min -1 ): 2000
[0055] Workpiece speed (min -1 ):301
[0056] Feed speed (μm / sec): 0.4
[0057] Residue(μm):10
[0058] Spark Out (time for the grinding stone to rotate without cutting at the end of grinding) (seconds): 10
[0059] The wear rate is calculated as follows.
[0060] Wear rate = change in super-hard abrasive layer height / change in workpiece thickness × 100 (%)
[0061] These results are shown in Table 3.
[0062] From this result, it was confirmed that the area ratio of the coarse glass needs to be 10% or less.
[0063] It is understood that when the area ratio of the coarse glass is 10% or less, the wear rate becomes extremely low, and the vitrified bond superabrasive grinding wheel becomes less prone to wear and has a long life.
[0064] In addition, it can be seen that in sample number 3-5, since the load current value is within the allowable range, the sharpness does not deteriorate.
[0065] The embodiments and examples disclosed herein are illustrative in all aspects and are not restrictive. The scope of the present invention is indicated by the claims rather than the above description, and is intended to include all modifications within the meaning and scope equivalent to the claims.
[0066] Explanation of symbols
[0067] 1. Vitrified bond superabrasive grinding wheel, 2. Vitrified bond, 3. Superabrasive grains, 4. Al2O3, 5. Pores, 6. Superabrasive grain layer, 100. Sintered body, 101. Front, 102. Top, 103. Back, 200. Field of view, 201. Area, 202. Holes.
Claims
1. A vitrified bond super-hard abrasive grinding wheel having a super-hard abrasive grain layer, The super-hard abrasive grain layer comprises super-hard abrasive grains, pores and a vitrified binder. In the super-hard abrasive layer, the area is 30 μm 2 The area ratio of the above coarse ceramic binder particles is 10% or less.
2. The vitrified bond superabrasive grinding wheel according to claim 1, in, The super-hard abrasive layer further contains fillers, including 5 volume % to 20 volume % of the ceramic binder and 50 volume % to 70 volume % of the pores, with the remainder being the super-hard abrasive and the fillers.