Method for producing water-absorbent resin powder
By controlling the gel pulverizing parameters using a multi-screw mixer and a continuous gel pulverizing device, the problems of gel particle size and equipment adhesion were solved, resulting in the production of highly efficient water-absorbing resin powder.
Patent Information
- Application Number
- CN202380029405.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-08-04
- Filing Date
- 2023-03-28
- Publication Date
- 2024-11-08
AI Technical Summary
Existing technologies struggle to produce gel particles with diameters smaller than a few millimeters to a few centimeters, and gel pulverizers are prone to sticking to equipment, leading to equipment damage and time-consuming cleaning.
A multi-screw mixer was used for gel pulverization, with the gel pulverization coefficient controlled to be above 0.02 J/g·s and below 3 J/g·s, and the mass-average particle size below 500 μm. A continuous gel pulverization device was used to produce granular hydrogels.
This technology enables the production of water-absorbing resin powder with excellent water absorption speed, reduces the amount of residual monomer, and decreases equipment adhesion and cleaning time.
Smart Images

Figure CN118922476A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing water-absorbent resin powder. Background Art
[0002] Super absorbent polymer (SAP) is a water-swellable, water-insoluble polymer gelling agent, and is commonly used in various fields such as absorbent articles such as disposable diapers and sanitary napkins, water-retaining agents for agriculture, forestry and horticulture, and industrial water-stopping agents.
[0003] Among the water-absorbent resins mentioned above, a large amount of monomers and hydrophilic polymers are used as raw materials. From the viewpoint of water absorption performance, polyacrylic acid (salt)-based water-absorbent resins using acrylic acid and / or its salt as monomers are most commonly produced industrially.
[0004] As the main purpose of disposable diapers is becoming more high-performance, various functions (higher physical properties) are required for the water-absorbent resin. Specifically, in addition to the water absorption rate without pressure and the water absorption rate under pressure as basic physical properties, the water-absorbent resin is also required to have various physical properties such as gel strength, water-soluble components, water content, water absorption rate, liquid permeability, particle size distribution, urine resistance, antibacterial properties, damage resistance, powder fluidity, deodorization, coloring resistance, low dust, and low residual monomers. In particular, in the use of sanitary products such as disposable diapers, as the products become thinner, it is expected that the water absorption rate will be further improved.
[0005] The commercial production method of the above-mentioned powdered or granular water-absorbent resin typically includes the following steps: a polymerization step; a gel pulverization (fine granulation) step performed after or during the polymerization; a drying step of the finely granulated gel; a pulverization step of the dried product; a classification step of the pulverized product; a recovery step of fine powders produced by pulverization and classification; and a surface cross-linking step of the classified water-absorbent resin powder.
[0006] As one of the methods for producing water-absorbent resins proposed so far, there is a method for simultaneously performing a polymerization step and a gel pulverization step using a polymerization device having a pulverization mechanism. In the case of this production method, while the liquid monomer is polymerized, the generated hydrogel is pulverized, and the hydrogel in fine particles is discharged from the polymerization device. As specific examples thereof, methods using a batch kneader or a continuous kneader are described in Patent Documents 1 to 3.
[0007] However, the size of the gel particles obtained by these devices is about several mm to several cm, and in recent years, the gel pulverization is insufficient under the situation that further improvement of water absorption speed is required, and an additional gel pulverization device is required. Patent document 4 proposes a method of wet pulverizing the gel particles to a size smaller than the product particle size of the water-absorbent resin using a batch kneader or a continuous kneader, but the size of the device becomes too large, which is not realistic.
[0008] In addition, in the polymerization process, the hydrogel with high adhesion during the polymerization reaction of the monomer is crushed by gel. Therefore, the hydrogel is easy to adhere to the components inside the device, and then reacts in the adhered state, so the hydrogel is fixed, which may cause damage to the components or take time to clean during maintenance.
[0009] Prior art literature
[0010] Patent Literature
[0011] Patent Document 1: Japanese Patent Application Laid-Open No. 57-34101
[0012] Patent Document 2: Japanese Patent Application Laid-Open No. 60-55002
[0013] Patent Document 3: International Publication No. 2001 / 038402
[0014] Patent Document 4: Japanese Patent Application Laid-Open No. 05-112654 Summary of the invention
[0015] In recent years, in order to obtain a water-absorbent resin having an excellent water absorption rate, which is particularly sought after, it is necessary to grind the hydrogel into a particle size smaller than that of conventional methods in the gel grinding step. However, in conventional so-called kneader polymerization in which a polymerization step and a gel grinding step are simultaneously performed using a kneading machine having a plurality of screws, it is impossible to obtain a hydrogel having a desired particle size.
[0016] Therefore, an object of the present invention is to provide a water-absorbent resin having an excellent water absorption rate. Another object of the present invention is to reduce residual monomers.
[0017] The present inventors first discovered that, when a hydrogel-like crosslinked polymer is conventionally obtained by using an extruder (a meat slicer) equipped with a porous plate (also referred to as a die, dies) to obtain a granular hydrogel-like crosslinked polymer (hereinafter also referred to as "granular hydrogel"), it is possible to continuously obtain a granular hydrogel by using a multi-screw kneader (particularly a twin-screw kneader) to grind the gel. The inventors further discovered that, by setting the polymerization rate of the hydrogel-like crosslinked polymer to 90% by mass or more, setting the gel grinding coefficient to 0.02 J / g·sec or more and 3 J / g·sec or less, and setting the solid content-converted mass average particle size of the granular hydrogel-like crosslinked polymer discharged from the multi-screw kneader to 500 μm or less, a water-absorbent resin powder having an excellent water absorption rate can be obtained, thereby completing the present invention.
[0018] That is, the present invention is a method for producing a water-absorbent resin powder, comprising the following steps: a polymerization step of polymerizing a monomer aqueous solution to obtain a hydrogel-like crosslinked polymer; and a gel pulverization step of pulverizing the hydrogel-like crosslinked polymer using a gel pulverizing device to obtain a particulate hydrogel-like crosslinked polymer after the polymerization step, the gel pulverizing device comprising an inlet, a discharge port, and a main body having a plurality of rotating shafts therein, each of the rotating shafts having a pulverizing unit, in the gel pulverization step, the hydrogel-like crosslinked polymer is continuously fed from the inlet, and the particulate hydrogel-like crosslinked polymer is continuously taken out from the discharge port, the polymerization rate of the hydrogel-like crosslinked polymer fed to the inlet having a polymerization rate of 90% by mass or more, a gel pulverization coefficient of 0.02 J / g·second or more and 3 J / g·second or less, and the particulate hydrogel-like crosslinked polymer discharged from the discharge port having a mass average particle size calculated as a solid content of 500 μm or less. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a partially cutaway side view showing an example of a gel grinding device used in the production method according to the embodiment of the present invention.
[0020] Figure 2 yes Figure 1 An enlarged view of the gel grinding device (view of the central part of the main body from above).
[0021] Figure 3 This is a diagram showing an example of a specific configuration of a rotating shaft included in the gel grinding device used in the Examples.
[0022] Figure 4 This is a diagram showing an example of a specific configuration of a rotating shaft included in the gel grinding device used in the Examples.
[0023] Figure 5This is a diagram showing an example of a specific configuration of a rotating shaft included in the gel grinding device used in the Examples.
[0024] Figure 6 This is a diagram showing an example of a specific configuration of a rotating shaft included in the gel grinding device used in the Examples.
[0025] Figure 7 This is a diagram showing an example of a specific configuration of a rotating shaft included in the gel grinding device used in the Examples.
[0026] Figure 8 It is a front view showing an example of a disk. DETAILED DESCRIPTION
[0027] The present invention is described in detail below, but the scope of the present invention is not limited to these descriptions. In addition to the following examples, it can also be implemented by appropriately changing within the scope that does not damage the gist of the present invention. In addition, the present invention is not limited to the following embodiments, and various changes can be made within the scope indicated in the claims. Other embodiments obtained by appropriately combining the technical means disclosed for a plurality of embodiments are also included in the technical scope of the present invention.
[0028] [1] Definition of terms
[0029] 〔1-1〕"Water-absorbent resin"
[0030] The "water-absorbent resin" in the present invention refers to a water-swellable, water-insoluble polymer gelling agent that satisfies the following physical properties. That is, it refers to a polymer gelling agent that has a water-swellable CRC (centrifuge retention capacity) of 5 g / g or more as specified in NWSP 241.0.R2 (15), and a water-insolubility of 50% by mass or less as specified in NWSP 270.0.R2 (15).
[0031] [1-2] "Poly (meth) acrylic acid (salt)"
[0032] The "poly(meth)acrylic acid (salt)" in the present invention refers to a (co)polymer of (meth)acrylic acid and / or its salt, and refers to a cross-linked polymer that contains a structure derived from (meth)acrylic acid and / or its salt (hereinafter also referred to as "(meth)acrylic acid (salt)") as a main component as a repeating unit and contains a structure derived from an internal cross-linking agent as an optional component.
[0033] The above-mentioned "main component" means that the amount (content) of (meth)acrylic acid (salt) is preferably 50 mol% to 100 mol%, more preferably 70 mol% to 100 mol%, further preferably 90 mol% to 100 mol%, and particularly preferably substantially 100 mol%, relative to the total monomers used in the polymerization (all monomers excluding the cross-linking agent).
[0034] 〔1-3〕Definition of evaluation method
[0035] "NWSP" stands for "Non-Woven Standard Procedures-Edition 2015", which is a standard jointly issued by EDANA (European Disposables And Nonwovens Association) and INDA (Association of the Nonwoven Fabrics Industry) in the United States and Europe for the evaluation method of nonwoven fabrics and their products, and represents the standard measurement method of water-absorbent resin. Unless otherwise specified, the physical properties of water-absorbent resin are measured in accordance with "Non-Woven Standard Procedures-Edition 2015" in the present invention. For evaluation methods not described in NWSP, they are measured by the methods and conditions described in the Examples.
[0036] [1-3-1] "CRC" (NWSP 241.0.R2(15))
[0037] "CRC" is the abbreviation of Centrifuge Retention Capacity, which refers to the water absorption rate of a water-absorbent resin without pressure (sometimes also referred to as "water absorption rate"). Specifically, it refers to the water absorption rate (unit: g / g) after 0.2 g of a water-absorbent resin is put into a non-woven bag, immersed in a significantly excessive 0.9 mass % sodium chloride aqueous solution for 30 minutes to allow it to swell freely, and then drained by a centrifuge (250G) for 3 minutes. It should be noted that for the hydrogel-like cross-linked polymer after polymerization and / or gel crushing (hereinafter also referred to as "hydrogel"), 0.4 g of hydrogel is used, the measurement time is changed to 24 hours, and solid content correction is performed to obtain CRC.
[0038] [1-3-2] "Moisture Content" (NWSP 230.0.R2(15))
[0039] "Moisture Content" refers to the moisture content specified by the drying loss of the water-absorbent resin. Specifically, it refers to the value calculated from the drying loss when 4.0 g of the water-absorbent resin is dried at 105°C for 3 hours (unit: mass %). It should be noted that in the present invention, the water-absorbent resin after drying is specified by the drying loss of 1.0 g of the water-absorbent resin at 180°C for 3 hours, and the water-containing gel before drying is specified by the drying loss of 2.0 g of the water-containing gel at 180°C for 24 hours.
[0040] [1-3-3] "PSD" (NWSP 220.0.R2(15))
[0041] "PSD" is the abbreviation of Particle Size Distribution, which refers to the particle size distribution of the water-absorbent resin measured by sieving. It should be noted that the mass mean particle size (D50) and the logarithmic standard deviation (σζ) of the particle size distribution are measured by the same method as described in U.S. Patent No. 7,638,570. It should be noted that in the present invention, the particle size distribution (PSD) of the particulate hydrogel is specified by sieving in a wet manner using the method described below. Furthermore, the particle size (μm) converted to the solid content of the particulate hydrogel is specified based on the particle size (μm) of the particulate hydrogel and its solid content (mass %) and using the calculation method described below.
[0042] [1-3-4] "AAP" (NWSP 242.0.R2(15))
[0043] "AAP" is the abbreviation of Absorption Against Pressure, which refers to the water absorption rate of water-absorbent resin under pressure. Specifically, it means: 0.9g of water-absorbent resin is subjected to 2.06kPa (21g / cm 2 The water absorption ratio (unit: g / g) after swelling for 1 hour with a significantly excessive amount of 0.9 mass % sodium chloride aqueous solution under a load of 4.83 kPa (equivalent to about 49 g / cm 2 , about 0.7psi).
[0044] [1-3-5] "Vortex"
[0045] The term "Vortex" as used herein is an index indicating the water absorption rate of a water-absorbent resin, and refers to the time (unit: seconds) required for 2 g of the water-absorbent resin to absorb 50 ml of a 0.9 mass % sodium chloride aqueous solution to a predetermined state.
[0046] 〔1-4〕"Gel crushing"
[0047] The term "gel crushing" as used herein means an operation of applying shearing and compressive forces to reduce the size and increase the surface area of a hydrogel-like cross-linked polymer obtained in a polymerization step (preferably aqueous solution polymerization, non-stirring aqueous solution polymerization (stationary aqueous solution polymerization), and particularly preferably belt polymerization) for the purpose of facilitating drying of the polymer.
[0048] In addition, the shape of the obtained hydrogel may be different depending on the type of polymerization machine. For example, the shape of the hydrogel obtained in static polymerization (especially belt polymerization) is sheet-like or block-like. Here, sheet-like refers to a polymer having a thickness along a plane, and its thickness is preferably 1 mm to 30 cm, and particularly preferably 0.5 to 10 cm. Typically, a sheet-like hydrogel is obtained by belt polymerization, drum polymerization, and intermittent film polymerization. The length and width of the sheet-like hydrogel are appropriately determined according to the size of the polymerization device used. In the case of continuous polymerization (continuous belt polymerization or continuous drum polymerization), a sheet-like hydrogel with an endless length is obtained, and its width is the width of the belt or drum of the polymerization device, preferably 0.1 to 10 m, and more preferably 1 to 5 m. The endless sheet-like hydrogel can be appropriately cut along the length direction after polymerization for use, and further, it can be appropriately broken into several mm to several m square after cutting. In addition, a block-like hydrogel is obtained by tank polymerization, etc. The block-like hydrogel can be appropriately broken into several mm to several m square after polymerization. In contrast, in the case of kneader polymerization, the hydrogel generated by the polymerization is polymerized while being coarsely crushed in the same device in the polymerization step, so that a granulated hydrogel can be obtained. However, the particle size of the hydrogel particles obtained by kneader polymerization is about several cm to several mm, and is not finely granulated to the particle size obtained by the gel crushing step described in the present invention. In addition, in order to crush the hydrogel to the particle size obtained in the present invention by kneader polymerization, an overly large device is required, which is not realistic as an industrial production method. Therefore, gel crushing in such a polymerization step is not included in the concept of "gel crushing" in the present invention. In addition, in the present invention, the polymerization step is deemed to have ended at the stage where the polymerization rate reaches the range described below. The operation of crushing the hydrogel granulated to a particle size of about several cm to several mm by kneader polymerization or the like to the particle size required by the present invention is included in the concept of "gel crushing" in the present invention.
[0049] 〔1-5〕Others
[0050] In this specification, "X to Y" indicating a range means "above X and below Y". In addition, unless otherwise noted, "t (ton)" as a mass unit means "Metric ton", and "ppm" means "mass ppm" or "weight ppm". Furthermore, "mass" and "weight", "mass parts" and "weight parts", "mass %" and "weight %" are respectively regarded as synonyms. In addition, "acid (salt)" means "acid and / or its salt", and "(meth)acrylic acid" means "acrylic acid and / or methacrylic acid".
[0051] [2] Method for producing water-absorbent resin powder
[0052] The method for producing the water-absorbent resin powder of the present invention comprises a polymerization step and a gel pulverization step performed separately from the polymerization step. The method preferably further comprises a drying step, a cooling step, a pulverization step of the dried product, a classification step, a surface cross-linking step or a granulation step after the surface cross-linking. In addition, the method may include a monomer aqueous solution preparation step, a step of adding various additives, a fine powder removal step and a fine powder recycling step (fine powder recovery step), or a filling step. Furthermore, various known steps may be included depending on the purpose.
[0053] According to the production method of the present invention, a hydrogel cross-linked polymer having a polymerization rate of 90% by mass or more is subjected to gel pulverization using a kneading machine having a plurality of screws (particularly a twin-screw kneading machine). At this time, by controlling the gel pulverization coefficient to be between 0.020 J / g·sec and 3.0 J / g·sec, a granular hydrogel having a mass average particle size d1 of 500 μm or less in terms of solid content is produced, thereby obtaining a water-absorbent resin having an excellent water absorption rate and reduced residual monomers.
[0054] Hereinafter, each step will be described in detail.
[0055] [2-1] Step of preparing monomer aqueous solution
[0056] This step is an optional step of preparing an aqueous solution containing a monomer to be a raw material of a water-absorbent resin, preferably an aqueous solution containing an acid group-containing unsaturated monomer as a main component (hereinafter referred to as "monomer aqueous solution"). It should be noted that a slurry of monomers may be used as long as the water absorption performance of the obtained water-absorbent resin is not reduced, but in this section, for convenience, the monomer aqueous solution is described.
[0057] The above-mentioned "main component" means that the amount (content) of the acid group-containing unsaturated monomer used is usually 50 mol% or more, preferably 70 mol% or more, more preferably 90 mol% or more (the upper limit is 100 mol%) based on the total amount of monomers (excluding the internal crosslinking agent) used in the polymerization reaction of the water-absorbent resin.
[0058] (Unsaturated monomer containing acid group)
[0059] The acid group specified in the present invention is not particularly limited, and examples thereof include carboxyl, sulfone, phosphoric acid, etc. Examples of the unsaturated monomer containing the acid group include (meth) acrylic acid, maleic acid (anhydride), itaconic acid, cinnamic acid, vinyl sulfonic acid, allyl toluene sulfonic acid, vinyl toluene sulfonic acid, styrene sulfonic acid, 2-(meth) acrylamide-2-methylpropane sulfonic acid, 2-(meth) acrylyl ethanesulfonic acid, 2-(meth) acrylyl propane sulfonic acid, (meth) acrylyl phosphonic acid 2-hydroxyethyl ester, etc. From the viewpoint of water absorption performance, preferably (meth) acrylic acid, maleic acid (anhydride), itaconic acid, cinnamic acid, more preferably (meth) acrylic acid, and particularly preferably acrylic acid.
[0060] (Monomers other than unsaturated monomers containing an acid group)
[0061] As monomers other than unsaturated monomers containing an acid group, any compound that can form a water-absorbent resin by polymerization may be used. Examples thereof include unsaturated monomers containing amide groups such as (meth)acrylamide, N-ethyl (meth)acrylamide, and N,N-dimethyl (meth)acrylamide; unsaturated monomers containing amino groups such as N,N-dimethylaminoethyl (meth)acrylate, N,N-dimethylaminopropyl (meth)acrylate, and N,N-dimethylaminopropyl (meth)acrylamide; unsaturated monomers containing mercapto groups; unsaturated monomers containing phenolic hydroxyl groups; and unsaturated monomers containing lactam groups such as N-vinylpyrrolidone.
[0062] (Neutralizing Salt)
[0063] In the present invention, a neutralized salt in which a part or all of the acid groups contained in the unsaturated monomer containing an acid group are neutralized can be used. In this case, the salt of the unsaturated monomer containing an acid group is preferably a salt formed with a monovalent cation, more preferably at least one selected from an alkali metal salt, an ammonium salt and an amine salt, further preferably an alkali metal salt, further preferably at least one selected from a sodium salt, a lithium salt and a potassium salt, and particularly preferably a sodium salt.
[0064] (Neutralizer)
[0065] The neutralizing agent used to neutralize the unsaturated monomer containing an acid group is not particularly limited, and inorganic salts such as sodium carbonate and ammonium carbonate; alkaline substances such as sodium hydroxide, potassium hydroxide, and amine-based organic compounds having amino groups or imino groups can be appropriately selected and used. As the neutralizing agent, two or more salts or alkaline substances can be used in combination. It should be noted that the monomers in the present invention include the concept of neutralized salts unless otherwise specified.
[0066] (Neutralization rate)
[0067] From the viewpoint of water absorption performance, the molar number of the neutralized salt relative to the total molar number of the acid group-containing unsaturated monomer and its neutralized salt (hereinafter referred to as "neutralization ratio") is preferably 40 mol% or more, more preferably 40 mol% to 80 mol%, further preferably 45 mol% to 78 mol%, and particularly preferably 50 mol% to 75 mol%.
[0068] Examples of methods for adjusting the neutralization rate include: a method of mixing an unsaturated monomer containing an acid group with a neutralizing salt thereof; a method of adding a known neutralizing agent to an unsaturated monomer containing an acid group; a method of using a partially neutralized salt of an unsaturated monomer containing an acid group (i.e., a mixture of an unsaturated monomer containing an acid group and a neutralizing salt thereof) adjusted in advance to a predetermined neutralization rate, etc. In addition, these methods may be combined.
[0069] The above-mentioned adjustment of the neutralization rate can be performed before the polymerization reaction of the unsaturated monomer containing an acid group begins, can be performed during the polymerization reaction of the unsaturated monomer containing an acid group, and can also be performed on the hydrogel cross-linked polymer obtained after the polymerization reaction of the unsaturated monomer containing an acid group ends. In addition, the neutralization rate can be adjusted at any stage before the polymerization reaction begins, during the polymerization reaction, or after the polymerization reaction ends, or the neutralization rate can be adjusted in multiple stages. It should be noted that in the use of absorbent articles such as diapers that may come into direct contact with the human body, it is preferred to adjust the neutralization rate before the polymerization reaction begins and / or during the polymerization reaction, and it is more preferred to adjust the neutralization rate before the polymerization reaction begins.
[0070] (Internal crosslinking agent)
[0071] In the method for producing the water-absorbent resin powder, it is preferred to use an internal crosslinking agent, which is used to adjust the water absorption performance of the obtained water-absorbent resin, the gel strength when absorbing water, and the like.
[0072] The internal crosslinking agent may have two or more unsaturated bonds or reactive functional groups in total in one molecule. For example, examples of the internal crosslinking agent having a plurality of polymerizable unsaturated groups (copolymerizable with the monomer) in the molecule include N,N-methylenebis(meth)acrylamide, (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, glycerol (meth)acrylate, glycerol acrylate methacrylate, ethylene oxide-modified trimethylolpropane tri(meth)acrylate, pentaerythritol hexa(meth)acrylate, triallyl cyanurate, triallyl isocyanurate, triallyl phosphate, and the like. As internal crosslinking agents having multiple reactive functional groups (capable of reacting with the functional groups (e.g., carboxyl groups) of monomers) in the molecule, triallylamine, polyallyloxyalkane, (poly)ethylene glycol diglycidyl ether, glycerol diglycidyl ether, ethylene glycol, polyethylene glycol, propylene glycol, glycerol, 1,4-butanediol, pentaerythritol, ethylenediamine, ethylene carbonate, propylene carbonate, polyethyleneimine, etc. (It should be noted that, here, cyclic carbonates such as ethylene carbonate are crosslinking agents that further generate functional groups OH by reacting with carboxyl groups). In addition, as internal crosslinking agents having polymerizable unsaturated groups and reactive functional groups in the molecule, glycidyl (meth)acrylate, etc. can be listed. Among these, two or more can be used in combination.
[0073] Among these internal crosslinking agents, compounds having a plurality of polymerizable unsaturated groups in the molecule are preferred from the viewpoint of the effects of the present invention, compounds having a (poly)alkylene structural unit in the molecule are more preferred, and compounds having a polyethylene glycol structural unit are still more preferred.
[0074] The amount of the internal crosslinking agent used is appropriately set according to the types of monomers and the internal crosslinking agent. From the viewpoint of the gel strength of the obtained water-absorbent resin, it is preferably 0.001 mol% or more, more preferably 0.005 mol% or more, and further preferably 0.01 mol% or more relative to the monomer. From the viewpoint of improving the water absorption performance of the water-absorbent resin, it is preferably 5 mol% or less, more preferably 2 mol% or less. It should be noted that under polymerization conditions where the self-crosslinking reaction of the monomer is effective, the internal crosslinking agent may not be used.
[0075] (Inhibitor)
[0076] From the perspective of polymerization stability, the monomer used in the polymerization preferably contains a small amount of polymerization inhibitor. The preferred polymerization inhibitor is p-methoxyphenol. The amount of polymerization inhibitor contained in the monomer (especially acrylic acid and its salt) is usually 1 ppm to 250 ppm, preferably 10 ppm to 160 ppm, and more preferably 20 ppm to 80 ppm.
[0077] (Other substances)
[0078] In the production method according to the present invention, the substances exemplified below (hereinafter referred to as "other substances") may be added to the aqueous monomer solution within the range of achieving the object of the present invention.
[0079] Specific examples of other substances include chain transfer agents such as mercaptans, mercaptan acids, secondary alcohols, amines, and hypophosphites; foaming agents such as carbonates, bicarbonates, and azo compounds; chelating agents such as ethylenediaminetetrakis (methylenephosphinic acid) or its metal salts, ethylenediaminetetraacetic acid or its metal salts, diethylenetriaminepentaacetic acid or its metal salts; polyacrylic acid (salts) and their crosslinked products (such as water-absorbent resin powder to be recycled), starch, cellulose, starch-cellulose derivatives, polyvinyl alcohol, and other hydrophilic polymers and powders, etc. Other substances may be used alone or in combination of two or more.
[0080] The amount of other substances used is not particularly limited. In the case of fine powder to be recycled, it is 30% by mass or less relative to the monomer. In the case of other substances other than fine powder, the total concentration is preferably 10% by mass or less, more preferably 0.001% by mass to 5% by mass, and particularly preferably 0.01% by mass to 1% by mass, relative to the monomer.
[0081] (Monomer Concentration in Monomer Composition (Aqueous Monomer Solution))
[0082] In this step, from the viewpoint of the physical properties of the water-absorbent resin and productivity, the monomer concentration (=total monomer amount / (total monomer amount + total polymerization solvent amount (usually water)) in the monomer composition (monomer aqueous solution) is preferably 10% by mass to 90% by mass, more preferably 20% by mass to 80% by mass, further preferably 30% by mass to 70% by mass, and particularly preferably 40% by mass to 60% by mass. Hereinafter, the monomer concentration may be referred to as "monomer concentration".
[0083] (Polymerization initiator)
[0084] The polymerization initiator used in the present invention is appropriately selected according to the polymerization form, etc., and is not particularly limited. For example, a thermal decomposition type polymerization initiator, a photodecomposition type polymerization initiator, or a combination thereof, or a redox polymerization initiator obtained by using a reducing agent that promotes the decomposition of the polymerization initiator, etc. can be listed. Specifically, one or more of the polymerization initiators disclosed in U.S. Patent No. 7265190 can be used. It should be noted that from the viewpoint of the handling property of the polymerization initiator and the physical properties of the water-absorbing resin, it is preferred to use a peroxide or an azo compound, more preferably a peroxide, and even more preferably a persulfate.
[0085] The amount of the polymerization initiator used is preferably 0.001 mol% to 1 mol%, more preferably 0.001 mol% to 0.5 mol% relative to the monomer. In addition, when redox polymerization is performed as needed, the amount of the reducing agent used in combination with the oxidizing agent is preferably 0.0001 mol% to 0.02 mol% relative to the monomer.
[0086] (Dissolved oxygen content)
[0087] It should be noted that the dissolved oxygen in the aqueous monomer solution before polymerization can be reduced by raising the temperature or replacing it with an inert gas. For example, the dissolved oxygen is preferably reduced to 5 ppm or less, more preferably to 3 ppm or less, and particularly preferably to 1 ppm or less.
[0088] In addition, bubbles (especially the above-mentioned inert gas, etc.) may be dispersed in the monomer aqueous solution. In this case, the polymerization reaction becomes foaming polymerization.
[0089] 〔2-2〕Polymerization process
[0090] This step is a step of polymerizing the aforementioned monomer aqueous solution to obtain a hydrogel-like crosslinked polymer. Preferably, it is a step of obtaining a hydrogel that is a crosslinked product having poly(meth)acrylic acid (salt) as a main component.
[0091] It should be noted that, in addition to the method of carrying out the polymerization reaction by adding the above-mentioned polymerization initiator, there is also a method of irradiating active energy rays such as radiation, electron beams, and ultraviolet rays. In addition, it is also possible to combine irradiation with active energy rays based on the addition of a polymerization initiator.
[0092] (Aggregate form)
[0093] As the polymerization form, it is intermittent or continuous aqueous solution polymerization. In addition, it can be belt polymerization or kneader polymerization. Furthermore, continuous aqueous solution polymerization is more preferred, and both continuous belt polymerization and continuous kneader polymerization can be applied. As a specific polymerization form, continuous belt polymerization is disclosed in U.S. Patent No. 4893999, U.S. Patent No. 6241928, U.S. Patent Application Publication No. 2005 / 215734, etc., and continuous kneader polymerization is disclosed in U.S. Patent No. 6987151, U.S. Patent No. 6710141, etc. By adopting these continuous aqueous solution polymerizations, the production efficiency of the water-absorbent resin is improved.
[0094] In addition, as preferred forms of the above-mentioned continuous aqueous solution polymerization, "high-temperature start polymerization" and "high-concentration polymerization" can be listed. "High-temperature start polymerization" refers to a form in which polymerization is started at a temperature of preferably 30°C or higher, more preferably 35°C or higher, further preferably 40°C or higher, and particularly preferably 50°C or higher (the upper limit is the boiling point) of the monomer aqueous solution, and "high-concentration polymerization" refers to a form in which polymerization is carried out under conditions where the monomer concentration is preferably 30% by mass or higher, more preferably 35% by mass or higher, further preferably 40% by mass or higher, and particularly preferably 45% by mass or higher (the upper limit is the saturation concentration). These polymerization forms may also be used in combination.
[0095] (Polymerization rate of hydrogel)
[0096] The polymerization rate of the hydrogel cross-linked polymer introduced into the inlet of the gel grinding device obtained by the polymerization process is 90% by mass or more. The polymerization rate of the hydrogel cross-linked polymer introduced into the inlet of the gel grinding device is preferably 95% by mass or more, more preferably 98% by mass or more, and particularly preferably 99% by mass or more. When gel grinding is performed in a state of low polymerization rate (i.e., a state of polymerization rate less than 90% by mass) (for example, when polymerization and gel grinding are performed simultaneously like kneader polymerization), a large amount of unreacted monomers contained in the ground gel particles are polymerized, and the ground gel particles are bonded to each other, thereby generating large-sized gel particles again. Therefore, there is the following problem: when gel grinding is performed in the polymerization process, the regenerated large-sized gel particles need to be ground again, the energy required for grinding increases, and the polymerization device becomes too large. In addition, when the hydrogel with a low polymerization rate is crushed after the polymerization process and the drying process is carried out in a state containing a large amount of unreacted monomers, a polymerization reaction occurs during drying, and hydrogel particles with a large particle size are regenerated from gel particles with a small particle size. Therefore, the water absorption rate of the obtained water-absorbing resin decreases, and the particle size of the dried product increases. It should be noted that the upper limit of the polymerization rate is not particularly limited, and 100% by mass is ideal, but a high polymerization rate requires a long polymerization time and strict polymerization conditions, and sometimes also leads to a decrease in productivity and physical properties. The upper limit is 99.99% by mass, 99.95% by mass, and further 99.9% by mass, and usually about 99.8% by mass is sufficient. Typically, the polymerization rate of the hydrogel-like cross-linked polymer obtained by the polymerization process is 90 to 99.99% by mass, 95 to 99.99% by mass, 98 to 99.99% by mass, 98 to 99.95% by mass, 98 to 99.9% by mass, and 98 to 99.8% by mass.
[0097] 〔2-3〕Chopping process
[0098] The shredding process is an optional process for cutting or roughly pulverizing the hydrogel-like cross-linked polymer into a size that can be put into the gel pulverizing device after the polymerization process and before the gel pulverizing process. In particular, when the above-mentioned polymerization process is a belt polymerization and a sheet-like or block-like hydrogel is obtained, the shredding process is preferably implemented. Therefore, in one embodiment of the present invention, the hydrogel-like cross-linked polymer obtained after the polymerization process is in sheet form, and a shredding process for shredding the sheet-like hydrogel-like cross-linked polymer is also included before the gel pulverizing process. There is no particular limitation on the unit for cutting or roughly pulverizing the hydrogel in the shredding process, and a rotary cutter, a roller cutter, a guillotine cutter, a cutting mill, a screw extruder (such as a meat slicer, etc.) and the like are used in combination as needed. The size to be shredded is not particularly limited as long as it is within the range that can be put into the gel pulverizing device described later. The size of the hydrogel after shredding is preferably 0.8 mm to 3 m, more preferably 1 mm to 2.5 m, and particularly preferably 1 mm to 2 m. It should be noted that, when achieving the purpose of the present invention, the shredding step may not be performed.
[0099] In addition, in the shredding process, water and / or water vapor (preferably water and water vapor) may be supplied as specifically described in the gel pulverizing process described later. The supply of water and / or water vapor is performed by, for example, supplying water and water vapor to the inside of the device used in the shredding process. As a means for supplying water and / or water vapor, the device used in the shredding process may have a plurality of supply ports. The specific means and suitable ranges such as the method for adding water vapor, the pressure, the temperature of water and / or water vapor, and the supply amount of water and / or water vapor are the same as those described in the gel pulverizing process described later.
[0100] 〔2-4〕Gel crushing process
[0101] This step is a step of obtaining a granular hydrogel crosslinked polymer by pulverizing the hydrogel crosslinked polymer obtained by the polymerization step after the above-mentioned polymerization and granulating it. In this step, the particle size of the granular hydrogel is adjusted to a preferred range described below. In order to obtain a granular hydrogel of a predetermined particle size, this step may be performed twice or more.
[0102] (Gel crushing device)
[0103] In the manufacturing method of the present invention, Figure 1 , Figure 2As shown in FIG. 1 , in the gel pulverizing step after the polymerization step, a gel pulverizing device having an inlet, a main body with a plurality of rotating shafts built therein, and a discharge port is used. Each rotating shaft has a pulverizing unit. In the gel pulverizing device, the hydrous gel-like crosslinked polymer continuously fed from the inlet into the main body is pulverized by the pulverizing unit of each rotating shaft, and the hydrous gel-like crosslinked polymer is continuously taken out from the discharge port in the form of granular. In addition, in the present invention, the main body refers to the body part ( Figure 1 Symbol 208), also known as barrel, trough, casing, etc.
[0104] The gel grinding device used in the production method of the present invention can be a vertical type (the direction of the water-containing gel is the vertical direction), a horizontal type or a horizontal type (the direction of the water-containing gel is the horizontal direction or the horizontal direction) as long as it is a continuous type. In addition, the vertical type and the horizontal type gel grinding device can have an inclination of 0° to 90° relative to the horizontal direction. For example, in Figure 1 In the case of the horizontal continuous pulverizing device shown, the inclination is appropriately set as needed, and the inclination from the input port to the discharge port (i.e., relative to the advancing direction of the hydrogel) can be downward or upward. Usually, the inclination angle is 0° to 10°, preferably 0° to 1°, and particularly preferably 0°.
[0105] It should be noted that, in the case of an extruder (meat slicer) used for gel pulverization in a conventional production method, the hydrogel is substantially pulverized near the die provided at the extrusion port, and the gel pulverization is hardly performed in the screw portion involved in the transportation of the hydrogel. In contrast, in the case of a gel pulverization device (particularly a kneading machine) used in the production method described in the present invention, the hydrogel fed is continuously pulverized to a smaller particle size by the pulverizing unit of the rotating shaft from the feed port until it reaches the discharge port.
[0106] Specifically, in the gel grinding device, the hydrogel fed from the feed port is ground to a target particle size before being discharged from the discharge port. Therefore, in the gel grinding device, the hydrogel particles adjusted to the target particle size are taken out from the discharge port without being extruded from a die as in a conventional extruder (meat slicer). In the production method of the present invention, a water-absorbent resin having an excellent water absorption rate is obtained by using the gel grinding device.
[0107] From the viewpoint of continuously performing gel pulverization, the gel pulverization device preferably has a heating unit and / or a heat-retaining unit. The heating unit and / or the heat-retaining unit are not particularly limited, but from the viewpoint of preventing the adhesion and aggregation of the hydrogel and the granular hydrogel, a heating unit based on direct heat conduction and / or indirect heat conduction is preferred, wherein the direct heat conduction is based on convection heat conduction, and the indirect heat conduction is based on heat conduction from the heating surface (surface in contact with the hydrogel, heat source portion) of the gel pulverization device heated by the heat medium. As for a more preferred heating unit, a ventilation heating type is used in the case of direct heat conduction, and an outer wall heating type is used in the case of indirect heat conduction.
[0108] From the viewpoint of reducing damage to the hydrogel, it is preferred to provide a heating unit and / or a heat-insulating unit on the outer surface of the main body, and it is more preferred to provide a heating unit. As the heat-insulating unit, for example, a method of covering a part or all of the outer surface of the main body (preferably 50% or more of the outer surface (area) of the main body, more preferably 80% or more, and particularly preferably the entire surface) with an insulating material can be cited. In addition, as the heating unit, an electric trace, a steam trace, a jacket heated by a heat medium, etc. can be exemplified in a manner that covers a part or all of the outer surface of the main body (preferably 50% or more of the outer surface (area) of the main body, more preferably 80% or more, and particularly preferably the entire surface). The particle size of the granular hydrogel pursued in the present invention is significantly smaller than in the past. Therefore, the changes in the adhesion and fluidity of the hydrogel particles caused by temperature changes are large compared to the situation envisioned within the scope of the prior art. As a result, the energy required for pulverizing the hydrogel and the aggregation of the pulverized gel particles may vary significantly depending on the temperature. Therefore, as described later, there may be a suitable temperature range when the hydrogel cross-linked polymer is continuously pulverized. The gel pulverizing device can perform the gel pulverizing process within a more preferred temperature range by having the above-mentioned heating unit and / or heat-retaining unit. In addition, the deterioration of the quality of the gel pulverization caused by the temperature difference between seasons, day and night, etc. can be avoided. Furthermore, when the gel pulverizing device is started, it can also be smoothly induced to stable operation.
[0109] As long as the effects of the present invention can be obtained, the type of pulverizing unit possessed by each rotating shaft is not particularly limited. For example, as an object having a shearing effect on the aqueous gel, disks of various shapes can be listed. The disk is sometimes referred to as a chip, a paddle, an element, a kneading, a rotor, and the like. The shape of the disk is not particularly limited, and can be appropriately selected from a circular plate shape, a roughly elliptical shape, a roughly triangular shape, and the like. A shape having a major axis diameter X and a minor axis diameter Y is preferred, and a roughly elliptical shape is more preferred. It should be noted that the roughly elliptical shape includes, in addition to the elliptical shape, a bag shape, a truck type shape, and a shape in which a portion of them is deformed (for example, the shape described later). Figure 8 The major axis diameter X and the minor axis diameter Y are described later. Disks of different shapes may be used in combination, and their arrangement may be appropriately adjusted from the viewpoint of the particle size of the target granular hydrogel and the energy required for pulverization. In addition, as a pulverizing unit, an arm, a blade, a scraper, a cut disk (CD), etc. may be used in combination.
[0110] For example, in the case where each rotating shaft has a disk as a crushing unit, especially in the case of a disk in the shape of a circular plate or (roughly) elliptical shape, the ratio of the effective length L (Length, mm) inside the main body to the maximum diameter D (Diameter, mm; when multiple disks with different diameters / major axis diameters are used, the diameter of the largest disk / major axis diameter) of the disk is defined by L / D. The L / D is preferably greater than 5, more preferably greater than 6, and more preferably greater than 7. By making L / D greater than the above lower limit, the pressure applied to the hydrous gel in gel crushing is dispersed to the entire main body (barrel), and the maximum pressure on the hydrous gel is reduced, which is preferred. In addition, L / D is preferably less than 20, and more preferably less than 15. By making L / D less than the above upper limit, the crusher will not be overly enlarged, and the increase in the cost of the device can be suppressed, which is preferred. L / D is preferably greater than 5 and less than 20, more preferably greater than 6 and less than 15, and further preferably greater than 7 and less than 15. In addition, as Figure 1 As shown, the effective length L refers to the axial length (total length) of the main body (barrel) portion from the inlet port to the outlet port.
[0111] In addition, the effective length L (Length) inside the main body is, for example, 200 mm to 8000 mm, or 400 to 7000 mm. Furthermore, the maximum diameter D (Diameter; when using multiple disks with different diameters / long axis diameters, the diameter / long axis diameter of the largest disk) of the disk is, for example, 10 to 1000 mm, or 20 to 800 mm.
[0112] In addition, the distance (gap) between the disk and the main body (barrel) sometimes also varies depending on the location. When the distance between the outer circumference of the disk and the inner wall of the main body (barrel) is the shortest distance, it is recorded as the minimum gap C. The minimum gap C is preferably less than 20% relative to the maximum diameter D of the disk, more preferably less than 15%, further preferably less than 10%, and particularly preferably less than 5%. If it is below the above upper limit, the shear force between the barrel and the disk becomes stronger during gel crushing, and the gel crushing efficiency becomes good. In addition, the minimum gap C is preferably more than 0.2% relative to the maximum diameter D of the disk, more preferably more than 0.5%, and further preferably more than 1%. If it is above the above lower limit, the contact between the disk and the inner wall of the main body (barrel) is suppressed, and the mixing of metal foreign matter caused by wear is suppressed. A suitable form of the present invention is that the minimum gap C is 0.2 to 20% relative to the maximum diameter D of the disk.
[0113] As described later, in the gel pulverizing device, the hydrogel is pulverized to a predetermined particle size by the rotation of a plurality of rotating shafts having a pulverizing unit. The rotation speed of the plurality of rotating shafts may be uniform or non-uniform, and is appropriately set according to the device, preferably in the range of 1 rpm to 1000 rpm, more preferably in the range of 3 rpm to 500 rpm, and further preferably in the range of 5 rpm to 300 rpm. In addition, when the rotation speeds of the rotating shafts are different, the ratio of the rotation speeds of the other rotating shafts to the rotation speed of one rotating shaft is generally in the range of 1 to 10, preferably in the range of 1 to 2. In addition, the rotating shafts are preferably parallel.
[0114] In addition, when the multiple rotating shafts have a disk as a crushing unit, the circumferential speed (V) of the disk defined by the following (Formula 1) may be uniform or non-uniform, and is appropriately set according to the device, preferably 0.05m / s to 5m / s, more preferably 0.1m / s to 5m / s, further preferably 0.15m / s to 3m / s, and particularly preferably 0.2m / s to 2m / s. If it exceeds the above range, the shear force involved in the hydrogel becomes too large, and the physical properties of the hydrogel particles after crushing deteriorate and excessive compaction (agglomeration) occurs, so it is not preferred. In addition, if it is less than the above range, the processing amount per unit time in the gel crushing process is reduced, so it is not preferred. In addition, when the circumferential speeds of the disks possessed by each rotating shaft are different, the ratio of the circumferential speed of the other rotating shafts to the circumferential speed of one rotating shaft is generally in the range of 1 to 10, preferably in the range of 1 to 2.
[0115] Circumferential speed (V) (m / s) = πD × n / 60… (Formula 1)
[0116] Here, in (Equation 1), V is the peripheral speed of the disk (unit: m / s), D is the maximum diameter of the disk (unit: m), and n is the rotation speed of the disk per unit time (unit: rpm).
[0117] In addition, the rotation direction of the plurality of rotating shafts may be a unidirectional type in which each rotating shaft rotates in the same direction, or a heterodirectional type in which each rotating shaft rotates in opposite directions. In a unidirectional type device, self-cleaning properties can be expected, and in a heterodirectional type device, strong shearing force can be expected. The rotation direction of each rotating shaft can be appropriately selected by combining it with the arrangement (disc pattern) of the pulverizing unit described later.
[0118] The gel crushing device preferably has the function of supplying water and / or water vapor to the inside of the main body. By supplying water and / or water vapor (preferably water and water vapor) while performing gel crushing, a water-absorbent resin powder with a better water absorption rate can be obtained. In addition, just after the gel crushing starts, the discharged granular hydrogel-like cross-linked polymer contains a large number of coarse granular hydrogel-like cross-linked polymers with a particle size of more than 10 mm, but by supplying water and / or water vapor (preferably water and water vapor) while performing gel crushing, it is possible to reduce such coarse granular hydrogel-like cross-linked polymers with a particle size of more than 10 mm in a short time, and the amount of coarse gel mixed into the obtained granular hydrogel-like cross-linked polymer can also be reduced in a stable state. Therefore, according to one embodiment of the present invention, water and / or water vapor are supplied to the inside of the main body in the gel crushing process. In another preferred embodiment, water and water vapor are supplied to the inside of the main body in the gel crushing process. As a means for supplying water and / or water vapor, the gel crushing device can have multiple water and / or water vapor supply ports. The water and / or water vapor supply port is set at any position, and is preferably set at the side of the hydrogel inlet. In other words, water and / or water vapor is supplied from the vicinity of the hydrogel inlet. In addition, water and water vapor may be supplied from different supply ports.
[0119] When adding water vapor, there is no particular limitation, and gases such as air, dry air, and nitrogen can be mixed with water vapor and added in the form of a mixed gas. The pressure of the added water vapor is not particularly limited, but is preferably 0.2 to 0.8 MPa, and more preferably 0.3 to 0.7 MPa. The temperature of water and / or water vapor (including mixed gas) is not particularly limited, but is preferably 50°C or more, more preferably 60°C or more, further preferably 70°C or more, and particularly preferably 80°C or more. From the viewpoint of suppressing excessive temperature rise and drying of the hydrogel, it is preferably 200°C or less, more preferably 170°C or less, further preferably 150°C or less, further preferably 120°C or less, and particularly preferably 100°C or less. A preferred form is: the temperature of water and / or water vapor supplied to the inside of the body is 50 to 200°C, 50 to 170°C, 50 to 150°C, 50 to 120°C, 60 to 120°C, 70 to 120°C, 80 to 120°C. The temperature of the hydrogel and the granular hydrogel in the gel grinding device can also be adjusted by the temperature and supply amount of the water and / or water vapor (including the mixed gas) used. In this case, the water vapor and / or the mixed gas acts as a heat medium for direct heat conduction, and the hydrogel and the granular hydrogel in the body are heated or kept warm to a predetermined temperature. In addition, additives such as a gel-fluidizing agent, a cross-linking agent, an oxidizing agent, a reducing agent, and a polymerization initiator described later can be mixed into the added water and / or water vapor (including the mixed gas).
[0120] The amount of water and / or water vapor supplied is preferably 0.1% to 50% by mass, more preferably 0.5% to 40% by mass, and further preferably 1% to 30% by mass, based on the mass calculated on the solid content of the hydrogel.
[0121] The gel crushing device used in the production method described in the present invention is preferably equipped with a heating unit and / or a heat-insulating unit on the outer surface of the main body, and a liquid heat medium such as warm water or oil can be introduced into a jacket or the like provided on the outer surface of the main body, or a heated gas (hot air) can be introduced as a heat medium. These heat media act as heat media for indirect heat conduction. From the viewpoint of heating efficiency and / or heat-insulating efficiency of indirect heat conduction, the temperature of the heat medium is preferably 50°C or more, more preferably 60°C or more, further preferably 70°C or more, and particularly preferably 80°C or more. On the other hand, from the viewpoint of suppressing excessive temperature rise and drying of the hydrogel, the temperature of the heat medium is preferably 200°C or less, more preferably 170°C or less, further preferably 150°C or less, further preferably 130°C or less, and particularly preferably 110°C or less. A particularly preferred heat medium is warm water or steam. In addition, the temperature of the heat medium can be a constant temperature, or can be appropriately changed during the gel crushing process.
[0122] It is more preferred that the temperature of the inside (inner surface) of the main body is preferably heated to 50°C or higher, more preferably 60°C or higher, further preferably 70°C or higher, and further preferably 80°C or higher before the hydrogel is introduced into the gel grinding device. This can reduce the adhesion of the hydrogel to the inner surface of the main body. In addition, the water absorption rate of the water-absorbent resin powder obtained thereby is further improved. That is, in the production method of the present invention, it is preferred that the inner surface of the main body is heated to the above-mentioned temperature or higher before the hydrogel is introduced and / or when the gel grinding is started. It is more preferred that the inner surface of the main body and the outer surfaces of the plurality of rotating shafts and the grinding units of each rotating shaft are preferably heated to the above-mentioned temperature or higher. On the other hand, from the viewpoint of suppressing excessive temperature rise and drying of the hydrogel, the heating temperature of the inside (inner surface) of the main body is preferably 200°C or lower, more preferably 170°C or lower, further preferably 150°C or lower, further preferably 130°C or lower, and particularly preferably 110°C or lower before the hydrogel is introduced into the gel grinding device. For example, by circulating a heat medium inside a jacket provided in the main body and maintaining it, the temperature inside the main body (inner surface) can be adjusted to a desired range. From the viewpoint of maintaining the temperature of the gel in the gel crushing process, the temperature inside the main body (inner surface) is preferably maintained within the above range in the gel crushing process. Regarding a preferred embodiment, before the hydrogel is put into the gel crushing device, the heating temperature inside the main body (inner surface) is 50 to 200°C, 50 to 170°C, 50 to 150°C, 50 to 130°C, 50 to 110°C, 60 to 110°C, 70 to 110°C, 80 to 110°C.
[0123] From the viewpoint of continuously and satisfactorily performing gel pulverization, the temperature for continuously pulverizing the hydrogel-like crosslinked polymer is preferably 50° C. or higher, more preferably 60° C. or higher, further preferably 70° C. or higher, and further preferably 80° C. or higher.
[0124] The upper limit of the temperature for continuously pulverizing the hydrogel-like cross-linked polymer is not particularly limited, but is preferably 200°C or lower, more preferably 170°C or lower, further preferably 150°C or lower, further preferably 130°C or lower, and particularly preferably 110°C or lower, from the viewpoint of suppressing excessive temperature rise and drying of the hydrogel.
[0125] Here, for example, "continuously pulverizing the hydrogel crosslinked polymer at 50°C or higher" means: Figure 1 In the interval shown in (A), in other words, in the interval from passing through the inlet to reaching the outlet, the hydrous gel-like cross-linked polymer is continuously crushed while maintaining the temperature of the hydrous gel-like cross-linked polymer at 50°C or above. In other words, "continuously crushing the hydrous gel-like cross-linked polymer at 50°C or above by means of a crushing unit" means: "continuously crushing the hydrous gel-like cross-linked polymer by means of a crushing unit while maintaining the hydrous gel-like cross-linked polymer at 50°C or above". For example, if the temperature T1 of the hydrous gel-like cross-linked polymer introduced into the inlet of the gel crushing device is set to 50°C or above, and the temperature of the heat medium of the jacket provided on the outside of the device body is set to 50°C or above, then in Figure 1 In the interval (A), the temperature of the hydrogel crosslinked polymer can be maintained at 50°C or higher, and the hydrogel crosslinked polymer can be continuously pulverized at 50°C or higher. In addition, the following case is included: for example, even if the temperature T1 of the hydrogel crosslinked polymer fed into the inlet of the gel pulverizing device is 50°C or lower, by supplying high-temperature water and / or steam to the inlet portion, setting the jacket heat medium temperature of the device body to a high temperature, etc., the hydrogel crosslinked polymer is quickly heated to 50°C or higher in the (A) portion and continuously pulverized.
[0126] Furthermore, in the case of a large-scale gel grinding device, it is also preferable to circulate a heat medium inside a plurality of rotating shafts as a heating means and / or a heat-retaining means. This can shorten the time required to raise the temperature inside the main body when the gel grinding device is started.
[0127] The porosity V (hereinafter also referred to as the porosity V) of the gel grinding device calculated by the following (Formula 2) is preferably 40% or more, more preferably 45% or more. In addition, the porosity V is preferably 80% or less, more preferably 70% or less, further preferably 65% or less, and particularly preferably 60% or less. The porosity V of the gel grinding device is preferably 40% or more and 80% or less, more preferably 40% or more and 70% or less, further preferably 45% or more and 65% or less, and particularly preferably 45% or more and 60% or less.
[0128] Void ratio V = {(AB) / A} × 100 (Formula 2)
[0129] (Here, A is the main body portion after removing the portion corresponding to the inlet and outlet from the main body (barrel) in the length direction (i.e., Figure 1 The internal volume (m 3 ), B is Figure 1 The total volume (m 3 ). )
[0130] By making the porosity V below the upper limit, the hydrogel can be pulverized uniformly and the proportion of coarse particles can be reduced. In addition, by making the porosity V above the lower limit, excessive pressure on the hydrogel can be reduced, which can reduce the decrease in productivity.
[0131] In the gel pulverizing device used in the manufacturing method described in the present invention, it is most preferred not to use a mold (template), but as long as the effect of the present invention can be obtained, a mold may be provided at the discharge port. When a mold is used, the opening ratio of the mold is preferably 25% or more, more preferably 50% or more, further preferably 60% or more, further preferably 70% or more, and particularly preferably 80% or more. There is no particular upper limit to the opening ratio. An opening ratio of 100% is synonymous with the case where no mold is used. In addition, a mold (template) refers to a plate having (multiple) through holes for discharging the material inside the main body, which is disposed near the discharge port of the pulverizing device. In addition, the opening ratio refers to the ratio of the total top-view area of all the through holes to the top-view area of the mold. The larger the opening ratio, the more difficult it is for the material inside the main body to be clogged and the easier it is to be discharged, and therefore, the effect of the present invention becomes more significant. In addition, as an adjustment Figure 1 In order to adjust the size of the discharge port 210, a plate without a through hole can be provided to appropriately adjust the size of the discharge port.
[0132] Figure 1 and Figure 2 2 shows an example of a gel grinding device 200 used in the production method according to the present invention. Figure 1FIG. 2 is a partially cut-away side view of the gel grinding device 200. Figure 2 This is an enlarged view of the gel grinding device 200 (a view of the center of the main body viewed from above). Figure 1 and Figure 2 The basic structure and usage of the gel grinding device 200 will be described.
[0133] As shown in the figure, the gel grinding device 200 includes an inlet 204, a main body 208, two rotating shafts 206, an outlet 210, a driving device 214, and a gas supply port 216. The main body 208 is also called a barrel. Figure 1 In the figure, two rotating shafts 206 are arranged along the orthogonal direction of the paper surface. The two rotating shafts 206 are parallel. The rotating shaft 206 extends along the length direction of the main body 208. One end of the rotating shaft 206 penetrates the main body 208 and is connected to the driving device 214. Although not shown in the figure, in the gel crushing device 200, the other end of the rotating shaft 206 is supported by a bearing arranged at the rear thereof in a freely rotatable manner. In other words, the rotating shaft 206 is in a state where both ends are retained. Among them, the gel crushing device in the manufacturing method described in the present invention is not limited to this two-axis support form, as long as the purpose of the present invention is achieved, it can also be a so-called single-axis support structure without a bearing at the rear of the discharge port 210. The inlet 204, the gas supply port 216 and the discharge port 210 are respectively fixed to the main body 208 and are connected to the interior of the main body 208. Figure 1 The left-right direction in the figure is the length direction of the main body 208, which is the axial direction of the rotating shaft 206. Although not shown in the figure, the main body 208 has a jacket structure. The discharge port 210 can be as shown in FIG. Figure 1 As shown in the figure, it is arranged at the lower side of the main body, and it can also be arranged at the rear of the main body. By arranging it at the rear of the main body, even if the same device size is the same, the crushing interval can be extended.
[0134] Figure 2 FIG. 2 shows a portion of the main body 208 of the gel grinding device 200 . Figure 2 for Figure 1 An enlarged view of a gel pulverizing device (a view showing the central part of the main body viewed from above). As shown in the figure, in the gel pulverizing device 200, two rotating shafts 206 are built into the main body 208. The two rotating shafts 206 each have a screw 218 and a pulverizing unit 212 in order from the side close to the input port 204. In addition, although not shown in the figure, a reverse screw (reverse screw) for guiding the pulverized material to the discharge port 210 may be provided just in front of the bottom plate provided behind the discharge port 210. The pulverizing units 212 are provided on the outer circumferences of the two rotating shafts 206, respectively. That is, the pulverizing unit 212 and the rotating shaft 206 are configured as separate bodies. In this embodiment, the rotating shaft 206 has a plurality of disks as the pulverizing unit 212. Figure 2 The up-down direction in the figure is the width direction of the main body 208. Figure 2 The left-right direction in FIG. 2 is the length direction of the main body 208 and the axial direction of the rotating shaft 206 .
[0135] In a preferred embodiment of the gel pulverizing process using the gel pulverizing device 200, a heat medium is first circulated in a jacket (not shown) to heat the main body 208. Thereafter, each rotating shaft 206 is rotated by a driving device 214 (e.g., a motor). As the rotating shaft 206 rotates, the rotating shaft 206 and a plurality of disks as the pulverizing unit 212 rotate.
[0136] Next, the hydrogel is continuously fed into the feed port 204. At this time, water and / or water vapor may be simultaneously fed into the feed port 204. In addition, water vapor and / or water may be fed into the gas feed port 216. The hydrogel and the main body 208 are heated by the water and / or water vapor and are kept at a predetermined temperature.
[0137] The hydrogel introduced into the main body 208 contacts the screw 218. The hydrogel moves toward the discharge port 210 in the main body 208 due to the action of the rotating screw 218. A part of the hydrogel is roughly crushed by the rotation of the screw 218.
[0138] The hydrogel contacts the pulverizing unit 212 (i.e., a plurality of disks) in the main body 208. The hydrogel is granulated by the shearing action of the rotating plurality of disks. The hydrogel is pulverized by the conveying action of the screw 218 and the shearing action of the pulverizing unit 212 while moving toward the discharge port 210. At the discharge port 210, the granular hydrogel adjusted to a predetermined particle size is taken out. Figure 1 In order to take out the particulate hydrous gel from the bottom, the discharge port is arranged toward the bottom of the device, and in order to take out the particulate hydrous gel from the rear of the device, the discharge port can be arranged at the rear of the device.
[0139] The rotating shaft of the gel grinding device includes a plurality of screws having grinding units and different shapes and a plurality of disks. The shapes of the plurality of disks may be the same or different.
[0140] Here, the shape of the disk is not limited, and examples thereof include the disk disclosed in Japanese Patent Application Laid-Open No. 2013-139124. Figure 5 The shapes shown (flat disk, Figure 8 ), Japanese Patent Publication No. 2013-139124 Figure 6 An example of a flat disk is shown in Figure 8 . Figure 8The flat plate 10 is a front view, and in the front view, it is a shape that has a hole 11 that passes through the axis of the screw 218 in the central area of the roughly elliptical circular plate and a flat portion 12 along the long axis direction. The long axis diameter X refers to the maximum length of the straight line connecting any two points passing through the center, and the short axis diameter Y refers to the minimum length of the straight line connecting any two points passing through the center. Figure 8 In the figure, the major axis diameter X refers to the length of the straight line connecting the end points at the position of the point object existing in the flat portion 12. The spiral disk is the same as the flat disk except that the flat portion 12 is inclined along the thickness direction. The reverse spiral disk is the same as the spiral disk except that the inclination of the flat portion 12 is the same as the spiral disk.
[0141] Relative to the disk major axis diameter X (mm), the disk minor axis diameter Y (mm) preferably satisfies 0.2≤Y / X≤0.6, more preferably satisfies 0.3≤Y / X≤0.6, and further preferably satisfies 0.4≤Y / X≤0.6. By making Y / X above the above lower limit, the strength of the disk becomes sufficient, and there is no risk of disk breakage or the risk is small even when the gel crushing strength becomes high. In addition, by making Y / X below the above upper limit, the distance between axes is appropriate and the device size will not become too large, which is preferred in terms of device cost. It should be noted that when the major axis diameter and the minor axis diameter of each disk are different, the major axis diameter and the minor axis diameter of each disk preferably meet the above range.
[0142] In addition, similarly, the disk thickness T preferably satisfies 0.05≤T / X≤1.0 relative to the disk major axis diameter X, more preferably satisfies 0.05≤T / X≤0.8, and further preferably satisfies 0.07≤T / X≤0.5. By making T / X above the above lower limit, the strength of the disk becomes sufficient, and even if the gel crushing strength becomes high, there is no risk of disk breakage or the risk is small. In addition, by making T / X below the above upper limit, the disk pattern incorporated into the main body can be appropriately set, and the gel crushing strength can be easily adjusted. In addition, the weight of each disk will not be too heavy, and in particular, the load of the replacement operation is small even in the case of expansion. A suitable form is: relative to the disk major axis diameter X, the disk minor axis diameter Y satisfies 0.2≤Y / X≤0.6, and the disk thickness T satisfies 0.05≤T / X≤1.0.
[0143] The combination of the screw and the disk can be appropriately changed according to the physical properties of the hydrogel, the size of the hydrogel particles to be obtained, etc., with reference to, for example, patent documents (Japanese Unexamined Patent Publication No. 2005-35212). Figure 3The symbol FS is a feed screw, which is mainly responsible for conveying the input material into the main body. The symbol RS is a reverse screw, which is set in front of the bottom plate to reverse the flow path of the material and is responsible for guiding the material to the discharge port 210. The symbol F is a flat disk, which is mainly responsible for mixing. The symbol H is a spiral disk, which is responsible for both mixing and conveying. The symbol RH is a reverse spiral disk, which is responsible for mixing and reflux (material return). Figure 3 Detailed configuration of a rotating shaft included in a gel grinding device used in the examples described below is shown as an example. Figure 3 The numbers 1 to 4 shown are the phase angles of each disk. Figure 3 In the device, the phase difference of each disk is set to 45 degrees. Taking disk 1 as a reference, 2 refers to a state of being tilted 45 degrees in the direction opposite to the rotation direction of the rotation axis, 3 refers to a state of being tilted 90 degrees, and 4 refers to a state of being tilted 135 degrees. When disk 2 is used as a reference, 3 refers to a state of being tilted 45° in the direction opposite to the rotation direction of the rotation axis, 4 refers to a state of being tilted 90°, and 1 refers to a state of being tilted 135°. When disk 3 is used as a reference, 4 refers to a state of being tilted 45° in the direction opposite to the rotation direction of the rotation axis, 1 refers to a state of being tilted 90° in the rotation direction, and 2 refers to a state of being tilted 135° in the rotation direction. When disk 4 is used as a reference, 1 refers to a state of being tilted 45° in the direction opposite to the rotation direction of the rotation axis, 2 refers to a state of being tilted 90°, and 3 refers to a state of being tilted 135°. Furthermore, when the phase difference between the adjacent disks in the forward direction from the inlet toward the outlet is 45° in the rotation direction of the rotating shaft, the gel is returned in the direction opposite to the forward direction, and when the phase difference between the adjacent disks in the forward direction from the inlet toward the outlet is 90°, the gel stays at this position and is kneaded. When the phase difference between the adjacent disks in the forward direction from the inlet toward the outlet is 45° in the direction opposite to the rotation direction of the rotating shaft, the gel is sent out in the forward direction. Therefore, from the supply port toward the outlet, when the disks are arranged in 1→2→3→4→1, the feeding phase is presented, when the disks are arranged in 1→3→1→3 or 2→4→2→4, the kneading phase is presented, and when the disks are arranged in 4→3→2→1→4, the return phase is presented. The type, number, and arrangement of each disk are not limited to this specific example, and are appropriately changed according to the physical properties of the hydrogel, the size of the granular hydrogel to be obtained, etc. It should be noted that the phase difference is not limited to a scale of 45 degrees. For example, the phase difference may be a scale of 15°, a scale of 30°, or a scale of 60°. If the phase difference between the adjacent disks in the advancing direction from the input port toward the discharge port in the direction opposite to the rotation direction of the rotating shaft exceeds 0° and is less than 90°, it means a feed phase, if it is 90°, it means a kneading phase, and if it exceeds 90° and is less than 180°, it means a return phase, without being limited to a specific example.
[0144] In the present invention, in the arrangement of the pulverizing units of the gel pulverizing device, it is preferred to include one or more portions showing a return phase, wherein the phase difference between the adjacent disks in the advancing direction from the input port toward the discharge port is greater than 90° and less than 180°. When one or more portions having a phase greater than 90° and less than 180° are included, there is a portion showing a return phase and having the function of blocking the hydrogel inside the main body, so that immediately after the gel pulverization starts, the coarse particulate hydrogel-like crosslinked polymer having a particle size of 10 mm or more contained in the particulate hydrogel-like crosslinked polymer can be reduced from the discharge port 210 in a short time, and the amount of coarse gel mixed into the obtained particulate hydrogel-like crosslinked polymer can be reduced. The number of locations where the phase difference between adjacent disks in the arrangement of the grinding units of the gel grinding device exceeds 90° and is less than 180° can be appropriately set according to the size of the device, for example, in the preferred order of 2 or more, 4 or more, 5 or more, 7 or more, 10 or more, and 14 or more, and the upper limit can be 30 or less or 20 or less.
[0145] Examples of gel grinding devices include multi-screw mixers (kneaders) with two or more screws. Specifically, mixers with two screws, three screws, four screws, or eight screws are included. From the perspective of production efficiency, the gel grinding device is preferably used in a continuous manner. Specifically, examples of the gel pulverizing device include a CKH type continuous kneading machine (HONDA MACHINERY WORKS CO., LTD.), a two-screw extruder TEX (Japan Steel Works, Ltd.), a two-screw extruder TEX α III (Japan Steel Works, Ltd.), a continuous kneader (CONTINUOUS KNEADER, DALTON), a KRC hybrid reactor (KRC HYBRID REACTER, Kurimoto, Ltd.), a KRC kneader (KURIMOTO-READCO CONTINUOUS KNEADER, Kurimoto, Ltd.), a KEX extruder (KEX EXTRUDER, Kurimoto, Ltd.), a KEXD extruder (KEXD EXTRUDER, Kurimoto, Ltd.), a double-arm kneader ruder (KNEADER-RUDER, MORIYAMA), a two-screw kneading extruder TEX-SSG (Toshiba Machine Co., Ltd.), two-screw mixing extruder TEX-CS (Toshiba Machine Co., Ltd.), two-screw mixing extruder TEX-SX (Toshiba Machine Co., Ltd.), two-screw mixing extruder TEX-DS (Toshiba Machine Co., Ltd.), two-screw mixing extruder TEX-A (Toshiba Machine Co., Ltd.), two-screw mixing extruder TEX-B (ToshibaMachine Co., Ltd.), two-screw mixing extruder TEX-BS (Toshiba Machine Co., Ltd.), four-screw, eight-screw mixing extruder WDR series (TECHNOVEL company), etc. Therefore, in a preferred embodiment of the present invention, the gel pulverizing device is a continuous multi-screw type mixer.
[0146] (Gel crushing coefficient)
[0147] The gel crushing coefficient represents the energy applied to 1g of gel per unit time in the gel crushing device, in other words, the energy applied to 1g of water-containing gel per unit time in the gel crushing device, and is 0.02 J / g·second or more and 3.0 J / g·second or less. If the gel crushing coefficient is less than 0.02 J / g·second, the water absorption rate is slowed down and / or the amount of residual monomers is increased. If the gel crushing coefficient exceeds 3.0 J / g·second, the amount of residual monomers is increased.
[0148] The above-mentioned "time in the gel crushing device" refers to the average residence time of the hydrogel-like cross-linked polymer in the gel crushing device. The above-mentioned "energy applied to 1g of gel" refers to the gel crushing energy. That is, the gel crushing coefficient is expressed by gel crushing energy [J / g] / average residence time [s]. The average residence time and the gel crushing energy are described in detail below. It should be noted that when calculating the above-mentioned gel crushing coefficient, the gel crushing energy and the average residence time are calculated to the unit digit using the values obtained by rounding off the first decimal place, and the gel crushing coefficient is obtained by rounding off the third significant figure according to JIS Z8401:1999 to the second significant figure.
[0149] The gel crushing coefficient is preferably 0.030 J / g·sec or more, more preferably 0.040 J / g·sec or more, and further preferably 0.050 J / g·sec or more. From the viewpoint of increasing the water absorption rate, increasing AAP (absorption ratio under pressure) and reducing the amount of residual monomers, the gel crushing coefficient is preferably less than 2.9 J / g·sec, may be 2.0 J / g·sec or less, and may be 1.5 J / g·sec or less. The gel crushing coefficient is preferably 0.030 to 3.0 J / g·sec, more preferably 0.040 to 2.9 J / g·sec, further preferably 0.050 to 2.0 J / g·sec, and further preferably 0.080 to 1.5 J / g·sec.
[0150] (Gel crushing energy)
[0151] Gel Grinding Energy (GGE) refers to the mechanical energy per unit mass (unit mass of the hydrous gel) required by the gel grinding device when the hydrous gel is subjected to gel grinding, as described in International Publication No. 2011 / 126079 (corresponding to U.S. Patent Application Publication No. 2013 / 026412 and U.S. Patent Application Publication No. 2016 / 332141). In the present invention, the mechanical energy applied to the hydrous gel-like cross-linked polymer is important, and therefore, it is preferred to calculate the gel grinding energy by subtracting the current value of the gel grinding device when it is idling. In particular, when multiple devices are used to perform gel grinding, the total current value during idling becomes large, and therefore, a method of calculating by subtracting the current value during idling is suitable. The gel grinding energy when the gel grinding device is driven by three-phase AC power is calculated according to the following formula (1).
[0152] [Mathematical formula 1]
[0153] Formula (1)
[0154] Gel crushing energy [J / g] = {3 1 / 2 × voltage × (current value during gel grinding - current value during idling) × power factor × motor efficiency} / {mass of water-containing gel introduced into the gel grinding device within 1 second}
[0155] In the present application, in the calculation formula of the above formula (1), the value calculated by assuming that both the power factor and the motor efficiency are 1 is defined as gel grinding energy (GGE).
[0156] When the gel grinding device is driven by single-phase AC power, the 3 1 / 2 The calculation is performed by changing 1. In the above formula (1), the unit of voltage is [V], the unit of current is [A], and the unit of mass of the hydrogel is [g].
[0157] The "mass of the hydrogel fed into the gel mill in 1 second [g / s]" in the above formula (1) refers to, for example, when the hydrogel-like cross-linked polymer is continuously fed using a quantitative feeder, if the feed rate is [t / hr], then the value is converted into [g / s].
[0158] The gel grinding energy (GGE) is preferably 10 J / g or more, more preferably 15 J / g or more, and further preferably 20 J / g or more. The gel grinding energy (GGE) is preferably 250 J / g or less, more preferably 200 J / g or less, and further preferably 150 J / g or less. The gel grinding energy (GGE) is preferably 10 J / g or more and 250 J / g or less, more preferably 15 J / g or more and 200 J / g or less, and further preferably 20 J / g or more and 150 J / g or less. By making the gel grinding energy (GGE) above the lower limit, the particle size of the water-containing gel particles can be reduced, and the water absorption rate is further improved, so it is preferred. By making the gel grinding energy (GGE) below the upper limit, the increase in device cost can be suppressed, and the compaction (excessive aggregation) of the gel particles can be suppressed, and the water absorption rate is improved.
[0159] The gel grinding energy (GGE) can be determined by, for example, adjusting the disk pattern (= filling rate in the machine, Figure 3 to Figure 7 The type, number and arrangement of the disks shown in the figure), the amount of water / steam supplied to the gel grinding device, the rotation speed of the rotating shaft, etc. For example, if there are many return phases in the disk pattern, there is a tendency for the gel grinding energy (GGE) to increase.
[0160] (Average residence time)
[0161] From the viewpoint of reducing residual monomers, the average residence time of the hydrogel cross-linked polymer in the gel grinding device is preferably 20 seconds or more, 30 seconds or more, 35 seconds or more, 40 seconds or more, 45 seconds or more, and 50 seconds or more. From the viewpoint of productivity and device cost, the average residence time of the hydrogel cross-linked polymer in the gel grinding device is preferably 1200 seconds or less, 1000 seconds or less, 800 seconds or less, 700 seconds or less, and 600 seconds or less. The average residence time of the hydrogel cross-linked polymer in the gel grinding device is preferably 20 seconds or more and 1200 seconds or less, preferably 30 seconds or more and 1200 seconds or less, more preferably 30 seconds or more and 1000 seconds or less, further preferably 35 seconds or more and 800 seconds or less, particularly preferably 40 seconds or more and 700 seconds or less, and most preferably 45 seconds or more and 600 seconds or less. By making the average residence time of the hydrogel crosslinked polymer in the gel grinding device not less than the above lower limit, the compaction (excessive aggregation) of the gel particles is suppressed, and the water absorption rate is further improved, which is preferred. By making the average residence time of the hydrogel crosslinked polymer in the gel grinding device not more than the above upper limit, the productivity is improved and the mechanical damage to the hydrogel is reduced, which is preferred.
[0162] The average residence time of the hydrogel is determined by the ratio of the effective length L inside the gel grinding device body to the maximum diameter D of the disk (L / D), the disk pattern (= adjustment of the filling rate inside the device, Figure 3 to Figure 7 The average residence time tends to be longer if L / D is high, the rate of introduction of the hydrogel is slow, and the amount of water / steam supplied to the gel grinding device is large.
[0163] The average residence time of the hydrogel-like crosslinked polymer in the gel grinding device is a value measured by the method described in Examples.
[0164] (Gel Temperature)
[0165] In the gel grinding step, the temperature T1 of the hydrogel crosslinked polymer fed into the inlet of the gel grinding device (hereinafter also referred to as "gel temperature T1 at the inlet" or simply "gel temperature T1") is preferably 50°C or higher. By controlling the gel temperature T1 in this way, it is easy to continuously grind the hydrogel crosslinked polymer at 50°C or higher as a suitable mode. The gel temperature T1 is preferably measured by a thermometer provided at the inlet. From the viewpoint of preventing the hydrogels subjected to gel grinding from adhering to each other, the gel temperature T1 is preferably 60°C or higher, and from the viewpoint of further increasing the water absorption rate of the water-absorbent resin powder, it is more preferably 70°C or higher, and further preferably 80°C or higher. From the viewpoint of suppressing excessive drying, the gel temperature T1 is preferably 130°C or lower, more preferably 110°C or lower, further preferably 100°C or lower, and particularly preferably 90°C or lower. For the same reason, the gel temperature during grinding is preferably 130°C or lower. The gel temperature T1 can be adjusted to a desired range by keeping the hydrogel crosslinked polymer whose temperature rises due to the polymerization heat or by heating the obtained hydrogel crosslinked polymer fed into the gel grinding device.
[0166] From the viewpoint of suppressing the aggregation of the hydrogels that have been subjected to gel pulverization, the temperature T2 of the particulate hydrogel crosslinked polymer discharged from the gel pulverization device (hereinafter referred to as "gel temperature T2 at the discharge port" or simply "gel temperature T2") is preferably 60°C to 140°C, more preferably 70°C to 130°C, further preferably 80°C to 125°C, 85°C to 120°C, particularly preferably 90°C to 115°C, and most preferably 100°C to 115°C. It is preferred to set the temperature T2 in this temperature range and the temperature T1 in the aforementioned temperature range. The gel temperature T2 is preferably measured using a thermometer provided at the discharge port. It should be noted that the gel temperature T2 can be adjusted to a desired range by appropriately adjusting the set temperature of the heating unit and / or the heat-retaining unit of the gel pulverization device and the residence time of the hydrogel crosslinked polymer inside the gel pulverization device.
[0167] From the viewpoint of further increasing the water absorption rate of the water-absorbent resin powder, the gel temperature T2 at the discharge port is preferably higher than the gel temperature T1 at the input port. The difference ΔT = (T2-T1) is preferably 5°C or more, more preferably 8°C or more, and even more preferably 10°C or more. In addition, the difference ΔT = (T2-T1) is preferably 60°C or less, more preferably 50°C or less, even more preferably 40°C or less, and particularly preferably 35°C or less. It is preferably set so that the difference ΔT = (T2-T1) is within this temperature range and the temperature T1 and the temperature T2 are within the aforementioned temperature range. It should be noted that ΔT can be adjusted to a desired range by adjusting T1 and T2 separately as described above.
[0168] (Gel solid content)
[0169] In the gel grinding step, the solid content of the hydrogel introduced into the inlet of the gel grinding device (hereinafter referred to as the gel solid content) is determined by the measuring method described in the examples described later. From the viewpoints of the degree of aggregation of the hydrogels subjected to gel grinding, the energy required for grinding, the drying efficiency and the absorption performance, the gel solid content is preferably 25% to 75% by mass, more preferably 30% to 70% by mass, further preferably 35% to 65% by mass, and particularly preferably 40% to 60% by mass.
[0170] (Gel fluidizer)
[0171] In the production method described in the present invention, it is preferred to add a gel fluidizer before and / or during the gel pulverization step. Thus, a particulate hydrogel containing a gel fluidizer is taken out from the discharge port. That is, in one suitable embodiment of the present invention, the particulate hydrogel cross-linked polymer contains a gel fluidizer. By adding a gel fluidizer, the following effects are obtained: the strong adhesion or adhesion between the finely pulverized gel particles is suppressed, and the water absorption rate of the obtained water-absorbent resin is improved. In addition, the following effects are also obtained: the load in the crushing step in the pulverization step after the drying step and the granulation step is reduced, and the amount of fine powder generated is reduced. From the viewpoint that each particle of the obtained particulate hydrogel uniformly contains the gel fluidizer, it is more preferred to add it in the gel pulverization step, and it is further preferred to add it at the same time as the hydrogel is added (add it from the inlet of the hydrogel).
[0172] The amount of the gel fluidizer added can be appropriately set according to the solid content of the hydrogel or particulate hydrogel and the type of the gel fluidizer. The amount added is preferably 0.001% to 5% by mass, more preferably 0.01% to 3% by mass, further preferably 0.02% to 2% by mass, and particularly preferably 0.03% to 1% by mass relative to the solid content of the hydrogel.
[0173] Examples of the gel fluidizing agent include anionic, cationic, nonionic and amphoteric surfactants, and low-molecular or high-molecular surfactants thereof, polymer lubricants, etc. Among them, surfactants are preferred.
[0174] (Surfactant)
[0175] Specifically, examples of surfactants used in the gel fluidizing agent include (1) nonionic surfactants such as sucrose fatty acid esters, polyglycerol fatty acid esters, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene glycerol fatty acid esters, sorbitol fatty acid esters, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers, polyoxyethylene castor oils, polyoxyethylene hydrogenated castor oils, alkyl allyl formaldehyde condensation polyoxyethylene ethers, polyoxyethylene polyoxypropylene block copolymers, polyoxyethylene polyoxypropyl alkyl ethers, polyethylene glycol fatty acid esters, alkyl glucosides, N-alkyl glucamides, polyoxyethylene fatty acid amides, polyoxyethylene alkylamines, phosphate esters of polyoxyethylene alkyl ethers, and phosphate esters of polyoxyethylene alkyl allyl ethers; and (2) octyl dimethylamine. (1) alkyl dimethylaminoacetic acid betaines such as lauryl dimethylaminoacetic acid betaine, lauryl dimethylaminoacetic acid betaine, myristyl dimethylaminoacetic acid betaine, stearyl dimethylaminoacetic acid betaine; alkyl amidopropyl betaines such as lauric acid amidopropyl betaine, coconut oil fatty acid amidopropyl betaine, palm kernel oil fatty acid amidopropyl betaine, alkyl hydroxysulfobetaines such as lauryl hydroxysulfobetaine, alkyl carboxymethyl hydroxyethyl imidazolium betaine such as 2-alkyl-N-carboxymethyl-N-hydroxyethyl imidazolium betaine; (2) anionic surfactants such as alkyl aminodiacetic acid monoalkali metal salts such as laurylaminodiacetic acid monosodium, laurylaminodiacetic acid potassium, and myristylaminodiacetic acid sodium; (3) cationic surfactants such as long-chain alkyl dimethylaminoethyl quaternary ammonium salts, etc. Two or more of these may be used in combination. Among them, from the viewpoint of further increasing the water absorption rate of the water-absorbent resin powder, an amphoteric surfactant is preferred, and alkyldimethylaminoacetic acid betaine is more preferred.
[0176] (Polymer lubricant)
[0177] In the production method of the present invention, the polymer lubricants exemplified below may be added to the above-mentioned aqueous monomer solution or hydrogel within the range of achieving the object of the present invention.
[0178] As the above-mentioned polymer lubricant, specifically, maleic anhydride modified polyethylene, maleic anhydride modified polypropylene, maleic anhydride modified ethylene-propylene copolymer, maleic anhydride modified ethylene-propylene-diene terpolymer (EPDM), maleic anhydride modified polybutadiene, maleic anhydride-ethylene copolymer, maleic anhydride-propylene copolymer, maleic anhydride-ethylene-propylene copolymer, maleic anhydride-butadiene copolymer, polyethylene, polypropylene, ethylene-propylene copolymer, oxidized polyethylene, oxidized polypropylene, oxidized ethylene-propylene copolymer, ethylene-acrylic acid copolymer, ethyl cellulose, ethyl hydroxyethyl cellulose, polyoxyalkylenes such as polyethylene glycol, side chain and / or terminal polyether modified polysiloxanes, etc. can be listed. Their molecular weight (weight average molecular weight) is preferably selected in the range of 2 to 2 million, more preferably 4 to 1 million. Among these, two or more kinds can be used in combination.
[0179] In addition, as a gel fluidizing agent, these polymer lubricants and the above-mentioned surfactants can be used in combination. When a surfactant and a polymer lubricant are used in combination, the total amount added is appropriately set according to the polymerization form, the composition of the monomer aqueous solution, and the water content of the hydrogel. When added to the monomer aqueous solution, it is set in the form of concentration relative to the monomer component, when added to the hydrogel, it is set in the form of concentration relative to the solid content, and when added to both, it is set in the form of the above total.
[0180] The total amount of the surfactant and the polymer lubricant added is preferably 5% by mass or less, more preferably 3% by mass or less, and is preferably 0.001% by mass or more, particularly preferably 0.01% by mass or more, based on the solid content of the hydrogel.
[0181] (Surface tension)
[0182] The type and amount of the gel fluidizer can be appropriately adjusted in consideration of the aggregation inhibition of the granular hydrogel in the gel crushing process and the drying process. Based on the reflux amount of the absorbent article (diaper) of the obtained absorbent resin powder during actual use, it is preferred that the type and amount of gel fluidizer be such that the surface tension of the absorbent resin of the final product does not excessively decrease. For example, the type and amount of the gel fluidizer are selected in such a way that the surface tension of the absorbent resin (the surface tension of the dispersion of the absorbent resin in saline) is preferably 55 mN / m or more, more preferably 60 mN / m or more, and further preferably 65 mN / m or more. The surface tension is measured using the method described in WO2015 / 129917. As a gel fluidizer that can make the surface tension within this range, an amphoteric surfactant can be exemplified.
[0183] (Other additives)
[0184] In the gel grinding step or during the transition from the gel grinding step to the subsequent drying step, the surface crosslinking agent described in [2-7-1] or other additives described in [2-10] may be added.
[0185] (Particle size of granular aqueous gel)
[0186] In the production method of the present invention, from the viewpoint of the absorption rate of the water-absorbent resin powder to be produced, the mass average particle size d1 of the particulate hydrogel crosslinked polymer discharged from the discharge port of the gel grinding device, calculated on the basis of the solid content, is 500 μm or less. When d1 exceeds 500 μm, the water absorption rate slows down (Comparative Example 2 described later). d1 is preferably 460 μm or less, more preferably 400 μm or less, and further preferably 350 μm or less. The smaller d1 is, the more preferred it is, so its lower limit is not particularly limited, and is usually 1 μm or more, and can be 10 μm or more, 20 μm or more, 30 μm or more, or 50 μm or more. The mass average particle size d1 of the particulate hydrogel crosslinked polymer discharged from the discharge port of the gel grinding device, calculated on the basis of the solid content, can be controlled, for example, by the average residence time in the grinding device, the gel crushing energy (GGE), and the like. There is a tendency that d1 becomes larger as the average residence time becomes shorter. In addition, there is a tendency that d1 becomes larger as the gel crushing energy (GGE) becomes smaller. In addition, the solid content-equivalent mass average particle diameter d1 of the particulate hydrogel is defined by the physical property measurement method (g) described later.
[0187] In addition, as the particle size distribution of the particulate hydrogel, the content of the substance in the range of less than 150 μm in terms of solid content conversion is preferably 10% by mass or more, more preferably 25% by mass or more, and further preferably 40% by mass or more. In addition, as the particle size distribution of the particulate hydrogel, the content of the substance in the range of less than 850 μm in terms of solid content conversion is preferably 80% by mass or more, more preferably 85% by mass or more, further preferably 90% by mass or more, particularly preferably 95% by mass or more, and the upper limit is 100% by mass. The logarithmic standard deviation (σζ) of the particle size distribution is 0.2 to 1.0, more preferably 0.2 to 0.8, and further preferably 0.2 to 0.7.
[0188] (Solid content of granular hydrogel)
[0189] The solid content (solid content) of the granular hydrogel discharged from the discharge port of the gel grinding device is preferably 25% to 75% by mass, more preferably 30% to 70% by mass, further preferably 35% to 65% by mass, and particularly preferably 40% to 60% by mass. By subjecting the granular hydrogel having a solid content within the above range to the drying step, a granular dried product having a high CRC and little damage (such as an increase in water-soluble components) due to drying can be obtained.
[0190] (Polymerization rate of granular hydrogel)
[0191] The polymerization rate of the granular hydrogel discharged from the gel grinding device is within the range of the polymerization rate before being put into the above-mentioned gel grinding device, and further polymerization can be carried out in the gel grinding process. The degree of polymerization is appropriately adjusted by the heating and residence time in the gel grinding device, the residual amount of polymerization initiator in the hydrogel after polymerization, the amount of optional post-addition of polymerization initiator, etc. The polymerization rate after the gel grinding process is determined by the physical property measurement method described below in the same way as the polymerization rate before gel grinding. The polymerization rate of the granular hydrogel after gel grinding is 90% by mass or more, preferably 95% by mass or more, more preferably 98 to 99.99% by mass, and ideally 100% by mass. The granular hydrogel with a polymerization rate within the above range can avoid aggregation and adhesion during drying.
[0192] 〔2-5〕Drying process
[0193] This step is a step of drying a particulate hydrogel crosslinked polymer, preferably a particulate hydrogel crosslinked polymer containing a gel fluidizing agent, to a desired solid content to obtain a dried product. The "solid content" is a value calculated from the loss on drying (the change in mass when 1.0 g of a sample is dried at 180° C. for 3 hours).
[0194] The solid content of the dried product obtained after the drying process is preferably 80% by mass or more, more preferably 85% by mass to 99.8% by mass, further preferably 90% by mass to 99.7% by mass, further preferably 92% by mass to 99.5% by mass, particularly preferably 96% by mass to 99.5% by mass, and extremely preferably in the order of 98% by mass to 99.5% by mass. If the solid content after drying is too high, not only long-term drying is required, but also physical property degradation and coloring after drying may occur. In addition, when the solid content after drying is low, the productivity in the granulation process described later and the water absorption rate (CRC) are sometimes reduced. In the case of implementing the surface cross-linking process described later after the drying process, the physical properties are further improved by drying to the above-mentioned solid content, so it is preferred. It should be noted that the moisture content (=100-solid content) of the dried product is obtained based on the above-mentioned solid content.
[0195] The drying method in the drying step of the present invention is not particularly limited, and static drying, stirring drying, fluidized bed drying, etc. can be appropriately used. In addition, various drying methods such as heating drying, hot air drying, reduced pressure drying, infrared drying, microwave drying, drum drying, azeotropic dehydration drying with a hydrophobic organic solvent, and high-humidity drying using high-temperature steam can be used.
[0196] (Drying device)
[0197] As the drying device used in the drying process, there is no particular limitation, and one or more of a heat conduction dryer, a radiation heat conduction dryer, a hot air heat conduction dryer, an induction heating dryer, etc. can be appropriately selected. It can be intermittent or continuous. In addition, it can be a direct heating type or an indirect heating type. For example, heat conduction dryers such as ventilation belt type, ventilation circuit type, ventilation vertical type, parallel flow belt type, ventilation tunnel type, ventilation stirring type, ventilation rotary type, fluidized bed type, and air flow type can be listed. When implementing a belt drying (ventilation belt drying) in which hot air drying is carried out on a ventilation belt, the various conditions described in International Publication No. 2006 / 100300, International Publication No. 2011 / 025012, International Publication No. 2011 / 025013, and International Publication No. 2011 / 111657 can be appropriately applied.
[0198] The heating means is not particularly limited, but from the viewpoint of drying efficiency and reduction of heat damage to the water-absorbent resin, the heating means for the particulate hydrogel is preferably a heating means based on direct heat conduction and / or indirect heat conduction, wherein the direct heat conduction is based on convection heat conduction and the indirect heat conduction is based on heat conduction from a heating surface (surface in contact with the particulate hydrogel, heat source portion) of a dryer heated by a heat medium. More preferred heating means is a ventilation heating type in the case of direct heat conduction and an outer wall heating type or a tubular heating type in the case of indirect heat conduction.
[0199] In the drying process, gas can be introduced into the dryer. The gas is not particularly limited, and examples thereof include air, dry gas, nitrogen, water vapor, and mixed gases thereof. The gas acts as a carrier gas, and promotes drying by discharging the water vapor generated during drying to the outside of the dryer. Furthermore, when a heated gas is used, the gas also acts as a heat medium, thereby promoting drying. Preferably, nitrogen, water vapor, and a mixed gas thereof with air are used. When a mixed gas containing water vapor (hereinafter also referred to as a high-humidity mixed gas) is used, the inside of the dryer presents a low oxygen state, which inhibits oxidation and degradation during drying. As a result, improved performance and low coloration of the water-absorbent resin can be achieved. In addition, the moving direction of the gas can be cocurrent or countercurrent relative to the moving direction of the granular hydrogel to be dried, and they can also be mixed.
[0200] The drying conditions are appropriately selected according to the type of drying device and the solid content of the particulate hydrogel, and the drying temperature is preferably 100°C to 300°C, more preferably 150°C to 250°C, further preferably 160°C to 220°C, and particularly preferably 170°C to 200°C. When the drying temperature is lower than the above range, the drying time becomes too long, which is not economical. When the drying temperature exceeds the above range, the physical properties of the water-absorbent resin deteriorate and the coloring is significant, which is not preferred. In addition, the drying time is preferably 1 minute to 10 hours, more preferably 5 minutes to 2 hours, further preferably 10 minutes to 120 minutes, and particularly preferably 20 minutes to 60 minutes. When the drying temperature is lower than the above range, the drying temperature needs to be excessively increased, the physical properties of the water-absorbent resin deteriorate and the coloring is significant, which is not preferred. When the drying temperature exceeds the above range, the dryer becomes huge and the processing capacity is reduced, which is not economical.
[0201] In the present invention, as a preferred drying method, stirring drying using a stirring type dryer can also be adopted. This stirring drying is a type of drying operation based on heat conduction, and an indirect heating method can be used. It is preferred that the drying treatment of the dried object is continuously carried out. Therefore, there are advantages that the drying efficiency is high and the physical properties of the obtained water-absorbing resin can be suppressed from being reduced. The stirring method and form of the above-mentioned stirring type dryer are not particularly limited, and examples thereof include: a container rotating dryer in which the container itself that stores the contents rotates, vibrates, and shakes; a mechanical stirring dryer in which the contents are stirred by a rotating shaft equipped with stirring blades such as arms, blades, and paddles; a floating stirring dryer in which the contents are floated by a gas such as air; a flow path division dryer in which the flow path is divided by gravity and a partition; a high-speed shearing dryer; an impact dryer, etc. In the drying process of the present invention, a material stirring type drying in which the dried object is dried while stirring can also be suitably adopted. In the above-mentioned material stirring type drying, the adjacent dried object (particulate hydrogel) is replaced in sequence while stirring, so that one particle will contact a new particle one after another. Thus, the dried material (particulate hydrogel) is effectively heated by direct heat conduction and / or indirect heat conduction, and excessive aggregation and agglomeration of the particulate hydrogel are suppressed. When the stirring type dryer is used for stirring and drying, the conditions described in International Publication No. 2018 / 092863 and International Publication No. 2018 / 092864 can be appropriately applied.
[0202] Furthermore, in the present drying step, by adding a surface crosslinking agent described later, it is possible to carry out the drying of the particulate hydrogel and the heat treatment step of the surface crosslinking step in the same step.
[0203] 〔2-6〕Crushing and classification process
[0204] This step is a step of pulverizing and / or classifying the dried product obtained in the above-mentioned drying step to obtain a water-absorbent resin powder having a preferred specific particle size. It should be noted that this step is different from the above-mentioned gel pulverization step [2-4] in that the pulverized product undergoes a drying step.
[0205] This step is carried out before and / or after the surface cross-linking step [2-7], preferably before the surface cross-linking step [2-7], and may be carried out two or more times before and after the surface cross-linking step [2-7].
[0206] Examples of the machine (pulverizer) used in the pulverizing step of the present invention include high-speed rotary pulverizers such as roll mills, hammer mills, screw mills, and pin mills; vibration mills, knuckle pulverizers, and barrel agitators, which can be used in combination as needed.
[0207] (granularity)
[0208] From the viewpoint of water absorption rate and water absorption ratio under pressure, the mass average particle size (D50) of the water-absorbent resin powder before surface crosslinking is preferably 200 μm or more, more preferably 200 μm to 600 μm, further preferably 220 μm to 550 μm, and particularly preferably 250 μm to 500 μm.
[0209] The content of fine particles having a particle size of less than 150 μm as defined by standard sieve classification is preferably as low as possible and is preferably 0 to 5 wt %, more preferably 0 to 3 wt %, and even more preferably 0 to 2 wt % based on the total weight of the water-absorbent resin powder.
[0210] Furthermore, the smaller the amount of coarse particles having a particle size of 850 μm or more as defined by standard sieve classification, the better. From the viewpoint of water absorption rate, etc., the amount is preferably 0 to 5 wt %, more preferably 0 to 3 wt %, and even more preferably 0 to 1 wt % based on the total water-absorbent resin powder.
[0211] In addition, from the viewpoints of water absorption speed, water absorption ratio under pressure, etc., the proportion of particles having a particle size of 150 μm or more and less than 850 μm is preferably 90 wt % or more, more preferably 95 wt % or more, further preferably 98 wt % or more, and particularly preferably 99 wt % or more (the upper limit is 100 wt %) based on the entire water-absorbent resin powder.
[0212] 〔2-7〕Surface cross-linking process
[0213] This process is a process of adding a surface crosslinking agent that reacts with the functional groups (especially carboxyl groups) of the water-absorbent resin powder and causing a crosslinking reaction, and is also called a post-crosslinking process. In the manufacturing method described in the present invention, in this process, after adding a surface crosslinking agent to the water-absorbent resin powder, a heat treatment is performed to cause a crosslinking reaction. In the water-absorbent resin powder obtained by the constitution of the present invention, the aggregation and adhesion of the particles are suppressed, so that it is easy to form a layer based on the surface treatment agent on the surface of each particle as a whole, and even if it is crushed after the surface crosslinking process, it is easy to maintain the surface treatment layer. Therefore, the AAP (water absorption under pressure) of the obtained water-absorbent resin is easy to become high. Therefore, in a suitable form of the present invention, after the gel crushing process, a surface crosslinking process is also included. This process has a surface crosslinking agent adding process and a heat treatment process, and a cooling process can be provided after the heat treatment process as needed. In addition, the various conditions described in International Publication No. 2018 / 092863 can be appropriately applied. The surface crosslinking process can be performed, for example, at the same time as the drying process, after the drying process, after the crushing and classification process, etc.
[0214] 〔2-7-1〕Surface cross-linking agent adding step
[0215] This step is a step of preparing a water-absorbent resin powder containing a surface crosslinking agent to be supplied to the surface crosslinking step by mixing the water-absorbent resin powder and the surface crosslinking agent.
[0216] (Surface cross-linking agent)
[0217] As the surface crosslinking agent, a surface crosslinking agent that can react with multiple functional groups (preferably multiple carboxyl groups) of the water-absorbent resin can be used, and preferably a surface crosslinking agent that can form a covalent bond or an ionic bond, and further a covalent bond can be used. Specifically, polyol compounds such as ethylene glycol, diethylene glycol, propylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, 1,3-propylene glycol, dipropylene glycol, 2,2,4-trimethyl-1,3-pentanediol, polypropylene glycol, glycerol, polyglycerol, 2-butene-1,4-diol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,2-cyclohexanedimethanol, 1,2-cyclohexanol, trimethylolpropane, diethanolamine, triethanolamine, polyoxypropylene, ethylene oxide-propylene oxide block copolymer, pentaerythritol, and sorbitol can be listed; ethylene glycol Epoxy compounds such as alcohol diglycidyl ether, polyethylene glycol diglycidyl ether, glycerol polyglycidyl ether, diglycerol polyglycidyl ether, polyglycerol polyglycidyl ether, propylene glycol diglycidyl ether, polypropylene glycol polyglycidyl ether, glycidol, sorbitol polyglycidyl ether, pentaerythritol polyglycidyl ether, trimethylolpropane polyglycidyl ether, neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether; polyamine compounds such as ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, polyethyleneimine, and their inorganic or organic salts; 2,4-toluene diisocyanate cyanate, hexamethylene diisocyanate and other polyisocyanate compounds; aziridine compounds such as polyaziridine; polyoxazoline compounds such as 1,2-ethylenebisoxazoline, bisoxazoline, polyoxazoline; carbonic acid derivatives such as urea, thiourea, guanidine, dicyandiamide, 2-oxazolinone; 1,3-dioxolane-2-one (ethylene carbonate), 4-methyl-1,3-dioxolane-2-one, 4,5-dimethyl-1,3-dioxolane-2-one, 4,4-dimethyl-1,3-dioxolane-2-one, 4-ethyl-1,3-dioxolane-2-one, 4-hydroxymethyl-1,3-dioxolane Alkylene carbonate compounds such as oxolane-2-one, 1,3-dioxane-2-one, 4-methyl-1,3-dioxane-2-one, 4,6-dimethyl-1,3-dioxane-2-one, 1,3-dioxolane-2-one; halogenated epoxy compounds such as epichlorohydrin, epibromohydrin, α-methylepichlorohydrin and their polyamine adducts; oxetane compounds; silane coupling agents such as γ-glycidoxypropyltrimethoxysilane and γ-aminopropyltriethoxysilane; polyvalent metal compounds such as hydroxides, chlorides, sulfates, nitrates or carbonates of zinc, calcium, magnesium, aluminum, iron, zirconium, etc. Among these, two or more kinds may be used in combination.Among the above-mentioned surface cross-linking agents, one or more selected from polyol compounds, polyvalent metal ions, epoxy compounds, oxazoline compounds and alkylene carbonate compounds are preferred, and one or more selected from polyvalent metal ions, epoxy compounds, oxazoline compounds and alkylene carbonate compounds are more preferred.
[0218] (Surface crosslinking agent solution)
[0219] The amount of the surface crosslinking agent added is preferably 5% by mass or less, more preferably 3% by mass or less, further preferably 2% by mass or less, further preferably 1% by mass or less, and particularly preferably 0.1% by mass or less, based on the solid content of the water-absorbent resin. The lower limit is preferably 0.001% by mass or more, and more preferably 0.01% by mass or more.
[0220] The surface crosslinking agent may be added in its original form. From the perspective of ease of addition, it is preferably added in the form of a solution dissolved in water or an organic solvent. The concentration of the surface crosslinking agent solution is preferably 1% by mass or more, more preferably 2% by mass or more. The total amount of the solvent selected from water and an organic solvent is preferably 0 to 10% by mass, more preferably 0.1% to 8% by mass, and further preferably 0.5% to 5% by mass relative to the solid content of the water-absorbent resin. When water and an organic solvent are used in combination, water is preferably the main component.
[0221] When adding in the form of an aqueous solution, the concentration of the aqueous solution can be adjusted according to the water content of the water-absorbent resin powder at the time of contact with the surface crosslinking agent, which is preferred. When the surface crosslinking agent does not form a solution due to low solubility in water, it is preferred to add a hydrophilic solvent such as alcohol to form a uniform solution.
[0222] 〔2-6-2〕Heat treatment process
[0223] This step is a step of heat-treating the water-absorbent resin powder containing the surface crosslinking agent to obtain a surface-crosslinked dry product.
[0224] (Surface cross-linking temperature)
[0225] In this step, the water-absorbent resin powder containing the surface crosslinking agent is preferably heated to 100° C. or higher. The preferred maximum temperature varies depending on the type of the surface crosslinking agent, but is 100° C. to 250° C., more preferably 120° C. to 230° C., and even more preferably 150° C. to 210° C.
[0226] (time)
[0227] The time of the heat treatment process can be appropriately set according to the moisture content of the object of the heat treatment process, the type of the surface crosslinking agent, the thermal efficiency of the heating device, etc. As a rough benchmark, as long as the moisture content is heated to 10% by mass or less, the time is in the range of 10 minutes to 120 minutes, preferably 30 minutes to 90 minutes.
[0228] (Heating form)
[0229] The heating device used in the surface cross-linking step is not particularly limited, but a heating device of a conductive heat transfer type based on solid-solid contact and having a stirring mechanism is preferably used from the viewpoint of preventing uneven heating.
[0230] 〔2-7〕Cooling process
[0231] In the manufacturing method described in the present invention, it is preferred that: after the aforementioned drying process or surface cross-linking process and before the granulation process described later, there is a cooling process for forcibly cooling the dried product or the surface cross-linked dried product to adjust it to the desired temperature. The cooling process can be carried out using existing known cooling means. In addition, the cooling temperature can be appropriately adjusted. Regarding the cooling process [2-7] to the fine powder recycling process [2-9], the various conditions disclosed in International Publication No. 2018 / 092864 can be appropriately applied.
[0232] 〔2-8〕Pelletizing process
[0233] This step is a step of adjusting the particle size of the surface-crosslinked water-absorbent resin powder. Through this particle size adjustment step, a water-absorbent resin powder with a more positively controlled particle size or particle size distribution can be obtained.
[0234] The granulation process preferably includes a crushing step and / or a classification step. The crushing step is a step of using a crusher to disassemble the granules that have been slowly aggregated after the surface treatment process and adjust the particle size. The classification step is a step of using a classifier to remove coarse particles and fine powder from the surface-crosslinked granules or their crushed products.
[0235] As a crusher, there is no particular limitation, and examples thereof include a vibration mill, a roller granulator, a claw type pulverizer, a roller mill, a high-speed rotary pulverizer (pin mill, hammer mill, screw mill), a barrel agitator, etc. Preferably, a crusher that causes little damage to the dried product or the dried product cross-linked on the surface, specifically, a roller granulator (MATSUBO CORPORATION), a granulator (Kurimoto, Ltd.), a round mill (TOKUJU CORPORATION), etc. As a classifier, a vibrating or shaking sieve classifier using a screen is used.
[0236] 〔2-9〕Micro powder recycling process
[0237] "Micropowder recycling process" refers to a process in which the micropowder removed by the classification step is directly supplied to any process or supplied to any process after the micropowder is granulated. It is preferably a process in which the micropowder or micropowder granules are put into the process before the drying process and reused. As the process before the drying process, the monomer aqueous solution prepared by the monomer aqueous solution preparation process, the hydrogel during the polymerization process, the pulverization process of the hydrogel after the polymerization, the drying process of the granular hydrogel, etc. can be listed. Micropowder can be added directly to these processes, and it can also be added after the micropowder is swollen and gelled or granulated with water. In addition, water, a cross-linking agent, a binder other than water (such as a water-soluble polymer, a thermoplastic resin), a polymerization initiator, a reducing agent, a chelating agent, an anti-coloring agent, etc. can also be added together with the micropowder.
[0238] The preferred recovery amount of fine powder is appropriately set according to the target particle size.
[0239] 〔2-10〕Other processes
[0240] The production method of the present invention may further include a pulverizing step, a classification step, a rewetting step, a granulating step, a transportation step, a storage step, a packaging step, a custody step, etc., in addition to the above steps, as required.
[0241] (Other additives)
[0242] In addition to the optional surface crosslinking agent and gel fluidizing agent mentioned above, other additives may be further added before or after drying, such as polymer powder (for example, starch such as tapioca acetate starch), inorganic fine particles, anti-dust agents, dry water-absorbing resins (fine powders), liquid permeability improvers, reducing agents (for example, sodium sulfite) and other existing well-known ingredients.
[0243] [3] Physical properties of water-absorbent resin powder as a product
[0244] When the water-absorbent resin powder (particularly, the surface-crosslinked water-absorbent resin powder is also referred to as a water-absorbent) obtained by the production method of the present invention is used in absorbent articles, particularly disposable diapers, it is desirable that at least one, preferably two or more, more preferably three or more, and even more preferably all of the properties shown in (3-1) to (3-5) below be controlled within a desired range. If all of the following properties do not satisfy the following ranges, the effects of the present invention may not be fully achieved.
[0245] 〔3-1〕CRC (centrifuge holding capacity)
[0246] The CRC (centrifuge retention capacity) of the water-absorbent resin powder (water-absorbing agent) of the present invention is usually 5 g / g or more, preferably 15 g / g or more, more preferably 25 g / g or more, and even more preferably 30 g / g or more. The upper limit is not particularly limited, but a higher CRC is preferred. From the viewpoint of balance with other physical properties, the CRC is preferably 70 g / g or less, more preferably 50 g / g or less, and even more preferably 40 g / g or less.
[0247] When the CRC is less than 5 g / g, the absorption amount is small and it is not suitable as an absorbent body of absorbent articles such as diapers. In addition, when the CRC exceeds 70 g / g, the absorption rate of body fluids such as urine and blood is reduced, so it is not suitable for use in diapers with high water absorption rate. It should be noted that CRC can be controlled by changing the type and amount of internal crosslinking agents, surface crosslinking agents, etc.
[0248] 〔3-2〕Water content and solid content
[0249] The water content of the water-absorbent resin powder (water-absorbent) is preferably more than 0% by mass and less than 20% by mass, more preferably 1% to 15% by mass, further preferably 2% to 13% by mass, and particularly preferably 2% to 10% by mass. By setting the water content within the above range, a water-absorbent having excellent powder properties (e.g., fluidity, handling properties, damage resistance, etc.) is obtained. In addition, the solid content of the surface-crosslinked water-absorbent resin powder (water-absorbent) is preferably 80% by mass or more, more preferably 85% to 99% by mass, further preferably 87% to 99% by mass, and particularly preferably 90% to 99% by mass.
[0250] 〔3-3〕Particle size
[0251] The mass average particle size d3 (D50) of the water-absorbent resin powder (water-absorbing agent) is preferably 200 μm or more, more preferably 200 μm to 600 μm, further preferably 250 μm to 550 μm, and particularly preferably 300 μm to 500 μm. In addition, the proportion of particles having a particle size of less than 150 μm is preferably 10% by mass or less, more preferably 8% by mass or less, and further preferably 6% by mass or less. In addition, the proportion of water-absorbent resin powder having a particle size exceeding 850 μm is preferably 5% by mass or less, more preferably 3% by mass or less, and further preferably 1% by mass or less. The water-absorbing agent contains preferably 90% by mass or more, more preferably 95% by mass or more, further preferably 97% by mass or more, and particularly preferably 99% by mass or more of particles having a particle size of 150 μm to 850 μm. Ideally, it is 100% by mass. The logarithmic standard deviation (σζ) of the particle size distribution is preferably 0.20 to 0.50, more preferably 0.25 to 0.40, and further preferably 0.27 to 0.35.
[0252] 〔3-4〕AAP (absorption under pressure)
[0253] The AAP (absorption under pressure) of the water-absorbent resin powder (water-absorbing agent) is preferably 15 g / g or more, more preferably 20 g / g or more, further preferably 23 g / g or more, further preferably 24 g / g or more, particularly preferably 25 g / g or more, and most preferably 26 g / g or more. The upper limit is not particularly limited, but is preferably 35 g / g or less, and more preferably 30 g / g or less.
[0254] When the AAP is less than 15 g / g, the amount of liquid reflux (sometimes referred to as "Re-Wet") when pressure is applied to the absorbent increases, and therefore, it is not suitable as an absorbent for absorbent articles such as disposable diapers. It should be noted that the AAP can be controlled by adjusting the particle size, changing the surface crosslinking agent, etc. In addition, as described above, the water-absorbent resin powder obtained by the constitution of the present invention can easily increase the AAP (absorbency under pressure) of the obtained water-absorbent resin.
[0255] 〔3-5〕Vortex (water absorption speed)
[0256] The Vortex (water absorption rate) of the water-absorbent resin powder (water-absorbing agent) is preferably 65 seconds or less, 60 seconds or less, 50 seconds or less, 40 seconds or less, 30 seconds or less, 25 seconds or less, and less than 23 seconds, respectively. The lower limit is not particularly limited, but is preferably 5 seconds or more, and more preferably 10 seconds or more.
[0257] By setting Vortex in the above range, a predetermined amount of liquid can be absorbed in a short time. When used in an absorbent body of an absorbent article such as a disposable diaper, the user's skin feels wet for a shorter time, which is less likely to cause discomfort and can reduce leakage.
[0258] 〔3-6〕Residual monomer amount (content ratio)
[0259] The content of residual monomers in the water-absorbent resin powder (water-absorbent) is preferably 450 ppm or less, more preferably 430 ppm or less, and further preferably 420 ppm or less. With this form, even if the water-absorbent resin powder (water-absorbent) is used in sanitary materials, low skin irritation can be expected. The lower limit of the residual monomers is about 1 ppm. It should be noted that, regardless of the neutralization rate, the content is calculated as if unneutralized acrylic acid is present.
[0260] [4] Application of water-absorbent resin powder (water-absorbent)
[0261] The water-absorbent resin powder (water-absorbent) of the present invention can be used for the purpose of water absorption and can be widely used as an absorbent. In addition, it can be used as an absorbent article containing the absorbent. In particular, the water-absorbent of the present invention has excellent water absorption speed and reduced residual monomer content. Therefore, among absorbent articles, it is suitable for use as an absorbent suitable for sanitary articles worn on the body surface of humans or animals for absorbing body fluids such as urine or blood (hereinafter referred to as "wearing type absorbent"). In addition, it can also be suitably used as an absorbent suitable for sanitary articles configured on certain objects (such as floors, mattresses, etc.) for absorbing body fluids such as urine or blood of humans or animals (hereinafter referred to as "configuration type absorbent"). As a wearing type absorbent, for example, diapers, incontinence pads, sanitary napkins for physiological use, etc. can be listed, and as a configuration type absorbent, pet sheets, waterproof sheets for care, simple toilets for disasters, etc. can be listed. As an example of other absorbent articles, for example, cat litter, dripping absorbent materials, fresh-keeping materials, anti-condensation sheets, etc. can be listed. Other uses of water-absorbent resin powder (water-absorbent) include soil water-retaining agent, seedling-raising sheet, seed coating material, disposable hot pack, cooling handkerchief, cold-keeping agent, medical waste liquid solidifying agent, residual soil solidifying material, anti-water-damage waste liquid gelling agent, water-absorbent sandbag, wet compress material, cosmetic thickener, electrical / electronic material communication cable waterproof material, gasket filler, fertilizer slow-release agent, various slow-release agents (space sterilizing agent, fragrance, etc.), wound protection clothing material, anti-condensation building material, oil moisture remover, etc. In addition, the water-absorbent of the present invention can also be used as a coating, adhesive, anti-blocking agent, light diffusing agent, matting agent, decorative board additive, artificial marble additive, toner additive, etc., in the use of making it absorb water / swell and mix it with resin and substrate.
[0262] In addition, as a raw material of the absorbent body, an absorbent material such as pulp fiber may be used together with the absorbent resin powder (water absorbing agent). In this case, the content (core concentration) of the absorbent resin powder (water absorbing agent) in the absorbent body is preferably 30% to 100% by mass.
[0263] By setting the core concentration to the above range, when the absorbent is used in an absorbent article, skin irritation and dermatitis during use can be suppressed. Furthermore, the absorbent has excellent diffusivity of body fluids such as urine and blood, so it is expected that the absorption amount will be increased by effectively distributing the liquid.
[0264] Example
[0265] The present invention is described in more detail with reference to the following experimental examples. However, the present invention is not to be construed limitatively by these descriptions, and experimental examples obtained by appropriately combining the technical means disclosed in each experimental example are also included in the scope of the present invention.
[0266] In addition, the "water-absorbent resin" described below refers to a granular dry product that has undergone a drying process, a granular dry product that has been surface-crosslinked, or a water-absorbent resin powder, and a surface-crosslinked water-absorbent resin powder, and the "hydrogel" refers to a hydrogel-like crosslinked polymer that has not undergone a drying process or a granular hydrogel-like crosslinked polymer.
[0267] In addition, the electrical equipment used in the experimental examples (including the equipment for measuring the physical properties of the water-absorbent resin) used a power supply of 60 Hz and 200 V or 100 V unless otherwise noted. In addition, the physical properties of the water-absorbent resin and the hydrogel described below were measured at room temperature (20° C. to 25° C.) and a relative humidity of 50% RH±10% unless otherwise noted.
[0268] For convenience, "liter" may be expressed as "1" or "L", and "mass %" or "weight %" may be expressed as "wt %". When measuring trace components, the detection limit or less may be expressed as ND (Non Detected).
[0269] [Physical property measurement method]
[0270] (a) CRC (centrifuge retention capacity) of water-absorbent resin powder
[0271] The CRC (centrifuge retention capacity) of the water-absorbent resin powder was measured in accordance with NWSP 241.0.R2 (15).
[0272] (b) Water content and solid content of water-absorbent resin powder
[0273] The moisture content of the water-absorbent resin powder was measured according to NWSP 230.0.R2 (15). In the measurement, the mass of the sample was changed to 1.0 g, the drying temperature was changed to 180°C, and the moisture content and solid content of the water-absorbent resin powder were calculated from the drying loss after drying for 3 hours.
[0274] (c) Mass average particle size (d3) of water-absorbent resin powder
[0275] The mass average particle size (d3) of the water-absorbent resin powder was measured according to the method described in columns 27 and 28 of US Pat. No. 7,638,570.
[0276] (d) Polymerization rate of aqueous gel
[0277] 1.00 g of the sampled hydrogel is added to 1000 g of ion exchange water at room temperature (at this point, the polymerization reaction is substantially stopped), stirred at 300 rpm for 2 hours, and then filtered to remove the insoluble components. The amount of monomer extracted from the filtrate obtained by the above operation is measured using liquid chromatography. When the amount of the monomer is set as the residual monomer amount m (g), the polymerization rate C (mass %) of the hydrogel is calculated according to the following (Formula 3). In addition, it is preferred to measure the polymerization rate immediately after sampling the hydrogel. In the case where it takes time from sampling to measurement, it is necessary to perform the polymerization stop operation by forced cooling (contact with dry ice, liquid nitrogen, ice water, etc.).
[0278] C (mass %) = 100 × {1-m / (M × α / 100)} … (Formula 3)
[0279] In (Formula 3), M refers to the mass (g) of the hydrogel, and α refers to the solid content (mass %) of the hydrogel.
[0280] (e) Solid content of hydrogel
[0281] The water content of the hydrogel is measured according to NWSP 230.0.R2 (15). It should be noted that, during the measurement, the mass of the sample is changed to 2.0 g, the drying temperature is changed to 180°C, and the drying time is changed to 24 hours. Specifically, after 2.0 g of the hydrogel is put into an aluminum cup with a bottom diameter of 50 mm, the total mass W1 (g) of the sample (hydrogel and aluminum cup) is accurately weighed. Next, the sample is placed in an oven with an atmosphere temperature set to 180°C. After 24 hours, the sample is taken out of the oven and the total mass W2 (g) is accurately weighed. When the mass of the hydrogel used in this measurement is set to M (g), the solid content α (mass %) of the hydrogel is calculated according to the following (Formula 4).
[0282] α(mass %)=100-{(W1-W2) / M}×100…(Formula 4).
[0283] (f) Particle size of granular aqueous gel
[0284] The mass average particle size (D50) of the particulate aqueous gel was measured according to the method described in WO2016 / 204302.
[0285] That is, 20 g of a hydrogel (solid content α (mass %)) at a temperature of 20 to 25°C is added to 1000 g of a 20 mass % sodium chloride aqueous solution (hereinafter referred to as "EMAL aqueous solution") containing 0.08 mass % EMAL 20C (surfactant, manufactured by Kao Corporation) to prepare a dispersion, and the dispersion is stirred at 300 rpm for 16 hours using a rotor piece having a length of 50 mm and a diameter of 7 mm (using a cylindrical polypropylene container of about 1.14 L having a height of 21 cm and a diameter of 8 cm).
[0286] After the stirring was completed, the dispersion was poured into the center of a JIS standard sieve (inner diameter: 20 cm, mesh size: 8 mm / 4 mm / 2 mm / 1 mm / 0.60 mm / 0.30 mm / 0.15 mm / 0.075 mm) placed on a rotating disk. After all the hydrogel was washed out on the sieve using 100 g of the EMAL aqueous solution, the sieve was manually rotated (20 rpm) with respect to 6000 g of the EMAL aqueous solution, while a sprayer (72 holes, liquid volume: 6.0 [L / min]) was used from a height of 30 cm above the top to inject water over a range (50 cm 2 ) is uniformly poured with water throughout the entire sieve, and this operation is repeated 4 times to classify the hydrogel. After draining the water on the classified first-stage sieve for about 2 minutes, the hydrogel is weighed. The second and subsequent sieves are also classified by the same operation, and the hydrogel remaining on each sieve is weighed after draining the water. It should be noted that the type of the above-mentioned sieve is appropriately changed according to the particle size of the hydrogel. For example, when the particle size of the hydrogel is fine and the sieve with a mesh size of 0.15mm or 0.075mm is clogged, a JIS standard sieve with a larger diameter (diameter of 30cm, mesh size of 0.15mm and 0.075mm) is used.
[0287] The mass of the hydrogel remaining on each sieve is used to calculate the proportion (mass %) of the total hydrogel using the following (Formula 5). The mesh size of the sieve after water control is plotted on logarithmic probability paper according to the following (Formula 6). The plotted cumulative sieve %R is equivalent to a particle size of 50 mass % as the mass average particle size (D50) of the hydrogel with a solid content rate α (mass %).
[0288] X(%)=(w / W)×100 … (Formula 5)
[0289] R(α)(mm)=(20 / W) 1 / 3 ×r … (Formula 6)
[0290] In addition, here,
[0291] X: Mass % (%) of the hydrous gel remaining on each sieve after classification and water control
[0292] w: The mass (g) of the hydrous gel remaining on each sieve after classification and water control
[0293] W: Total mass of the hydrous gel remaining on each sieve after classification and water control (g)
[0294] R(α): Mesh size of the sieve when converted to a water-containing gel having a solid content ratio α (mass %) (mm)
[0295] r: The mesh size (mm) of the sieve through which the hydrogel after swelling in a 20 mass % sodium chloride aqueous solution was classified.
[0296] (g) Mass average particle size (d1) of the granular hydrogel in terms of solid content
[0297] According to WO2016 / 204302, based on the solid content α (mass %) of the granular hydrogel calculated in (e) above and the mass average particle size (D50) of the hydrogel having the solid content α (mass %) calculated in (f) above, the particle size d1 converted to the solid content of the granular hydrogel (the mass average particle size obtained by converting the solid content into the dried product of the granular hydrogel) is calculated according to the following (Formula 7).
[0298] SolidD50(d1)=GelD50×(α / 100) 1 / 3 … (Formula 7)
[0299] In addition, here,
[0300] GelD50: Mass average particle size (μm) of the granular hydrogel with solid content α (mass %)
[0301] α: Solid content of particulate hydrogel (mass %)
[0302] Solid D50 (d1): mass average particle size (μm) of the solid content converted into a hydrogel.
[0303] (h) Vortex (water absorption time) of water-absorbent resin powder
[0304] The Vortex (water absorption time) of the water-absorbent resin powder was measured as follows: First, 0.02 parts by mass of Food Blue No. 1 (Brilliant Blue) as a food additive was added to 1000 parts by mass of a previously prepared physiological saline solution (0.9% by mass sodium chloride aqueous solution), and the liquid temperature was adjusted to 30°C.
[0305] Next, 50 ml of the physiological saline solution was measured in a beaker with a capacity of 100 ml, and 2.0 g of water-absorbent resin powder was added while stirring at 600 rpm using a rotor piece having a length of 40 mm and a diameter of 8 mm. The time from the time when the water-absorbent resin powder was added to the time when the water-absorbent resin powder absorbed the physiological saline solution and covered the rotor piece was measured as Vortex (water absorption time) (unit: seconds).
[0306] (i) AAP (absorption under pressure) of water-absorbent resin powder
[0307] The AAP (absorption under pressure) of the water-absorbent resin powder was measured in accordance with NWSP 242.0.R2 (15). In the measurement, the load condition was changed to 4.83 kPa (0.7 psi).
[0308] (j) Average residence time
[0309] The average residence time (seconds) of the hydrogel in the gel grinding device was determined by the following method.
[0310] First, in Example 1 described later, except that Blue No. 1 was added to the monomer aqueous solution so as to be 1% by mass (relative to the monomer solution), polymerization was carried out in the same manner to prepare a blue-colored hydrogel. Next, an uncolored hydrogel was added to the gel grinding device at a predetermined feeding speed, and the device was operated stably. Without changing the feeding speed of the hydrogel, a blue-colored hydrogel was added instead of the hydrogel, and then an uncolored hydrogel was added at the same speed to continue the gel grinding. The time when the blue hydrogel was started to be added was regarded as 0 seconds, and the granular hydrogel discharged from the gel grinding device was sampled every 5 seconds.
[0311] After putting 15g of the sampled hydrogel into a polyethylene bag of size A with a zipper (produced by a Japanese company, 70mm long, 50mm wide, and 0.04mm thick), a weight (15kg) with a square bottom of 80mm long and wide is placed on the bag for 5 seconds to form it into a sheet. At this time, the air trapped in the bag is removed while forming. Next, the b value of the obtained sheet sample is measured using a spectrophotometer SZ-Σ80COLORMEASURING SYSTEM (produced by Nippon Denshoku Industries) under the conditions of reflection measurement / standard white plate No.1 / 30φ projection tube. Five measurements are performed on one sample, and the average value is calculated. In addition, a weight is placed in each measurement to adjust the shape of the sample. The b value is also calculated for the hydrogel sampled every 5 seconds. The bluer the hydrogel is, the smaller the b value (less than 0 and the larger the absolute value). The sampling time of the most blue (smallest b value) hydrogel is set as the average residence time (minutes). In addition, when the gel grinding step is performed multiple times, the average residence time of each time is measured, and the total is made into the average residence time (minutes).
[0312] (k) Residual monomer content
[0313] The residual monomer content of the water-absorbent resin was measured according to NWSP 210.0.R2 (15). Specifically, 1.0 g of the water-absorbent resin was added to 200 ml of a 0.9 mass % sodium chloride aqueous solution, stirred at 500 rpm for 1 hour using a 35 mm long stirrer piece, and then filtered, and the amount of monomer eluted into the filtrate was measured by high performance liquid chromatography. The residual monomer content was expressed as a mass ratio relative to the water-absorbent resin (unit: ppm).
[0314] (l) Evaluation of the amount of coarse gel
[0315] At a time point of twice the average residence time from the time when the hydrogel cross-linked polymer was added to the main body from the inlet of the gel grinding device, the granular hydrogel discharged from the gel grinding device was sampled. 100 g of the sampled granular hydrogel was added to 5000 g of a 20% sodium chloride aqueous solution (hereinafter referred to as "EMAL aqueous solution") containing 0.08% by mass EMAL 20C (surfactant, manufactured by Kao Corporation) to prepare a dispersion, and a small stirrer piece of 50 mm in length × 7 mm in diameter was stirred at 500 rpm for 16 hours. After the stirring was completed, the above dispersion was added to the center of a JIS standard sieve (inner diameter 20 cm, mesh size 16 mm), and the number of hydrogels on the sieve was measured. The number of the above granular hydrogels was 1 or less, set to 0, the number of 2 or more and 3 or less was set to △, and the number of 4 or more was set to ×.
[0316] [Example 1]
[0317] (Step of Preparing Monomer Aqueous Solution)
[0318] A monomer aqueous solution containing 300 parts by mass of acrylic acid, 100 parts by mass of a 48.5% by mass sodium hydroxide aqueous solution, 0.65 parts by mass of polyethylene glycol diacrylate (average n number: 9), 16.4 parts by mass of a 0.1% by mass trisodium diethylenetriaminepentaacetate aqueous solution, and 273.2 parts by mass of deionized water was prepared.
[0319] Next, 150.6 parts by mass of a 48.5% by mass sodium hydroxide aqueous solution was continuously mixed by line mixing while the monomer aqueous solution whose temperature was adjusted to 38° C. was continuously fed by a metering pump. At this time, the liquid temperature of the monomer aqueous solution rose to 87° C. due to the heat of neutralization.
[0320] (Polymerization process)
[0321] Furthermore, after 13.2 parts by mass of a 4% by mass sodium persulfate aqueous solution was continuously mixed by pipeline mixing, the mixture was continuously supplied to a continuous polymerization machine having a planar polymerization belt with baffles at both ends in a manner to a thickness of 10 mm. Thereafter, polymerization was continuously carried out for a polymerization time of 3 minutes to obtain a strip-shaped hydrogel (1a). The obtained strip-shaped hydrogel (1a) was cut according to the processing speed and input interval in the gel crushing device described later to obtain a short strip-shaped hydrogel (1b) having a width of several centimeters. The polymerization rate of the short strip-shaped hydrogel (1b) was 98.5% by mass and the solid content was 53% by mass.
[0322] (Gel crushing process)
[0323] As a gel grinding device, a device having a main body (barrel) with two rotating shafts rotating in the same direction and at the same speed is used to grind the short strip of water-containing gel (1b). Figure 3 The structure shown in the figure is provided with a feed screw (FS) and a reverse screw (RS), and a flat disk (F), a spiral disk (H) and a reverse spiral disk (RH) as a pulverizing unit. Figure 3 The numbers 1 to 4 shown are the phase angles of each disk. Taking disk 1 as the reference, 2 refers to a state in which the disk is tilted 45 degrees in the direction opposite to the rotation direction of the rotation axis, 3 refers to a state in which the disk is tilted 90 degrees, and 4 refers to a state in which the disk is tilted 135 degrees. Figure 3 In the structure shown, the return phase is 1 position. The diameter of each disk is 50 mm. The ratio L / D of the effective length of the main body (effective length in the barrel) L to the maximum diameter D of the disk is 13.5, and the porosity V is 50%. The barrel is a jacket structure, and has a gas supply port that penetrates the jacket and injects water vapor into the main body.
[0324] First, the heat medium was circulated inside the jacket and maintained at 105°C. Thereafter, the rotation speed was set to 50 rpm, and the short-shaped hydrogel (1b) heated to 80°C was fed into the feed port of the gel grinding device at a rate of 0.25 kg / min (a rate of one short-shaped hydrogel (1b) every 5 seconds). At this time, a 10% by mass lauryldimethylaminoacetic acid betaine aqueous solution and 90°C water were supplied from the feed port simultaneously with the hydrogel (1b), and further, 0.6 MPa water vapor was supplied from the gas supply port. The supply amount of lauryldimethylaminoacetic acid betaine in terms of solid content was 0.08% by mass relative to the solid content of the short-shaped hydrogel (1b). The supply amount of 90°C water was 14.5% by mass relative to the solid content of the short-shaped hydrogel (1b). The supply amount of 0.6 MPa water vapor was 26.1% by mass relative to the solid content of the short-shaped hydrogel (1b). The gel grinding conditions are shown in Table 1. Tables 2 and 4 show the properties of the particulate hydrogel (1c) taken out from the outlet of the gel grinding device.
[0325] (Drying process)
[0326] The obtained granular hydrogel (1c) was dried using a hot air dryer. The dryer was equipped with a cage (bottom size 30 cm×20 cm) formed of a metal mesh with a mesh size of 1.2 mm. 500 g of the granular hydrogel (1c) was spread roughly evenly on the bottom of the cage, and hot air at 190° C. was sent from below for 30 minutes to obtain a dried product (1A′).
[0327] (Crushing and classification process)
[0328] The cooled dried product (1A') was supplied to a roll mill and pulverized to obtain a water-absorbent resin (1A) having a mass average particle size (d2) of 600 μm.
[0329] (Surface cross-linking process)
[0330] Next, a surface crosslinking agent solution containing 0.025 parts by mass of ethylene glycol diglycidyl ether, 0.3 parts by mass of ethylene carbonate, 0.5 parts by mass of propylene glycol and 2.0 parts by mass of deionized water was sprayed into 100 parts by mass of the water-absorbent resin (1A) and mixed. The mixture was heated at 200°C for 30 minutes to obtain a surface-crosslinked water-absorbent resin (1B). The water-absorbent resin (1B) was supplied to a roll mill and pulverized, and the components that passed through a sieve of 850 μm but did not pass through a sieve of 150 μm were collected to obtain a water-absorbent resin (1C). The physical properties of the water-absorbent resin (1C) are shown in Table 3.
[0331] [Example 2]
[0332] (Step of Preparing Monomer Aqueous Solution)
[0333] In the same manner as in Example 1 (step of preparing an aqueous monomer solution), an aqueous monomer solution was prepared.
[0334] (Polymerization process)
[0335] A short-shaped water-containing gel (2b) was obtained in the same manner as in the (polymerization step) of Example 1. The polymerization rate of the short-shaped water-containing gel (2b) was 98.5% by mass and the solid content was 53% by mass.
[0336] (Gel crushing process)
[0337] The same operation as in Example 1 (gel crushing step) was performed except that the feeding rate of the short-strip hydrogel (2b) was set to 0.45 kg / min (a speed of one short-strip hydrogel (2b) every 5 seconds), the feeding amount of 90°C water was changed to 13.5% by mass relative to the solid content of the short-strip hydrogel (2b), and the feeding amount of 0.6 MPa water vapor was changed to 14.5% by mass relative to the solid content of the short-strip hydrogel (2b). Granular hydrogel (2c) was obtained. The gel crushing conditions are shown in Table 1. The properties of the granular hydrogel (2c) taken out from the discharge port of the gel crushing device are shown in Tables 2 and 4.
[0338] (Drying process)
[0339] The same procedure as in Example 1 (drying step) was carried out to obtain a dried product (2A').
[0340] (Crushing and classification process)
[0341] The same operation as in Example 1 (crushing and classification step) was carried out to obtain a water-absorbent resin (2A) having a mass average particle size (d2) of 615 μm.
[0342] (Surface cross-linking process)
[0343] The water-absorbent resin (2C) was obtained in the same manner as in the (surface crosslinking step) of Example 1. Table 3 shows the physical properties of the surface-crosslinked water-absorbent resin (2C).
[0344] [Example 3]
[0345] (Step of Preparing Monomer Aqueous Solution)
[0346] A monomer aqueous solution was prepared in the same manner as in Example 1 (step of preparing a monomer aqueous solution), except that polyethylene glycol diacrylate (average n number: 9) was changed to 1.07 parts by mass and trisodium diethylenetriaminepentaacetate was changed to pentasodium ethylenediaminetetramethylenephosphonate.
[0347] (Polymerization process)
[0348] A short-shaped water-containing gel (3b) was obtained in the same manner as in the (polymerization step) of Example 1. The polymerization rate of the short-shaped water-containing gel (3b) was 98.5% by mass and the solid content was 53% by mass.
[0349] (Gel crushing process)
[0350] In the gel crushing device, two rotating shafts rotate in the same direction. Figure 4 The structure shown is provided with a feed screw (FS) and a flat disc (F) as a pulverizing unit (in Figure 4 In the structure shown, the return phase is 14 positions), the diameter of each disk is changed to 123 mm, the ratio L / D of the effective length of the main body (effective length in the barrel) L to the maximum diameter D of the disk is changed to 10.2, the temperature of the heat medium of the jacket is changed to 80°C, the rotation speed is changed to 70 rpm, the feeding rate of the short strip of water-containing gel (3b) is changed to 3.0 kg / min (a speed of one short strip of water-containing gel (3b) every 5 seconds), the supply amount of lauryl dimethylaminoacetic acid betaine is changed to 0.04% by mass relative to the solid content of the short strip of water-containing gel (3b), the supply amount of 90°C water is changed to 12.3% by mass relative to the solid content of the short strip of water-containing gel (3b), and the supply amount of 0.6 MPa water vapor is changed to 5.3% by mass relative to the solid content of the short strip of water-containing gel (3b). Except for this, the same operation as in Example 1 (gel crushing step) is performed to obtain a granular water-containing gel (3c). The gel grinding conditions are shown in Table 1. The properties of the granular hydrogel (3c) taken out from the outlet of the gel grinding device are shown in Tables 2 and 4. Figure 4 As shown, the discharge port of the gel grinding device is arranged at the rear of the device.
[0351] (Drying process)
[0352] The same procedure as in Example 1 (drying step) was carried out to obtain a dried product (3A').
[0353] (Crushing and classification process)
[0354] The same operation as in Example 1 (crushing and classification step) was carried out to obtain a water-absorbent resin (3A) having a mass average particle size (d2) of 605 μm.
[0355] (Surface cross-linking process)
[0356] The water-absorbent resin (3C) was obtained in the same manner as in the (surface crosslinking step) of Example 1. Table 3 shows the physical properties of the surface-crosslinked water-absorbent resin (3C).
[0357] [Example 4]
[0358] (Step of Preparing Monomer Aqueous Solution)
[0359] A monomer aqueous solution was prepared in the same manner as in Example 1 (step of preparing a monomer aqueous solution) except that the amount of polyethylene glycol diacrylate (average n number: 9) was changed to 0.85 parts by mass.
[0360] (Polymerization process)
[0361] A short-shaped hydrogel (4b) was obtained in the same manner as in the (polymerization step) of Example 1. The polymerization rate of the short-shaped hydrogel (4b) was 98.5% by mass and the solid content was 53% by mass.
[0362] (Gel crushing process)
[0363] Two axes of rotation rotating in the same direction Figure 5 The structure shown is provided with a feed screw (FS) and a reverse screw (RS), and a flat disk (F), a spiral disk (H) and a reverse spiral disk (RH) as a pulverizing unit (in Figure 5 In the configuration shown, the return phase is one part), except that the same operation as in Example 2 (gel grinding step) was performed to obtain a granular hydrogel (4c). The gel grinding conditions are shown in Table 1. The properties of the granular hydrogel (4c) taken out from the discharge port of the gel grinding device are shown in Tables 2 and 4.
[0364] (Drying process)
[0365] The same procedure as in Example 1 (drying step) was carried out to obtain a dried product (4A').
[0366] (Crushing and classification process)
[0367] The same operation as in Example 1 (crushing and classification step) was carried out to obtain a water-absorbent resin (4A) having a mass average particle size (d2) of 583 μm.
[0368] (Surface cross-linking process)
[0369] The water-absorbent resin (4C) was obtained in the same manner as in the (surface crosslinking step) of Example 1. Table 3 shows the physical properties of the surface-crosslinked water-absorbent resin (4C).
[0370] [Example 5]
[0371] (Step of Preparing Monomer Aqueous Solution)
[0372] A monomer aqueous solution was prepared in the same manner as in Example 1 (step of preparing a monomer aqueous solution) except that the amount of polyethylene glycol diacrylate (average n number: 9) was changed to 1.07 parts by mass.
[0373] (Polymerization process)
[0374] A short-shaped water-containing gel (5b) was obtained in the same manner as in the (polymerization step) of Example 1. The polymerization rate of the short-shaped water-containing gel (5b) was 98.5% by mass and the solid content was 53% by mass.
[0375] (Gel crushing process)
[0376] In the gel crushing device, two rotating shafts rotate in the same direction. Figure 6 The structure shown is provided with a feed screw (FS) and a flat disc (F) as a pulverizing unit (in Figure 6 In the structure shown, the return phase is 5 positions), the diameter of each disk is changed to 53 mm, the ratio L / D of the effective length of the main body (effective length in the barrel) L to the maximum diameter D of the disk is changed to 8.4, the heat medium temperature of the jacket is changed to 80°C, the rotation speed is changed to 165 rpm, the feeding speed of the short strip of hydrous gel (5b) is changed to 1.04 kg / min (a speed of one short strip of hydrous gel (5b) every 5 seconds), the supply amount of lauryl dimethylaminoacetic acid betaine is changed to 0.04 mass% relative to the solid content of the short strip of hydrous gel (5b), the supply amount of 90°C water is changed to 26.1 mass% relative to the solid content of the short strip of hydrous gel (5b), and the supply amount of 0.6 MPa water vapor is changed to 5.0 mass% relative to the solid content of the short strip of hydrous gel (5b). Except for this, the same operation as in Example 1 (gel crushing step) is performed to obtain a granular hydrous gel (5c). The gel grinding conditions are shown in Table 1. The properties of the granular hydrogel (5c) taken out from the outlet of the gel grinding device are shown in Tables 2 and 4. Figure 6 As shown, the discharge port of the gel grinding device is arranged at the rear of the device.
[0377] (Drying process)
[0378] The same procedure as in Example 1 (drying step) was carried out to obtain a dried product (5A').
[0379] (Crushing and classification process)
[0380] The same operation as in Example 1 (crushing and classification step) was carried out to obtain a water-absorbent resin (5A) having a mass average particle size (d2) of 624 μm.
[0381] (Surface cross-linking process)
[0382] The water-absorbent resin (5C) was obtained in the same manner as in the (surface crosslinking step) of Example 1. Table 3 shows the physical properties of the surface-crosslinked water-absorbent resin (5C).
[0383] [Example 6]
[0384] (Step of Preparing Monomer Aqueous Solution)
[0385] In the same manner as in Example 1 (step of preparing an aqueous monomer solution), an aqueous monomer solution was prepared.
[0386] (Polymerization process)
[0387] The same operation as in Example 1 (polymerization process) is performed to obtain a strip-shaped hydrogel (6a). The obtained strip-shaped hydrogel (6a) is cut to obtain a short strip-shaped hydrogel (6b) having a width of several centimeters. Thereafter, the obtained short strip-shaped hydrogel (6b) is put into a screw extruder for further shredding. As the screw extruder, a meat cutter is used in which the outer diameter of the screw shaft is 86 mm and a porous plate having a diameter of 100 mm, a thickness of 10 mm, 6 holes, and an opening rate of 30% is provided at the front end (extrusion port). While the screw shaft speed of the meat slicer was set to 115 rpm, the short-strip hydrogel (6b) was supplied at 4.6 kg / min, and 80°C warm water with a solid content of 4.6% by mass relative to the short-strip hydrogel (6b) and 0.6 MPa steam with a solid content of 4.1% by mass relative to the short-strip hydrogel (6b) were supplied, respectively, to obtain a chopped hydrogel (6b'). The obtained chopped hydrogel (6b') had a polymerization rate of 98.9% by mass and a solid content of 51% by mass.
[0388] (Gel crushing process)
[0389] The same operation as in Example 2 (gel crushing step) was performed on the chopped hydrogel (6b') to obtain a granular hydrogel (6c). It should be noted that 37.5 g of the chopped hydrogel (6b') was added every 5 seconds so that the feeding rate became 0.45 kg / min. The gel crushing conditions are shown in Table 1. The properties of the granular hydrogel (6c) taken out from the discharge port of the gel crushing device are shown in Tables 2 and 4.
[0390] (Drying process)
[0391] The same procedure as in (drying step) of Example 1 was carried out to obtain a dried product (6A').
[0392] (Crushing and classification process)
[0393] The same operation as in Example 1 (crushing and classification step) was carried out to obtain a water-absorbent resin (6A) having a mass average particle size (d2) of 605 μm.
[0394] (Surface cross-linking process)
[0395] The water-absorbent resin (6C) was obtained in the same manner as in the (surface crosslinking step) of Example 1. Table 3 shows the physical properties of the surface-crosslinked water-absorbent resin (6C).
[0396] [Example 7]
[0397] (Step of Preparing Monomer Aqueous Solution)
[0398] In the same manner as in Example 3 (step of preparing an aqueous monomer solution), an aqueous monomer solution was prepared.
[0399] (Polymerization process)
[0400] The same operation as in Example 1 (polymerization process) is performed to obtain a strip-shaped hydrogel (7a). The obtained strip-shaped hydrogel (7a) is cut to obtain a short strip-shaped hydrogel (7b) having a width of several centimeters. Thereafter, the obtained short strip-shaped hydrogel (7b) is put into a screw extruder for further shredding. As the screw extruder, a meat cutter is used in which the outer diameter of the screw shaft is 86 mm and a porous plate having a diameter of 100 mm, a thickness of 10 mm, 15 holes, and an opening rate of 29% is provided at the front end (extrusion port). While the screw shaft speed of the meat slicer was set to 115 rpm, the short-strip hydrogel (7b) was supplied at 4.6 kg / min, and 80°C warm water with a solid content of 4.6% by mass and 0.6 MPa steam with a solid content of 4.1% by mass were supplied to obtain a chopped hydrogel (7b'). The obtained chopped hydrogel (7b') had a polymerization rate of 99.0% by mass and a solid content of 51% by mass.
[0401] (Gel crushing process)
[0402] The same operation as in Example 3 (gel crushing step) was performed on the chopped hydrogel (7b') to obtain a granular hydrogel (7c). It should be noted that 0.25 kg of the chopped hydrogel (7b') was added every 5 seconds at a rate of 3.0 kg / min. The gel crushing conditions are shown in Table 1. The properties of the granular hydrogel (7c) taken out from the discharge port of the gel crushing device are shown in Tables 2 and 4. It should be noted that Figure 4 As shown, the discharge port of the gel grinding device is arranged at the rear of the device.
[0403] (Drying process)
[0404] The same procedure as in Example 1 (drying step) was carried out to obtain a dried product (7A').
[0405] (Pulverization and classification process of dried product)
[0406] The same operation as in Example 1 (crushing and classification step) was carried out to obtain a water-absorbent resin (7A) having a mass average particle size (d2) of 610 μm.
[0407] (Surface cross-linking process)
[0408] The water-absorbent resin (7C) was obtained in the same manner as in the (surface crosslinking step) of Example 1. Table 3 shows the physical properties of the surface-crosslinked water-absorbent resin (7C).
[0409] [Example 8]
[0410] (Step of Preparing Monomer Aqueous Solution)
[0411] A monomer aqueous solution was prepared in the same manner as in Example 1 (step of preparing a monomer aqueous solution) except that the amount of polyethylene glycol diacrylate (average n number: 9) was changed to 0.61 parts by mass.
[0412] (Polymerization process)
[0413] The same operation as in Example 1 (polymerization process) is performed to obtain a strip-shaped hydrogel (8a). The obtained strip-shaped hydrogel (8a) is cut to obtain a short strip-shaped hydrogel (8b) having a width of several centimeters. Thereafter, the obtained short strip-shaped hydrogel (8b) is put into a screw extruder for further shredding. As the screw extruder, a meat cutter is used in which the outer diameter of the screw shaft is 86 mm and a porous plate having a diameter of 100 mm, a thickness of 10 mm, 18 holes, and an opening rate of 29% is provided at the front end (extrusion port). While the screw shaft speed of the meat slicer was set to 115 rpm, the short-strip hydrogel (8b) was supplied at 4.6 kg / min, and 80°C warm water with a solid content of 4.6% by mass relative to the short-strip hydrogel (8b) and 0.6 MPa steam with a solid content of 4.1% by mass relative to the short-strip hydrogel (8b) were supplied, respectively, to obtain a chopped hydrogel (8b'). The obtained chopped hydrogel (8b') had a polymerization rate of 99.0% by mass and a solid content of 51.1% by mass.
[0414] (Gel crushing process)
[0415] Two axes of rotation rotating in the same direction Figure 7 The structure shown is provided with a feed screw (FS) and a reverse screw (RS), and a flat disk (F), a spiral disk (H) and a reverse spiral disk (RH) as a pulverizing unit (in Figure 7In the configuration shown, the return phase is 0 positions), the temperature of the heat medium in the jacket is changed to 80°C, the rotation speed is changed to 40 rpm, the feeding rate of the chopped hydrogel (8b') heated to 70°C is set to 0.64 kg / min (a rate of 53.33 g every 5 seconds), the supply amount of 90°C water is changed to 13.5% by mass relative to the solid content of the chopped hydrogel (8b'), and the feeding amount of 0.6 MPa water vapor is changed to 14.5% by mass relative to the solid content of the chopped hydrogel (8b'). Except for this, the same operation as in Example 1 (gel crushing step) is performed to obtain a granular hydrogel (8c). The gel crushing conditions are shown in Table 1. The properties of the granular hydrogel (8c) taken out from the discharge port of the gel crushing device are shown in Tables 2 and 4.
[0416] (Drying process)
[0417] The same procedure as in Example 1 (drying step) was carried out to obtain a dried product (8A').
[0418] (Crushing and classification process)
[0419] The same operation as in Example 1 (crushing and classification step) was carried out to obtain a water-absorbent resin (8A) having a mass average particle size (d2) of 605 μm.
[0420] (Surface cross-linking process)
[0421] A water-absorbent resin (8C) was obtained in the same manner as in Example 1 (surface crosslinking step). Table 3 shows the physical properties of the surface-crosslinked water-absorbent resin (8C).
[0422] [Comparative Example 1]
[0423] In Comparative Example 1, the surface-crosslinked water-absorbent resin (9C) was obtained in the same manner as in Experimental Example 3 disclosed in PCT / JP2021 / 034800. Specifically, the following is described.
[0424] (Step of Preparing Monomer Aqueous Solution)
[0425] A monomer aqueous solution was prepared in the same manner as in Example 1 (step of preparing a monomer aqueous solution) except that the amount of polyethylene glycol diacrylate (average n number: 9) was changed to 0.61 parts by mass.
[0426] (Polymerization process)
[0427] The same procedure as in Example 1 (polymerization step) was carried out to obtain a short-strip water-containing gel (9b).
[0428] (Gel crushing process)
[0429] Two axes of rotation rotating in the same direction Figure 5 The structure shown is provided with a feed screw (FS) and a reverse screw (RS), and a flat plate (F), a spiral plate (H) and a reverse spiral plate (RH) as a pulverizing unit, the rotation speed is changed to 100 rpm, the feeding speed of the short-strip hydrogel (9b) is changed to 0.64 kg / min (a speed of one short-strip hydrogel (9b) every 2.5 seconds), the supply amount of 90°C water is changed to 11.8% by mass relative to the solid content of the short-strip hydrogel (9b), and the supply amount of 0.6 MPa water vapor is changed to 9.7% by mass relative to the solid content of the short-strip hydrogel (9b). Except for this, the same operation as in Example 1 (gel pulverizing step) is performed to obtain a granular hydrogel (9c). The gel pulverizing conditions are shown in Table 1. The properties of the granular hydrogel (9c) taken out from the discharge port of the gel pulverizing device are shown in Tables 2 and 4.
[0430] (Drying process)
[0431] The same procedure as in Example 1 (drying step) was carried out to obtain a dried product (9A').
[0432] (Crushing and classification process)
[0433] The cooled dried product (9A') was supplied to a roll mill, pulverized, and classified using JIS standard sieves with mesh sizes of 850 μm and 150 μm. The components that passed through the 850 μm sieve but not through the 150 μm sieve were collected to obtain a water-absorbent resin (9A").
[0434] (Surface cross-linking process)
[0435] Next, a surface crosslinking agent solution containing 0.025 parts by mass of ethylene glycol diglycidyl ether, 0.3 parts by mass of ethylene carbonate, 0.5 parts by mass of propylene glycol and 2.0 parts by mass of deionized water was sprayed onto 100 parts by mass of the water-absorbent resin (9A") and mixed. The mixture was heated at 200°C for 30 minutes to obtain a surface-crosslinked water-absorbent resin (9C). The physical properties of the surface-crosslinked water-absorbent resin (9C) are shown in Table 3.
[0436] [Comparative Example 2]
[0437] In Comparative Example 2, the surface-crosslinked water-absorbent resin (10C) was obtained in the same manner as in Experimental Example 4 disclosed in PCT / JP2021 / 034800. Specifically, the following is described.
[0438] (Step of Preparing Monomer Aqueous Solution)
[0439] A monomer aqueous solution was prepared in the same manner as in Example 1 (step of preparing a monomer aqueous solution) except that the amount of polyethylene glycol diacrylate (average n number: 9) was changed to 0.61 parts by mass.
[0440] (Polymerization process)
[0441] The same operation as in Example 1 (polymerization step) was carried out to obtain a short-strip water-containing gel (10b).
[0442] (Gel crushing process)
[0443] Two axes of rotation rotating in the same direction Figure 7 The structure shown is provided with a feed screw (FS) and a reverse screw (RS), and a flat disk (F), a spiral disk (H) and a reverse spiral disk (RH) as a pulverizing unit (in Figure 7 In the configuration shown, the return phase is 0 position), the temperature of the heat medium in the jacket is changed to 80°C, the rotation speed is changed to 40 rpm, the feeding rate of the short strip of hydrous gel (10b) heated to 70°C is changed to 0.64 kg / min (a rate of one short strip of hydrous gel (10b) every 2.5 seconds), and water and steam are not supplied. Except for this, the same operation as in Example 1 (gel crushing step) is performed to obtain a granular hydrous gel (10c). The gel crushing conditions are shown in Table 1. The properties of the granular hydrous gel (10c) taken out from the discharge port of the gel crushing device are shown in Table 2.
[0444] (Drying process)
[0445] The same procedure as in (drying step) of Example 1 was carried out to obtain a dried product (10A').
[0446] (Crushing and classification process)
[0447] The same procedure as in Comparative Example 1 (crushing and classification steps) was carried out to obtain a water-absorbent resin (10A”).
[0448] (Surface cross-linking process)
[0449] The surface-crosslinked water-absorbent resin (10C) was obtained in the same manner as in the (surface crosslinking step) of Comparative Example 1. Table 3 shows the physical properties of the surface-crosslinked water-absorbent resin (10C).
[0450] [Comparative Example 3]
[0451] (Step of Preparing Monomer Aqueous Solution)
[0452] In the same manner as in Example 3 (step of preparing an aqueous monomer solution), an aqueous monomer solution was prepared.
[0453] (Polymerization process)
[0454] The same operation as in Example 1 (polymerization step) was carried out to obtain a short-strip water-containing gel (11b).
[0455] (Gel crushing process)
[0456] Two axes of rotation rotating in the same direction Figure 6 The structure shown is provided with a feed screw (FS) and a reverse screw (RS), and a flat plate (F), a spiral plate (H) and a reverse spiral plate (RH) as a pulverizing unit. Except that the feeding speed of the short-strip hydrogel (11b) is changed to 1.0 kg / min (a speed of one short-strip hydrogel (11b) every 5 seconds), the same operation as in Example 3 (gel pulverizing step) is performed to obtain a granular hydrogel (11c). The gel pulverizing conditions are shown in Table 1. The properties of the granular hydrogel (11c) taken out from the discharge port of the gel pulverizing device are shown in Tables 2 and 4.
[0457] (Drying process)
[0458] The same procedure as in (drying step) of Example 1 was carried out to obtain a dried product (11A').
[0459] (Crushing and classification process)
[0460] The same operation as in Example 1 (crushing and classification step) was carried out to obtain a water-absorbent resin (11A) having a mass average particle size (d2) of 608 μm.
[0461] (Surface cross-linking process)
[0462] A water-absorbent resin (11C) was obtained in the same manner as in Example 1 (surface crosslinking step). Table 3 shows the physical properties of the surface-crosslinked water-absorbent resin (11C).
[0463] [Table 1]
[0464]
[0465] [Table 2]
[0466] (Table 2) Properties of granular hydrogel
[0467]
[0468] [Table 3]
[0469]
[0470] [Table 4]
[0471] (Table 4)
[0472]
[0473] As shown above, the water-absorbent resins of the Examples have a high water absorption rate and a low residual monomer content. In contrast, the water-absorbent resin of Comparative Example 1 having a gel crushing coefficient exceeding 3.0 J / g·sec has a larger residual monomer content than that of the Examples, and the water-absorbent resin of Comparative Example 2 having a mass average particle size of more than 500 μm in terms of solid content of the particulate hydrogel crosslinked polymer and the water-absorbent resin of Comparative Example 3 having a gel crushing coefficient of less than 0.020 J / g·sec have a lower water absorption rate than that of the Examples and a larger residual monomer content than that of the Examples.
[0474] This application is based on Japanese Patent Application No. 2022-056292 filed on March 30, 2022 and Japanese Patent Application No. 2022-124526 filed on August 4, 2022, the disclosures of which are incorporated herein by reference in their entirety.
[0475] Industrial Applicability
[0476] The water-absorbent resin powder obtained by the present invention is suitable for use as an absorbent body in sanitary products such as disposable diapers.
[0477] Description of Reference Numerals
[0478] 10…Flat plate
[0479] 11…hole
[0480] 12…Flat part
[0481] 200…Gel crushing device
[0482] 204…Inlet
[0483] 206…Rotation axis
[0484] 208…Main body (barrel)
[0485] 210…Discharge outlet
[0486] 212…Crushing unit
[0487] 214…Driver
[0488] 216…Gas supply port
[0489] 218…Screw
Claims
1. A method for producing a water-absorbent resin powder, comprising the following steps: A polymerization step of polymerizing the monomer aqueous solution to obtain a hydrogel-like cross-linked polymer; and After the polymerization step, a gel pulverizing step is performed in which the hydrous gel-like crosslinked polymer is pulverized using a gel pulverizing device to obtain a granular hydrous gel-like crosslinked polymer. The gel grinding device comprises an inlet, an outlet, and a main body having a plurality of rotating shafts built therein, wherein each of the rotating shafts has a grinding unit. In the gel pulverization step, the hydrous gel-like crosslinked polymer is continuously fed from the feed port, and the hydrous gel-like crosslinked polymer is continuously taken out from the discharge port in a granular form. The polymerization rate of the hydrogel cross-linked polymer introduced into the introduction port is 90% by mass or more, The gel crushing coefficient is 0.020 J / g·sec or more and 3.0 J / g·sec or less, The particulate hydrogel crosslinked polymer discharged from the discharge port has a mass average particle size of 500 μm or less in terms of solid content.
2. The manufacturing method according to claim 1, wherein: The average residence time of the hydrogel-like cross-linked polymer in the gel grinding device is 30 seconds to 1200 seconds.
3. The manufacturing method according to claim 1 or 2, wherein: The hydrogel-like cross-linked polymer obtained after the polymerization step is in a sheet form, and the production method further includes a pulverizing step of pulverizing the sheet-like hydrogel-like cross-linked polymer before the gel pulverizing step.
4. The production method according to any one of claims 1 to 3, wherein The particulate aqueous gel-like cross-linked polymer contains a gel fluidizing agent.
5. The manufacturing method according to claim 4, wherein: The gel fluidizing agent is added to the hydrogel-like cross-linked polymer before and / or during the gel pulverization step.
6. The production method according to any one of claims 1 to 5, wherein The rotating shaft has a disk, and a ratio L / D of an effective length L inside the body to a maximum diameter D of the disk (when a plurality of disks of different diameters are used, the diameter of the largest disk) is 5 or more and 20 or less.
7. The manufacturing method according to claim 6, wherein: With respect to the disk major axis diameter X, the disk minor axis diameter Y satisfies 0.2≤Y / X≤0.6, and the disk thickness T satisfies 0.05≤T / X≤1.
0.
8. The production method according to any one of claims 1 to 7, wherein The porosity V of the gel grinding device calculated by the following formula is 40% or more and 80% or less, V={(AB) / A}×100 Here, A is the internal volume (m 3 ), B is the total volume of the plurality of rotating shafts and the pulverizing unit existing in the main body portion after removing the portion corresponding to the inlet and the outlet from the main body in the length direction (m 3 ).
9. The production method according to any one of claims 1 to 8, wherein The arrangement of the grinding units of the gel grinding device includes one or more portions showing a return phase in which the phase difference between adjacent disks in the advancing direction from the inlet toward the outlet is greater than 90° and less than 180°.
10. The production method according to any one of claims 1 to 9, wherein: The solid content of the hydrogel-like cross-linked polymer introduced into the introduction port is 25 to 75% by mass.
11. The production method according to any one of claims 1 to 10, wherein The solid content of the particulate hydrogel crosslinked polymer discharged from the discharge port is 25 to 75% by mass.
12. The production method according to any one of claims 1 to 11, wherein The hydrogel-like cross-linked polymer is a cross-linked body containing poly(meth)acrylic acid (salt) as a main component.
13. The production method according to any one of claims 1 to 12, wherein: After the gel pulverization step, a surface cross-linking step is further included.
Citation Information
Cited By
Superabsorbent polymers and method of fabricating the same
TWI919698B