Aromatic polycarbonate resin composition and molded article thereof

By reasonably proportioning epoxy-containing compounds and glycerol monofatty acid esters in aromatic polycarbonate resins and adding aromatic phosphite-based heat stabilizers, the aromatic polycarbonate resins in the prior art are solved. The problem of insufficient properties and molding heat resistance achieves higher humidity and heat resistance and molding heat resistance, and is suitable for high-demand industrial applications.

CN118922495APending Publication Date: 2024-11-08TEIJIN LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380026962.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-15
Filing Date
2023-02-27
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing aromatic polycarbonate resins have shortcomings in terms of moisture and heat resistance and molding heat resistance, especially under the requirements of high functionalization and high performance, pentaerythritol, aliphatic carboxylic acid esters and glycerol monofats in the prior art. The amount of acid ester added is insufficient, resulting in insufficient moisture and heat resistance and molding heat resistance.

Method used

By reasonably proportioning the epoxy-containing compound and glycerol monofat acid esters in the aromatic polycarbonate resin, the specific ratio is 0.02 to 0.04 parts by weight of the aromatic polycarbonate resin and 100 parts by weight of the aromatic polycarbonate resin and 0.06 to 0.15 parts by weight of glycerol monofatty acid ester, and an aromatic phosphite-based heat stabilizer is added to optimize the moisture and heat resistance of the resin composition and the molding heat resistance.

Benefits of technology

The heat resistance and heat resistance of aromatic polycarbonate resins have been significantly improved, and are suitable for high-demand industrial applications, especially molded products that are steam sterilized in medical and food applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005038176090000041
    Figure BDA0005038176090000041
  • Figure BDA0005038176090000151
    Figure BDA0005038176090000151
  • Figure BDA0005038176090000161
    Figure BDA0005038176090000161
Patent Text Reader

Abstract

Provided is an aromatic polycarbonate resin composition which is characterized by containing 0.02-0.04 parts by weight of (B) an epoxy group-containing compound (component B) and 0.06-0.15 parts by weight of (C) a glycerin monofatty acid ester (component C) per 100 parts by weight of (A) an aromatic polycarbonate resin (component A), and which has excellent wet heat resistance and molding heat resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an aromatic polycarbonate resin composition having excellent moisture heat resistance and molding heat resistance and a molded product thereof. Background Art

[0002] Aromatic polycarbonate resin is a material with relatively excellent heat resistance among polymer materials. However, in order to improve the functionality and performance of the material, it is necessary to further improve the moisture and heat resistance and molding heat resistance.

[0003] Patent Document 1 is known as a technique for using fatty acid esters and epoxy compounds in combination. However, the esters of pentaerythritol and aliphatic carboxylic acids shown in the Examples do not have sufficient moist heat resistance, and the molding heat resistance is not sufficient at the addition amount of glycerol monofatty acid ester shown in the Comparative Examples.

[0004] In Patent Document 2, the amount of epoxy-containing compound added shown in the examples is 0.0075 parts by mass or less relative to 100 parts by mass of the polycarbonate resin, and the moist heat resistance is not sufficient in the added region.

[0005] In Patent Documents 3 and 4, the amount of glycerol monofatty acid ester added is 0.05 parts by mass or less, and the mold release property is insufficient, resulting in problems in moldability.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent No. 5542810

[0009] Patent Document 2: Japanese Patent Application Publication No. 2020-132840

[0010] Patent Document 3: Japanese Patent Application Publication No. 2021-134286

[0011] Patent Document 4: Japanese Patent Application Publication No. 2021-120458 Summary of the invention

[0012] An object of the present invention is to provide an aromatic polycarbonate resin composition having excellent moisture heat resistance and molding heat resistance, and a molded product thereof.

[0013] The present inventors have conducted intensive studies to solve the above problems and have found that an aromatic polycarbonate resin composition obtained by blending an epoxy-containing compound and a glycerol monofatty acid ester in a specific ratio with an aromatic polycarbonate resin and a molded article thereof achieves the above object, thereby completing the present invention.

[0014] That is, according to the present invention, the following (Configuration 1) to (Configuration 4) are provided.

[0015] (Composition 1)

[0016] A polycarbonate resin composition comprises 0.02 to 0.04 parts by weight of (B) an epoxy group-containing compound (component B) and 0.06 to 0.15 parts by weight of (C) a glycerol monofatty acid ester (component C) based on 100 parts by weight of (A) an aromatic polycarbonate resin (component A).

[0017] (Composition 2)

[0018] The resin composition according to Configuration 1, wherein the (D) aromatic phosphite-based heat stabilizer (component D) is contained in an amount of 0.01 to 0.02 parts by weight based on 100 parts by weight of the component A.

[0019] (Composition 3)

[0020] The resin composition according to configuration 1 or 2, wherein the component B is a copolymer of styrene and glycidyl methacrylate.

[0021] (Composition 4)

[0022] A molded article formed from the aromatic polycarbonate resin composition according to any one of configurations 1 to 3.

[0023] The aromatic polycarbonate resin composition of the present invention is excellent in moisture heat resistance and molding heat resistance, and therefore can be used in various applications where aromatic polycarbonate resin compositions are used, and has a very high industrial value. DETAILED DESCRIPTION

[0024] Hereinafter, the present invention will be described in detail.

[0025] <Aromatic polycarbonate resin (component A)>

[0026] The aromatic polycarbonate resin used as the component (A) in the present invention is obtained, for example, by reacting a dihydric phenol with a carbonate precursor by an interfacial polymerization method (solution method) or a melt method.

[0027] Representative examples of the dihydric phenols used herein include hydroquinone, resorcinol, 4,4'-dihydroxybiphenyl, 1,4-dihydroxynaphthalene, bis(4-hydroxyphenyl)methane, bis{(4-hydroxy-3,5-dimethyl)phenyl}methane, 1,1-bis(4-hydroxyphenyl)ethane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 2,2-bis(4-hydroxyphenyl)propane (commonly known as bisphenol A), 2,2-bis{(4-hydroxy-3-methyl)phenyl}propane , 2,2-bis{(4-hydroxy-3,5-dimethyl)phenyl}propane, 2,2-bis{(3,5-dibromo-4-hydroxy)phenyl}propane, 2,2-bis{(3-isopropyl-4-hydroxy)phenyl}propane, 2,2-bis{(4-hydroxy-3-phenyl)phenyl}propane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)-3-methylbutane, 2,2-bis(4-hydroxyphenyl)-3,3-dimethylbutane, 2,4-bis (4-Hydroxyphenyl)-2-methylbutane, 2,2-bis(4-hydroxyphenyl)pentane, 2,2-bis(4-hydroxyphenyl)-4-methylpentane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-4-isopropylcyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 9,9-bis(4-hydroxyphenyl)fluorene, 9,9-bis{(4-hydroxy-3-methyl)phenyl}fluorene, α,α'-bis(4 α,α'-bis(4-hydroxyphenyl)-o-diisopropylbenzene, α,α'-bis(4-hydroxyphenyl)-m-diisopropylbenzene, α,α'-bis(4-hydroxyphenyl)-p-diisopropylbenzene, 1,3-bis(4-hydroxyphenyl)-5,7-dimethyladamantane, 4,4'-dihydroxydiphenyl sulfone, 4,4'-dihydroxydiphenyl sulfoxide, 4,4'-dihydroxydiphenyl sulfide, 4,4'-dihydroxydiphenyl ketone, 4,4'-dihydroxydiphenyl ether and 4,4'-dihydroxydiphenyl ester. Preferred dihydric phenols are bis(4-hydroxyphenyl)alkanes, and bisphenol A is particularly preferred.

[0028] As the carbonate precursor, a carbonyl halide, a carbonate ester, a halogenated format, or the like can be used. Specific examples thereof include phosgene, diphenyl carbonate, and a dihalogenated format of a dihydric phenol.

[0029] When making above-mentioned dihydric phenol and carbonate precursor reaction and manufacturing aromatic polycarbonate resin by interfacial polymerization or melting method, dihydric phenol can be used alone or use more than 2 kinds, also can use the antioxidant of catalyzer, end-capping agent, dihydric phenol etc. as required.In addition, aromatic polycarbonate resin can also be the branched polycarbonate resin that the multifunctional aromatic compound copolymerization of trifunctional or more is formed.In addition, can also be the mixture of aromatic polycarbonate resin more than 2 kinds.

[0030] The reaction based on the interfacial polymerization method is usually a reaction between a dihydric phenol and phosgene, and the reaction is carried out in the presence of an acid binder and an organic solvent. As the acid binder, for example, an alkali metal hydroxide such as sodium hydroxide or potassium hydroxide or an amine compound such as pyridine can be used. As the organic solvent, for example, a halogenated hydrocarbon such as dichloromethane or chlorobenzene can be used. In addition, in order to promote the reaction, a catalyst such as a tertiary amine or a quaternary ammonium salt can also be used. At this time, the reaction temperature is usually 0 to 40°C, and the reaction time is about several minutes to about 5 hours.

[0031] The reaction based on the melting method is usually an ester exchange reaction between dihydric phenol and diphenyl carbonate. Dihydric phenol and diphenyl carbonate are mixed in the presence of an inert gas and reacted at 120 to 350°C under reduced pressure. The degree of reduced pressure changes in stages and eventually reaches 1.3×10 2 The phenols generated when the reaction temperature is less than Pa are removed from the system. The reaction time is usually about 1 to 4 hours.

[0032] In addition, in the polymerization reaction, monofunctional phenols can be used as end-capping agents. In particular, when phosgene is used as a reaction of a carbonate precursor, monofunctional phenols are generally used as end-capping agents for regulating molecular weight, and since the ends of the obtained aromatic polycarbonate resin are end-capped by groups based on monofunctional phenols, thermal stability is excellent compared to situations where this is not the case. As the above-mentioned monofunctional phenols, as long as they can be used as end-capping agents for polycarbonates, they are generally phenol or low alkyl substituted phenols, and can be shown as monofunctional phenols represented by the following formula (1).

[0033]

[0034] [In the formula, R represents a hydrogen atom or an alkyl group or a phenylalkyl group having 1 to 9 carbon atoms, and m is an integer of 1 to 5, preferably 1 to 3.]

[0035] Specific examples of the monofunctional phenols include phenol, p-tert-butylphenol, p-cumylphenol, and isooctylphenol.

[0036] The molecular weight of the aromatic polycarbonate resin in the present invention is preferably 10000 to 50000, more preferably 14000 to 35000, in terms of viscosity average molecular weight (M). Aromatic polycarbonate resins having such a viscosity average molecular weight are preferred because they maintain relatively good fluidity during extrusion and molding and provide a certain mechanical strength to the resulting molded product.

[0037] The viscosity average molecular weight of the aromatic polycarbonate resin in the present invention is first determined by using an Ostwald viscometer from a solution obtained by dissolving 0.7 g of a polycarbonate resin material in 100 ml of dichloromethane at 20° C. to obtain a specific viscosity (η) which can be calculated from the following formula: SP ),

[0038] Specific viscosity (η SP )=(t-t0) / t0

[0039] [t0 is the falling seconds of dichloromethane, t is the falling seconds of the sample solution]

[0040] According to the calculated specific viscosity (η SP ) The viscosity average molecular weight Mv is calculated by the following mathematical formula.

[0041] η SP / c=[η]+0.45×[η] 2 c (where [η] is limiting viscosity)

[0042] [η] = 1.23 × 10 -4 Mv 0.83

[0043] c=0.7

[0044] <Epoxy-containing compound (component B)>

[0045] The epoxy group-containing compound used in the present invention is a compound blended mainly to improve moisture and heat resistance, and basically any compound having an epoxy functional group can be used.

[0046] Specific examples of preferred epoxy group-containing compounds include 3',4'-epoxycyclohexylcarboxylic acid-3,4-epoxycyclohexylmethyl ester, 1,2-epoxy-4-(2-oxacyclopropyl)cyclohexane adduct of 2,2-bis(hydroxymethyl)-1-butanol, copolymers of methyl methacrylate and glycidyl methacrylate, copolymers of styrene and glycidyl methacrylate, etc. Preferably, it is a copolymer containing a glycidyl group, and more preferably, it is a copolymer of styrene and glycidyl methacrylate. As a commercially available product of a copolymer of styrene and glycidyl methacrylate, Marproof G-0250SP manufactured by NOF Corporation can be cited.

[0047] The epoxy group-containing compound used in the present invention is blended in an amount of 0.02 to 0.04 parts by weight, preferably 0.02 to 0.03 parts by weight, based on 100 parts by weight of the aromatic polycarbonate resin. Within the above range, moisture heat resistance and molding heat resistance are good.

[0048] <Glycerol monofatty acid ester (ingredient C)>

[0049] The glycerol monofatty acid ester used in the present invention is a condensate of an aliphatic monocarboxylic acid and glycerol. Examples of the aliphatic monocarboxylic acid include saturated or unsaturated aliphatic monocarboxylic acids, and the aliphatic monocarboxylic acid may be any of a chain aliphatic monocarboxylic acid and a cyclic aliphatic monocarboxylic acid, preferably a chain aliphatic monocarboxylic acid. The carbon number of the aliphatic monocarboxylic acid is preferably 6 to 40, more preferably 8 to 32, and even more preferably 12 to 24.

[0050] Examples of saturated aliphatic monocarboxylic acids include capric acid, neodecanoic acid, lauric acid, myristic acid, palmitic acid, stearic acid, arachidic acid, behenic acid, and lignoceric acid. Examples of unsaturated aliphatic carboxylic acids include undecylenic acid, oleic acid, elaidic acid, erucic acid, nervonic acid, linoleic acid, γ-linolenic acid, arachidonic acid, α-linolenic acid, octadecatetraenoic acid, eicosapentaenoic acid, and docosahexaenoic acid.

[0051] Among the above, as the aliphatic monocarboxylic acid, lauric acid, myristic acid, palmitic acid, stearic acid and behenic acid are preferred, palmitic acid, stearic acid and behenic acid are more preferred, and stearic acid is further preferred.

[0052] As the glycerol monofatty acid ester used in the present invention, glyceryl monostearate is preferred. Examples of commercially available products of glyceryl monostearate include Rikemal S-100A manufactured by Riken Vitamin Co., Ltd.

[0053] The amount of the glycerol monofatty acid ester used in the present invention is 0.06 to 0.15 parts by weight, preferably 0.07 to 0.13 parts by weight, and more preferably 0.09 to 0.11 parts by weight relative to 100 parts by weight of the aromatic polycarbonate resin. Within the above range, mold release, moisture and heat resistance, and molding heat resistance are good.

[0054] <Aromatic phosphite-based heat stabilizer (component D)>

[0055] As aromatic phosphite heat stabilizers preferably used in the present invention, for example, triphenyl phosphite, tricresyl phosphite, tris(ethylphenyl) phosphite, tris(2,4-di-tert-butylphenyl) phosphite, tris(nonylphenyl) phosphite, tris(hydroxyphenyl) phosphite and other triaryl phosphites; aryl phosphites such as phenyl didecyl phosphite, diphenyldecyl phosphite, diphenyl isooctyl phosphite, phenyl isooctyl phosphite, 2-ethylhexyl diphenyl phosphite and other aralkyl phosphites can be mentioned. Among the aromatic phosphite heat stabilizers, tris(2,4-di-tert-butylphenyl) phosphite is preferred. As a commercially available product of tris(2,4-di-tert-butylphenyl) phosphite, Irgafos168 manufactured by BASF can be mentioned.

[0056] The amount of the aromatic phosphite heat stabilizer preferably used in the present invention is preferably 0.01 to 0.02 parts by weight, more preferably 0.012 to 0.018 parts by weight, and further preferably 0.014 to 0.016 parts by weight relative to 100 parts by weight of the aromatic polycarbonate resin. Within the above range, moisture heat resistance and molding heat resistance are excellent.

[0057] (Other additives)

[0058] In order to improve the flame retardancy, oxidation resistance, and light stability (ultraviolet stability) of the resin composition of the present invention, additives for these improvements are advantageously used. These additives are specifically described below.

[0059] (I) Flame retardant

[0060] Various compounds known as flame retardants for polycarbonate resins can be formulated in the resin composition of the present invention. The formulation of the above-mentioned compounds will improve flame retardancy, but in addition, it will also improve antistatic properties, fluidity, rigidity and thermal stability according to the properties of each compound. As the above-mentioned flame retardant, (i) organic metal salt flame retardants (such as organic sulfonic acid alkali (earth) metal salts, organic boric acid metal salt flame retardants and organic stannic acid metal salt flame retardants, etc.); (ii) organic phosphorus flame retardants (for example, monophosphate compounds containing organic groups, phosphate oligomers, phosphonate oligomers, phosphazene oligomers and phosphoramide compounds, etc.); (iii) organic silicon flame retardants composed of organic silicon compounds; (iv) fibrillated PTFE, among which organic metal salt flame retardants and organic phosphorus flame retardants are preferred.

[0061] (i) Organic metal salt flame retardants

[0062] The organic metal salt compound is preferably an alkali (earth) metal salt of an organic acid having 1 to 50 carbon atoms, preferably 1 to 40 carbon atoms, preferably an alkali (earth) metal salt of an organic sulfonic acid. The organic sulfonic acid alkali (earth) metal salt includes: a metal salt of a perfluoroalkylsulfonic acid having 1 to 10 carbon atoms, preferably 2 to 8 carbon atoms, and an alkali metal or alkaline earth metal, such as a metal salt of a fluorine-substituted alkylsulfonic acid; and a metal salt of an aromatic sulfonic acid having 7 to 50 carbon atoms, preferably 7 to 40 carbon atoms, and an alkali metal or alkaline earth metal. As alkali metals constituting the metal salt, lithium, sodium, potassium, rubidium and cesium can be cited, and as alkaline earth metals, beryllium, magnesium, calcium, strontium and barium can be cited. Alkali metals are more preferred. Among the above alkali metals, rubidium and cesium with larger ionic radii are preferred when higher transparency is required, but on the other hand, since they are not widely used and difficult to purify, the result is a cost disadvantage. On the other hand, metals with smaller ionic radii such as lithium and sodium are disadvantageous in flame retardancy. In consideration of these, the alkali metal in the sulfonic acid alkali metal salt can be used separately, and the potassium sulfonic acid salt is most preferred because it has an excellent balance of properties in all aspects. The above potassium salt and the sulfonic acid alkali metal salt composed of other alkali metals can also be used in combination.

[0063] As a specific example of perfluoroalkylsulfonic acid alkali metal salt, potassium trifluoromethanesulfonate, potassium perfluorobutanesulfonate, potassium perfluorohexanesulfonate, potassium perfluorooctanesulfonate, sodium pentafluoroethanesulfonate, sodium perfluorobutanesulfonate, sodium perfluorooctanesulfonate, lithium trifluoromethanesulfonate, lithium perfluorobutanesulfonate, lithium perfluoroheptanesulfonate, cesium trifluoromethanesulfonate, cesium perfluorobutanesulfonate, cesium perfluorooctanesulfonate, cesium perfluorohexanesulfonate, rubidium perfluorobutanesulfonate, and rubidium perfluorohexanesulfonate, etc., can be cited, these can be used one or two or more. Here, the carbon number of the perfluoroalkyl group is preferably in the range of 1 to 18, more preferably in the range of 1 to 10, and further preferably in the range of 1 to 8. Among them, potassium perfluorobutanesulfonate is particularly preferred. In the perfluoroalkylsulfonic acid alkali (earth) metal salt composed of an alkali metal, a lot of fluoride ions (F-) are usually mixed. The presence of the fluoride ions will become an important factor in reducing flame retardancy, so it is preferably reduced as much as possible. The ratio of the above-mentioned fluoride ions can be measured by ion chromatography. The content of fluoride ions is preferably less than 100ppm, more preferably less than 40ppm, and particularly preferably less than 10ppm. In addition, in terms of manufacturing efficiency, it is preferably more than 0.2ppm. The perfluoroalkylsulfonic acid alkali (earth) metal salt with reduced fluoride ion amount can be manufactured by a known method, and is manufactured by the following method, wherein the method is a method for reducing the amount of fluoride ions contained in the raw materials when manufacturing fluorine-containing organic metal salts, a method for removing the hydrogen fluoride obtained by the reaction by gas generated during the reaction or heating, and a method for reducing the amount of fluoride ions by purification methods such as recrystallization and reprecipitation in the manufacture of fluorine-containing organic metal salts. In particular, since organic metal salt flame retardants are relatively soluble in water, they are preferably manufactured by the following process: using ion exchange water, especially water satisfying a resistance value of 18 MΩ·cm or more, i.e., a conductivity of about 0.55 μS / cm or less, and dissolving it at a temperature higher than room temperature for washing, and then cooling it for recrystallization.

[0064] Specific examples of the aromatic sulfonic acid alkali (earth) metal salt include, for example, disodium diphenyl sulfide-4,4'-disulfonate, dipotassium diphenyl sulfide-4,4'-disulfonate, potassium 5-sulfoisophthalate, sodium 5-sulfoisophthalate, polysodium polyethylene terephthalate polysulfonate, calcium 1-methoxynaphthalene-4-sulfonate, disodium 4-dodecylphenyl ether disulfonate, polysodium poly(2,6-dimethylphenylene ether) polysulfonate, polysodium poly(1,3-phenylene ether) polysulfonate, polysodium poly(1,4-phenylene ether) polysulfonate, polypotassium poly(2,6-diphenylphenylene ether) polysulfonate, lithium poly(2-fluoro-6-butylphenylene ether) polysulfonate, potassium sulfonate of benzene sulfonate, benzene sulfonate, Sodium sulfonate, strontium benzenesulfonate, magnesium benzenesulfonate, dipotassium terephthalene disulfonate, dipotassium naphthalene-2,6-disulfonate, calcium biphenyl-3,3'-disulfonate, sodium diphenyl sulfone-3-sulfonate, potassium diphenyl sulfone-3-sulfonate, dipotassium diphenyl sulfone-3,3'-disulfonate, dipotassium diphenyl sulfone-3,4'-disulfonate, sodium α,α,α-trifluoroacetophenone-4-sulfonate, dipotassium benzophenone-3,3'-disulfonate, disodium thiophene-2,5-disulfonate, dipotassium thiophene-2,5-disulfonate, calcium thiophene-2,5-disulfonate, sodium benzothiophene sulfonate, potassium diphenyl sulfoxide-4-sulfonate, formalin condensate of sodium naphthalenesulfonate, and formalin condensate of sodium anthracenesulfonate. Among these aromatic sulfonic acid alkali (earth) metal salts, potassium salts are particularly preferred. Among these aromatic sulfonic acid alkali (earth) metal salts, potassium diphenyl sulfone-3-sulfonate and dipotassium diphenyl sulfone-3,3'-disulfonate are preferred, and a mixture thereof (the weight ratio of the former to the latter is 15 / 85 to 30 / 70) is particularly preferred.

[0065] As organic metal salts other than sulfonic acid alkali (earth) metal salts, alkali (earth) metal salts of sulfates and alkali (earth) metal salts of aromatic sulfonamides can be preferably exemplified. As alkali (earth) metal salts of sulfates, alkali (earth) metal salts of sulfates of monohydric and / or polyhydric alcohols can be particularly cited, and as the sulfates of the above-mentioned monohydric and / or polyhydric alcohols, methyl sulfate, ethyl sulfate, lauryl sulfate, hexadecyl sulfate, sulfates of polyoxyethylene alkylphenyl ether, monosulfate, disulfate, trisulfate, tetrasulfate of pentaerythritol, sulfates of lauric acid monoglyceride, sulfates of palmitic acid monoglyceride, and sulfates of stearic acid monoglyceride can be cited. As alkali (earth) metal salts of these sulfates, alkali (earth) metal salts of lauryl sulfate can be preferably cited. As the alkali (earth) metal salt of aromatic sulfonamide, for example, saccharin, N-(p-tolylsulfonyl)-p-toluenesulfonyl imide, N-(N'-benzylaminocarbonyl)sulfonyl imide and alkali (earth) metal salt of N-(phenylcarboxyl)sulfonyl imide can be mentioned. The content of the organic metal salt flame retardant is preferably 0.001 to 1 part by weight, more preferably 0.005 to 0.5 part by weight, further preferably 0.01 to 0.3 part by weight, and particularly preferably 0.03 to 0.15 part by weight relative to 100 parts by weight of component A.

[0066] (ii) Organic phosphorus flame retardants

[0067] As the organophosphorus flame retardant, an aryl phosphate compound is preferred. This is because the above-mentioned phosphate compounds generally have excellent color tones. In addition, since the phosphate compounds have a plasticizing effect, they are advantageous in improving molding processability. The above-mentioned phosphate compounds can use various phosphate compounds that are conventionally known as flame retardants. The amount of the organophosphorus flame retardant is preferably 0.01 to 20 parts by weight, more preferably 2 to 10 parts by weight, and further preferably 2 to 7 parts by weight relative to 100 parts by weight of component A.

[0068] (II) Hindered phenol stabilizer

[0069] The resin composition of the present invention may further be formulated with a hindered phenol stabilizer. The above formulation exerts effects such as suppressing the deterioration of color tone during molding and long-term use. Examples of hindered phenol compounds include α-tocopherol, butylhydroxytoluene, sinapyl alcohol, vitamin E, n-octadecyl β-(4'-hydroxy-3',5'-di-tert-butylphenyl) propionate, 2-tert-butyl-6-(3'-tert-butyl-5'-methyl-2'-hydroxybenzyl)-4-methylphenyl acrylate, 2,6-di-tert-butyl-4-(N,N-dimethylaminomethyl)phenol, diethyl 3,5-di-tert-butyl-4-hydroxybenzylphosphonate, 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 2,2'-methylenebis(4-ethyl-6-tert-butylphenol), 4,4'-methylenebis(2,6-di-tert-butylphenol), 2,2'-methylenebis(4-ethyl-6-tert-butylphenol), bis(4-methyl-6-cyclohexylphenol), 2,2'-dimethylene-bis(6-α-methyl-benzyl-p-cresol), 2,2'-ethylidene-bis(4,6-di-tert-butylphenol), 2,2'-butylidene-bis(4-methyl-6-tert-butylphenol), 4,4'-butylidene-bis(3-methyl-6-tert-butylphenol), triethylene glycol-N-bis-3-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate, 1,6-hexanediol bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], bis[2-tert-butyl-4-methyl-6-(3-tert-butyl-5-methyl-2-hydroxybenzyl)phenyl] terephthalate, 3,9-bis{2- [3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1,-dimethylethyl}-2,4,8,10-tetraoxaspiro[5,5]undecane, 4,4'-thiobis(6-tert-butyl-m-cresol), 4,4'-thiobis(3-methyl-6-tert-butylphenol), 2,2'-thiobis(4-methyl-6-tert-butylphenol), bis(3,5-di-tert-butyl-4-hydroxybenzyl) sulfide, 4,4'-dithiobis(2,6-di-tert-butylphenol), 4,4'-trithiobis(2,6-di-tert-butylphenol), 2,2-thiodiethylenebis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 2,4-bis n-Octylthio-6-(4-hydroxy-3',5'-di-tert-butylanilino)-1,3,5-triazine, N,N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxyhydrocinnamic acid), N,N'-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine, 1,1,3-tri(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tri(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, tri(3,5-di-tert-butyl-4-hydroxyphenyl)isocyanurate, tri(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanurate, 1,3,5-tri(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl) isocyanurate, 1,3,5-tris[3(3,5-di-tert-butyl-4-hydroxyphenyl)propionyloxy]ethyl isocyanurate, and tetrakis[methylene-3-(3',5'-di-tert-butyl-4-hydroxyphenyl)propionate]methane, etc. These are all easily available. The above hindered phenol stabilizers can be used alone or in combination of two or more. ,

[0070] The amount of the hindered phenol stabilizer to be added is preferably 0.0001 to 1 part by weight, more preferably 0.001 to 0.5 part by weight, and even more preferably 0.005 to 0.3 part by weight, based on 100 parts by weight of the component A.

[0071] (III) Other thermal stabilizers

[0072] The resin composition of the present invention may contain other heat stabilizers other than the aromatic phosphite stabilizer and the hindered phenol stabilizer. As the other heat stabilizer, for example, a typical lactone stabilizer for the reaction product of 3-hydroxy-5,7-di-tert-butylfuran-2-one and o-xylene can be preferably exemplified. The details of the stabilizer are described in Japanese Patent Publication No. 7-233160. The compound is commercially available as Irganox HP-136 (trademark, manufactured by CIBASPECIALTY CHEMICALS), and the compound can be used. In addition, stabilizers obtained by mixing the compound with various phosphite compounds and hindered phenol compounds are also commercially available. For example, Irganox HP-2921 manufactured by the above company can be preferably exemplified. The amount of the lactone stabilizer is preferably 0.0005 to 0.05 parts by weight, and more preferably 0.001 to 0.03 parts by weight, relative to 100 parts by weight of component A. In addition, as other stabilizers, sulfur-containing stabilizers such as pentaerythritol tetrakis (3-mercaptopropionate), pentaerythritol tetrakis (3-lauryl thiopropionate) and glycerol-3-stearyl thiopropionate can be exemplified. The amount of the sulfur-containing stabilizer is preferably 0.001 to 0.1 parts by weight, more preferably 0.01 to 0.08 parts by weight, based on 100 parts by weight of component A.

[0073] (IV) UV absorber

[0074] The resin composition of the present invention may contain an ultraviolet absorber in order to impart light resistance.

[0075] Specific examples of the ultraviolet absorber include benzophenone-based agents such as 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-octyloxybenzophenone, 2-hydroxy-4-benzyloxybenzophenone, 2-hydroxy-4-methoxy-5-sulfonic acid benzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone-5-sodium sulfonate, bis(5-benzoyl-4-hydroxy-2-methoxyphenyl)methane, 2-hydroxy-4-n-dodecyloxybenzophenone, and 2-hydroxy-4-methoxy-2'-carboxybenzophenone.

[0076] Examples of the benzotriazole series include 2-(2-hydroxy-5-methylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole, 2-(2-hydroxy-3,5-dicumylphenyl)phenylbenzotriazole, 2-(2-hydroxy-3-tert-butyl-5-methylphenyl)-5-chlorobenzotriazole, 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazol-2-yl)phenol], 2-(2-hydroxy-3,5-di-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-3,5-di-tert-butylphenyl)-5-chlorobenzotriazole, 2-(2-hydroxy-3,5-di-tert-amylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole, and 2-(2 2-(2-hydroxy-5-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-4-octyloxyphenyl)benzotriazole, 2,2'-methylenebis(4-cumyl-6-benzotriazolephenyl), 2,2'-p-phenylenebis(1,3-benzoxazin-4-one), and 2-[2-hydroxy-3-(3,4,5,6-tetrahydrophthalimidomethyl)-5-methylphenyl]benzotriazole, and copolymers of 2-(2'-hydroxy-5-methacryloyloxyethylphenyl)-2H-benzotriazole and vinyl monomers copolymerizable with the monomer, and copolymers of 2-(2'-hydroxy-5-acryloyloxyethylphenyl)-2H-benzotriazole and vinyl monomers copolymerizable with the monomer, etc. having a 2-hydroxyphenyl-2H-benzotriazole skeleton, etc.

[0077] Examples of hydroxyphenyltriazine-based compounds include 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-hexyloxyphenol, 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-methoxyphenol, 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-ethoxyphenol, 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-propoxyphenol, and 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-butoxyphenol. Examples include compounds in which the phenyl group of the above-mentioned compounds is a 2,4-dimethylphenyl group, such as 2-(4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine-2-yl)-5-hexyloxyphenol.

[0078] Examples of cyclic iminoesters include 2,2'-p-phenylenebis(3,1-benzo Oxazine-4-one), 2,2'-m-phenylenebis(3,1-benzo Oxazine-4-one) and 2,2'-diphenylenebis(3,1-benzo Oxazine-4-one) etc.

[0079] Examples of cyanoacrylates include 1,3-bis-[(2′-cyano-3′,3′-diphenylacryloyl)oxy]-2,2-bis{[(2-cyano-3,3-diphenylacryloyl)oxy]methyl}propane and 1,3-bis-[(2-cyano-3,3-diphenylacryloyl)oxy]benzene.

[0080] In addition, the above-mentioned ultraviolet absorber can also be a polymer type ultraviolet absorber obtained by copolymerizing the above-mentioned ultraviolet absorbing monomer and / or light-stable monomer with monomers such as (meth) alkyl acrylate by adopting the structure of a monomer compound that can be subjected to free radical polymerization. As the above-mentioned ultraviolet absorbing monomer, compounds containing a benzotriazole skeleton, a benzophenone skeleton, a triazine skeleton, a cyclic imino ester skeleton and a cyanoacrylate skeleton in the ester substituent of (meth) acrylate can be preferably exemplified. Among them, in terms of ultraviolet absorption ability, benzotriazole and hydroxyphenyl triazine systems are preferred, and in terms of heat resistance and color tone, cyclic imino ester systems and cyanoacrylate systems are preferred. Specifically, for example, Chemipro Chemical (strain) "Kemisorb79" and the like can be cited. The above-mentioned ultraviolet absorber can be used alone or in a mixture of two or more.

[0081] The content of the ultraviolet absorber is preferably 0.01 to 3 parts by weight, more preferably 0.02 to 2 parts by weight, further preferably 0.03 to 1 part by weight, and particularly preferably 0.05 to 0.5 parts by weight, based on 100 parts by weight of the component A.

[0082] (V) Other additives

[0083] In addition to the above, in the resin composition of the present invention, in order to impart various functions to the molded article and improve the properties, as long as the object of the present invention is not impaired, a small proportion of additives known per se can be incorporated. Examples of the above additives include antistatic agents, flow modifiers, infrared absorbers (heat ray absorbers), and bluing agents.

[0084] <Manufacturing method of polycarbonate resin composition>

[0085] The method of incorporating additives into the polycarbonate resin composition of the present invention is not particularly limited, and known methods can be used. As the most general method, the following method can be cited: The polycarbonate resin and the additive are pre-mixed and then fed into an extruder for melt-kneading. The extruded strand is cooled and cut by a granulator to produce a granular molding material.

[0086] Either a single-screw extruder or a twin-screw extruder can be used as the extruder in the above method, but from the viewpoints of productivity and kneading property, a twin-screw extruder is preferred. As a representative example of the above twin-screw extruder, TEX (manufactured by Japan Steel Works, Ltd., trade name) can be cited. As specific examples of the same type, TEX (manufactured by Japan Steel Works, Ltd., trade name), TEM (manufactured by Toshiba Machine Co., Ltd., trade name), KTX (manufactured by Kobe Steel, Ltd., trade name), ZSK (manufactured by Werner & Pfleiderer, trade name), etc. can be cited. As the extruder, an extruder having an exhaust port capable of removing moisture in the raw material and volatile gases generated from the melt-kneaded resin is preferably used. A vacuum pump for efficiently discharging the generated moisture and volatile gases from the exhaust port to the outside of the extruder is preferably provided. In addition, a screen for removing foreign substances mixed in the extrusion raw material, etc. can be provided in the area near the die head of the extruder to remove foreign substances from the resin composition. Examples of the above screen include a wire mesh, a screen changer, and a sintered metal plate (such as a disk filter).

[0087] In addition, the additive can also be independently supplied to the extruder, but it is preferably pre-mixed with the resin raw material as described above. Among the above pre-mixing means, Nauta mixers, V-type mixers, Henschel mixers, mechanochemical devices, and extrusion mixers can be exemplified. A more preferred method is as follows: For example, a part of the raw material resin and the additive are mixed using a high-speed mixer such as a Henschel mixer to produce a masterbatch, and then the above masterbatch and all the remaining resin raw materials are mixed using a non-high-speed mixer such as a Nauta mixer.

[0088] <Molded article>

[0089] The aromatic polycarbonate resin composition of the present invention can be formed into a desired molded article by a known molding method such as injection molding, blow molding, extrusion molding, rotational molding, etc.

[0090] Examples of the molded article preferably used in the present invention include molded articles subjected to steam sterilization for medical use or food use.

[0091] Example

[0092] Hereinafter, the present invention will be described in more detail based on examples, but the present invention is not limited to the following examples unless it exceeds the gist of the present invention.

[0093] The raw materials used in the following Examples and Comparative Examples are as follows.

[0094] <(A) Aromatic polycarbonate resin>

[0095] PC: Panlite L-1225WP manufactured by Teijin Co., Ltd. (polycarbonate resin obtained from bisphenol A, viscosity average molecular weight 22400)

[0096] <(B) Epoxy-containing compounds>

[0097] B-1: Marproof G0250SP manufactured by NOF Corporation (copolymer of styrene and glycidyl methacrylate)

[0098] <(C) Glycerol monofatty acid ester>

[0099] C-1: Riken Vitamin Co., Ltd. Rikemal S-100A (glyceryl monostearate)

[0100] C-2 (Comparative Example): Unister H-476-S (pentaerythritol tetrastearate) manufactured by NOF Corporation

[0101] <(D) Aromatic phosphite-based heat stabilizer>

[0102] D-1: Irgafos 168 (tris(2,4-di-tert-butylphenyl)phosphite) manufactured by BASF

[0103] The evaluation methods used in Examples and Comparative Examples are as follows.

[0104] (1) Moisture and heat resistance

[0105] The granular molding material obtained by each composition of the embodiment was dried at 120°C for 5 hours using a hot air circulation dryer, and was molded into a molded plate with a width of 50 mm, a length of 90 mm, and a thickness of 2 mm using an injection molding machine [J85-ELIII manufactured by The Nippon Steel Works, Ltd.] at a molding temperature of 350°C and a mold temperature of 80°C. The molded plate was subjected to a wet heat treatment (temperature 130°C, 24 hours) using a steam sterilizer [SN-510 of YAMATO Scientific Co., Ltd.], and the Haze and viscosity average molecular weight (Mv) before and after the wet heat treatment were measured. The value obtained by subtracting the Haze before the wet heat treatment from the Haze after the wet heat treatment was calculated as ΔHaze, and the value obtained by subtracting the viscosity average molecular weight (Mv) after the wet heat treatment from the viscosity average molecular weight (Mv) before the wet heat treatment was calculated as ΔMv. The smaller the ΔHaze and ΔMv, the better. The Haze of the molded plate was measured in accordance with JIS-K7361-1, and the viscosity average molecular weight (Mv) was measured by the following method.

[0106] Determination of viscosity average molecular weight (Mv)

[0107] The specific viscosity (η) was calculated from the following formula using an Ostwald viscometer from a solution obtained by dissolving 0.7 g of the molded plate in 100 ml of dichloromethane at 20°C. SP ), according to the obtained specific viscosity (η SP ) The viscosity average molecular weight Mv is calculated by the following mathematical formula.

[0108] Specific viscosity (η SP )=(t-t0) / t0

[0109] [t0 is the falling seconds of dichloromethane, t is the falling seconds of the sample solution]

[0110] η SP / c=[η]+0.45×[η] 2 c (where [η] is limiting viscosity)

[0111] [η] = 1.23 × 10 -4 Mv 0.83

[0112] c=0.7

[0113] (2) Molding heat resistance ΔE

[0114] When the test piece is molded in (1) above, the color tone (L * 、a * , b * ) and hue (L * '、a * ', b *') The color difference ΔE of the test piece was calculated using the following formula (a) using a spectrophotometer CE-7000A manufactured by Sakata Inx Eng Co., Ltd. with a D65 light source and a 10-degree field of view. The smaller the ΔE, the better.

[0115] ΔE={(ΔL * ) 2 +(Δa * ) 2 +(Δb * ) 2} 1 / 2 …Formula (a)

[0116] Color tone of "Forming board before retention": L * 、a * , b *

[0117] Color tone of "Forming board after retention": L * '、a * ', b * '

[0118] ΔL * :L * -L * '

[0119] Δa * :a * -a * '

[0120] Δb * :b * -b * '

[0121] [Examples 1 to 4 and Comparative Examples 1 to 6]

[0122] After blending the raw materials in the ratios shown in Tables 1 and 2, the raw materials were melt-kneaded at a barrel temperature of 280°C using a twin-screw extruder TEX30α with a vent and a screw diameter of 30 mm manufactured by Nippon Steel Corporation, and the strands were cut to obtain pelletized molding materials. The test pieces for evaluation were molded under the above conditions, and the above evaluations were performed. The evaluation results are shown in Tables 1 and 2.

[0123]

[0124] [Table 2]

[0125]

[0126] Industrial Applicability

[0127] The aromatic polycarbonate resin composition of the present invention has excellent moisture and heat resistance and molding heat resistance. Therefore, it can be applied to various uses using aromatic polycarbonate resins, and is particularly useful as a molded product subjected to steam sterilization in medical and food applications.

Claims

1. An aromatic polycarbonate resin composition comprising 0.02 to 0.04 parts by weight of (B) an epoxy group-containing compound (component B) and 0.06 to 0.15 parts by weight of (C) a glycerol monofatty acid ester (component C), based on 100 parts by weight of (A) an aromatic polycarbonate resin (component A).

2. The aromatic polycarbonate resin composition according to claim 1, wherein (D) an aromatic phosphite-based heat stabilizer, that is, component D, is contained in an amount of 0.01 to 0.02 parts by weight based on 100 parts by weight of component A.

3. The aromatic polycarbonate resin composition according to claim 1 or 2, wherein The component B is a copolymer of styrene and glycidyl methacrylate. 4 . A molded article formed from the aromatic polycarbonate resin composition according to claim 1 .