Resin composition for coating optical fiber, colored coating material for optical fiber, optical fiber, and optical fiber ribbon
By using a resin composition of bisphenol skeleton epoxy di(meth)acrylate and alkylene oxide modified tri(meth)acrylate, combined with titanium oxide, the peeling and warm water properties of the fiber-optic resin layer are solved, and the problem of colored resin layer of the fiber is achieved. It is a fiber-optic coating material that is not easy to peel off and has a warm water resistance.
Patent Information
- Application Number
- CN202380028756.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-06
- Filing Date
- 2023-03-07
- Publication Date
- 2024-11-08
AI Technical Summary
When removing the tape, the optical fiber tape is prone to peeling of the colored resin layer, and the coating of the resin layer in warm water may peel off, resulting in an increase in transmission loss.
The photopolymerizable compound of epoxy di(meth)acrylate containing bisphenol skeleton and alkylene oxide modified tri(meth)acrylate is used as the resin composition, and the Young's modulus of the resin layer is adjusted and colored Titanium oxide is added to the resin layer to form an optical fiber clad material that is not easy to peel and is warm and water-resistant.
It effectively prevents color peeling and improves the temperature and water resistance of the optical fiber, making the optical fiber tape not easy to peel off when taken out, and has low transmission loss in a warm water environment.
Smart Images

Figure CN118922391A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a resin composition for coating an optical fiber, a colored coating material for an optical fiber, an optical fiber, and an optical fiber ribbon.
[0002] This application claims the priority based on Japanese application No. 2022-063430 filed on April 6, 2022, and all the contents described in the above Japanese application are cited. Background Art
[0003] Generally, an optical fiber has a coating resin layer for protecting a glass fiber as a light transmission body. The coating resin layer includes, for example, a primary resin layer and a secondary resin layer. The outermost layer of the coating resin layer includes a colored resin layer for identifying the optical fiber (for example, see Patent Documents 1 to 3).
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Laid-Open No. 6-242355
[0007] Patent Document 2: Japanese Patent Application Publication No. 2003-279811
[0008] Patent Document 3: International Publication No. 2016 / 047002 Summary of the invention
[0009] A resin composition for optical fiber coating according to one embodiment of the present disclosure contains a photopolymerizable compound and a photopolymerization initiator. The photopolymerizable compound includes epoxy di(meth)acrylate having a bisphenol skeleton and alkylene oxide-modified tri(meth)acrylate. The content of the alkylene oxide-modified tri(meth)acrylate is 0.5% by mass or more and less than 40% by mass based on the total amount of the photopolymerizable compound. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] Figure 1 It is a schematic cross-sectional view showing an example of the optical fiber according to the present embodiment.
[0011] Figure 2 It is a schematic cross-sectional view showing an example of the optical fiber according to the present embodiment.
[0012] Figure 3 It is a schematic cross-sectional view showing an example of the optical fiber ribbon according to the present embodiment. DETAILED DESCRIPTION
[0013] [Technical Problems to be Solved by the Present Disclosure]
[0014] Optical fibers are sometimes used in the form of optical fiber ribbons, which are formed by arranging a plurality of optical fibers and integrating them with a ribbon resin. When using an optical fiber ribbon having an optical fiber with a colored resin layer, when removing the ribbon to take out the optical fiber, the colored resin layer may peel off from the optical fiber, which is called "color peeling". In particular, color peeling is more likely to occur when the line speed when forming the colored resin layer is increased. In addition, when the optical fiber is immersed in warm water, the coating resin layer may peel off from the glass fiber, resulting in an increase in transmission loss.
[0015] An object of the present disclosure is to provide a resin composition, an optical fiber colored coating material, an optical fiber, and an optical fiber ribbon capable of producing an optical fiber that is less susceptible to color flaking and has excellent hot water resistance.
[0016] [Effects of the present disclosure]
[0017] According to the present disclosure, a resin composition, a colored coating material for an optical fiber, an optical fiber, and an optical fiber ribbon capable of producing an optical fiber that is less susceptible to color flaking and has excellent hot water resistance can be provided.
[0018] [Description of Embodiments of the Present Disclosure]
[0019] First, the contents of the embodiments of the present disclosure will be described by way of example.
[0020] (1) A resin composition for optical fiber coating according to one embodiment of the present disclosure contains a photopolymerizable compound and a photopolymerization initiator. The photopolymerizable compound includes an epoxy di(meth)acrylate having a bisphenol skeleton and an alkylene oxide-modified tri(meth)acrylate. The content of the alkylene oxide-modified tri(meth)acrylate is 0.5 mass % or more and less than 40 mass % based on the total amount of the photopolymerizable compound.
[0021] Such a resin composition can produce an optical fiber that is less susceptible to color flakes and has excellent warm water resistance by using a (meth)acrylate compound having a specific structure as a photopolymerizable compound instead of the commonly used urethane (meth)acrylate.
[0022] (2) In the above (1), from the viewpoint of adjusting the Young's modulus of the resin layer, the alkylene oxide-modified di(meth)acrylate may have at least one selected from the group consisting of ethylene oxide chains and propylene oxide chains.
[0023] (3) In the above (1) or (2), the resin composition according to the present embodiment may further contain titanium oxide from the viewpoint of coloring the resin layer.
[0024] (4) An optical fiber colored coating material according to one aspect of the present disclosure includes the resin composition as described in any one of (1) to (3). By using the resin composition according to this embodiment for the colored resin layer, an optical fiber that is less susceptible to color flaking and has excellent warm water resistance can be produced.
[0025] (5) An optical fiber according to one embodiment of the present disclosure comprises: a glass fiber including a core and a cladding; a primary resin layer that is in contact with the glass fiber and covers the glass fiber; a secondary resin layer that covers the primary resin layer; and a colored resin layer that covers the secondary resin layer; wherein the colored resin layer comprises a cured product of the resin composition described in any one of (1) to (3) above. By using the resin composition according to this embodiment for the colored resin layer, the hot water resistance of the optical fiber can be improved without causing color flakes.
[0026] (6) An optical fiber according to one embodiment of the present disclosure comprises: a glass fiber including a core and a cladding; a primary resin layer that is in contact with the glass fiber and covers the glass fiber; and a secondary resin layer that covers the primary resin layer; wherein the secondary resin layer comprises a cured product of the resin composition described in any one of (1) to (3) above. By using the resin composition according to this embodiment for the secondary resin layer, the warm water resistance of the optical fiber can be improved without causing color flakes.
[0027] (7) An optical fiber ribbon according to one embodiment of the present disclosure is formed by arranging a plurality of optical fibers as described in (5) or (6) above and coating the plurality of optical fibers as described in (5) or (6) above with a ribbon resin. This optical fiber ribbon has excellent resistance to warm water and can easily identify the optical fibers without causing color flakes when removing the optical fibers.
[0028] [Details of the embodiments of the present disclosure]
[0029] Specific examples of the resin composition and optical fiber involved in the embodiments of the present disclosure are described with reference to the drawings as needed. Furthermore, the present disclosure is not limited to these examples, but is represented by the claims, and is intended to include all changes within the meaning and scope of the claims and equivalents. In the following description, the same elements are marked with the same symbols in the description of the drawings, and repeated descriptions are omitted. (Meth)acrylate in this specification refers to acrylate or its corresponding methacrylate. The same applies to other similar expressions such as (meth)acryloyl.
[0030] (Resin composition)
[0031] The resin composition for optical fiber coating involved in this embodiment contains a photopolymerizable compound and a photopolymerization initiator, the photopolymerizable compound includes epoxy di(meth)acrylate having a bisphenol skeleton and alkylene oxide-modified tri(meth)acrylate, and the content of alkylene oxide-modified tri(meth)acrylate is 0.5 mass% or more and less than 40 mass% based on the total amount of the photopolymerizable compound.
[0032] From the viewpoint of further suppressing color peeling, the content of the alkylene oxide-modified tri(meth)acrylate may be 0.8% by mass or more, 1% by mass or more, 2% by mass or more, or 4% by mass or more. From the viewpoint of further improving warm water resistance, the content of the alkylene oxide-modified tri(meth)acrylate may be 36% by mass or less, 34% by mass or less, 32% by mass or less, or 30% by mass or less.
[0033] From the viewpoint of adjusting the Young's modulus of the resin layer, the alkylene oxide-modified tri(meth)acrylate involved in the present embodiment may also have at least one selected from the group consisting of an ethylene oxide (EO) chain and a propylene oxide (PO) chain. The ethylene oxide chain may be denoted as "(EO)n", and the propylene oxide chain may be denoted as "(PO)n". n is an integer greater than or equal to 1, and may also be greater than or equal to 2, greater than or equal to 3, greater than or equal to 6, greater than or equal to 8, or greater than or equal to 10, and may also be less than or equal to 30, less than or equal to 25, less than or equal to 20, less than or equal to 18, or less than or equal to 16. The number of alkylene oxides possessed by the alkylene oxide-modified tri(meth)acrylate may also be 3 to 21, 3 to 18, or 3 to 15.
[0034] Examples of the alkylene oxide-modified tri(meth)acrylate include trimethylolpropane tri(meth)acrylate, trimethyloloctane tri(meth)acrylate, trimethylolpropane polyethoxy tri(meth)acrylate, trimethylolpropane polypropoxy tri(meth)acrylate, trimethylolpropane polyethoxy polypropoxy tri(meth)acrylate, isocyanuric acid tris[(meth)acryloyloxyethyl] ester, and pentaerythritol tri(meth)acrylate. From the viewpoint of further suppressing color peeling, the alkylene oxide-modified tri(meth)acrylate according to the present embodiment may be trimethylolpropane polyethoxy tri(meth)acrylate (trimethylolpropane EO addition triacrylate).
[0035] As the epoxy di(meth)acrylate according to the present embodiment, a reaction product of a diglycidyl ether compound having a bisphenol skeleton and a compound having a (meth)acryloyl group such as (meth)acrylic acid can be used.
[0036] Examples of the epoxy di(meth)acrylate include (meth)acrylic acid adducts of bisphenol A diglycidyl ether, (meth)acrylic acid adducts of bisphenol AF diglycidyl ether, and (meth)acrylic acid adducts of bisphenol F diglycidyl ether.
[0037] From the viewpoint of improving the strength of the resin layer, the content of the epoxy di(meth)acrylate may be 30% by mass or more, 40% by mass or more, or 45% by mass or more, and may be 75% by mass or less, 70% by mass or less, 65% by mass or less, 60% by mass or less, or 55% by mass or less, based on the total amount of the photopolymerizable compound.
[0038] From the viewpoint of improving the toughness of the resin layer, the photopolymerizable compound according to the present embodiment may further contain an alkylene-modified di(meth)acrylate having a bisphenol skeleton. Examples of the alkylene-modified di(meth)acrylate having a bisphenol skeleton include EO-modified di(meth)acrylate of bisphenol A, PO-modified di(meth)acrylate of bisphenol A, and EO-PO-modified di(meth)acrylate of bisphenol A.
[0039] The photopolymerizable compound according to the present embodiment may further include a photopolymerizable compound (hereinafter referred to as a “monomer”) other than epoxy di(meth)acrylate having a bisphenol skeleton, alkylene oxide-modified tri(meth)acrylate, and alkylene-modified di(meth)acrylate having a bisphenol skeleton.
[0040] As the monomer, a monofunctional monomer having one polymerizable group or a polyfunctional monomer having two or more polymerizable groups can be used. Two or more monomers may be mixed and used.
[0041] Examples of the monofunctional monomer include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, isopentyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, 1,2-dimeth ... -3-phenoxybenzyl ester, phenoxydiethylene glycol acrylate, phenoxypolyethylene glycol acrylate, 4-tert-butylcyclohexanol acrylate, tetrahydrofurfuryl (meth)acrylate, benzyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, dicyclopentane (meth)acrylate, nonylphenol polyethylene glycol (meth)acrylate, nonylphenoxypolyethylene glycol (meth)acrylate, isobornyl (meth)acrylate and other (meth)acrylate monomers; (meth)acrylic acid, (meth)acrylic acid dimer, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, ω-carboxy-polyhexane Monomers containing carboxyl groups, such as lactone (meth)acrylates; monomers containing heterocyclic rings, such as N-(meth)acryloylmorpholine, N-vinylpyrrolidone, N-vinylcaprolactam, N-(meth)acryloylpiperidine, N-(meth)acryloylpyrrolidine, (meth)acrylate-3-(3-pyridyl)propyl, cyclic trimethylolpropane formal acrylate; maleimide monomers, such as maleimide, N-cyclohexylmaleimide, and N-phenylmaleimide; (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-hexyl(meth)acrylamide, N-methyl(meth)acrylamide Amide monomers such as acrylamide, N-ethyl (meth)acrylamide, N-butyl (meth)acrylamide, N-methylol (meth)acrylamide, and N-methylolpropane (meth)acrylamide; aminoalkyl (meth)acrylate monomers such as aminoethyl (meth)acrylate, aminopropyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, and tert-butylaminoethyl (meth)acrylate; and succinimide monomers such as N-(meth)acryloyloxymethylenesuccinimide, N-(meth)acryloyl-6-oxyhexamethylenesuccinimide, and N-(meth)acryloyl-8-oxyoctamethylenesuccinimide.
[0042] Examples of the polyfunctional monomer include ethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,12-dodecanediol di(meth)acrylate, 1,14-tetradecanediol di(meth)acrylate, 1,16 - Hexadecanediol di(meth)acrylate, 1,20-eicosandiol di(meth)acrylate, isopentaediol di(meth)acrylate, 3-ethyl-1,8-octanediol di(meth)acrylate, pentaerythritol polyethoxy tetra(meth)acrylate, pentaerythritol polypropoxy tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, di-trimethylolpropane tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and caprolactone-modified isocyanuric acid tris[(meth)acryloyloxyethyl] ester.
[0043] The photopolymerization initiator can be appropriately selected from known free radical photopolymerization initiators and used. Examples of the photopolymerization initiator include 1-hydroxycyclohexyl phenyl ketone (Omnirad 184, manufactured by IGM Resins), 2,2-dimethoxy-2-phenylacetophenone, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropane-1-one, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinyl-propane-1-one (Omnirad 907, manufactured by IGM Resins), 2,4,6-trimethylbenzoyldiphenylphosphine oxide (Omnirad TPO, manufactured by IGM Resins), and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (Omnirad 819, manufactured by IGM Resins).
[0044] The content of the photopolymerization initiator may be 1 to 10 parts by mass, 2 to 8 parts by mass, or 3 to 7 parts by mass, based on 100 parts by mass of the total amount of the photopolymerizable compound.
[0045] The resin composition may further contain a silane coupling agent, a leveling agent, a defoaming agent, an antioxidant, a sensitizer, and the like.
[0046] The silane coupling agent is not particularly limited as long as it does not hinder the curing of the resin composition. Examples of the silane coupling agent include tetramethyl silicate, tetraethyl silicate, mercaptopropyl trimethoxysilane, vinyl trichlorosilane, vinyl triethoxysilane, vinyl tri(β-methoxy-ethoxy)silane, β-(3,4-epoxycyclohexyl)-ethyl trimethoxysilane, dimethoxydimethylsilane, diethoxydimethylsilane, 3-acryloxypropyl trimethoxysilane, γ-glycidyloxypropyl trimethoxysilane, γ-glycidyloxypropyl methyl diethoxysilane, γ-methacryloxypropyl trimethoxysilane, N-(β-
[0043] The invention also includes bis-[3-(triethoxysilyl)propyl]tetrasulfide, bis-[3-(triethoxysilyl)propyl]disulfide, γ-trimethoxysilylpropyldimethylthiocarbamoyl tetrasulfide, and γ-trimethoxysilylpropylbenzothiazolyl tetrasulfide.
[0047] From the perspective of coloring the resin layer, the resin composition of the present embodiment may further contain titanium oxide particles. The titanium oxide particles may also be surface-treated titanium oxide particles. The surface-treated titanium oxide particles are particles obtained by surface-treating titanium oxide with an inorganic substance, and have excellent dispersibility in the resin composition.
[0048] As inorganic substances used for surface treatment, for example, aluminum oxide, silicon dioxide, and zirconium dioxide can be cited. The surface-treated titanium oxide particles have a surface treatment layer containing at least one selected from the group consisting of aluminum oxide, silicon dioxide, and zirconium dioxide, thereby further improving dispersibility. The surface treatment layer can be formed on at least a portion of the surface of the titanium oxide, or on the entire surface of the titanium oxide. The surface treatment layer is formed by surface treatment of the titanium oxide.
[0049] From the viewpoint of improving dispersibility, the amount of the surface treatment layer in the surface-treated titanium oxide particles may be 1% by mass or more, 1.5% by mass or more, or 2% by mass or more, and from the viewpoint of improving hiding power, it may be 10% by mass or less, 9% by mass or less, or 8% by mass or less. The amount of the surface treatment layer can be calculated by measuring the amount of titanium element and inorganic elements other than titanium contained in the surface-treated titanium oxide particles by inductively coupled mass spectrometry (ICP-MS).
[0050] From the perspective of improving the lateral pressure resistance of the coating resin layer, the average primary particle size of the surface-treated titanium oxide particles may also be 300 nm or less, 295 nm or less, or 290 nm or less. From the perspective of improving the hiding power, the average primary particle size of the surface-treated titanium oxide particles may also be 100 nm or more, 150 nm or more, or 200 nm or more, or 200 nm or more and 300 nm or less. The average primary particle size may be measured, for example, by image analysis of electron microscope photographs, light scattering, BET (Brunauer-Emmett-Teller) method, etc.
[0051] From the perspective of improving the visibility of the resin layer, the content of the surface-treated titanium oxide particles may be 0.6% by mass or more, 1% by mass or more, 2% by mass or more, or 3% by mass or more based on the total amount of the resin composition. From the perspective of improving the curability of the resin composition, the content of the surface-treated titanium oxide particles may be 20% by mass or less, 15% by mass or less, 10% by mass or less, or 8% by mass or less based on the total amount of the resin composition.
[0052] If 900mJ / cm 2 Above and 1100mJ / cm 2 The following cumulative light intensity makes the elongation at break of the resin film formed by curing the resin composition involved in this embodiment 6% or more and 50% or less at 23° C., and a resin layer with excellent toughness can be formed. The elongation at break of the resin film may be 6.5% or more, 7% or more, or 10% or more, and may be 45% or less, 40% or less, or 30% or less.
[0053] From the viewpoint of improving the warm water resistance of the optical fiber, the Young's modulus of the resin film may be 1000 MPa or more, 1100 MPa or more, or 1150 MPa or more at 23° C. From the viewpoint of forming a resin layer having excellent toughness, the Young's modulus of the resin film may be 2000 MPa or less, 1900 MPa or less, or 1800 MPa or less at 23° C.
[0054] The resin composition according to the present embodiment can be suitably used as a colored coating material for an optical fiber. By forming the outermost layer of the coating resin layer using the colored coating material including the resin composition according to the present embodiment, the warm water resistance of the optical fiber can be improved.
[0055] (optical fiber)
[0056] Figure 1 1 is a schematic cross-sectional view showing the structure of an optical fiber according to one embodiment. Figure 1 As shown, the optical fiber 1 of the present embodiment includes a glass fiber 10 and a coating resin layer 20 that is in contact with the glass fiber 10 and covers the outer circumference of the glass fiber 10 .
[0057] The glass fiber 10 is a light-conducting optical transmission body that transmits the light introduced into the optical fiber 1. The glass fiber 10 is a glass member, for example, composed of a base material (main component) of silica (SiO2) glass. The glass fiber 10 includes a core 12 and a cladding 14 covering the core 12. The glass fiber 10 transmits the light introduced into the optical fiber 1. The core 12 is, for example, arranged in a region including the central axis of the glass fiber 10. The core 12 is, for example, composed of pure SiO2 glass, or composed of glass containing GeO2 and / or fluorine elements in SiO2 glass. The cladding 14 is arranged in a region surrounding the core 12. The cladding 14 has a refractive index lower than that of the core 12. The cladding 14 is, for example, composed of pure SiO2 glass, or composed of SiO2 glass to which fluorine elements are added. The outer diameter of the glass fiber 10 is about 100 μm to 125 μm, and the diameter of the core 12 constituting the glass fiber 10 is about 7 μm to 15 μm.
[0058] The coating resin layer 20 is an ultraviolet curing resin layer covering the coating 14. The coating resin layer 20 includes a primary resin layer 22 covering the outer periphery of the glass fiber 10, and a secondary resin layer 24 covering the outer periphery of the primary resin layer 22. The primary resin layer 22 is in contact with the outer peripheral surface of the coating 14 and covers the entire coating 14. The secondary resin layer 24 is in contact with the outer peripheral surface of the primary resin layer 22 and covers the entire primary resin layer 22. The thickness of the primary resin layer 22 is, for example, not less than 10 μm and not more than 50 μm. The thickness of the secondary resin layer 24 is, for example, not less than 10 μm and not more than 40 μm.
[0059] The resin composition involved in this embodiment can be used for the secondary resin layer 24. The secondary resin layer 24 can be formed by curing the above-mentioned resin composition. The secondary resin layer 24 includes a cured product of the resin composition involved in this embodiment, so that the single core separation and warm water resistance of the optical fiber can be improved without causing color peeling.
[0060] The primary resin layer 22 can be formed by curing a resin composition containing, for example, urethane (meth)acrylate, a monomer, a photopolymerization initiator, and a silane coupling agent. A conventionally known technique can be used for the resin composition for the primary resin layer.
[0061] The coating resin layer 20 may further include a colored resin layer 26 that covers the outer periphery of the secondary resin layer 24 . Figure 2 1 is a schematic cross-sectional view showing the structure of an optical fiber according to one embodiment. Figure 2 As shown, the optical fiber 1A of this embodiment includes a glass fiber 10 and a coating resin layer 20 that is connected to the glass fiber 10 and covers the outer periphery of the glass fiber 10. The coating resin layer 20 includes a primary resin layer 22, a secondary resin layer 24, and a colored resin layer 26. The thickness of the colored resin layer 26 is, for example, 3 μm or more and 10 μm or less.
[0062] The resin composition involved in this embodiment can be used for the colored resin layer 26. The colored resin layer 26 can be formed by curing the above-mentioned resin composition. The colored resin layer 26 includes a cured product of the resin composition involved in this embodiment, so that the single core separation and warm water resistance of the optical fiber can be improved without color peeling. The secondary resin layer 24 in the optical fiber 1A can be formed using a conventionally known resin composition, for example, by curing a resin composition containing urethane (meth) acrylate, a monomer, and a photopolymerization initiator.
[0063] (Fiber Optic Ribbon)
[0064] The optical fiber according to the present embodiment can be used to produce an optical fiber ribbon. The optical fiber ribbon is formed by arranging a plurality of the above optical fibers and coating the plurality of the above optical fibers with a tape resin.
[0065] Figure 3 1 is a schematic cross-sectional view showing an optical fiber ribbon according to the present embodiment. The optical fiber ribbon 100 includes a plurality of optical fibers 1A and a connecting resin layer 40 in which the optical fibers 1A are connected by coating them with a ribbon resin. Figure 3 In FIG. 4 , four optical fibers are shown as an example, but the number is not particularly limited.
[0066] As the tape resin, resin materials widely known as tape materials can be used. From the viewpoint of damage resistance of the optical fiber, ease of cutting, etc., the tape resin may also contain a thermosetting resin such as silicone resin, epoxy resin, polyurethane resin; or an ultraviolet curing resin such as epoxy acrylate, urethane acrylate, polyester acrylate.
[0067] The optical fiber ribbon according to the present embodiment uses the above optical fibers, and can easily identify the optical fibers without causing color flakes when removing the connecting resin layer from the optical fiber ribbon to take out the optical fibers.
[0068] Example
[0069] Hereinafter, the present disclosure will be described in more detail by showing the results of evaluation tests using examples and comparative examples according to the present disclosure. In addition, the present disclosure is not limited to these examples.
[0070] [Resin composition for colored resin layer]
[0071] (Photopolymerizable compound)
[0072] As the photopolymerizable compound, bisphenol A epoxy diacrylate (EA) and the following alkylene oxide-modified acrylate compounds were prepared.
[0073] BPA(EO)4DA: EO modified bisphenol A di(meth)acrylate (EO number: 4)
[0074] TMP(EO)3TA: Trimethylolpropane EO addition triacrylate (EO number: 3)
[0075] TMP(EO)6TA: Trimethylolpropane EO addition triacrylate (EO number: 6)
[0076] TMP(EO)9TA: Trimethylolpropane EO addition triacrylate (EO number: 9)
[0077] TMP (EO) 15 TA: Trimethylolpropane EO addition triacrylate (EO number: 15)
[0078] PE(EO)nTTA: Ethoxylated pentaerythritol tetraacrylate (EO number: 5)
[0079] As photopolymerization initiators, 2,4,6-trimethylbenzoyldiphenylphosphine oxide (Omnirad TPO) and 1-hydroxycyclohexyl phenyl ketone (Omnirad 184) were prepared.
[0080] As titanium oxide particles, surface-treated titanium oxide particles having a surface-treated layer containing aluminum oxide (Al2O3) were prepared. The average primary particle size of the surface-treated titanium oxide particles was 200 to 300 nm, and the amount of Al2O3 calculated by ICP-MS measurement was 2.5 mass %.
[0081] The resin composition was prepared by mixing the photopolymerizable compound and the photopolymerization initiator in the amounts (parts by mass) shown in Table 1, and then mixing so that the content of the surface-treated titanium oxide particles in the resin composition was 5% by mass. Test Examples 1 to 9 correspond to Examples, and Test Examples 10 and 11 correspond to Comparative Examples.
[0082] (Young's modulus)
[0083] The resin composition was applied onto a polyethylene terephthalate (PET) film using a spin coater, and then an electrodeless UV (Ultraviolet) lamp system ("VPS600 (D-bulb)" manufactured by Heraeus) was used to irradiate the film at 1000±100 mJ / cm 2 The resin layer was cured under the conditions of , thereby forming a resin layer with a thickness of 50±5 μm on the PET film. The resin layer was peeled off from the PET film to obtain a resin film.
[0084] The resin film was punched into a dumbbell shape of type 5 of JIS K 7127, and stretched at 23±2°C and 50±10%RH (relative humidity) using a tensile tester at a stretching speed of 1mm / min and a line spacing of 25mm to obtain a stress-strain curve. The Young's modulus was calculated using the 2.5% secant line.
[0085] (Resin composition for primary resin layer)
[0086] A urethane acrylate oligomer obtained by reacting polypropylene glycol having a molecular weight of 4000, isophorone diisocyanate, hydroxyethyl acrylate and methanol was prepared. 75 parts by mass of the urethane acrylate oligomer, 12 parts by mass of nonylphenol EO-modified acrylate, 6 parts by mass of N-vinyl caprolactam, 2 parts by mass of 1,6-hexanediol diacrylate, 1 part by mass of Omnirad TPO, and 1 part by mass of 3-mercaptopropyltrimethoxysilane were mixed to prepare a resin composition P.
[0087] (Resin composition for secondary resin layer)
[0088] Resin composition S was prepared by mixing 40 parts by mass of a urethane acrylate oligomer which was a reaction product of polypropylene glycol having a molecular weight of 600, 2,4-toluene diisocyanate and 2-hydroxyethyl acrylate, 35 parts by mass of isobornyl acrylate, 24 parts by mass of epoxy acrylate which was an acrylic acid adduct of bisphenol A diglycidyl ether, 1 part by mass of Omnirad TPO, and 1 part by mass of Omnirad 184.
[0089] (Resin composition for belt)
[0090] 18 parts by mass of urethane acrylate which is a reaction product of bisphenol A-ethylene oxide addition glycol, toluene diisocyanate and hydroxyethyl acrylate, 10 parts by mass of urethane acrylate which is a reaction product of polytetramethylene glycol, toluene diisocyanate and hydroxyethyl acrylate, 15 parts by mass of tricyclodecane dimethanol diacrylate, 10 parts by mass of N-vinyl pyrrolidone, 10 parts by mass of isobornyl acrylate, 5 parts by mass of bisphenol A-ethylene oxide addition glycol diacrylate, 0.7 parts by mass of 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propane-1-one (Omnirad 907), and 1.3 parts by mass of Omnirad TPO were mixed to prepare a resin composition R.
[0091] [Fabrication of optical fiber]
[0092] A primary resin layer with a thickness of 17.5 μm was formed on the periphery of a glass fiber having a core and a cladding and a diameter of 125 μm using a resin composition P, and a secondary resin layer with a thickness of 15 μm was further formed on the periphery using a resin composition S to produce an optical fiber. Subsequently, after temporarily winding up the optical fiber, the optical fiber was rewound while a colored resin layer with a thickness of 5 μm was formed on the periphery of the secondary resin layer using the resin composition of Test Examples 1 to 11 using a coloring machine, thereby producing an optical fiber having a colored resin layer and a diameter of 200 μm (hereinafter referred to as a "colored optical fiber"). The line speed when forming each resin layer was 1500 m / min.
[0093] [Fabrication of optical fiber ribbon]
[0094] Four colored optical fibers were prepared, coated with the tape resin composition R, and then irradiated with ultraviolet rays for curing to form a connecting resin layer, thereby producing an optical fiber ribbon.
[0095] (Warm water test)
[0096] After measuring the transmission loss of the optical fiber ribbon, the optical fiber ribbon was immersed in warm water at 60°C for 60 days. The transmission loss of the optical fiber ribbon at a wavelength of 1.55 μm before and 30 days after immersion in warm water was measured by the OTDR (Optical Time Domain Reflection) method. When the difference between the transmission loss before immersion in warm water and the transmission loss after immersion in warm water for 60 days was less than 0.05 dB / km, it was evaluated as "A", and when it exceeded 0.05 dB / km, it was evaluated as "B".
[0097] (Color peeling test)
[0098] After the optical fiber ribbon was stored at 85°C and 85% RH (in the dark) for 30 days, the optical fibers were separated from the optical fiber ribbon according to Telcordia GR-20 5.3.1. The color resin layer was evaluated for peeling. If the color resin layer did not peel, it was evaluated as "A", and if it peeled, it was evaluated as "B".
[0099] [Table 1]
[0100]
[0101] Description of Reference Numerals
[0102] 1.1A optical fiber
[0103] 10. Fiberglass
[0104] 12 cores
[0105] 14 cladding
[0106] 20 coating resin layer
[0107] 22 primary resin layer
[0108] 24 Secondary resin layer
[0109] 26 Colored resin layer
[0110] 40 bonding resin layer
[0111] 100 fiber optic ribbon.
Claims
1. A resin composition for optical fiber coating, comprising a photopolymerizable compound and a photopolymerization initiator, The photopolymerizable compound includes epoxy di(meth)acrylate and alkylene oxide-modified tri(meth)acrylate having a bisphenol skeleton. The content of the alkylene oxide-modified tri(meth)acrylate is 0.5 mass % or more and less than 40 mass % based on the total amount of the photopolymerizable compound.
2. The resin composition according to claim 1, wherein The alkylene oxide-modified tri(meth)acrylate has at least one selected from the group consisting of ethylene oxide chains and propylene oxide chains. The resin composition according to claim 1 , further comprising titanium oxide.
4. A colored coating material for an optical fiber, comprising the resin composition according to any one of claims 1 to 3.
5. An optical fiber having: Glass fiber, including core and cladding; a primary resin layer, which is in contact with the glass fiber and covers the glass fiber; a secondary resin layer covering the primary resin layer; and a colored resin layer covering the secondary resin layer, and The colored resin layer comprises a cured product of the resin composition according to any one of claims 1 to 3.
6. An optical fiber having: Glass fiber, including core and cladding; a primary resin layer, in contact with the glass fibers and covering the glass fibers; and A secondary resin layer covers the primary resin layer, and The secondary resin layer comprises a cured product of the resin composition according to any one of claims 1 to 3.
7. An optical fiber ribbon, comprising: arranging a plurality of optical fibers according to claim 5 and coating the plurality of optical fibers according to claim 5 with a ribbon resin.
8. An optical fiber ribbon, comprising: arranging a plurality of optical fibers according to claim 6 and coating the plurality of optical fibers according to claim 6 with a ribbon resin.
Citation Information
Patent Citations
Optical fiber core wire
CN107001129A
Puncture-resistant reduced-diameter multimode optical fiber
CN113728259A
Resin composition, optical fiber secondary coating material, optical fiber and manufacturing method of optical fiber
CN113993921A
Coloring composition for optical fiber, colored element wire and colored unit using the same
JP2003279811A
Resin composition, optical fiber and method for producing optical fiber
TW202111031A