Crosslinked resin particles and method for producing same
By using peroxide crosslinked polyhydroxyalkanoate resin in the aqueous dispersion, small-particle-sized crosslinked resin particles with biodegradability were produced, and the failure of biodegradable small particles in the prior art was solved. The problem of crosslinking resin particles in diameter has achieved improved hardness and heat resistance of the resin and good biodegradation performance.
Patent Information
- Application Number
- CN202380029876.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-29
- Filing Date
- 2023-03-24
- Publication Date
- 2024-11-08
AI Technical Summary
At present, no small particle size crosslinked resin particles composed of biodegradable plastics can be produced.
Polyhydroxyalkanoate resin is used as the main component, and crosslinking is performed by using peroxide in the aqueous dispersion to produce crosslinking with a gel fraction of more than 50%, a volume average particle size of more than 0.1 μm and less than 10 μm. Resin particles.
It has successfully provided novel cross-linked resin particles with biodegradability, which has improved the hardness, heat resistance and solvent resistance of the resin, and has shown good biodegradation performance.
Smart Images

Figure BDA0005056792200000171 
Figure BDA0005056792200000172 
Figure BDA0005056792200000173
Abstract
Description
Technical Field
[0001] The present invention relates to crosslinked resin particles and a method for producing the same. Background Art
[0002] It is known that by introducing a cross-linked structure into a resin, the hardness, heat resistance, solvent resistance, etc. of the resin can be improved. Resin particles having a small particle size and composed of a resin having such a cross-linked structure have been used in various applications such as a modifier, spacer, anti-blocking agent, and matting agent for thermoplastic resins.
[0003] As resin materials constituting such crosslinked resin particles, acrylic resins, acrylic silicone resins, polystyrene, and the like are known (for example, refer to Patent Documents 1 and 2).
[0004] On the other hand, plastic waste has become a burden on the global environment, affecting the ecosystem, generating harmful gases when burned, and causing global warming due to the large amount of heat from combustion. Biodegradable plastics are being actively developed as materials that can solve these problems.
[0005] Patent Document 3 describes that poly(3-hydroxyalkanoate), which is one type of biodegradable plastic, is melt-kneaded in the presence of an organic peroxide to crosslink the resin. However, the description is that the crosslinked resin produced by such melt-kneading is used to form a film or sheet, and there is no description of producing small-diameter crosslinked resin particles.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2009-56770
[0009] Patent Document 2: Japanese Patent Application Publication No. 2003-82191
[0010] Patent Document 3: International Publication No. 2019 / 022008 Summary of the invention
[0011] Problems to be solved by the invention
[0012] Until now, there has been no known cross-linked resin particles having a small particle size which are composed of a biodegradable plastic and exhibit biodegradability.
[0013] In view of the above-mentioned current situation, an object of the present invention is to provide novel crosslinked resin particles having biodegradability.
[0014] Solution to the problem
[0015] The present inventors have conducted intensive studies and have succeeded in producing novel crosslinked resin particles using a polyhydroxyalkanoate resin which is a biodegradable resin, thereby completing the present invention.
[0016] That is, the present invention relates to crosslinked resin particles comprising a polyhydroxyalkanoate resin, having a gel fraction of 50% or more and a volume average particle size of 0.1 μm or more and 10 μm or less.
[0017] Furthermore, the present invention also relates to an aqueous dispersion in which the crosslinked resin particles are dispersed in an aqueous medium.
[0018] The present invention also relates to a method for producing the crosslinked resin particles, comprising: crosslinking the polyhydroxyalkanoate resin in the presence of a peroxide in an aqueous dispersion of the polyhydroxyalkanoate resin particles.
[0019] Effects of the Invention
[0020] According to the present invention, novel cross-linked resin particles having biodegradability can be provided. DETAILED DESCRIPTION
[0021] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to the following embodiments.
[0022] <Cross-linked resin particles>
[0023] The crosslinked resin particles of the present embodiment are particles composed of a polyhydroxyalkanoate resin as a main resin component. Hereinafter, the polyhydroxyalkanoate resin may be abbreviated as "PHA".
[0024] <PHA>
[0025] "PHA" is a general term for polymers containing hydroxyalkanoic acid as a monomer unit, and is generally biodegradable. PHA is an aliphatic polyester, preferably a polyester without an aromatic ring.
[0026] PHA is not particularly limited, and examples thereof include polyglycolic acid, poly(3-hydroxyalkanoate) resins, poly(4-hydroxyalkanoate) resins, and the like. As PHA, only one type may be used, or two or more types may be used in combination. Among them, poly(3-hydroxyalkanoate) resins are preferred. Hereinafter, poly(3-hydroxyalkanoate) resins may be referred to as "P3HA".
[0027] The above-mentioned P3HA is a 3-hydroxyalkanoic acid repeating unit represented by the chemical formula: [-CHR-CH2-CO-O-] (wherein R is C n H 2n+1The P3HA preferably contains 50 mol % or more of the 3-hydroxyalkanoic acid repeating unit in all monomer repeating units (100 mol %), and more preferably contains 70 mol % or more.
[0028] P3HA is not particularly limited, and examples thereof include poly(3-hydroxybutyrate) (abbreviated as P3HB), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (abbreviated as P3HB3HH), etc. As P3HA, only one type may be used, or two or more types may be used in combination.
[0029] P3HA can be produced by microorganisms. Such microbial production of P3HA is usually composed of only D-form (R-form) hydroxyalkanoic acid repeating units. Among the microbial production of P3HA, P3HB and P3HB3HH are preferred from the viewpoint of easy industrial production, and P3HB3HH is more preferred.
[0030] In the case where P3HA contains 3-hydroxybutyric acid (3HB) repeating units, from the viewpoint of the balance between flexibility and strength, the composition ratio of 3HB repeating units in all monomer repeating units (100 mol%) is preferably 60 to 99 mol%, more preferably 65 to 97 mol%, and further preferably 67 to 95 mol%. By making the composition ratio of 3HB repeating units 60 mol% or more, the rigidity of the cross-linked resin particles can be further improved. On the other hand, by making the composition ratio of 3HB repeating units 99 mol% or less, there is a tendency for the softness of the cross-linked resin particles to be further improved. It should be noted that the monomer composition ratio of P3HA can be measured by gas chromatography, etc. (for example, refer to International Publication No. 2014 / 020838). As P3HA, two or more compositions having different composition ratios of 3HB repeating units can be used in combination.
[0031] As a microorganism producing P3HA, it is not particularly limited as long as it is a microorganism with the ability to produce P3HA. For example, as a P3HB producing bacterium, the earliest one was Bacillus megaterium discovered in 1925. Other examples include natural microorganisms such as Cupriavidus necator (old classification: Alcaligenes eutrophus, Ralstonia eutropha), and Alcaligenes latus. Among these microorganisms, it is known that P3HB accumulates in the bacteria.
[0032] In addition, as a producer of copolymers of 3HB and other hydroxyalkanoates, Aeromonas caviae, which is a P3HB3HH producer, is known. In particular, in order to improve the productivity of P3HB3HH, preferably Alcaligenes eutrophus AC32 strain (Alcaligenes eutrophus AC32, FERM BP-6038) (T. Fukui, Y. Doi, J. Bateriol., 179, p4821-4830 (1997)) into which the genes of the P3HA synthase group are introduced is used. Microbial cells in which these microorganisms are cultured under appropriate conditions to accumulate P3HA in the cell body can be used. In addition, in addition to the above, genetically recombinant microorganisms into which various P3HA synthesis-related genes are introduced according to the P3HA to be produced can be used, and the culture conditions including the substrate type can also be optimized.
[0033] The molecular weight of PHA is not particularly limited, and the weight average molecular weight is preferably 50,000 to 3,000,000, preferably 100,000 to 2,000,000, and more preferably 150,000 to 1,500,000. By making the weight average molecular weight above 50,000, the tendency of the strength of the cross-linked resin particles to decrease can be avoided, or the tendency of stickiness due to low molecular weight components can be avoided. On the other hand, PHA having a weight average molecular weight exceeding 3,000,000 is sometimes difficult to prepare itself or difficult to handle for the purpose of the present invention. The numerical value of the weight average molecular weight is a value measured before the cross-linking treatment of PHA is performed.
[0034] The weight average molecular weight can be determined by gel permeation chromatography (GPC) (Shimadzu Corporation "High Performance Liquid Chromatography 20A System"), using a polystyrene gel (Showa Denko K.K. "KG 4A", "K-806M", etc.) as a column, using chloroform as a mobile phase, and obtaining the molecular weight in terms of polystyrene. At this time, a calibration curve can be prepared using polystyrene with weight average molecular weights of 31400, 197000, 668000, and 1920000. As a column in the GPC, a column suitable for measuring the above molecular weight can be used.
[0035] <Gel fraction>
[0036] The cross-linked resin particles of the present embodiment have a cross-linked structure formed by bonding molecular chains of PHA. Since the cross-linked structure has a certain amount or more, the cross-linked resin particles of the present embodiment have a high gel fraction, specifically, a gel fraction of 50% or more. By showing a high gel fraction in this way, the hardness, heat resistance, solvent resistance, etc. of the resin particles containing PHA are improved.
[0037] The gel fraction is preferably 60% or more, more preferably 70% or more, further preferably 75% or more, and particularly preferably 80% or more. Alternatively, it may be 85% or more, or 90% or more. The upper limit of the gel fraction is not particularly limited as long as it is 100% or less. From the viewpoint of the production efficiency of the cross-linked resin particles, it is preferably 99.5% or less, more preferably 99% or less. Alternatively, it may be 98% or less, or 97% or less, or 96% or less.
[0038] The gel fraction is a value measured as follows. The dried cross-linked resin particles are added to chloroform at a concentration of 0.7% by weight and dissolved at 60°C for 30 minutes to obtain a chloroform solution. Then, after standing at room temperature for 3 hours, the chloroform solution is filtered using a membrane filter with a pore size of 0.45 μm. The gel on the filter is dried, and the weight is measured together with the filter, and the gel fraction is calculated by the following formula.
[0039] Formula: Gel fraction = (weight of the filter including the dried gel - weight of the filter alone) / weight of the cross-linked resin particles used in the measurement × 100 (%)
[0040] <Average particle size>
[0041] The volume average particle size of the cross-linked resin particles of the present embodiment is within the range of 0.1 μm or more and 10 μm or less. By having such a particle size, it can be used for various purposes described later. From the perspective of practical use opportunities, the lower limit of the above particle size is preferably 0.1 μm or more, more preferably 0.3 μm or more, and further preferably 0.5 μm or more. In addition, from the perspective of productivity (production of PHA, cross-linking treatment, etc.), the upper limit of the above particle size is preferably 8 μm or less, more preferably 5 μm or less.
[0042] The volume average particle size is a value measured in a state where the crosslinked resin particles are dispersed in an aqueous solvent. As a measuring device, a general-purpose measuring device can be used, and an example of such a device is Microtrac MT3300EXII manufactured by Nikkiso Co., Ltd.
[0043] <Peroxide>
[0044] The crosslinking form in the crosslinked resin particles of this embodiment is not particularly limited, and crosslinking using peroxide is preferred. When peroxide is used, free radicals generated by decomposition of the peroxide act on PHA molecules, and molecular chains of PHA are directly bonded to each other, thereby forming the above-mentioned crosslinked structure.
[0045] The peroxide may be an organic peroxide or an inorganic peroxide. In order to more efficiently increase the gel fraction, an organic peroxide is preferred.
[0046] The organic peroxide is preferably at least one selected from diacyl peroxides, alkyl peroxides, dialkyl peroxides, hydroperoxides, peroxyketals, peroxycarbonates and peroxydicarbonates in consideration of heating temperature and time during crosslinking treatment.
[0047] Specific examples of such organic peroxides include butyl peroxyneododecanoate, octanoyl peroxide, dilauroyl peroxide, succinyl peroxide, a mixture of methylbenzoyl peroxide and benzoyl peroxide, benzoyl peroxide, bis(butylperoxy)trimethylcyclohexane, butyl peroxylaurate, dimethyldi(benzoylperoxy)hexane, bis(butylperoxy)methylcyclohexane, bis(butylperoxy)cyclohexane, butyl peroxybenzoate, butyl peroxyvalerate, diisopropylbenzene peroxide, di-tert-hexyl peroxide, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxyisobutyrate, tert-butyl peroxypivalate, tert-hexyl peroxypivalate, tert-butyl peroxymethylmonocarbonate. , tert-amyl peroxymethyl monocarbonate, tert-hexyl peroxymethyl monocarbonate, tert-heptyl peroxymethyl monocarbonate, tert-octyl peroxymethyl monocarbonate, 1,1,3,3-tetramethylbutyl peroxymethyl monocarbonate, tert-butyl peroxyethyl monocarbonate, tert-amyl peroxyethyl monocarbonate, tert-hexyl peroxyethyl monocarbonate, tert-heptyl peroxyethyl monocarbonate, tert-octyl peroxyethyl monocarbonate, 1,1,3,3-tetramethylbutyl peroxyethyl monocarbonate, tert-butyl peroxy-n-propyl monocarbonate, tert-amyl peroxy-n-propyl monocarbonate, tert-hexyl peroxy-n-propyl monocarbonate, tert-heptyl peroxy-n-propyl monocarbonate, tert-octyl peroxy-n-propyl monocarbonate, 1,1 ,3,3-Tetramethylbutyl peroxyn-propyl monocarbonate, tert-butyl peroxyisopropyl monocarbonate, tert-amyl peroxyisopropyl monocarbonate, tert-hexyl peroxyisopropyl monocarbonate, tert-heptyl peroxyisopropyl monocarbonate, tert-octyl peroxyisopropyl monocarbonate, 1,1,3,3-Tetramethylbutyl peroxyisopropyl monocarbonate, tert-butyl peroxyn-butyl monocarbonate, tert-amyl peroxyn-butyl monocarbonate, tert-hexyl peroxyn-butyl monocarbonate, tert-heptyl peroxyn-butyl monocarbonate, tert-octyl peroxyn-butyl monocarbonate, 1,1,3,3-Tetramethylbutyl peroxyn-butyl monocarbonate, tert-butyl peroxyisobutyl monocarbonate, tert-amyl peroxyisobutyl monocarbonate , tert-hexyl peroxyisobutyl monocarbonate, tert-heptyl peroxyisobutyl monocarbonate, tert-octyl peroxyisobutyl monocarbonate, 1,1,3,3-tetramethylbutyl peroxyisobutyl monocarbonate, tert-butyl peroxysec-butyl monocarbonate, tert-amyl peroxysec-butyl monocarbonate, tert-hexyl peroxysec-butyl monocarbonate, tert-heptyl peroxysec-butyl monocarbonate, tert-octyl peroxysec-butyl monocarbonate, 1,1,3,3-tetramethylbutyl peroxysec-butyl monocarbonate, tert-butyl peroxytert-butyl monocarbonate, tert-amyl peroxytert-butyl monocarbonate, tert-hexyl peroxytert-butyl monocarbonate, tert-heptyl peroxytert-butyl monocarbonate, tert-octyl peroxytert-butyl monocarbonate, 1,1,3,3-tetramethylbutyl peroxysec-butyl monocarbonate,3-Tetramethylbutyl peroxy tert-butyl monocarbonate, tert-butyl peroxy 2-ethylhexyl monocarbonate, tert-amyl peroxy 2-ethylhexyl monocarbonate, tert-hexyl peroxy 2-ethylhexyl monocarbonate, tert-heptyl peroxy 2-ethylhexyl monocarbonate, tert-octyl peroxy 2-ethylhexyl monocarbonate, 1,1,3,3-tetramethylbutyl peroxy 2-ethylhexyl monocarbonate, diisobutyl peroxide, isopropyl peroxyneodecanoate, di-n-propyl peroxydicarbonate, diisopropyl peroxydicarbonate, di-sec-butyl peroxydicarbonate, 1,1,3,3-tetramethylbutyl peroxyneodecanoate, bis(4-tert-butylcyclohexyl) peroxydicarbonate, bis(2-ethylhexyl) peroxydicarbonate, tert-hexyl peroxyneodecanoate, tert-butyl peroxyneodecanoate, tert-butyl peroxyneoheptanoate, tert-hexyl peroxypivalate, peroxy tert-Butyl pivalate, di(3,5,5-trimethylhexanoyl) peroxide, dilauroyl peroxide, 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate, disuccinic acid peroxide, 2,5-dimethyl-2,5-bis(2-ethylhexanoyl peroxide)hexane, tert-hexyl peroxy-2-ethylhexanoate, di(4-methylbenzoyl) peroxide, dibenzoyl peroxide, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxyisopropyl carbonate, 1,6-bis(tert-butylperoxycarbonyloxy)hexane, tert-butyl peroxy-3,5,5-trimethylhexanoate, tert-butyl peroxyacetate, tert-butyl peroxybenzoate, tert-amyl peroxy-3,5,5-trimethylhexanoate, 2,2-bis(4,4-di-tert-butylperoxycyclohexyl)propane, 2,2-di-tert-butylperoxybutane, etc. The organic peroxide may be used alone or in combination of two or more.
[0048] Among them, tert-butyl peroxyisopropyl monocarbonate, tert-amyl peroxyisopropyl monocarbonate, tert-hexyl peroxyisopropyl monocarbonate, tert-butyl peroxy-2-ethylhexyl monocarbonate, tert-amyl peroxy-2-ethylhexyl monocarbonate, tert-hexyl peroxy-2-ethylhexyl monocarbonate, tert-amyl peroxyisopropyl monocarbonate, di-tert-hexyl peroxide, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxyisobutyrate, tert-hexyl peroxy-2-ethylhexanoate, 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate, tert-butyl peroxypivalate, tert-hexyl peroxypivalate, tert-butyl peroxyneodecanoate, tert-hexyl peroxyneodecanoate, and 1,1,3,3-tetramethylbutyl peroxyneodecanoate are preferred organic peroxides because they can efficiently crosslink PHA.
[0049] The peroxide can set the heating temperature during the crosslinking treatment to a low level, and therefore, the peroxide preferably has a one-hour half-life temperature of 200°C or lower, more preferably 170°C or lower, and further preferably 140°C or lower. The lower limit may be 50°C or higher, 60°C or higher, or 70°C or higher.
[0050] Particularly preferred organic peroxides showing such a one-hour half-life temperature are tert-butyl peroxyisopropyl monocarbonate, tert-butyl peroxy 2-ethylhexyl monocarbonate, di-sec-butyl peroxydicarbonate, tert-butyl peroxy 2-ethylhexanoate, tert-butyl peroxyisobutyrate, tert-hexyl peroxy 2-ethylhexanoate, 1,1,3,3-tetramethylbutyl peroxy 2-ethylhexanoate, tert-butyl peroxypivalate, tert-hexyl peroxypivalate, tert-butyl peroxyneodecanoate, tert-hexyl peroxyneodecanoate, and 1,1,3,3-tetramethylbutyl peroxyneodecanoate.
[0051] When the above-mentioned peroxide is an inorganic peroxide, as the inorganic peroxide, considering the heating temperature and time during the crosslinking treatment, for example, hydrogen peroxide, potassium peroxide, calcium peroxide, sodium peroxide, magnesium peroxide, potassium persulfate, sodium persulfate, ammonium persulfate, etc. can be listed. Among them, from the viewpoint of the decomposition temperature of the heating temperature during the ease of operation and the heating temperature suitable for the crosslinking treatment, hydrogen peroxide, potassium persulfate, sodium persulfate and ammonium persulfate are preferably used. One inorganic peroxide can be used alone, or two or more can be used in combination. In addition, organic peroxide and inorganic peroxide can also be used in combination.
[0052] <Multifunctional compounds>
[0053] The crosslinked structure in the crosslinked resin particles of the present embodiment may be introduced using only a peroxide or using both a peroxide and a polyfunctional compound. The latter can increase the gel fraction of the crosslinked resin particles with a small amount of peroxide.
[0054] The polyfunctional compound is a compound having two or more functional groups capable of crosslinking PHA in one molecule. Although not particularly limited, it is preferably a compound reactive with free radicals generated by peroxides, and particularly preferably a compound having two or more radical reactive groups in one molecule. The radical reactive group is preferably at least one selected from vinyl, allyl, acryloyl, or methacryloyl.
[0055] Such a multifunctional compound is not particularly limited, and examples thereof include: allyl (meth)acrylate; allyl alkyl (meth)acrylates; allyloxyalkyl (meth)acrylates; multifunctional (meth)acrylates having two or more (meth)acrylate groups, such as ethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, and pentaerythritol (meth)acrylate; divinylbenzene, diallyl phthalate, triallyl cyanurate, triallyl isocyanurate, and divinylbenzene. Preferred are allyl methacrylate, triallyl isocyanurate, butanediol di(meth)acrylate, and divinylbenzene, and particularly preferred are allyl methacrylate and triallyl isocyanurate.
[0056] When a cross-linked structure is formed in the presence of a polyfunctional compound, the obtained cross-linked resin particles may generally contain a structure derived from the polyfunctional compound. In this case, molecular chains of PHA are bonded to each other via the structure derived from the polyfunctional compound.
[0057] The cross-linked resin particles of the present embodiment may be composed only of PHA having a cross-linked structure, or may further contain components other than PHA having a cross-linked structure. As components other than PHA having a cross-linked structure, for example, resins other than PHA, antioxidants, hydrolysis inhibitors, anti-blocking agents, crystal nucleating agents, ultraviolet absorbers, etc. may be listed.
[0058] The ratio of PHA in the cross-linked resin particles of the present embodiment is not particularly limited and may be 50% by weight or more, preferably 70% by weight or more, more preferably 80% by weight or more, further preferably 90% by weight or more, and particularly preferably 95% by weight or more. It may be 99% by weight or more. The upper limit is not particularly limited and may be 100% by weight or less.
[0059] As resins other than PHA, for example, aliphatic polyesters formed by polycondensation of aliphatic diols and aliphatic dicarboxylic acids, aliphatic aromatic polyesters using both aliphatic compounds and aromatic compounds as monomers, etc. Examples of the former include polyethylene succinate, polybutylene succinate (PBS), polyhexamethylene succinate, polyethylene adipate, polybutylene adipate, polyhexamethylene adipate, polybutylene succinate adipate (PBSA), polyethylene sebacate, polybutylene sebacate, etc. Examples of the latter include poly(butylene adipate-co-butylene terephthalate) (PBAT), poly(butylene sebacate-co-butylene terephthalate), poly(butylene azelaate-co-butylene terephthalate), poly(butylene succinate-co-butylene terephthalate) (PBST), etc. The other resins may be used alone or in combination of two or more.
[0060] It is preferred that the cross-linked resin particles of the present embodiment are unfoamed, that is, substantially do not contain bubbles inside the particles, unlike the foamed resin particles disclosed in International Publication Nos. 2007 / 049694 and 2019 / 146555.
[0061] In the case of not foaming, the apparent density of the crosslinked resin particles of the present embodiment shows a large value, preferably greater than 0.6 g / cm 3 , more preferably 0.7 g / cm 3 More preferably, 0.9 g / cm 3 The apparent density of the crosslinked resin particles can be determined by the method described in JIS K0061 (method for measuring density and specific gravity of chemical products) or JIS Z8807 (method for measuring density and specific gravity of solids).
[0062] The average weight per particle of the crosslinked resin particles of the present embodiment is not particularly limited, but is a value far below 0.1 mg because the volume average particle size of the crosslinked resin particles is as small as 10 μm or less.
[0063] The crosslinked resin particles of the present embodiment may be dried. The shape after drying may be powdery, granular, crumbly, flake, or the like, depending on the drying method.
[0064] <Aqueous dispersion>
[0065] One aspect of the present embodiment may be an aqueous dispersion in which the crosslinked resin particles are dispersed in an aqueous medium.
[0066] The aqueous medium contained in the aqueous dispersion may be water alone or a mixed solvent of water and an organic solvent compatible with water. The concentration of the organic solvent compatible with water in the mixed solvent is not particularly limited as long as it is less than the solubility of the organic solvent used in water.
[0067] As the above-mentioned organic solvent, there is no particular limitation, and examples thereof include: alcohols such as methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, isobutanol, pentanol, hexanol, heptanol, etc.; ketones such as acetone, methyl ethyl ketone, etc.; ethers such as tetrahydrofuran, dioxane, etc.; nitriles such as acetonitrile, propionitrile, etc.; amides such as dimethylformamide, acetamide, etc.; dimethyl sulfoxide, pyridine, piperidine, etc. Among them, from the viewpoint of easy removal, methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, isobutanol, acetone, methyl ethyl ketone, tetrahydrofuran, dioxane, acetonitrile, propionitrile, etc. are preferred. In addition, from the viewpoint of easy availability, methanol, ethanol, 1-propanol, 2-propanol, butanol, acetone, etc. are more preferred. In addition, methanol, ethanol, and acetone are particularly preferred.
[0068] The water content in the total aqueous medium constituting the aqueous dispersion is preferably 5 to 100% by weight, preferably 10% by weight or more, more preferably 30% by weight or more, further preferably 50% by weight or more, particularly preferably 70% by weight or more, and may be 90% by weight or more, or 95% by weight or more.
[0069] The concentration of the crosslinked resin particles in the aqueous dispersion is not particularly limited, and may be, for example, about 1 to 60% by weight. In addition, the aqueous dispersion may contain a dispersant as described below.
[0070] <Method for producing cross-linked resin particles>
[0071] An example of a method for producing the crosslinked resin particles of the present embodiment is specifically described. The crosslinked resin particles of the present embodiment can be produced by crosslinking PHA in an aqueous dispersion containing PHA particles before crosslinking treatment in the presence of a peroxide. In order to efficiently crosslink PHA, the aqueous dispersion of PHA particles containing a peroxide is preferably heated to a temperature suitable for the decomposition of the peroxide.
[0072] More specifically, the method for producing crosslinked resin particles preferably comprises: a step (1) of preparing an aqueous dispersion of PHA particles in which PHA particles before crosslinking treatment are dispersed in water; a step (2) of adding a peroxide to the aqueous dispersion of PHA particles so that the peroxide is impregnated into the PHA particles; and a step (3) of heating the aqueous dispersion of PHA particles impregnated with the peroxide to a heating temperature to crosslink the PHA. More preferably, the method further comprises a step (4) of maintaining the heating temperature after all the peroxide has been added.
[0073] In step (1), the aqueous dispersion of PHA particles may be an aqueous dispersion obtained by culturing PHA-producing microorganisms to accumulate PHA in the microorganisms, destroying the microorganisms in the culture solution, and separating and removing the microorganism components; or an aqueous dispersion obtained by concentrating or diluting the aqueous dispersion. According to such a method, the PHA particles can be prepared from the time of crosslinking treatment when culturing the PHA-producing microorganisms without separating the PHA particles from water.
[0074] Alternatively, the aqueous dispersion of PHA particles may be prepared by dispersing dried PHA particles in water. The aqueous dispersion may contain the above-mentioned organic solvent compatible with water in addition to water.
[0075] In the above-mentioned aqueous dispersion, the volume average particle size of the PHA particles is preferably within the same range as the volume average particle size of the above-mentioned cross-linked resin particles. In the case of PHA particles produced by PHA-producing microorganisms, the volume average particle size thereof can generally be within the above-mentioned range, and therefore, even without performing a special process for adjusting the particle size, an aqueous dispersion of PHA particles having a desired volume average particle size can be obtained.
[0076] The concentration of the PHA particles in the aqueous dispersion is not particularly limited and can be appropriately set, and may be, for example, about 1 to 70% by weight, preferably about 5 to 50% by weight.
[0077] In order to improve the dispersibility of PHA particles and make the cross-linking reaction proceed uniformly, it is preferred that the aqueous dispersion of PHA particles contains a dispersant. As a dispersant, for example, anionic surfactants such as sodium sulfosuccinate dioctyl ester, sodium lauryl sulfate, sodium lauryl sulfate, sodium oleate, etc.; cationic surfactants such as dodecyl trimethylammonium chloride; nonionic surfactants such as glycerol fatty acid esters, sorbitan fatty acid esters, sucrose fatty acid esters, polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers, polyoxyethylene polyoxypropylene glycols; polyvinyl alcohol, ethylene-modified polyvinyl alcohol, polyvinyl pyrrolidone, methyl cellulose, ethyl cellulose, hydroxymethyl cellulose, hydroxyethyl cellulose, polyacrylic acid, sodium polyacrylate, potassium polyacrylate, polymethacrylic acid, sodium polymethacrylate, etc. Water-soluble polymers, etc., can be used. These dispersants can be used alone or in combination of two or more.
[0078] When a dispersant is used, the amount thereof added is not particularly limited, and may be, for example, 0.1 to 10 parts by weight, preferably 0.5 to 5 parts by weight, and particularly preferably 0.5 to 3 parts by weight, relative to 100 parts by weight of the PHA particles.
[0079] In step (2), peroxide is added to the aqueous dispersion of PHA particles obtained in step (1) to impregnate the PHA particles with the peroxide. As the peroxide, the above-mentioned peroxides can be used. The peroxide can be added in various forms such as solid and liquid. In addition, liquid peroxide diluted with a diluent or the like can also be added. The peroxide can be added all at once, or can be added continuously or in divided portions.
[0080] When a peroxide and the above-mentioned multifunctional compound are used in combination, in the step (2), the multifunctional compound is preferably also added to the aqueous dispersion of the PHA particles. As the multifunctional compound, the above-mentioned multifunctional compound can be used. The multifunctional compound can be added in various forms such as solid and liquid. In addition, a liquid multifunctional compound diluted with a diluent or the like can also be added. The multifunctional compound can be added all at once, or can be added continuously or in divided portions.
[0081] In order to impregnate the PHA particles with the peroxide and any polyfunctional compound, after adding these compounds to the aqueous dispersion of the PHA particles, or while adding them, the temperature of the aqueous dispersion is set to, for example, 0° C. or higher and lower than a temperature suitable for decomposition of the peroxide used in the next step (3), and the aqueous dispersion is stirred and maintained at this temperature for, for example, about 1 minute to 5 hours. Specifically, the temperature of the aqueous dispersion during impregnation can be about 10 to 60° C.
[0082] The amount of peroxide used can be appropriately set in consideration of the gel fraction of the crosslinked resin particles, and is, for example, preferably 0.01 to 10 parts by weight, more preferably 0.1 to 8 parts by weight, further preferably 0.3 to 5 parts by weight, and particularly preferably 0.5 to 3 parts by weight, relative to 100 parts by weight of the PHA particles.
[0083] According to the manufacturing method of crosslinking PHA particles in an aqueous dispersion using a peroxide, crosslinking is performed while maintaining the particle size (volume) before crosslinking, and crosslinked resin particles are easily obtained. On the other hand, the method of crosslinking the resin by melt kneading in the presence of a peroxide is sometimes difficult to achieve this effect.
[0084] In addition, according to the production method of crosslinking PHA particles in an aqueous dispersion using a peroxide, it is easy to control the temperature rise caused by the heat generated in the crosslinking reaction, which is advantageous in obtaining crosslinked resin particles having a stable crosslinked structure (quality) safely and efficiently.
[0085] In addition, the amount of the multifunctional compound can also be appropriately set in consideration of the gel fraction of the cross-linked resin particles. For example, it is preferably 0.01 to 20 parts by weight, more preferably 0.05 to 15 parts by weight, further preferably 0.1 to 10 parts by weight, further preferably 0.2 to 5 parts by weight, and particularly preferably 0.3 to 3 parts by weight relative to 100 parts by weight of the PHA particles.
[0086] In step (3), the aqueous dispersion of PHA particles impregnated with peroxide is heated to a temperature suitable for the decomposition of the peroxide. The heating temperature is preferably within a range of about 25°C based on the 1-hour half-life temperature of the peroxide described above. Specifically, the heating temperature is preferably 30 to 140°C, more preferably 50 to 135°C, and even more preferably 60 to 130°C. According to the present method, PHA can be crosslinked at a temperature lower than the melting temperature of PHA, so that the deterioration of PHA caused by heating during the crosslinking treatment can be avoided.
[0087] Next, in step (4), the heating temperature is preferably maintained. This allows the crosslinking reaction using the peroxide to proceed sufficiently. The time for maintaining the heating temperature is not particularly limited, but is preferably 1 minute to 15 hours, more preferably 1 hour to 10 hours.
[0088] After the crosslinking reaction is completed, the crosslinked resin particles are separated from the aqueous dispersion and water is removed, thereby obtaining dried crosslinked resin particles. The method for separating the crosslinked resin particles is not particularly limited, and for example, filtration, centrifugal separation, heat drying, freeze drying, spray drying, etc. can be used. For example, when spray drying is used, the dried crosslinked resin particles can be directly obtained from the aqueous dispersion. In addition, by extruding the crosslinked resin particles separately after separation from the aqueous dispersion, the crosslinked resin particles can also be obtained in a granular shape while completely removing the residual water. In addition, a coagulation process using a coagulant or pH adjustment can also be implemented.
[0089] However, the aqueous dispersion itself after the crosslinking reaction is completed, or an aqueous dispersion obtained by concentrating the aqueous dispersion after the crosslinking reaction to increase the concentration of the crosslinked resin particles, or an aqueous dispersion obtained by adding an aqueous medium to the aqueous dispersion after the crosslinking reaction is completed and diluting it also constitutes one embodiment of the present invention.
[0090] <Applications of cross-linked resin particles>
[0091] The use of the cross-linked resin particles of this embodiment is not particularly limited, and can be used in the use of conventionally known cross-linked resin particles. Specifically, the cross-linked resin particles can be used as resin modifiers, rheology modifiers for coatings or adhesives, coating pigments, paper coating agents, matting agents, anti-blocking agents, cosmetic additives, toner additives, liquid crystal spacers, coating agents, adhesive tape fillers, fiber processing agents, medical diagnostic inspection particles, fillers, etc., but are not limited thereto.
[0092] Since the crosslinked resin particles of the present embodiment are composed of biodegradable PHA, the crosslinked resin particles can be expected to be useful as crosslinked resin particles that can address the problem of plastic waste and are friendly to the global environment.
[0093] In the following items, preferred aspects of the present disclosure are listed, but the present invention is not limited to the following items.
[0094] [Project 1]
[0095] A cross-linked resin particle comprising a polyhydroxyalkanoate resin,
[0096] The cross-linked resin particles have a gel fraction of 50% or more and a volume average particle size of 0.1 μm or more and 10 μm or less.
[0097] [Project 2]
[0098] The crosslinked resin particles according to item 1, wherein the polyhydroxyalkanoate resin is a poly(3-hydroxyalkanoate) resin.
[0099] [Item 3]
[0100] The crosslinked resin particles according to item 1 or 2, wherein the crosslinked resin particles are crosslinked using a peroxide.
[0101] [Item 4]
[0102] The crosslinked resin particles according to any one of items 1 to 3, wherein the crosslinked resin particles are further crosslinked in the presence of a polyfunctional compound.
[0103] [Item 5]
[0104] The crosslinked resin particles according to any one of items 1 to 4, wherein the crosslinked resin particles are not foamed.
[0105] [Item 6]
[0106] The crosslinked resin particles according to any one of items 1 to 5, wherein a ratio of the polyhydroxyalkanoate-based resin in the crosslinked resin particles is 80% by weight or more.
[0107] [Item 7]
[0108] The crosslinked resin particles according to any one of items 1 to 6, wherein the gel fraction is 70 to 100%.
[0109] [Item 8]
[0110] An aqueous dispersion comprising the crosslinked resin particles according to any one of items 1 to 7 dispersed in an aqueous medium.
[0111] [Item 9]
[0112] A production method, which is a method for producing the crosslinked resin particles according to any one of items 1 to 7, comprising:
[0113] A step of crosslinking the polyhydroxyalkanoate type resin in the presence of a peroxide in an aqueous dispersion of polyhydroxyalkanoate type resin particles.
[0114] Example
[0115] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to these Examples at all.
[0116] [1] Measurement conditions
[0117] 1-1. Weight average molecular weight
[0118] The resin to be measured was dissolved in chloroform, heated in a hot water bath at 60°C for 30 minutes, the soluble component was filtered using a PTFE disposable filter with a pore size of 0.45 μm, and the filtrate was used to perform GPC measurement under the following conditions to determine the weight average molecular weight.
[0119] GPC measurement equipment: High performance liquid chromatography 20A system manufactured by Shimadzu Corporation
[0120] Column: KG 4A (1 piece), K-806M (2 pieces) manufactured by Showa Denko K.K.
[0121] Sample concentration: 1mg / ml
[0122] Eluent: Chloroform solution
[0123] Eluent flow rate: 1.0ml / min
[0124] Sample injection volume: 100μL
[0125] Analysis time: 30 minutes
[0126] Standard sample: Standard polystyrene
[0127] 1-2. Volume average particle size
[0128] The volume average particle size of the crosslinked resin particles or base resin particles was measured in the state of resin particle latex. Microtrac MT3300EXII manufactured by Nikkiso Co., Ltd. was used as a measuring device.
[0129] 1-3. Gel fraction
[0130] The dried product of cross-linked resin particles or base resin particles was added to a concentration of 0.7% by weight relative to chloroform, and dissolved at 60°C for 30 minutes to obtain a chloroform solution. Then, after standing at room temperature for 3 hours, the chloroform solution was filtered using a membrane filter with a pore size of 0.45 μm. Chloroform was added several times inside the container and on the filter to fully wash and filter, thereby preventing loss. The gel remaining on the filter was dried, and the weight was measured together with the filter, and the gel fraction was calculated by the following formula.
[0131] Formula: Gel fraction = (weight of the filter including the dried gel - weight of the filter alone) / weight of the cross-linked resin particles or base resin particles used in the measurement × 100 (%)
[0132] 1-4. (Biochemical oxygen demand (BOD) test)
[0133] 25 mg of the frozen and pulverized sample was added to 250 ml of seawater to which 0.05 g / L of ammonium chloride and 0.1 g / L of potassium dihydrogen phosphate were added, and the BOD value was measured after maintaining the conditions at 30°C and constant stirring for 91 days.
[0134] The BOD value was measured by measuring the pressure loss caused by the absorption of CO2 generated by the respiration of microorganisms by KOH tablets using Oxitop (manufactured by Xylem) which can measure the pressure drop of the gas phase in a closed container under constant temperature conditions using a pressure sensor.
[0135] The biodegradation degree (%) in seawater was calculated by dividing the obtained BOD value by the theoretical oxygen demand (the amount of oxygen required for complete decomposition into water and carbon dioxide).
[0136] [2] Raw materials for cross-linked resin particles
[0137] 2-1. Base resin particles
[0138] PHA-1: poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), (3-hydroxybutyrate) / (3-hydroxyhexanoate) = 72 / 28 (mol / mol), weight average molecular weight Mw: 700,000 to 1.5 million
[0139] PHA-2: poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), (3-hydroxybutyrate) / (3-hydroxyhexanoate) = 89 / 11 (mol / mol), weight average molecular weight Mw: 500,000
[0140] PHA-3: Poly(3-hydroxybutyrate-co-3-hydroxyhexanoate): (3-hydroxybutyrate) / (3-hydroxyhexanoate) = 68 / 32 (mol / mol), weight average molecular weight Mw: 700,000 to 1.5 million
[0141] PHA-4: poly(3-hydroxybutyrate-co-3-hydroxyhexanoate): (3-hydroxybutyrate) / (3-hydroxyhexanoate) = 75 / 25 (mol / mol), weight average molecular weight Mw: 600,000 to 1.5 million
[0142] 2-2. Peroxide
[0143] PO-1: tert-butyl peroxypivalate ("LUPEROX 11" manufactured by ARKEMA Yoshitomi Co., Ltd., 1-hour half-life temperature: 76°C)
[0144] PO-2: tert-butyl peroxy 2-ethylhexanoate ("LUPEROX 26" manufactured by ARKEMA Yoshitomi Co., Ltd., 1-hour half-life temperature: 95°C)
[0145] PO-3: tert-Butyl peroxy-2-ethylhexyl monocarbonate ("Perbutyl E" manufactured by NOF Corporation, 1-hour half-life temperature: 119°C)
[0146] PO-4: di-sec-butyl peroxydicarbonate ("LUPEROX 225" manufactured by ARKEMA Yoshitomi Co., Ltd., 1-hour half-life temperature: 69°C)
[0147] 2-3. Multifunctional compounds
[0148] CA-1: Allyl methacrylate
[0149] CA-2: Triallyl isocyanurate
[0150] [3] Method for producing cross-linked resin particles
[0151] The crosslinked resin particles of Examples 1 to 29 were produced by the following procedures using the raw materials of the types described in the tables in the amounts described in the tables.
[0152] Into an autoclave equipped with a stirrer, baffles, nitrogen inlet / outlet, and a thermometer, an aqueous dispersion of base resin particles dispersed in water (100 parts by weight in terms of solid content), 200 parts by weight of deionized water, a given amount of peroxide, 2 parts by weight of sodium dioctyl sulfosuccinate, and a given amount of a polyfunctional compound were added, and stirring was started at room temperature while nitrogen substitution was performed in the autoclave.
[0153] Then, the contents in the autoclave are stirred at the temperature and time of the impregnation conditions described in the table to impregnate the base resin particles with the peroxide and the polyfunctional compound, and then the temperature is raised to the reaction temperature of the crosslinking conditions described in the table. After reaching the reaction temperature, the reaction is carried out at the reaction temperature for the reaction time of the crosslinking conditions described in the table, thereby obtaining an aqueous dispersion in which the crosslinked resin particles are dispersed in water.
[0154] After adjusting the pH of the aqueous dispersion, the dispersion was dried in an oven to obtain solidified crosslinked resin particles.
[0155] The volume average particle size and gel fraction of the crosslinked resin particles obtained in each example were measured by the above-mentioned method, and the results are shown in the table.
[0156] In Comparative Example 1, the volume average particle size and gel fraction of the base resin particles before the crosslinking reaction were measured by the above-mentioned methods.
[0157] In addition, the biodegradability in seawater of the crosslinked resin particles obtained in Examples 20 and 22 and commonly available cellulose (microcrystalline cellulose, manufactured by Merck) (reference example) was measured by the above-mentioned method.
[0158] surface
[0159] [Table 2]
[0160]
[0161] [Table 3]
[0162]
[0163] As can be seen from Tables 1 to 3, crosslinked resin particles containing polyhydroxyalkanoate resin, having a gel fraction of 50% or more and a volume average particle size of 0.1 to 10 μm were obtained in Examples 1 to 29. On the other hand, in Comparative Example 1 in which no crosslinking reaction was performed, the gel fraction of the resin particles was extremely low, namely 0%.
[0164] In addition, as shown in Table 3, the crosslinked resin particles obtained in Examples 20 and 22 have a higher biodegradability in seawater in about 3 months than cellulose (reference example) as a biodegradable material, and thus exhibit good biodegradability.
Claims
1. A cross-linked resin particle comprising a polyhydroxyalkanoate resin, The cross-linked resin particles have a gel fraction of 50% or more and a volume average particle size of 0.1 μm or more and 10 μm or less.
2. The crosslinked resin particles according to claim 1, in, The polyhydroxyalkanoate resin is a poly(3-hydroxyalkanoate) resin.
3. The crosslinked resin particles according to claim 1 or 2, in, The cross-linked resin particles are cross-linked using peroxide.
4. The crosslinked resin particles according to claim 3, in, The crosslinked resin particles are further crosslinked in the presence of a polyfunctional compound.
5. The crosslinked resin particles according to claim 1 or 2, in, The cross-linked resin particles are not foamed.
6. The crosslinked resin particles according to claim 1 or 2, in, The ratio of the polyhydroxyalkanoate resin in the cross-linked resin particles is 80% by weight or more.
7. The crosslinked resin particles according to claim 1 or 2, in, The gel fraction is 70-100%. 8 . An aqueous dispersion comprising the crosslinked resin particles according to claim 1 or 2 dispersed in an aqueous medium.
9. A method for producing the crosslinked resin particles according to claim 1 or 2, wherein the method include: A step of crosslinking the polyhydroxyalkanoate type resin in the presence of a peroxide in an aqueous dispersion of polyhydroxyalkanoate type resin particles.