Polymerizable solutions for obtaining furan polymer impregnated materials

By adjusting the composition in a polymerizable solution of furan polymer impregnating wood, controlling the pH range and using condensate as a carrier, the problems of poor stability and insufficient environmental friendliness in the prior art are solved, and high-performance furan polymer impregnation is achieved Reuse of wood and condensate.

CN118922472APending Publication Date: 2024-11-08KENBONI GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380026792.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-23
Filing Date
2023-03-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the prior art, the polymerizable solution of furan polymer impregnated wood has poor stability, insufficient environmental friendliness, and difficulty in reusing condensate during storage and use, resulting in poor polymerization reactivity and unstable final product performance.

Method used

Polymerizable solution containing 25-75% furfurol, 0.01-0.15 mol/kg of carboxylic acid, 0.25-4% maleic anhydride and water-soluble alkali salts was used by controlling the initial pH in the range of 3-5, using The condensate of the wood curing process acts as a carrier, combines an appropriate amount of water-soluble alkali salt to stabilize the solution, and prepares a polymerizable solution through specific compositional proportions and steps.

Benefits of technology

Provides a stable polymerizable solution for storage at ambient temperature for at least 7 days, improving the dimensional stability, mechanical strength, leaching resistance and weather resistance of furan polymer-impregnated wood, reducing production costs, and achieving effective condensate Use again.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention relates to a polymerizable solution for impregnating wood, a method of impregnating wood using said solution and impregnated wood impregnated with said solution. The polymerizable solution comprises:-furfuryl alcohol in the range of 25 to 75 wt.%, based on the total weight of the solution,-carboxylic acid in the range of 0.01 to 0.15 mol / kg, based on the total weight of the solution,-maleic anhydride in the range of 0.25 to 4 wt.%, based on the total weight of the solution,-condensate from a previous curing process of wood in the range of 24 to 74 wt.%, based on the total weight of the solution, and-an amount of a water-soluble alkali salt to obtain a pH in the range of 3 to 5 at the point in time at which the solution is formed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to polymerizable solutions for obtaining furan polymer impregnation of materials, such as wood.

[0002] In particular, the invention relates to the reuse of condensates from previous drying and curing processes as carriers in polymerizable solutions. Background Art

[0003] Furan polymer impregnated wood is known in the art. Furan polymer impregnated wood is typically produced by applying / impregnating the wood with a suitable amount of a polymerizable solution / liquid and then heating and curing the wood so that the polymerizable compounds of the polymerizable solution polymerize / cure into the furan polymer in the wood units.

[0004] The polymerizable solution generally includes a low molecular weight furan derivative (eg, furfural, furfuryl alcohol, bis(hydroxymethyl)furan), or a combination thereof, and optionally a catalyst, an initiator, and a stabilizer.

[0005] Furfuryl alcohol polymerizes (resinsifies) in an acidic medium, wherein the acid initiates and accelerates the polymerization reaction. The presence of strong acids is undesirable, since this may lead to violent self-condensation polymerization of furfuryl alcohol which is difficult to control. Therefore, it is necessary to use a weak acid, such as an organic acid, in the polymerizable solution, which does not separate from the furfuryl alcohol during impregnation and polymerization / curing. It is advantageous to select a weak acid which also has a chemical affinity for the material to be impregnated, such as wood. A non-separating mixture with an enhanced affinity for wood is known from WO 02 / 30638.

[0006] For certain uses, it is desirable to impregnate porous materials (such as wood) with more dilute solutions of initiated furfuryl alcohol, providing better control and economy than disclosed in WO02 / 30638. It has been found that lower concentrations of furfuryl alcohol polymers (also known as furan polymers or furan resins) in wood still provide useful properties at lower cost and with less change in appearance. Wood prepared according to WO02 / 30638 is very dark in color. Using lower concentrations of furfuryl alcohol, colors ranging from light tan to dark brown can be obtained.

[0007] In the polymerizable solution, the concentration of furan polymer in the final cured product can be controlled by using a liquid carrier for furfuryl alcohol. The carrier is applied to the product together with furfuryl alcohol before the polymerization process begins.

[0008] Several carriers are known in the prior art, such as water, or water and ethanol. Furfuryl alcohol is soluble in water, so water can be used as a carrier for the diluted, uninduced furfuryl alcohol. Water is an environmentally friendly, inexpensive substance and is therefore generally a preferred carrier.

[0009] As mentioned above, the polymerizable solution includes an initiator for initiating the polymerization reaction. When the organic acid initiator is mixed with furfuryl alcohol and water (water as a carrier), the solution becomes very reactive, which may lead to polymerization of the furfuryl alcohol. Therefore, a stabilizer is required to provide a stable solution suitable for storage or at least impregnation before polymerization, which is the basis of WO 02 / 060660.

[0010] The first useful chemical stabilizers discovered were borax and the sodium salt of lignin sulfonic acid (lignin sulfonic acid). However, the sodium salt of lignin sulfonic acid exhibits low solubility and is expensive and difficult to handle, and is therefore not a preferred stabilizer. Borax can be used to form a buffer and is also a biocide (adding protection against biodegradation to the final furan polymer impregnated product). However, borax as a biocide is undesirable for environmental reasons because it is easily washed out of the final impregnated material and deposited in the environment.

[0011] Efforts have been made to prepare stable polymerizable solutions without using the above stabilizers. Such stable polymerizable solutions should be kept within a certain pH range during storage, because overly acidic polymerizable solutions will polymerize rapidly resulting in phase separation and, since this reaction is irreversible, will destroy the solution. On the other hand, overly basic polymerizable solutions will delay or hinder the polymerization reaction of the polymerizable solution during use, and thus fail to provide the desired reactivity and target properties of the final impregnated product.

[0012] One method of providing such a stable polymerizable solution includes using stable co-solvents disclosed in WO 2004 / 011216. Such co-solvents may be methanol, ethanol, acetone or other volatile solvents. These co-solvents are good solvents for furfuryl alcohol and are also good swelling agents for wood. Co-solvents dilute the acid concentration during storage and impregnation, thereby extending the shelf life of the polymerizable solution. When they are removed from the wood after impregnation, i.e. before curing, the reactivity of the solution increases (pH decreases) as the co-solvent evaporates from the wood. An effective co-solvent removal step should be added to the process. This removal step is preferably a vacuum drying process with a co-solvent recovery system so that the co-solvent can be reused. By using such a stable co-solvent, no further stabilizer is required and the ratio of initiator: furfuryl alcohol can be reduced. This is conducive to reducing the amount of leachable substances in the final impregnated wood product. Further, experiments have shown that stable co-solvents maintain the pH in the polymerizable solution until after the wood is impregnated. The pH then decreases (becomes more acidic), which promotes curing.

[0013] However, the use of such co-solvents is more expensive and places greater demands on safety and process equipment than the use of water, making them less desirable. These co-solvents are also considered volatile, difficult to recover, and flammable. The use of such flammable co-solvents in enclosed spaces (typically process equipment) that contain oxidants (such as oxygen from air) can result in the formation of an explosive atmosphere.

[0014] A conventional polymerization process for obtaining an impregnated wood product is known from inter alia EP 2435223 A1 (incorporated herein by reference). The process involves the use of an apparatus, i.e. a drying and curing chamber, for combined drying and curing. The process comprises applying a polymerizable solution to the material to be impregnated, such as wood, before the wood is introduced into the apparatus. The apparatus generally comprises a drain which allows a so-called "bottom condensate" formed by compounds in the polymerizable solution and compounds in the wood, such as water, furfuryl alcohol, organic compounds, polymers and resins, to be drawn off from the apparatus during the heating phase and to a lesser extent during the subsequent curing phase. Further, the main mechanism for removing water and other chemicals (the so-called "top condensate") is by means of a condenser which is introduced into the drying and curing chamber along its upper surface. This top condensate is formed mainly by recondensing evaporated water, furfuryl alcohol and volatile organic compounds (VOCs) from the polymerizable solution and the wood. The top condensate is then conveyed to a condensate tank for reuse. The bottom condensate is conveyed to a separation tank which separates the reusable portion of the condensate from the unusable high density polymer. Thereafter, the reusable portion is transferred to a condensate tank for reuse.

[0015] However, the reuse of such condensates, i.e. the top condensate as well as the reusable part of the bottom condensate, as a carrier, is challenging to provide a stable polymerizable solution suitable for obtaining the final impregnated wood product. This is partly due to the fact that the resinified and oligomerized components in the condensate originating from the polymerizable solution become increasingly non-polar during the curing process as the degree of polymerization increases. Since such components are soluble in furfuryl alcohol, the presence of these components in the condensate reduces the solubility of the organic furfuryl alcohol phase in water when the condensate is used as a carrier. This reduction in solubility manifests itself as an increase in the cloud point temperature, which is undesirable because the cloud point temperature of the initial polymerizable solution must be below the storage temperature of the solution to avoid phase separation. The condensate also has a low pH because acidic by-products are formed during the polymerization reaction. The low pH accelerates the polymerization reaction and therefore shortens the storage life of the polymerizable solution.

[0016] Furthermore, the impregnation of wood, especially the presence of an organic solvent as a carrier in the condensate, can extract non-polar components such as terpenes (e.g., α-pinene). Such non-polar components also affect water solubility, thereby increasing the cloud point temperature with increasing concentration.

[0017] It is therefore a first object of the present invention to provide polymerizable solutions for impregnating materials such as wood which overcome the disadvantages of the prior art.

[0018] A second object of the present invention is to provide a polymerizable solution which is cheaper and more environmentally friendly than known solutions.

[0019] A third object of the present invention is to provide a polymerizable solution which is stable when stored in a closed container at ambient temperature, typically 15 to 30°C, for at least 7 days, preferably at least 10 days, more preferably at least 14 days, and even more preferably at least 21 days.

[0020] A fourth object of the present invention is to provide furan polymer impregnated / chemically modified products, such as wood, having advantageous or improved properties, such as dimensional stability, mechanical strength, leaching resistance, decay resistance and weather resistance. Summary of the invention

[0021] In a first aspect, there is provided a polymerizable solution for impregnating wood, wherein the polymerizable solution comprises:

[0022] - furfuryl alcohol in the range of 25 to 75% by weight, based on the total weight of the solution,

[0023] - a carboxylic acid in the range of 0.01 to 0.15 mol / kg, based on the total weight of the solution,

[0024] - maleic anhydride in the range of 0.25 to 4 wt. %, based on the total weight of the solution,

[0025] - a water-soluble alkaline salt in an amount such that the pH of the initial composition is in the range of 3 to 5, and

[0026] - in the range of 24 to 74% by weight, based on the total weight of the solution, of condensate from a previous curing process of the wood, and

[0027] - an amount of a water-soluble alkaline salt to obtain a pH in the range of 3 to 5 at the point in time when the solution is formed.

[0028] In one embodiment according to the first aspect, a water-soluble base salt is added to obtain a pH in the range of 3 to 4.5, more preferably 3.5 to 4.

[0029] In one embodiment according to the first aspect, the amount of furfuryl alcohol is in the range of 30 to 60 wt%, preferably 35 to 60 wt%.

[0030] In one embodiment according to the first aspect, the water-soluble alkali salt is selected from at least one of a metal hydroxide salt, a metal bicarbonate salt and a metal carbonate salt.

[0031] In one embodiment according to the first aspect, the carboxylic acid is selected from at least one of citric acid, fumaric acid, malic acid, malonic acid, oxalic acid, tartaric acid, 2-furoic acid, benzoic acid, levulinic acid and salicylic acid, preferably citric acid.

[0032] In one embodiment according to the first aspect, the total amount of carboxylic acid and maleic anhydride is equal to or less than 4.5 wt %.

[0033] In a second aspect, there is provided an impregnated wood impregnated with a polymerizable solution according to the first aspect and any embodiment thereof.

[0034] In a third aspect, a method for preparing a polymerizable solution is provided, wherein the method comprises the following subsequent steps:

[0035] - providing the condensate from the solidification process in a container,

[0036] - Add furfuryl alcohol to the container,

[0037] - Add carboxylic acid, maleic anhydride and water soluble base salt to a container.

[0038] In one embodiment according to the third aspect, a certain amount of water-soluble alkali salt is added to obtain a pH in the range of 3 to 5 when preparing the solution.

[0039] In a fourth aspect, there is provided a polymerizable solution for impregnating wood, comprising:

[0040] - furfuryl alcohol in the range of 25 to 75% by weight, based on the total weight of the solution,

[0041] - a carboxylic acid in the range of 0.01 to 0.15 mol / kg, based on the total weight of the solution,

[0042] - maleic anhydride in the range of 0.25 to 4 wt. %, based on the total weight of the solution,

[0043] - in the range of 24 to 74% by weight, based on the total weight of the solution, of condensate from a previous curing process of the wood, and

[0044] - an amount of a water-soluble alkaline salt to obtain a pH in the range of 3 to 5 at the point in time when the solution is formed, and

[0045] - wherein the polymerizable solution is obtained by the process according to the third aspect.

[0046] In a fifth aspect, there is provided the use of the polymerizable solution according to the first aspect and any embodiment thereof for impregnating wood. DETAILED DESCRIPTION

[0047] The present invention will be described in more detail below with reference to the examples provided. However, the present invention is not limited to these examples.

[0048] Unless specifically defined herein, all technical and scientific terms used have the same meanings as commonly understood by one of ordinary skill in the art of polymer engineering and wood impregnation.

[0049] In order to mitigate environmental challenges particularly with regard to the disposal of condensate generated during the curing / polymerization process, the present invention provides a polymerizable solution for impregnating materials such as wood such that such condensate is reusable as a carrier in the polymerizable solution.

[0050] Thus, the present invention provides an optimized furan polymerizable solution which is suitable for storage, inexpensive and environmentally friendly, and further provides a furan polymer impregnated wood having favorable or improved properties such as dimensional stability, mechanical strength, resistance to leaching, rot and weathering, and uniform color and density, and can utilize condensate as a carrier in the solution.

[0051] Thus, in a first aspect, there is provided a polymerizable solution for impregnating wood, wherein the polymerizable solution comprises:

[0052] - furfuryl alcohol in the range of 25 to 75% by weight, based on the total weight of the solution,

[0053] - a carboxylic acid in the range of 0.01 to 0.15 mol / kg, based on the total weight of the solution,

[0054] - maleic anhydride in the range of 0.25 to 4 wt. %, based on the total weight of the solution,

[0055] - a water-soluble alkaline salt in an amount such that the pH of the initial composition is in the range of 3 to 5, and

[0056] - in the range of 24 to 74% by weight, based on the total weight of the solution, of condensate from a previous curing process of the wood, and

[0057] - an amount of a water-soluble alkaline salt to obtain a pH in the range of 3 to 5 at the point in time when the solution is formed.

[0058] Also described herein is a polymerizable solution for impregnating a material such as wood having a composition comprising:

[0059] - furfuryl alcohol in the range of 25 to 75% by weight, based on the total weight of the composition of the polymerizable solution,

[0060] - a carboxylic acid in the range of 0.01 to 0.15 mol / kg, based on the total weight of the composition of the polymerizable solution,

[0061] - maleic anhydride in the range of 0.25 to 4 wt. %, based on the total weight of the composition of the polymerizable solution,

[0062] - a water-soluble alkaline salt in an amount such that the pH of the initial composition is in the range of 3 to 5, and

[0063] - in the range of 24 to 74 wt. % water and / or condensate, based on the total weight of the composition of the polymerizable solution.

[0064] The water-soluble base salt is always present in the polymerizable solution because the pH of the initial composition without the water-soluble base salt is always less than 3.

[0065] The polymerizable solution of the above composition is suitable for storage, meaning that the solution can be stored in a closed container under ambient conditions for at least 7 days, preferably at least 10 days, more preferably at least 14 days or even more preferably at least 21 days without separation.

[0066] Since the condensate used as a carrier in the polymerizable solution is acidic and may have a pH of less than 3, when it is added as an alternative carrier to water in a conventional furan polymerizable solution, it will accelerate the polymerization of the solution, thus providing a solution that separates rapidly. A solution that separates rapidly, such as for example within 48 hours, is undesirable because the application / impregnation of the material must be performed before any such separation occurs. The composition of the polymerizable solution of the present invention alleviates this problem, since the polymerizable solution includes an organic buffer provided by the presence of a carboxylic acid as a buffer and a controlled amount of a water-soluble alkali salt for adjusting the pH of the initial polymerizable solution to a target pH range of 3 to 5, or more preferably within a pH range of 3 to 4.5, or even more preferably within a pH range of 3.5 to 4, as this range has been shown to provide the most stable polymerizable solution and further maintains good reactivity when heated during the polymerization process.

[0067] The carboxylic acid added to the polymerization solution of the present invention does not act as an initiator, but rather as a buffer to keep the pH as stable as possible during storage, so that the acidity of the condensate does not affect the pH stability of the solution, providing a less sensitive and more stable polymerization solution. Experiments have shown that the amount of carboxylic acid in the polymerizable solution must be in the range of 0.01 to 0.15 mol / kg based on the total mass of the polymerizable solution.

[0068] Overly acidic polymerizable solutions, such as solutions with a pH value of less than 3, will rapidly polymerize resulting in phase separation and, since this reaction is irreversible, will destroy the solution. On the other hand, overly basic polymerizable solutions, such as solutions with a pH value of greater than 5, will delay or hinder the polymerization reaction of the polymerizable solution during use and thus fail to provide the desired reactivity and target properties of the final impregnated product. It is therefore important to provide a polymerizable solution in which the pH of the initial solution can be controlled to a pH value in the range of 3 to 5, which would not be considered overly acidic or overly basic. Due to the acidity of the condensate in the polymerizable solution, the amount of water-soluble alkaline salt added will depend on its acidity and the buffering range and buffering capacity of the acid added.

[0069] The water-soluble base salt may advantageously be selected from at least one of a metal hydroxide salt, a metal bicarbonate salt and a metal carbonate salt, since for all practical purposes these merely add cations and OH to the polymerizable solution. - , thereby mainly affecting the pH of the polymerizable solution. Preferably, the water-soluble alkali salt is sodium carbonate (Na2CO3), which is environmentally friendly, easily available and inexpensive.

[0070] It is generally known that a buffer solution has the ability to resist changes in pH with changes in acid or base concentration. The buffer capacity (β) is a quantitative measure of this and for solutions of simple carboxylic acids it can be expressed as:

[0071]

[0072] in:

[0073] [H + ] is H + The equilibrium concentration of ions,

[0074] C CA is the total concentration of carboxylic acids in solution,

[0075] K a is the acid dissociation constant of the carboxylic acid, and

[0076] K W is the dissociation constant of water.

[0077] The above equation shows that the buffer capacity of this solution depends mainly on the carboxylic acid concentration. For monocarboxylic acids, when pH = pK a The buffer capacity is maximum when pH = pK a ± 1, the buffer capacity drops to 33% of the maximum value, when pH = pK a ± 1.5, the buffer capacity drops to 12% of the maximum value, when pH = pK a ± 2, the buffer capacity drops to 4% of the maximum value. Therefore, for dicarboxylic acids, when pK a1+ 1 = pH = pK a2 − 1, pK a The difference of 2 will result in a total buffer capacity of 66%, while pK a A difference of 3 in value would provide a 24% buffer capacity at the midpoint.

[0078] Therefore, the pK of the carboxylic acid in the polymerizable solution is a value, or if more than one pK a The value may preferably be within ± 1.5 of the target pH or within ± 1.5 of one of the end points of the target pH range (buffer zone). Preferably, the pK of the carboxylic acid of the polymerizable solution is a value, or if more than one pK a The value may preferably be within ± 1 of the target pH or within ± 1 of one of the endpoints of the target pH range.

[0079] Furthermore, with several pK a Polycarboxylic acids having values ​​that differ by ≤ 3 (ie, Δ ≤ 3) have an enhanced buffering capacity, which is beneficial and is therefore preferred.

[0080] Carboxylic acids suitable as buffering agents may include, but are not limited to, at least one of the following: monocarboxylic acids, such as acetic acid, propionic acid, and butyric acid; unsaturated carboxylic acids, such as crotonic acid and sorbic acid; hydroxycarboxylic acids, such as glycolic acid and lactic acid; ketocarboxylic acids, such as pyruvic acid and levulinic acid; heteroaromatic carboxylic acids, such as 2-furoic acid; phenylcarboxylic acids, such as benzoic acid, salicylic acid, and gallic acid; dicarboxylic acids, such as oxalic acid, malonic acid, and succinic acid; unsaturated dicarboxylic acids, such as fumaric acid; hydroxydicarboxylic acids, such as malic acid and tartaric acid; and tricarboxylic acids, such as propane-1,2,3-tricarboxylic acid, aconitic acid, and citric acid.

[0081] The carboxylic acid of the polymerizable solution of the present invention may preferably be at least one selected from citric acid, fumaric acid, malic acid, malonic acid, oxalic acid, tartaric acid, 2-furoic acid, levulinic acid, benzoic acid and salicylic acid.

[0082] As described above, the total amount of carboxylic acid added to the total composition is in the range of 0.01 to 0.15 mol / kg, based on the total composition of the polymerizable solution. As known to those skilled in the art, this amount would correspond to about 0.25 to 3 wt% citric acid, about 0.15 to 1.8 wt% fumaric acid, about 0.17 to 2.1 wt% malic acid, about 0.14 to 1.6 wt% malonic acid, about 0.12 to 1.4 wt% oxalic acid, about 0.20 to 2.3 wt% tartaric acid, about 0.15 to 1.8 wt% 2-furoic acid, about 0.15 to 1.8 wt% levulinic acid, about 0.18 to 2.2 wt% salicylic acid, and about 0.16 to 1.9 wt% benzoic acid, all based on the weight of the total composition of the polymerizable solution.

[0083] Non-carboxylic acids, such as phosphoric acid and sulfuric acid, are not suitable buffers because the solution will separate rapidly. a The values ​​are 2.1, 7.2 and 12.4, thus having a Δ>3 makes it less suitable than, for example, citric acid which meets this criterion. Sulfuric acid is not a weak acid and would therefore accelerate the polymerisation process and is therefore unsuitable.

[0084] Other favorable characteristics of carboxylic acids that may also affect polymerizable solutions are properties such as the partition coefficient (log P), dipole moment (Ð), proticness, and hydrogen bonding, which may be properties that indicate the polarity and intermolecular forces of the compound, subsequently determining solubility properties and solvation.

[0085] Citric acid is considered to be preferably suitable because it is highly soluble in both water and furfuryl alcohol and further has a pK a value, which stabilizes the pH of the polymerizable solution within the above range and thus has a greater buffering capacity. Further, citric acid is inexpensive and is considered environmentally friendly when released into nature.

[0086] Experiments have shown that the amount of carboxylic acid should be limited, i.e. should not exceed 0.15 mol / kg of the total composition, since too high an amount will reduce the storage time of the polymerizable solution, i.e. the time for phase separation, thus allowing the carboxylic acid to act more as an initiator than as a buffer and thus providing a less stable polymerizable solution that is less suitable for storage.

[0087] Therefore, maleic anhydride is added to the solution as an initiator in the polymerization solution. Maleic anhydride is a well-known initiator having very good initiation properties and wood affinity and is more environmentally friendly than other initiators known in the prior art, such as phthalic anhydride.

[0088] Advantageously, in order to limit the acceleration of the polymerization of the polymerizable solution, the total amount of carboxylic acid and maleic anhydride in the polymerizable solution may be equal to or less than 4.5% by weight, even more preferably less than 4.

[0089] Another problem associated with the reuse of condensate from conventional furan polymerizable solutions relates to the presence of oligomers and possibly other compounds in the condensate, which are not soluble in water. Such compounds must be dissolved in the polymerizable solution prior to storage and impregnation to ensure uniform density and uniform surface structure of the final impregnated product, thus providing better weather resistance, mechanical strength properties, etc.

[0090] The polymerizable solutions of the present invention are prepared by having a sufficient amount of furfuryl alcohol in the polymerizable solution to dissolve the compound.

[0091] In general, for all polymerizable solutions suitable for storage, it is also important that the cloud point temperature (Cp) of the initial polymerizable solution be below the storage temperature of the solution. The cloud point temperature is defined as the temperature at which the onset of phase separation, where turbidity of the solution can be visually observed, occurs. The presence of oligomers in the solution contributes to an increase in the cloud point temperature of the polymerizable solution, while an increase in the presence of furfuryl alcohol decreases the cloud point temperature.

[0092] Therefore, in addition to being an essential component for the polymerization of the polymerizable solution, the amount of furfuryl alcohol is also important to provide a stable polymerizable solution suitable for storage.

[0093] The amount of furfuryl alcohol should be at least 25% by weight of the total composition of the polymerizable solution to provide this property.

[0094] The amount of furfuryl alcohol in the most stable polymerizable solution for storage is from 25 to 75 wt %, preferably in the range of 30 to 60 wt %, even more preferably in the range of 35 to 60 wt % of the total composition of the polymerizable solution.

[0095] Wood and wood materials are the primary products impregnated and polymerized by the polymerizable solutions of the present invention, but other porous materials such as brick, Portland cement, concrete and stone may also be similarly impregnated.

[0096] In a third aspect, there is provided impregnated wood impregnated with the polymerizable solution according to the first aspect and embodiments thereof.

[0097] A fourth aspect of the present invention provides a method for preparing the polymerizable solution according to the first aspect.

[0098] The method includes the following subsequent steps:

[0099] - the condensate from the solidification process is placed in a container,

[0100] - add furfuryl alcohol to the vessel containing the condensate,

[0101] - Add carboxylic acid, maleic anhydride and water soluble base salt to the vessel containing furfuryl alcohol and condensate.

[0102] In other words, the method may include adding the carrier in the form of a condensate to a container. Furfuryl alcohol may then be added to the same container, preferably during stirring. The carboxylic acid, maleic anhydride and water-soluble base salt may then be added simultaneously or nearly simultaneously while measuring the pH of the initial polymerizable solution.

[0103] In one embodiment, an amount of the water-soluble alkali metal salt is added to obtain a pH in the range of 3 to 5 when the solution is prepared.

[0104] The pH of the initial polymerizable solution can be measured by any conventional method known in the art.

[0105] The method may further include stirring or mixing during each step and / or between each step.

[0106] Depending on the process equipment, the entire process may take from about 5 minutes to several hours.

[0107] If the container is stored at non-ambient temperatures, the container is preferably made of a material that protects the contents therein from the surrounding environment.

[0108] In a fourth aspect, there is provided a polymerizable solution for impregnating wood, comprising:

[0109] - furfuryl alcohol in the range of 25 to 75% by weight, based on the total weight of the solution,

[0110] - a carboxylic acid in the range of 0.01 to 0.15 mol / kg, based on the total weight of the solution,

[0111] - maleic anhydride in the range of 0.25 to 4 wt. %, based on the total weight of the solution,

[0112] - in the range of 24 to 74% by weight, based on the total weight of the solution, of condensate from a previous curing process of the wood, and

[0113] - an amount of a water-soluble alkaline salt to obtain a pH in the range of 3 to 5 at the time of preparation of the solution, and

[0114] - wherein the polymerizable solution is obtained by the method according to the third aspect.

[0115] Also provided is a polymerizable solution for impregnating a material, such as wood, wherein the solution comprises:

[0116] - furfuryl alcohol in the range of 25 to 75 wt. %, based on the total composition weight of the polymerizable solution,

[0117] - a carboxylic acid in the range of 0.01 to 0.15 mol / kg, based on the total composition weight of the polymerizable solution,

[0118] - maleic anhydride in the range of 0.25 to 4 wt. %, based on the total composition weight of the polymerizable solution,

[0119] - a water-soluble alkaline salt in an amount such that the pH of the initial composition is in the range of 3 to 5, and

[0120] - condensate in the range of 24 to 74 wt. %, based on the total composition weight of the polymerizable solution, and

[0121] - wherein the polymerizable solution is obtained by the above method.

[0122] In a fifth aspect, the present invention discloses the use of the polymerizable solution of the first aspect and embodiments thereof for impregnating wood to obtain a final impregnated wood product.

[0123] The term "initial composition / initial polymerizable solution" should be interpreted as the starting composition of the polymerizable solution before storage. Thus, it is the composition of the polymerizable solution after addition and mixing of all ingredients.

[0124] The term "impregnating" should be interpreted as the act of applying a polymerizable solution to a material (eg wood) in a process of obtaining an impregnated product (eg impregnated wood).

[0125] The term "final furan polymer impregnated product / impregnated product" should be interpreted as the product / material obtained after the material has been impregnated and cured / polymerized. Thus, the material comprises furan polymer, for example, furan polymer impregnated wood.

[0126] The term "condensate" is to be interpreted as a liquid solution comprising the so-called "top condensate" and the reused part of the so-called "bottom condensate" obtained during the drying and curing of impregnated wood with the polymerizable solution according to the invention. The condensate thus mainly comprises water, furfuryl alcohol, residues of organic compounds and acids obtained from the previous curing of wood with the polymerizable solution according to the invention.

[0127] The term "stable solution" is to be interpreted as a polymerizable solution that does not phase separate. Thus, a stable solution can be stored at ambient temperature and pressure for at least 7 days without phase separation, preferably 10 days, more preferably 14 days, even more preferably 21 days.

[0128] The ranges mentioned herein should be interpreted as being inclusive of the endpoints.

[0129] Ambient temperature is to be interpreted as a temperature of 15 to 30° C. Ambient pressure is to be interpreted as atmospheric pressure. The term “ambient conditions” is to be interpreted as conditions where the temperature is 15 to 30° C. and the pressure is atmospheric pressure.

[0130] In the first experiment below, the polymerizable solutions were prepared with water as carrier for the purpose of comparing the varying amounts of the components in the polymerizable solutions. As already mentioned, the composition of the condensates differed, since each polymerization process produced a condensate of different composition.

[0131] Therefore, as shown in Table 1, experiments were performed using polymerizable solutions of different compositions.

[0132] Table 1:

[0133]

[0134] In the experiment, furfuryl alcohol (FA), maleic anhydride (MA), carboxylic acid buffer (represented by citric acid (CA)), water-soluble alkali salt (represented by anhydrous sodium carbonate (SC)) and water were mixed together and stored at 27°C and ambient pressure for up to 21 days. The amounts of FA, MA, CA and SC in the solution are expressed as weight % (wt%), and the remaining ingredient is water, so that the amounts of all ingredients add up to 100 wt%, which is the total composition of the polymerizable solution.

[0135] Table 1 shows that the initial pH of the polymerizable solution was about 3.8 to 3.9. This was the pH of the solution after all components were added together and stirred until a homogeneous solution was obtained, and was therefore the pH when the solution was initially placed in storage.

[0136] Table 1 also shows that the storage time for 1 day (d1) and 14 days (d 14 ), as well as the pH on the day of storage (d0) and after 14 days of storage (d 14 ) after the pH value difference ΔpH (d0-d 14 ).

[0137] The solutions were also stored for 1 day (d1) and 14 days (d 14 ) after the cloud point temperature (Cp).

[0138] The last few columns of the table indicate the storage of the solutions for 1 day (d1), 7 days (d7), 14 days (d 14 ) and 21 days (d 21 ), wherein "N" indicates that no phase separation occurs, and "Y" indicates that phase separation occurs.

[0139] Experiments No. 1-6, 10 and 11 show that the first 14 days (d 14 ). Therefore, these solutions are considered stable.

[0140] Further, it is shown from the table that adding too much carboxylic acid initiator to the composition, for example equal to or higher than 4 wt%, provides a solution with poor stability, resulting in phase separation within 14 days of storage, as shown in Experiment Nos. 7, 12 and 13. Therefore, it is important to control the total amount of added acid to avoid premature initiation of the polymerization process.

[0141] Further, the experiments showed that solutions with less than 20 wt% furfuryl alcohol (experiment numbers 8 and 9) also phase separated within 14 days of storage. This is because the small amount of furfuryl alcohol has a lower tolerance to the presence of oligomers and polymers that accumulate over time before phase separation occurs, thus causing its cloud point (Cp) to rise faster than similar solutions with more FA. Therefore, the polymerizable solution should contain at least 25 wt% furfuryl alcohol to provide a stable polymerizable solution.

[0142] Furthermore, the experiment also completed the comparison of the initial cloud point temperature of the polymerizable solution, using water or condensate as a carrier, and not adding carboxylic acid as a buffer. For comparison reasons, the experimental polymerizable solution includes 35 wt% furfuryl alcohol, 1 wt% maleic anhydride (MA) and a water-soluble alkali salt (expressed as anhydrous sodium carbonate (SC)) for adjusting the initial pH, see Table 2 below.

[0143] Table 2:

[0144]

[0145] As shown in Table 2, when water is used as a carrier, the initial cloud point is significantly lower than the initial cloud point for the condensate as a carrier. Therefore, under the same conditions, using water as a carrier provides a more stable polymerizable solution than using a condensate as a carrier. Therefore, Table 2 illustrates the challenges involved in providing a stable polymerizable solution when using a condensate as a carrier.

[0146] Table 3 below lists examples of preferred carboxylic acids, their pK a value or if more than 1 at least one pK a value, within ± 1 of the target pH or within ± 1 of one of the end points of the target pH range (buffer).

[0147] Furthermore, the pK of the preferred polycarboxylic acid is a The value difference is ≤ 3, that is, Δ ≤ 3.

[0148] Table 3:

[0149] .

Claims

1. A polymerizable solution for impregnating wood, characterized in that The solution comprises: - furfuryl alcohol in the range of 25 to 75% by weight, based on the total weight of the solution, - a carboxylic acid in the range of 0.01 to 0.15 mol / kg, based on the total weight of the solution, - maleic anhydride in the range of 0.25 to 4 wt. %, based on the total weight of the solution, - a water-soluble alkaline salt in an amount such that the initial composition comprises a pH in the range from 3 to 5, and - in the range of 24 to 74% by weight, based on the total weight of the solution, of condensate from a previous curing process of the wood, and - an amount of a water-soluble alkaline salt to obtain a pH ranging from 3 to 5 at the time of preparing the solution.

2. The polymerizable solution according to claim 1, wherein the water-soluble base salt is added to obtain a pH in the range of 3 to 4.5, more preferably 3.5 to 4.

3. The polymerizable solution according to any one of the preceding claims, wherein the amount of furfuryl alcohol is in the range of 30 to 60 wt%, preferably 35 to 60 wt%.

4. The polymerizable solution according to any one of the preceding claims, wherein the water-soluble alkali salt is selected from at least one of a metal hydroxide salt, a metal bicarbonate salt and a metal carbonate salt.

5. The polymerizable solution according to any one of the preceding claims, wherein the carboxylic acid is selected from at least one of citric acid, fumaric acid, malic acid, malonic acid, oxalic acid, tartaric acid, 2-furoic acid, benzoic acid, levulinic acid and salicylic acid, preferably citric acid.

6. The polymerizable solution according to any one of the preceding claims, wherein the total amount of carboxylic acid and maleic anhydride is equal to or less than 4.5 wt%.

7. Impregnated wood impregnated with the polymerizable solution according to any one of claims 1 to 6.

8. A method for preparing a polymerizable solution according to any one of claims 1 to 6, wherein the method comprises the following subsequent steps: - providing the condensate from the solidification process in a container, - adding furfuryl alcohol to said container, - Add carboxylic acid, maleic anhydride and water soluble base salt to the container.

9. A polymerizable solution for impregnating wood, the solution comprising: - furfuryl alcohol in the range of 25 to 75% by weight, based on the total weight of the solution, - a carboxylic acid in the range of 0.01 to 0.15 mol / kg, based on the total weight of the solution, - maleic anhydride in the range of 0.25 to 4 wt. %, based on the total weight of the solution, - in the range of 24 to 74% by weight, based on the total weight of the solution, of condensate from a previous curing process of the wood, - an amount of a water-soluble alkaline salt to obtain a pH in the range of 3 to 5 at the time of preparing the solution, and -in, The polymerizable solution is obtained by the method according to claim 8.

10. Use of the polymerizable solution according to any one of claims 1 to 6 for impregnating wood.