Silicone rubber adhesive

By cleaning and activate the inorganic substrate using a specific adhesive regulator composition and applying silicone rubber directly, the bonding problem between the silicone elastomer and the inorganic substrate is solved, and a strong bonding and environmentally friendly process is achieved.

CN118922506APending Publication Date: 2024-11-08DOW SILICONES CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202380029592.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-29
Filing Date
2023-03-27
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Prior art When preparing composite materials of silicone elastomers and inorganic substrates, the lack of adhesion between the two leads to bonding problems, especially the presence of unreliability and volatile organic solvents when using primers. Environmental issues.

Method used

Adhesive regulator compositions comprising trialkoxysilane, platinum group metal catalyst, alkoxy titanium compound and polyorganosiloxane are used to clean and activate the surface of the inorganic substrate and to bond without drying Silicone rubber is applied with the conditioner layer and directly cured to form the composite material.

Benefits of technology

The strong bonding of silicone elastomer and inorganic substrate is achieved, avoiding the unreliability of the primer and the volatile organic solvents, simplifying the process flow, and reducing environmental pollution.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present disclosure relates to a process for adhering a silicone elastomer prepared from a hydrosilylation curable silicone rubber composition to an inorganic substrate using a suitable adhesion modifier, the use of the adhesion modifier for the process, and to a composite material comprising an inorganic substrate adhered to a silicone elastomer using the aforementioned adhesion modifier composition.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present disclosure relates to a method of adhering a silicone elastomer prepared from a hydrosilylation-curable silicone rubber composition to an inorganic substrate using a suitable adhesion modifier, use of the adhesion modifier for the method, and to a composite material comprising an inorganic substrate adhered to the silicone elastomer using the aforementioned adhesion modifier composition.

[0002] The hydrosilylation-curable silicone rubber composition is cured via a hydrosilylation (addition) cure process to provide a silicone elastomeric material (also referred to as silicone rubber).

[0003] The silicone elastomer obtained by curing the hydrosilylation-curable silicone rubber composition can be used in a variety of applications including, for example, power supplies (e.g., high voltage electrical insulation materials), electronic devices, automotive applications, and consumer applications (including, for example, food contact applications) because of their highly reliable properties.

[0004] In many such applications, it is increasingly desirable to produce molded composite parts comprising silicone elastomers and other materials, such as inorganic materials, e.g., metals, metal alloys, glasses, and ceramics. However, the preparation of such composite materials has proven difficult due to the lack of adhesion between the silicone elastomer and many inorganic materials that would be used as substrates, particularly if the inorganic material is substantially unreactive toward the silicone elastomer, or the silicone elastomer is substantially unreactive toward the inorganic material. Thus, the ability to provide composite materials of silicone elastomer materials and such inorganic substrates is limited by the inability to form a sufficiently strong bond between the two.

[0005] The application of a primer to the substrate surface (with or without pre-activation of the substrate) was initially used to overcome this lack of adhesion. The primer is a preliminary coating applied to the substrate and then dried and / or cured to provide improved adhesion between the substrate and the hydrosilylation-curable silicone rubber composition subsequently applied thereto in this case. Unless, for example, a solvent, an ultrasonic bath and / or a special treatment (such as flame, corona or plasma treatment) are used for cleaning and / or activation, the primer cannot always establish adhesion with the inorganic substrate. Typically, depending on the nature of the primer, the primer is applied to the substrate surface with a suitable thickness of less than 10 μm to 1 mm. After application and solvent evaporation at room temperature or elevated temperature, many primers require pre-curing at a temperature between 60 and 130° C. for 20 to 120 minutes. However, the use of a method requiring a primer produces several problems. The use of primers for composite parts / articles is generally not preferred because these primers can be unreliable, can have quality control and reliability issues, and traditionally contain high proportions of organic solvents that evaporate during the drying / curing process, often resulting in undesirable volatile organic compound (VOC) environmental issues.

[0006] The use of such primers has proven to be particularly problematic in the preparation of composite parts / articles for highly regulated applications such as skin contact and food contact applications.

[0007] Composite parts / articles made from one or more inorganic substrates and one or more silicone elastomers are typically prepared by injection molding methods, including overmolding (e.g., injection molding a hydrosilylation-curable silicone rubber composition on an inorganic substrate) or 2K injection molding methods used when the inorganic substrate and the hydrosilylation-curable silicone rubber composition are molded into a composite silicone elastomer / inorganic substrate article or part by using a 2k injection molding machine. Historically, the use of most primers has been prevented by their composition, particularly volatile organic solvents.

[0008] It is an object of the present disclosure to provide a method for adhering a silicone elastomer to an inorganic substrate using a suitable adhesion modifier composition.

[0009] The present disclosure relates to a method for preparing a composite material of a silicone elastomer and an inorganic substrate, the method comprising the following steps:

[0010] (a) optionally cleaning and / or activating the surface of an inorganic substrate;

[0011] (b) treating the optionally cleaned and / or activated inorganic substrate surface with an adhesion regulator composition;

[0012] (c) applying a hydrosilylation-curable silicone rubber composition to the treated surface obtained in step (b);

[0013] (d) curing the hydrosilylation-curable silicone rubber composition,

[0014] It is characterized in that the adhesion regulator composition comprises:

[0015] (i) Formula Si(OR)3R 1 A trialkoxysilane wherein each R may be the same or different and is an alkyl group having at least two carbon atoms, and each R 1 which may be the same or different and are unsaturated groups selected from alkenyl groups or alkynyl groups;

[0016] The trialkoxysilane is present in an amount of 20 wt. % to 45 wt. % of the adhesion modifier composition;

[0017] (ii) a platinum group metal-based hydrosilylation catalyst, wherein the platinum group metal is present in an amount of 0.1 wt.% to 1.5 wt.% of the adhesion modifier composition;

[0018] (iii) an alkoxy titanium compound having 2 to 4 alkoxy groups, the alkoxy titanium compound being present in an amount of 1 wt.% of the adhesion regulator composition

[0019] to 10wt.%;

[0020] (iv) Formula Si(OR 2 )4 tetraalkoxysilane, wherein each R 2 which may be the same or different and are alkyl groups having at least two carbons per group, the tetraalkoxysilane being present in an amount of 5 wt.% to 20 wt.% of the adhesion modifier composition; and

[0021] (v) any of the following:

[0022] (a') a polyorganosiloxane containing at least two unsaturated groups selected from alkenyl groups and alkynyl groups per molecule and prepared using a Brookfield having an RV-4 spindle TM The viscometer has a viscosity in the range of 50 mPa.s to 9000 mPa.s at 25°C at 20 rpm; or

[0023] (b') a mixture of two or more polyorganosiloxanes containing at least two unsaturated groups selected from alkenyl groups and alkynyl groups per molecule, the mixture being prepared using a Brookfield 1000 having an RV-4 spindle TM The viscometer has a viscosity in the range of 50 mPa.s to 9000 mPa.s at 25°C at 20 rpm;

[0024] Wherein the component (v) is present in an amount of 25 wt.% to 60 wt.% of the adhesion regulator composition.

[0025] The total weight percent (wt.%) of the adhesion regulator composition used in the method in any combination is 100 wt.%. It is not necessary to wait for the adhesion regulator layer to dry or cure, and in fact it is preferred to apply the hydrosilylation-curable silicone rubber composition before the adhesion regulator layer cures or solidifies. Also provided is the use of the adhesion regulator composition as described above in the preparation of silicone elastomers and inorganic composite materials.

[0026] Also provided is a composite part or article obtained or obtainable by a method for preparing a composite material of a silicone elastomer and an inorganic substrate, the method comprising the steps of:

[0027] (a) optionally cleaning and / or activating the surface of an inorganic substrate;

[0028] (b) treating the optionally cleaned and / or activated inorganic substrate surface with an adhesion regulator composition;

[0029] (c) applying a hydrosilylation-curable silicone rubber composition to the treated surface obtained in step (b);

[0030] (d) curing the hydrosilylation-curable silicone rubber composition,

[0031] It is characterized in that the adhesion regulator composition comprises:

[0032] (i) Formula Si(OR)3R 1 A trialkoxysilane wherein each R may be the same or different and is an alkyl group having at least two carbon atoms, and each R 1 which may be the same or different and are unsaturated groups selected from alkenyl groups or alkynyl groups;

[0033] The trialkoxysilane is present in an amount of 20 wt. % to 45 wt. % of the adhesion modifier composition;

[0034] (ii) a platinum group metal-based hydrosilylation catalyst, wherein the platinum group metal is present in an amount of 0.1 wt.% to 1.5 wt.% of the composition;

[0035] (iii) an alkoxy titanium compound having 2 to 4 alkoxy groups, the alkoxy titanium compound being present in an amount of 1 wt.% of the adhesion regulator composition

[0036] to 10wt.%;

[0037] (iv) Formula Si(OR 2 )4 tetraalkoxysilane, wherein each R 2 which may be the same or different and are alkyl groups having at least two carbons per group, the tetraalkoxysilane being present in an amount of 5 wt. % to 20 wt. % of the adhesion modifier composition, and

[0038] (v) any of the following:

[0039] (a') a polyorganosiloxane containing at least two unsaturated groups selected from alkenyl groups and alkynyl groups per molecule and prepared using a Brookfield having an RV-4 spindle TM The viscometer has a viscosity in the range of 50 mPa.s to 9000 mPa.s at 25°C at 20 rpm; or

[0040] (b') a mixture of two or more polyorganosiloxanes containing at least two unsaturated groups selected from alkenyl groups and alkynyl groups per molecule, the mixture being prepared using a Brookfield 1000 having an RV-4 spindle TMThe viscometer has a viscosity in the range of 50 mPa.s to 9000 mPa.s at 25°C at 20 rpm;

[0041] Wherein the component (v) is present in an amount of 25 wt.% to 60 wt.% of the adhesion regulator composition.

[0042] Advantageously, the method of adhering silicone elastomers to inorganic substrates using the above-described adhesion modifier composition allows for immediate overmolding and does not rely on primer pre-cure treatments or solvent evaporation, ie, it is designed to not involve major volatile organic compounds (VOCs), such as organic solvents.

[0043] Any suitable inorganic substrate can be utilized. In one embodiment, the inorganic substrate is selected from metals, such as aluminum, steel, copper, zinc and alloys thereof (such as brass), glass, ceramic materials (such as silicon oxide, aluminum oxide, zirconium dioxide, aluminum silicate, cerium oxide and composites thereof). When the inorganic substrate is glass, the glass substrate on which the composition is applied can be almost any glass substrate, such as borosilicate glass, soda-lime glass, silica glass, alkali-barium glass, aluminosilicate glass, lead glass, phosphate glass, alkali borosilicate glass, xena glass and / or fluorosilicate glass. The substrate can alternatively be pretreated glass, such as, a vacuum-deposited reflective metal-coated flat glass, which can be used, for example, in commercial buildings and architectural spandrel applications.

[0044] In the method described in this article, there are four steps:

[0045] (a) optionally cleaning and / or activating the surface of an inorganic substrate;

[0046] (b) treating the optionally cleaned and / or activated inorganic substrate surface with an adhesion regulator composition;

[0047] (c) applying a hydrosilylation-curable silicone rubber composition to the treated surface obtained in step (b);

[0048] (d) curing the hydrosilylation-curable silicone rubber composition.

[0049] Step (a)

[0050] As previously mentioned, step (a) of the method described herein, i.e., cleaning and / or activating the surface of the inorganic substrate, is optional. If desired, the cleaning and / or activation step can be performed by, for example, plasma treatment, corona discharge treatment, UV-C / ozone or vacuum-UV irradiation, flame pyrolytic deposition of amorphous silica, or flame treatment.

[0051] The term "plasma" encompasses a wide range of systems with densities and temperatures that differ by many orders of magnitude. Some plasmas are very hot and all their microscopic matter (ions, electrons, etc.) is close to thermal equilibrium, and the energy input into the system is widely distributed by collisions at the atomic / molecular level. However, other plasmas, particularly those used at room temperature and pressure or under vacuum (wherein collisions are relatively infrequent), have constituent substances at widely different temperatures and are referred to as "non-thermal equilibrium" plasmas, in which free electrons are very hot, with temperatures of thousands of degrees Kelvin, while neutral and ion substances remain cool. Because free electrons have almost negligible mass, the total system heat content is low, and plasmas (e.g., atmospheric pressure plasma discharges, such as atmospheric pressure dielectric barrier discharges and atmospheric pressure glow discharges) operate at near room temperature, thereby allowing processing of temperature-sensitive materials, such as plastics or polymers, without applying destructive heat loads to the sample. However, hot electrons generate a rich source of free radicals and excited species with high chemical potential energy through high-energy collisions, which are capable of deep chemical and physical reactivity, and are therefore suitable for many technical applications, such as surface activation in this case.

[0052] Corona discharge is an electrical discharge caused by the ionization of a fluid, such as air surrounding a conductor carrying a high voltage. It represents a localized area where the air (or other fluid) has undergone electrical breakdown and become conductive, allowing charge to continue to leak from the conductor into the air and can be used for cleaning and / or activation purposes.

[0053] UV-C radiation is particularly advantageously provided at a wavelength of 100 nm to 280 nm, preferably 150 nm to 260 nm and particularly preferably 170 nm to 260 nm and can be used to clean and / or activate the surface of suitable inorganic substrates and to improve the adhesion of silicone on their surface after application of a coating of an adhesion regulator composition as described above.

[0054] The flame pyrolytic deposition of amorphous silicon dioxide can be carried out by any suitable method, such as the "PYROSIL TM A method in which a substrate is fed through a substrate doped with a silicon-containing precursor material (PYROSIL TM ) gas flame, the precursor burns in the flame and is deposited on the surface as a very thin but dense and firmly adhered silicon oxide coating (5nm-100nm).

[0055] In the case of each radiation cleaning and / or activation method used, the radiation is preferably generated by a suitable radiation source, wherein the radiation source moves over the surface of the inorganic substrate during irradiation. Alternatively, the radiation source can be fixed and / or the substrate can be moved relative to it, for example.

[0056] The irradiation of the surface of the inorganic substrate material by UV-C radiation is further advantageously carried out simultaneously with the formation of ozone, wherein the ozone interacts with the surface during the irradiation. It has been found that when the inorganic material is irradiated with UV-C radiation, ozone is formed by interaction with the air atmosphere, which in turn produces a significant improvement in the surface activation in the interaction with the surface of the inorganic material. The ozone formed is therefore additionally used to improve the adhesion of the silicone on the surface of the inorganic material.

[0057] If the irradiation is carried out in a closed space, in particular in an irradiation chamber that is darkened toward the outside, the advantage achieved in particular in combination with ozone is that the ozone remains in the region of the inorganic substrate close to the surface and can interact with the surface accordingly. In order to enhance this effect, the irradiation chamber can also be optimized accordingly to ensure the strongest possible interaction of the ozone with the surface. The dimensions of the irradiation chamber are selected, for example, to be so small that the highest possible ozone concentration is present above the surface of the inorganic substrate.

[0058] The duration of irradiation may be, for example, 0.1 seconds to fifteen minutes; alternatively 0.1 seconds to ten minutes; alternatively three seconds to seven minutes; alternatively three seconds to five minutes; alternatively 0.1 seconds to one minute; alternatively 0.4 seconds to 30 seconds.

[0059] For the cleaning and / or activation steps of the present invention, UV-C or particularly corona discharge are preferred methods for step (a) of the process, particularly for metals, as they can oxidize the surface of substrates, such as the metals described herein.

[0060] Step (b)

[0061] After step (a) cleaning and / or activation is completed, when necessary, the above-mentioned adhesion regulator composition layer is applied to the inorganic substrate surface according to step (b). Any suitable method can be used, that is, by spraying, brushing, roller coating, overflow (flooding) and scraping (squeegeeing), applying with a scraper coater or by wiping or transfer printing with a sponge or punching, or in some cases can be dipped in the bath of the adhesion regulator composition to dip the substrate, depending on the size and shape of the substrate. In the laboratory, it is found that once the adhesion regulator composition has been applied by a pipette, it is completely sufficient to only wipe the surface of the inorganic substrate. After being applied on the substrate, the adhesion regulator composition coating is usually in a region of 0.001mm to 3mm thick, alternatively 0.001mm to 2mm thick, alternatively 0.001mm to 1mm thick.

[0062] Step (b) of the method requires the use of the above-described adhesion regulator composition, the components of which are discussed below:

[0063] Component (i)

[0064] Component (i) of the adhesion modifier composition is of the formula Si(OR)3R 1 wherein each R group may be the same or different and is an alkyl group having at least two carbons per group, alternatively 2 to 20 carbons per group, alternatively 2 to 15 carbons per group, alternatively 2 to 10 carbons per group; alternatively, each R group may be selected from an alkyl group having 2 to 6 carbons per group, such as ethyl, propyl, n-butyl, tert-butyl, pentyl or hexyl; alternatively ethyl, propyl, n-butyl, isobutyl or tert-butyl, alternatively ethyl or propyl, and

[0065] Each R 1 may be the same or different and are unsaturated groups selected from alkenyl groups or alkynyl groups, alternatively, each R 1 may be the same or different and are unsaturated groups selected from alkenyl groups or alkynyl groups, in either case the alkenyl groups or alkynyl groups have 2 to 20 carbons per group, alternatively 2 to 15 carbons per group, alternatively 2 to 10 carbons per group; alternatively, each R 1 are alkenyl groups which may be identical or different and are selected from ethenyl, propenyl, n-butenyl, pentenyl or hexenyl.

[0066] In one embodiment, component (i) trialkoxysilane is present in an amount of 20 wt.% to 40 wt.% of the adhesion modifier composition, alternatively 25 wt.% to 38 wt.% of the adhesion modifier composition, alternatively 25 wt.% to 35 wt.% of the adhesion modifier composition.

[0067] In a preferred embodiment, the trialkoxysilane of component (i) is of the formula Si(OR)3R 1 A trialkoxysilane wherein each R is an alkyl group having 2 to 4 carbons per group, such as ethyl, propyl, n-butyl, isobutyl or tert-butyl, alternatively ethyl or propyl, and each R 1 is an alkenyl group which may be the same or different, each group having 2 to 6 carbon atoms, such as ethenyl, propenyl, n-butenyl, pentenyl or hexenyl; alternatively, each R 1 is a vinyl group.

[0068] Component (ii)

[0069] The component (ii) of the adhesion regulator composition is a hydrosilylation curing catalyst based on a platinum group metal. These catalysts are generally selected from catalysts of platinum group metals (platinum, ruthenium, osmium, rhodium, iridium and palladium), or compounds of one or more metals in such metals. Alternatively, due to the high activity level of these catalysts in the hydrosilylation reaction, platinum and rhodium compounds are preferred, wherein platinum compounds are most preferred. In the hydrosilylation (or addition) reaction, the hydrosilylation catalyst such as component (ii) herein catalyzes the reaction between an unsaturated group (usually an alkenyl group, for example vinyl) and a Si-H group.

[0070] The component (ii) catalyst may be a platinum group metal, a platinum group metal deposited on a carrier such as activated carbon, a metal oxide such as alumina or silica, silica gel or charcoal powder, or a compound or complex of a platinum group metal. Preferably the platinum group metal is platinum.

[0071] Examples of preferred hydrosilylation catalysts (ii) are platinum-based catalysts, such as platinum black, platinum oxide (Adams catalyst), platinum on various solid supports, chloroplatinic acid, such as hexachloroplatinic acid (Pt oxidation state IV) (Speier catalyst), chloroplatinic acid in solution in alcohols, such as isooctyl or amyl alcohol (Lamoreaux catalyst), and complexes of chloroplatinic acid with ethylenically unsaturated compounds, such as olefins, and organosiloxanes containing ethylenically unsaturated silicon-bonded hydrocarbon groups, such as tetravinyltetramethylcyclotetrasiloxane-platinum complex (Ashby catalyst). Soluble platinum compounds that can be used include, for example, platinum-olefin complexes of the formula (PtCl2.olefin)2 and H(PtCl3.olefin), in this context preferably using olefins having 2 to 8 carbon atoms, such as ethylene, propylene, isomers of butene and isomers of octene, or cycloalkanes having 5 to 7 carbon atoms, such as cyclopentene, cyclohexene and cycloheptene. Other soluble platinum catalysts are, for example, platinum-cyclopropane complexes of formula (PtCl2C3H6)2, reaction products of hexachloroplatinic acid with alcohols, ethers and aldehydes or mixtures thereof, or reaction products of hexachloroplatinic acid and / or its conversion products with vinyl-containing siloxanes (e.g., methylvinylcyclotetrasiloxane) in the presence of an ethanolic solution containing sodium bicarbonate. Platinum catalysts with phosphorus, sulfur and amine ligands, such as (Ph3P)2PtCl2, and complexes of platinum with vinyl siloxanes, such as symmetrical divinyltetramethyldisiloxane, can also be used.

[0072] Thus, specific examples of suitable platinum-based catalysts include:

[0073] (i') complexes of chloroplatinic acid and organosiloxanes containing ethylenically unsaturated hydrocarbon groups as described in US Pat. No. 3,419,593;

[0074] (ii') chloroplatinic acid in the form of its hexahydrate or in its anhydrous form;

[0075] (iii') a platinum-containing catalyst obtained by a process comprising the steps of: reacting chloroplatinic acid with an aliphatically unsaturated organosilicon compound such as divinyltetramethyldisiloxane;

[0076] (iv') olefin-platinum-silyl complexes such as (COD)Pt(SiMeCl2)2 as described in US Pat. No. 6,605,734, wherein "COD" is 1,5-cyclooctadiene; and / or

[0077] (v') Karstedt catalysts, i.e. platinum divinyltetramethyldisiloxane complexes, typically containing about 1 wt.% platinum in a vinylsiloxane polymer. Solvents such as toluene and similar organic solvents have historically been used as alternatives, but the use of vinylsiloxane polymers is by far the preferred choice. These are described in US 3,715,334 and US 3,814,730. In a preferred embodiment, component (ii) may be selected from coordination compounds of platinum. In one embodiment, hexachloroplatinic acid and its conversion products with vinyl-containing siloxanes, Karstedt catalysts and Speier catalysts are preferred.

[0078] The catalyst may be added as a single substance or as a mixture of two or more different substances. Typically, the amount of platinum group metal present, alternatively the amount of platinum metal present will be in the range of 0.1 wt.% - 1.5 wt.% of the composition, alternatively 0.1 wt.% - 1.0 wt.% of the composition, alternatively 0.1 wt.% - 0.5 wt.% of the composition, depending on the form / concentration in which the catalyst is provided.

[0079] Component (iii)

[0080] Component (iii) of the adhesion regulator composition is an alkoxytitanium compound having 2 to 4 alkoxy groups, such as Ti(OR 3 )4、Ti(OR 3 )3R 4 、Ti(OR 3 )2R 4 2, or chelated alkoxytitanium molecules, such as esters of enolates of titanic acid and acetoacetate; wherein R 3 is a straight or branched chain alkyl group having 1 to 20 carbons, alternatively 1 to 15 carbons, alternatively 1 to 10 carbons, alternatively 1 to 6 carbons. 3 Examples of include, but are not limited to, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, branched secondary alkyl groups such as 2,4-dimethyl-3-pentyl. When present, R4 is an organic group, such as an alkyl group having 1 to 10 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an alkynyl group having 2 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, or an aromatic group having 6 to 20 carbon atoms, such as a phenyl group, or a mixture thereof. 4 R may be the same or different and is selected from an alkyl group, an alkenyl group or an alkynyl group, alternatively an alkyl group, an alkenyl group, alternatively an alkyl group, in each case each group having up to 10 carbons, alternatively up to 6 carbons. 4 Examples of may include, but are not limited to, methyl, ethyl, propyl, butyl, vinyl, cyclohexyl, phenyl, tolyl groups.

[0081] In Ti(OR 3 )4、Ti(OR 3 )3R 4 Or Ti(OR 3 )2R 4 2, suitable examples of component (iii) include, for example, tetramethyl titanate, tetraethyl titanate, tetra-n-propyl titanate, tetra-n-butyl titanate, tetra-tert-butyl titanate, tetraisobutyl titanate, and tetraisopropyl titanate. When component (iii) is Ti(OR 3 )3R 4 When the component (iii) is a chelated titanium, examples include, but are not limited to, trimethoxyalkyltitanium, triethoxyalkyltitanium, tri-n-propoxyalkyltitanium, tri-n-butoxyalkyltitanium, tri-t-butoxyalkyltitanium and triisopropoxyalkyl titanate. When component (iii) is a chelated titanium, it may include an ester of an enolate of titanic acid and acetoacetate.

[0082] In one embodiment, component (iii) may be selected from the structure Ti(OR 3 )4、Ti(OR 3 )3R 4 、Ti(OR 3 )2R 4 2 titanate, wherein each R 4 As mentioned above, R 3 is an isobutyl group or an n-butyl group, or component (iii) is an ester of an enolate of titanic acid and acetoacetate.

[0083] Component (iii) of the adhesion modifier composition, i.e. the alkoxytitanium compound having 2 to 4 alkoxy groups, may be present in an amount of 1 to 10 wt.%, alternatively 2 to 8 wt.%, alternatively 2 to 7 wt.% of the composition.

[0084] Component (iv)

[0085] Component (iv) of the adhesion regulator composition is of the formula Si(OR 2 )4 tetraalkoxysilane, wherein each R 2 can be the same or different and are alkyl groups having at least two carbons per group, alternatively alkyl groups having 2 to 20 carbons per group, alternatively alkyl groups having 2 to 15 carbons per group, alternatively alkyl groups having 2 to 10 carbons per group, alternatively ethyl, propyl, isopropyl, n-butyl, isobutyl, tert-butyl, pentyl or hexyl, alternatively ethyl, propyl, isopropyl, n-butyl, isobutyl, tert-butyl; component (iv) is present in the adhesion regulator composition in an amount of 5wt.% to 20wt.%, alternatively 5wt.% to 15wt.%, alternatively 7wt.% to 15wt.% of the composition.

[0086] Component (v)

[0087] Component (v) of the adhesion regulator composition is any of the following:

[0088] (a') a polyorganosiloxane containing at least two unsaturated groups selected from alkenyl groups and alkynyl groups per molecule and prepared using a Brookfield having an RV-4 spindle TM The viscometer has a viscosity in the range of 50 mPa.s to 9000 mPa.s at 25°C at 20 rpm; or

[0089] (b') a mixture of two or more polyorganosiloxanes containing at least two unsaturated groups selected from alkenyl groups and alkynyl groups per molecule, the mixture being prepared using a Brookfield 1000 having an RV-4 spindle TM The viscometer has a viscosity in the range of 50 mPa.s to 9000 mPa.s at 25°C at 20 rpm;

[0090] wherein the component (v) is present in an amount of 25 wt.% to 60 wt.% of the composition.

[0091] In (v)(a') a polyorganosiloxane containing at least two unsaturated groups selected from alkenyl groups and alkynyl groups per molecule and in (v)(b') a mixture of two or more polyorganosiloxanes containing at least two unsaturated groups selected from alkenyl groups and alkynyl groups per molecule, a Brookfield 1000 having an RV-4 spindle was used. TM The viscometer has a viscosity in the range of 50 mPa.s to 9000 mPa.s at 25°C at 20 rpm; a Brookfield with RV-4 spindle may alternatively be used. TMThe viscometer has a viscosity in the range of 100 mPa.s to 9000 mPa.s at 25°C at 20 rpm; a Brookfield with RV-4 spindle may alternatively be used. TM The viscometer has a viscosity in the range of 100 mPa.s to 8000 mPa.s at 25°C at 20 rpm; a Brookfield with RV-4 spindle may alternatively be used. TM The viscometer has viscosities ranging from 100 mPa.s to 7500 mPa.s at 25°C at 20 rpm; a Brookfield with RV-4 spindle may alternatively be used. TM The viscometer has a viscosity in the range of 100 mPa.s to 7000 mPa.s at 25°C at 20 rpm; a Brookfield with RV-4 spindle may alternatively be used. TM The viscometer has a viscosity in the range of 200 mPa.s to 7000 mPa.s at 25°C at 20 rpm; a Brookfield with RV-4 spindle may alternatively be used. TM The viscometer has a viscosity in the range of 300 to 5000 mPa.s at 25° C. at 20 rpm.

[0092] In the case of (v)(b'), the mixture may comprise a polyorganosiloxane containing at least two unsaturated groups selected from alkenyl groups and alkynyl groups per molecule and having a viscosity in the range of 50 mPa.s to 60,000 mPa.s at 25°C, alternatively 50 mPa.s to 25,000 mPa.s at 25°C, 100 mPa.s to 25,000 mPa.s at 25°C, alternatively 100 mPa.s to 15,000 mPa.s at 25°C, alternatively 100 mPa.s to 10,000 mPa.s at 25°C, provided that the viscosity of the resulting mixture is measured using a Brookfield with an RV-4 spindle. TM The viscometer has a viscosity ranging from 50 to 9000 mPa.s at 25°C at 20 rpm in an amount of 25 to 60 wt.% of the composition, alternatively 30 to 60 wt.% of the composition, alternatively 35 to 55 wt.% of the composition.

[0093] (v) The viscosity of individual polymers in (b') having a viscosity greater than 10,000 mPa.s measured at 25°C can be determined using a Brookfield LV-4 spindle (designed for viscosities in the range of 10,000 mPa.s to 2,000,000 mPa.s). TMThe rotational viscometer is used to adjust the speed according to the viscosity of the polymer, for example, to measure at 6 rpm.

[0094] Each polyorganosiloxane of component (v) is a polydiorganosiloxane having at least two unsaturated groups per molecule, the unsaturated groups being selected from alkenyl groups or alkynyl groups. Alternatively, each polyorganosiloxane of component (v) has at least three unsaturated groups per molecule.

[0095] The unsaturated groups of each polyorganosiloxane of component (v) can be terminal groups, side groups or at these two positions. The alkenyl group can have 2 to 30, alternatively 2 to 24, alternatively 2 to 20, alternatively 2 to 12, alternatively 2 to 10, alternatively 2 to 6 carbon atoms. The alkenyl group is illustrated by but not limited to the following: vinyl group, allyl group, methallyl group, propenyl group and hexenyl group and cyclohexenyl group. The alkynyl group can be illustrated by but not limited to the following: ethynyl group, propynyl group and butynyl group. The alkynyl group can have 2 to 30, alternatively 2 to 24, alternatively 2 to 20, alternatively 2 to 12, alternatively 2 to 10, alternatively 2 to 6 carbon atoms.

[0096] Each polyorganosiloxane of component (v) has a plurality of units of formula (I): R' a SiO (4-a) / 2 (I)

[0097] Wherein each R 'is independently selected from aliphatic hydrocarbon groups, aliphatic non-halogenated organic groups (i.e., any aliphatic organic substituent group having one free valence at a carbon atom, regardless of the type of functional group). Saturated aliphatic hydrocarbon groups are exemplified by, but not limited to, alkyl groups such as methyl, ethyl, propyl, pentyl, octyl, undecyl and octadecyl, and cycloalkyl groups such as cyclohexyl. Examples of unsaturated aliphatic hydrocarbon groups include, but are not limited to, the above-mentioned alkenyl groups and alkynyl groups. Aliphatic non-halogenated organic groups are exemplified by, but not limited to, suitable nitrogen-containing groups such as acylamino, imino groups; oxygen-containing groups (such as polyoxyalkylene groups, carbonyl groups, alkoxy groups and hydroxyl groups). Additional organic groups may include sulfur-containing groups, phosphorus-containing groups, and boron-containing groups. Subscript "a" is 0, 1, 2 or 3.

[0098] The siloxy units can be described by shorthand (abbreviated) nomenclature, i.e., "M," "D," "T," and "Q," where R' is as described above, alternatively an alkyl group, typically a methyl group. The M unit corresponds to a siloxy unit, where a = 3, i.e., R'3SiO 1 / 2 ; The D unit corresponds to a siloxy unit, where a = 2, i.e. R'2SiO 2 / 2 ; T unit corresponds to a siloxy unit, where a = 1, i.e. R'1SiO 3 / 2; Q unit corresponds to a siloxy unit, where a = 0, i.e. SiO 4 / 2 Each polyorganosiloxane of component (v) is substantially linear but may contain a certain proportion of branches due to the presence of T units in the molecule (as described previously), so that the average value of a in structure (I) is about 2.

[0099] Examples of typical groups on each polyorganosiloxane of component (v) as described above include at least two unsaturated groups (typically alkenyl groups) selected from alkenyl groups and alkynyl groups per molecule, and having a viscosity within the range described above, mainly including alkenyl, alkynyl and / or alkyl groups, alternatively alkenyl and / or alkyl groups. The group may be in a side position (on a D or T siloxy unit) or may be terminal (on an M siloxy unit).

[0100] Each polyorganosiloxane of component (v) may be selected from polydimethylsiloxanes, alkylmethylpolysiloxanes, alkylarylpolysiloxanes or copolymers thereof containing, for example, alkenyl groups and / or alkynyl groups (wherein the reference to alkyl means any suitable alkyl group, alternatively an alkyl group having two or more carbons), and may have any suitable terminal groups, for example, they may be trialkyl terminated, alkenyldialkyl terminated, alkynyldialkyl terminated or may be terminated with any other suitable combination of terminal groups, provided that each polymer contains at least two unsaturated groups selected from alkenyl groups and alkynyl groups per molecule. In one embodiment, the terminal groups of such polymers do not include any silanol terminal groups.

[0101] Thus, each polyorganosiloxane of component (v) may, for example, be:

[0102] Dialkyl alkenyl terminated polydimethylsiloxanes, such as dimethylvinyl terminated polydimethylsiloxanes; dialkyl alkenyl terminated dimethylmethylphenylsiloxanes, such as dimethylvinyl terminated dimethylmethylphenylsiloxanes; trialkyl terminated dimethylmethylvinyl polysiloxanes; dialkyl vinyl terminated dimethylmethylvinyl polysiloxane copolymers; dialkyl vinyl terminated methylphenyl polysiloxanes, dialkyl alkenyl terminated methylvinylmethylphenylsiloxanes;

[0103] Dialkyl alkenyl terminated methylvinyl diphenyl siloxane; dialkyl alkenyl terminated methylvinyl methylphenyl dimethyl siloxane; trimethyl terminated methylvinyl methylphenyl siloxane; trimethyl terminated methylvinyl diphenyl siloxane; or trimethyl terminated methylvinyl methylphenyl dimethyl siloxane.

[0104] Thus, the adhesion modifier composition for use in the methods herein may comprise:

[0105] (i) Formula Si(OR)3R 1 A trialkoxysilane wherein each R may be the same or different and is an alkyl group having at least two carbon atoms, and each R 1 may be the same or different and are unsaturated groups selected from alkenyl groups or alkynyl groups; the trialkoxysilane is present in an amount of 20 wt.% to 40 wt.% of the composition, alternatively 25 wt.% to 38 wt.% of the adhesion modifier composition, alternatively 25 wt.% to 35 wt.% of the adhesion modifier composition;

[0106] (ii) a platinum group metal-based hydrosilylation reaction catalyst in an amount of 0.1 wt.% to 1.5 wt.% of the composition, alternatively 0.1 wt.% to 1.0 wt.% of the composition, alternatively 0.1 wt.% to 0.5 wt.% of the composition;

[0107] (iii) an alkoxy titanium compound having 2 to 4 alkoxy groups, the alkoxy titanium compound being present in an amount of 1 to 10 wt. %, alternatively 2 wt. % of the composition

[0108] to 8wt.%, alternatively 2wt.% to 7wt.%;

[0109] (iv) Formula Si(OR 2 )4 tetraalkoxysilane, wherein each R 2 The tetraalkoxysilane may be the same or different and each group has at least two carbon atoms, and the tetraalkoxysilane is present in an amount of 5 wt.% to 5 wt.% of the composition.

[0110] 20 wt.%, alternatively 5 wt.% to 15 wt.%, alternatively 7 wt.% to 15 wt.%; and

[0111] (v) any of the following:

[0112] (a') a polyorganosiloxane containing at least two unsaturated groups selected from alkenyl groups and alkynyl groups per molecule and having a relative humidity of 50 mPa.s to 50 mPa.s

[0113] 9000mPa.s; alternatively, 100mPa.s to

[0114] s; alternatively a viscosity in the range of 100 mPa.s to 8000 mPa.s; alternatively a viscosity in the range of 100 mPa.s to 7500 mPa.s; alternatively a viscosity in the range of 100 mPa.s to 7000 mPa.s; alternatively a viscosity in the range of 200 mPa.s to 7000 mPa.s; alternatively a viscosity in the range of 300 mPa.s to 5000 mPa.s; in each case the viscosity is measured using a Brookfield with an RV-4 spindle. TM Viscometer measured at 20 rpm at 25°C; or

[0115] (b') a mixture of two or more polyorganosiloxanes containing at least two unsaturated groups per molecule selected from alkenyl groups and alkynyl groups, the mixture having a viscosity in the range of 50 mPa.s to 9000 mPa.s; alternatively a viscosity in the range of 100 mPa.s to 9000 mPa.s; alternatively a viscosity in the range of 100 mPa.s to 8000 mPa.s; alternatively a viscosity in the range of 100 mPa.s to 7500 mPa.s; alternatively a viscosity in the range of 100 mPa.s to 7000 mPa.s; alternatively a viscosity in the range of 200 mPa.s to 7000 mPa.s; alternatively a viscosity in the range of 300 mPa.s to 5000 mPa.s; in each case the viscosity is measured using a Brookfield 3000 mm thick liquid chromatography (HPLC) with an RV-4 spindle. TM The viscometer was measured at 25°C at 20 rpm;

[0116] Wherein the component (v) is present in an amount of 25 wt.% to 60 wt.% of the composition, alternatively 30 wt.% to 60 wt.% of the composition, alternatively 35 wt.% to 55 wt.% of the composition.

[0117] Any suitable combination of components (i) to (v) may be used with or without additives, but whether or not additives are included, the total wt.% of the composition is 100 wt.%.

[0118] In one embodiment of the disclosure herein, the adhesion modifier composition used in the methods herein may comprise:

[0119] (i) Formula Si(OR)3R 1 A trialkoxysilane wherein each R may be the same or different and is an alkyl group having at least two carbon atoms, and each R 1may be the same or different and are unsaturated groups selected from alkenyl groups or alkynyl groups; the trialkoxysilane is present in an amount of 20 wt.% to 40 wt.% of the composition, alternatively 25 wt.% to 38 wt.% of the adhesion modifier composition, alternatively 25 wt.% to 35 wt.% of the adhesion modifier composition;

[0120] (ii) a platinum group metal-based hydrosilylation reaction catalyst, the platinum group metal-based hydrosilylation reaction catalyst is selected from one or more coordination compounds of platinum, the amount of the platinum group metal-based hydrosilylation reaction catalyst is 0.1 wt.%-1.5 wt.% of the composition, alternatively 0.1 wt.%-1.0 wt.% of the composition, alternatively 0.1 wt.% to 0.5 wt.% of the composition;

[0121] (iii) an alkoxy titanium compound having 2 to 4 alkoxy groups, the alkoxy titanium compound being selected from Ti(OR 3 )4、Ti(OR 3 )3R 4 、Ti(OR 3 )2R 4 2, where each R 4 are the same or different and are selected from an alkyl group, an alkenyl group or an alkynyl group, and each R 3 is selected from an isobutyl group or an n-butyl group, or component (iii) is an ester of titanic acid and an enolate of acetoacetate; the amount of the alkoxytitanium compound is 1 wt.% to 10 wt.%, alternatively 2 wt.% to 8 wt.%, alternatively 2 wt.% to 7 wt.% of the composition;

[0122] (iv) Formula Si(OR 2 )4 tetraalkoxysilane, wherein each R 2 may be the same or different and are alkyl groups, the tetraalkoxysilane being present in an amount of 5 wt.% to 20 wt.%, alternatively 5 wt.% to 15 wt.%, alternatively 7 wt.% to 15 wt.% of the composition; and

[0123] (v) any of the following:

[0124] (a') a polyorganosiloxane containing at least two unsaturated groups per molecule selected from alkenyl groups and alkynyl groups and having a viscosity in the range of 50 mPa.s to 9000 mPa.s; alternatively in the range of 100 mPa.s to 9000 mPa.s; alternatively in the range of 100 mPa.s to 8000 mPa.s; alternatively in the range of 100 mPa.s to 7500 mPa.s; alternatively in the range of 100 mPa.s to 7000 mPa.s; alternatively in the range of 200 mPa.s to 7000 mPa.s; alternatively in the range of 300 mPa.s to 5000 mPa.s; in each case the viscosity is measured using a Brookfield 3000 ft sq. m. with an RV-4 spindle. TM The viscometer was run at 20 rpm at 25°C using a Brookfield with an RV-4 spindle. TM Viscometer measured at 20 rpm at 25°C; or

[0125] (b') a mixture of two or more polyorganosiloxanes containing at least two unsaturated groups per molecule selected from alkenyl groups and alkynyl groups, the mixture having a viscosity in the range of 50 mPa.s to 9000 mPa.s; alternatively a viscosity in the range of 100 mPa.s to 9000 mPa.s; alternatively a viscosity in the range of 100 mPa.s to 8000 mPa.s; alternatively a viscosity in the range of 100 mPa.s to 7500 mPa.s; alternatively a viscosity in the range of 100 mPa.s to 7000 mPa.s; alternatively a viscosity in the range of 200 mPa.s to 7000 mPa.s; alternatively a viscosity in the range of 300 mPa.s to 5000 mPa.s; in each case the viscosity is measured using a Brookfield 3000 ft / s dryer with an RV-4 spindle. TM The viscometer was run at 20 rpm at 25°C using a Brookfield with an RV-4 spindle. TM The viscometer was measured at 25°C at 20 rpm;

[0126] Wherein the component (v) is present in an amount of 25 wt.% to 60 wt.% of the composition, alternatively 30 wt.% to 60 wt.% of the composition, alternatively 35 wt.% to 55 wt.% of the composition.

[0127] Any suitable combination of components (i) to (v) may be used with or without additives, but whether or not additives are included, the total wt.% of the composition is 100 wt.%.

[0128] The adhesion modifier composition used in the methods herein may be uniformly mixed using any suitable mixing device and, for laboratory purposes, the composition may be mixed manually in a container of appropriate size using a spoon or spatula or the like.

[0129] From our point of view, the adhesion regulator composition used in the method of this article is not a primer because its function is different. Standard primers are preparatory coatings applied to the substrate and then dried and / or cured in a basic step before adding the next layer. In the present disclosure, the adhesion regulator composition does not undergo the necessary drying / curing steps to provide improved adhesion between the substrate and the silicone elastomer. In addition, the composition does not contain harmful or toxic solvents designed to evaporate (as part of the drying process). In the method of this article, there is no need to wait for the adhesion regulator layer to dry or cure. In fact, in one embodiment, it is preferred to apply a hydrosilylation-curable silicone rubber composition before the adhesion regulator layer solidifies or cures. This significantly reduces the environmental problems caused by the release of volatile organic compounds (VOCs) usually associated with the use of primers, as well as regulatory issues such as skin contact and food contact applications. Instead, a non-volatile reactive diluent (component (v)) is used. The adhesion regulator as a whole will react and be incorporated into the LSR / composite product.

[0130] Once the adhesion regulator composition is applied to the inorganic substrate, the hydrosilylation-curable silicone rubber composition can be immediately applied on top of the adhesion regulator composition, followed by curing the hydrosilylation-curable silicone rubber composition at a suitable temperature and pressure to form a composite part / article. The fact that no drying step is required has the additional effect of shorter processing time and higher productivity compared to conventional primer solutions.

[0131] Step (c)

[0132] In step (c), the hydrosilylation-curable silicone rubber composition is applied to the substrate treated with the adhesion modifier composition in step (b). Preferably, this can be done immediately upon applying the adhesion modifier composition to the optionally activated substrate. By directly performing this step, the adhesion modifier composition is able to penetrate the surface of the hydrosilylation-curable silicone rubber composition at the inorganic substrate / hydrosilylation-curable silicone rubber composition interface, so that the adhesion modifier composition and the hydrosilylation-curable silicone rubber composition are effectively "cured" together at the surface of the inorganic material during step (d).

[0133] Any suitable hydrosilylation-curable silicone rubber composition may be applied to the inorganic substrate coated with the adhesion modifier composition. A standard hydrosilylation-curable silicone rubber (or LSR) composition for application to an inorganic substrate treated with an adhesion modifier composition may include:

[0134] (I) one or more polyorganosiloxane polymers, for example one or more polydiorganosiloxane polymers having a chemical structure as described in component (v) of the adhesion regulator composition above, the one or more polydiorganosiloxane polymers having a viscosity of 1000 mPa.s to 100,000 mPa.s at 25°C;

[0135] (II) optionally one or more finely divided reinforcing fillers, alternatively in an amount of 5 wt.% of the composition

[0136] to 40 wt.% of one or more finely divided reinforcing fillers;

[0137] (III) an organohydrogenpolysiloxane having at least two, alternatively at least three Si—H groups per molecule;

[0138] (IV) a platinum group metal-based hydrosilylation catalyst, such as the catalyst described above in component (ii) of the adhesion modifier composition; and optionally

[0139] (V) Curing inhibitor.

[0140] Component (I)

[0141] Component (I) of the standard hydrosilylation-curable silicone rubber (or LSR) composition is one or more polyorganosiloxane polymers, for example having a chemical structure as described above in component (v) of the adhesion modifier composition, but having a viscosity of 1000 mPa.s to 100,000 mPa.s at 25° C. measured as previously described. In the case of component (I), the polymer is present in the composition in an amount of 35 wt.% to 85 wt.% of the composition.

[0142] Component (II)

[0143] Component (II) of a standard hydrosilylation-curable silicone rubber (or LSR) composition is one or more reinforcing fillers, which are preferably provided in finely divided form.

[0144] The reinforcing fillers of component (II) can be exemplified by fumed silica and / or precipitated silica (in each case preferably finely divided) and / or suitable silicone resins.

[0145] Precipitated silica, fumed silica and / or colloidal silica are preferred because of their relatively high surface areas (usually at least 50 m 2 / g (BET method according to ISO 9277:2010)), so they are particularly preferred. Typically, materials with a surface area of ​​50 to 450 m2 / g (according to BET method of ISO 9277:2010), alternatively 50 to 300 m 2 / g (BET method according to ISO 9277:2010) of filler. All these types of silica are commercially available.

[0146] When the reinforcing filler (II) is naturally hydrophilic (such as untreated silica filler), it is usually treated with a treating agent to render it hydrophobic. These surface-modified reinforcing fillers (II) do not agglomerate and can be uniformly incorporated into the polydiorganosiloxane polymer (v) described below because the surface treatment makes the filler easily wetted by the polydiorganosiloxane polymer (v).

[0147] In general, the reinforcing filler (II) may be surface treated with any low molecular weight organosilicon compound disclosed in the art to be suitable for preventing wrinkling of the LSR composition during processing, for example, organosilanes, polydiorganosiloxanes or organosilazanes, such as hexaalkyldisilazane, short chain siloxane diols, to render the filler hydrophobic and thus easier to handle and obtain a homogeneous mixture with the other ingredients. Specific examples include, but are not limited to, silanol terminated trifluoropropylmethylsiloxane, silanol terminated vinylmethyl (ViMe) siloxane, silanol terminated methylphenyl (MePh) siloxane, liquid hydroxydimethyl terminated polydiorganosiloxanes containing an average of 2 to 20 repeating units of diorganosiloxane per molecule, hydroxydimethyl terminated phenylmethylsiloxane, hexaorganodisiloxanes such as hexamethyldisiloxane, divinyltetramethyldisiloxane; hexaorganodisilazanes such as hexamethyldisilazane (HMDZ), divinyltetramethyldisilazane and tetramethylbis(trifluoropropyl)disilazane; hydroxydimethyl terminated polydimethylmethylvinylsiloxane, octamethylcyclotetrasiloxane and silanes including, but not limited to, methyltrimethoxysilane, dimethyldimethoxysilane, vinyltrimethoxysilane, methyltriethoxysilane, vinyltriethoxysilane, trimethylchlorosilane, dimethyldichlorosilane, trichloromethylsilane.

[0148] In one embodiment, the treating agent may be selected from silanol terminated vinylmethyl (ViMe) siloxanes, liquid hydroxydimethyl terminated polydiorganosiloxanes containing an average of 2 to 20 diorganosiloxane repeating units per molecule, hexaorganodisiloxanes such as hexamethyldisiloxane, divinyltetramethyldisiloxane; hexaorganodisilazanes such as hexamethyldisilazane (HMDZ), divinyltetramethyldisilazane; and hydroxydimethyl terminated polydimethylmethylvinylsiloxane, octamethylcyclotetrasiloxane and silanes including but not limited to methyltriethoxysilane, dimethyldiethoxysilane and / or vinyltriethoxysilane. A small amount of water may be added along with the silica treating agent as a processing aid.

[0149] The surface treatment of the untreated reinforcing filler (II) can be performed prior to introduction into the composition or in situ (i.e., in the presence of at least a portion of the other ingredients of the composition herein, by blending the ingredients together at room temperature or higher until the filler is completely treated). Typically, the untreated reinforcing filler (II) is treated in situ with a treating agent in the presence of a polydiorganosiloxane polymer (I), which results in the preparation of a silicone rubber matrix material that can subsequently be mixed with the other ingredients.

[0150] Reinforcing filler (II) is optionally present in an amount up to 40 wt.% of the composition, alternatively 1.0 wt.% to 40 wt.% of the composition, alternatively 5.0 wt.% to 35 wt.% of the composition, alternatively 10.0 wt.% to 35 wt.% of the composition.

[0151] Component (III)

[0152] Component (III) of the standard hydrosilylation-curable silicone rubber (or LSR) composition is a crosslinking agent in the form of a polyorganosiloxane containing at least two or three silicon-bonded hydrogen atoms per molecule. Component (III) typically contains three or more silicon-bonded hydrogen atoms, so that the hydrogen atoms can react with the unsaturated alkenyl or alkynyl groups of polymer (I) to form a network structure, and thereby cure the polymer. When polymer (I) has more than two unsubstituted groups per molecule, some or all of component (III) may alternatively have two silicon-bonded hydrogen atoms per molecule.

[0153] The molecular configuration of the polyorganosiloxane containing at least two or three silicon-bonded hydrogen atoms per molecule (III) is not particularly limited, and it may be linear, linear with some branches, cyclic, or silicone resin-based.

[0154] Although the molecular weight of component (III) is not particularly limited, the viscosity is generally 15 mPa.s to 50,000 mPa.s at 25°C, depending on a Brookfield with an LV-4 spindle (designed for viscosities in the range of 1,000 mPa.s to 2,000,000 mPa.s). TM Rotational viscometer or Brookfield with LV-1 spindle (designed for viscosities in the range of 15 mPa.s - 20,000 mPa.s) TM The rotational viscometer is used for viscosities of less than 1000 mPa.s and the speed is adjusted according to the viscosity of the polymer in order to obtain good miscibility with polymer (I).

[0155] The silicon-bonded organic group used in component (III) can be exemplified by: an alkyl group such as methyl, ethyl, propyl, n-butyl, tert-butyl, pentyl, hexyl; a phenyl, tolyl, xylyl or similar aryl group; a 3-chloropropyl, 3,3,3-trifluoropropyl or similar halogenated alkyl group, wherein methyl and phenyl groups are preferred. Preferably, the silicon-bonded organic group used in component (III) is an alkyl group, alternatively a methyl, ethyl or propyl group.

[0156] Examples of polyorganosiloxanes containing at least two or three silicon-bonded hydrogen atoms per molecule of (III) include, but are not limited to:

[0157] (a") trimethylsiloxy-terminated methylhydrogenpolysiloxane,

[0158] (b") trimethylsiloxy-terminated polydimethylsiloxane-methylhydrogensiloxane,

[0159] (c") a dimethylsiloxane-methylhydrogensiloxane copolymer terminated with dimethylhydrogensiloxy groups,

[0160] (d") dimethylsiloxane-methylhydrogensiloxane cyclic copolymer,

[0161] (e") is composed of (CH3)2HSiO 1 / 2 Unit, (CH3)3SiO 1 / 2 Unit and SiO 4 / 2 Unit composed of copolymers and / or silicone resins,

[0162] (f”) is composed of (CH3)2HSiO 1 / 2 Unit and SiO 4 / 2 Unit composed of copolymers and / or silicone resins,

[0163] (g") methylhydrogensiloxane cyclic homopolymers having 3 to 10 silicon atoms per molecule;

[0164] Alternatively, the component B crosslinking agent can be a filler, such as silica treated with one of the above-mentioned materials, and mixtures thereof.

[0165] Component (III) can be exemplified by the following compounds: methylhydrogenpolysiloxane terminated at both molecular ends with trimethylsiloxy groups; copolymers of methylhydrogensiloxane and dimethylsiloxane terminated at both molecular ends with trimethylsiloxy groups; dimethylsiloxane terminated at both molecular ends with dimethylhydrogensiloxy groups; copolymers of methylhydrogensiloxane and dimethylsiloxane terminated at both molecular ends with dimethylhydrogensiloxy groups; copolymers of methylhydrogensiloxane and methylphenylsiloxane terminated at both molecular ends with dimethylphenylsiloxy groups; cyclic methylhydrogenpolysiloxane; (CH3)2HSiO 1 / 2 Siloxane units and SiO 4 / 2 Copolymer composed of (CH3)2HSiO 1 / 2 Siloxane unit, (CH3)3SiO 1 / 2 Siloxane units and SiO 4 / 2 Units, copolymers composed of the aforementioned polyorganosiloxanes, wherein a part or all of the methyl groups are substituted by ethyl, propyl or similar alkyl groups; phenyl, tolyl, or similar aryl groups; 3,3,3,-trifluoropropyl, or similar halogenated alkyl groups; or a mixture of two or more of the aforementioned polyorganosiloxanes. In one embodiment, component (III) is selected from methylhydrogenpolysiloxanes terminated with trimethylsiloxy groups at both molecular ends; copolymers of methylhydrogensiloxane and dimethylsiloxane terminated with trimethylsiloxy groups at both molecular ends; dimethylsiloxane terminated with dimethylhydrogensiloxane at both molecular ends; copolymers of methylhydrogensiloxane and dimethylsiloxane terminated with dimethylhydrogensiloxane at both molecular ends.

[0166] The polyorganosiloxane crosslinker (III) is typically present in the curable silicone elastomer composition such that the molar ratio of the total number of silicon-bonded hydrogen atoms in component (III) to the total number of alkenyl and / or alkynyl groups in polymer (v) is from 0.5:1 to 20:1. When the ratio is less than 0.5:1, a well-cured composition is not obtained. When the ratio exceeds 20:1, there is a tendency for the hardness of the cured composition to increase when heated. Preferably, the amount is such that the ratio of the number of moles of silicon-bonded hydrogen atoms of component (III) to the number of moles of alkenyl groups of component (I) is in the range of 0.7:1.0 to 5.0:1.0, preferably 0.9:1.0 to 2.5:1.0, and most preferably 0.9:1.0 to 2.0:1.0.

[0167] The silicon-bonded hydrogen (Si-H) content of component (III) is determined using quantitative infrared analysis according to ASTM E 168. In this case, when relying on a hydrosilylation cure process, the ratio of silicon-bonded hydrogen to alkenyl (vinyl) and / or alkynyl groups is important.

[0168] Generally, this is determined by calculating the total weight % of alkenyl groups (e.g., vinyl groups) [V] in the composition and the total weight % of silicon-bonded hydrogen [H] in the composition, and assuming that the molecular weight of hydrogen is 1 and the molecular weight of vinyl groups is 27, then the molar ratio of silicon-bonded hydrogen to vinyl groups is 27 [H] / [V].

[0169] Typically, depending on the number of unsaturated groups in component (I) and the number of Si-H groups in component (III), component (III) will be present in an amount of 0.1 wt % to 25 wt % of the LSR composition, alternatively 0.1 wt % to 20 wt % of the LSR composition, alternatively 0.1 wt % to 15 wt % of the LSR composition, and alternatively 0.5 wt % to 10 wt % of the LSR composition.

[0170] Component (IV)

[0171] The component (IV) of standard hydrosilylation curable silicone rubber (or LSR) composition is a hydrosilylation reaction catalyst based on platinum group metals, such as the catalyst described in the component (ii) of the above-mentioned adhesion regulator composition. Alternatively, component (IV) can be a UV-platinum catalyst system. It is usually provided with respect to reactive ingredients, i.e., the weight of components (I) and (III) in an amount of 0.1ppm to 500ppm (parts per million) of platinum atoms. The catalyst can be added as a single substance or as a mixture of two or more different substances. Typically, according to the form / concentration of providing the catalyst, the amount of the catalyst present will be in the range of 0.05wt.%-1.5wt.% of the composition, alternatively 0.05wt.%-1.0wt.%, alternatively 0.1wt.%-1.0wt.%, alternatively 0.1wt.% to 0.5wt.% of the composition, wherein the platinum catalyst is provided in a masterbatch of a polymer (such as (I) and (v) as described above).

[0172] In one embodiment, the hydrosilylation catalyst is a coordination compound of platinum and the final composite contains up to 50 mg platinum / kg, typically the cumulative total amount of platinum present in the above-mentioned adhesion modifier and silicone rubber material applied to the inorganic substrate, the amount of adhesion modifier herein.

[0173] Component (V)

[0174] The component (V) of standard hydrosilane addition curing silicone rubber (or LSR) composition is one or more optional curing inhibitors. When needed, curing inhibitor is used to prevent or delay the addition reaction curing process, especially during storage. The optional addition reaction inhibitor based on the catalyst of platinum is well known in the art and includes hydrazine, triazole, phosphine, mercaptan, organic nitrogen compound, alkynol, methane silylation alkynol, maleate, fumarate, ethylenic or aromatic unsaturated amide, ethylenic unsaturated isocyanate, olefinic siloxane, unsaturated hydrocarbon monoester and diester, conjugated alkene-alkynes, hydroperoxide, nitrile and diaziridine. The siloxane substituted with alkenyl as described in US3989667 can be used, wherein preferred cyclic methyl vinyl siloxane.

[0175] One class of known hydrosilylation reaction inhibitors are the acetylenic compounds disclosed in US 3445420. Alkynols such as 2-methyl-3-butyn-2-ol constitute a class of preferred inhibitors which will inhibit the activity of platinum-containing catalysts at 25° C. Compositions containing these inhibitors generally require heating at temperatures of 70° C. or above in order to cure at an achievable rate.

[0176] Examples of alkynols and their derivatives include 1-ethynyl-1-cyclohexanol (ETCH), 2-methyl-3-butyn-2-ol, 3-butyn-1-ol, 3-butyn-2-ol, propargyl alcohol, 1-phenyl-2-propyn-1-ol, 3,5-dimethyl-1-hexyn-3-ol, 1-ethynylcyclopentanol, 3-methyl-1-pentene-4-yn-3-ol, and mixtures thereof. Alkynol derivatives may include those compounds having at least one silicon atom.

[0177] When present, inhibitor concentrations as low as 1 mole inhibitor per mole of catalyst metal will in some cases impart satisfactory storage stability and cure rates. In other cases, inhibitor concentrations of up to 500 moles inhibitor per mole of catalyst metal are required. The optimum concentration of a given inhibitor in a given composition is readily determined by routine experimentation. When present in the composition, the inhibitor is typically present in an amount of 0.0125% to 10% by weight of the composition, depending on the concentration and form in which the selected inhibitor is provided / commercially available.

[0178] In one embodiment, when present, the inhibitor is selected from 1-ethynyl-1-cyclohexanol (ETCH) and / or 2-methyl-3-butyn-2-ol and is present in an amount from greater than zero to 0.1% by weight of the composition.

[0179] Depending on the intended use, such compositions may also contain one or more optional additives. Examples include release agents, non-reinforcing fillers, adhesion catalysts, peroxides, pigments, conductive fillers, thermally conductive fillers, pot life extenders, flame retardants, lubricants, release agents, UV stabilizers, bactericides, wetting agents, heat stabilizers, compression set additives and plasticizers, etc. In one embodiment, the composition does not contain optional additives other than the above-mentioned component (V).

[0180] The above hydrosilylation-curable silicone rubber composition is usually stored in two or more parts before use. In the case of a two-part composition, the two parts are usually referred to as part (A) and part (B):

[0181] In addition to the polyorganosiloxane (I) and the filler (II) (when present), part (A) generally contains a catalyst (IV), and

[0182] Part (B) generally comprises component (III) and, when present, component (V) the inhibitor and the remainder of the polyorganosiloxane (I) and / or filler (II).

[0183] It is important to store the catalyst (IV) separately from the crosslinker (III) to prevent premature curing during storage.

[0184] Any optional additives may be in either part (A) or part (B) or in both parts, provided that they do not adversely affect the storage of any essential ingredients present in the respective parts.

[0185] Various hydrosilylation-curable silicone compositions that can be used in the methods herein are commercially available. For example, these include Silastic TM RBL-9200-20(-70)LSR; Xiameter TM RBL 2004-20(-75)LSR; Silastic TM NPC 9300-40 / -50 / -70LSR; Silastic TM LTC 9400-40 / -50 LSR and Silastic TM 3D3335 LSR, all available from Dow Silicones Corporation of Midland, Michigan. Other hydrosilylation-curable silicone compositions that can be used in the methods herein include moldable silicones such as those described in US 8,691,910 B2, US 8,853,332 B2, and US 8,859,693 B2.

[0186] The uniform mixing of the components of the hydrosilylation-curable silicone rubber composition used herein can be carried out using a suitable mixing device, such as a kneader mixer, a static mixer in a liquid injection molding machine, a Z-blade mixer, a two-roll mill (open mill), a three-roll mill, a Haake TM Rheomix OS Lab mixer, screw extruder or twin-screw extruder etc. High-speed mixers as sold, for example, by Hauschild as DC 150.1 FV, DAC 400 FVZ or DAC 600 FVZ may alternatively be used.

[0187] After the inorganic substrate material is coated with the adhesion regulator composition in step (b), the silicone rubber composition that can be cured by silanization is applied to the surface of the inorganic substrate in step (c). The silicone rubber composition that can be cured by silanization can be applied by any suitable means, such as roller coating, spreading, 3-D printing, etc. Therefore, the silicone rubber composition that can be cured by silanization used in the method described herein can be applied to the treated inorganic substrate and solidified by any suitable means, such as by injection molding, using, for example, 2K type injection molding, compression molding, extrusion molding, transfer molding, pressurization vulcanization or calendering. In one embodiment, a 2K type injection molding unit is used to prepare a composite material by injection molding. After the inorganic substrate material is coated with the adhesion regulator composition, the silicone rubber composition that can be cured by silanization as described above can be applied to the surface of the inorganic substrate.

[0188] In the case of using a 3-D printing method, a typical method for forming a three-dimensional (3-D) product may include multiple steps. For example, after applying the adhesion modifier composition to the surface of the inorganic substrate, the method may include (i) printing a first hydrosilane curable silicone rubber composition with a 3-D printer to form a layer on top of the treated inorganic substrate. The method may also include (ii) heating the layer to form an at least partially cured layer. In addition, the method may include (iii) printing a second heat-curable silicone composition on the at least partially cured layer with a 3-D printer to form a subsequent layer. The method may also include (iv) heating the subsequent layer to form an at least partially cured subsequent layer. Optionally, steps iii) and iv) can be repeated to form a 3-D composite product by independently selecting a hydrosilane curable silicone rubber composition for any additional layer. If desired, the inorganic substrate may be cleaned and / or activated or partially activated before step (i) (for example, only the unmasked area is activated due to masking of the portion of the inorganic substrate surface).

[0189] Thus, in one embodiment of the method defined above, step (c) of the method may be performed by 3-D printing the hydrosilylation-curable silicone rubber composition onto an inorganic substrate surface (e.g., an inorganic substrate surface previously treated with the adhesion modifier composition described herein). In this case, steps (c) and (d) may be as follows:

[0190] printing the first hydrosilylation-curable silicone rubber composition as described above with a 3-D printer to form a layer on the optionally cleaned and / or activated inorganic substrate treated with the adhesion regulator composition obtained from steps (a) and (b);

[0191] i heating the layer to form an at least partially cured layer;

[0192] ii. Printing the second hydrosilylation-curable silicone rubber composition on at least

[0193] on the partially cured layer to form a subsequent layer;

[0194] iii. heating the subsequent layer to form an at least partially cured subsequent layer; and

[0195] iv. Optionally, re-coating with an independently selected heat-curable silicone composition for any additional layers

[0196] Steps iii) and iv) are repeated to form a 3-D article.

[0197] Step (d)

[0198] Finally, in step (d), the hydrosilylation-curable silicone rubber composition is cured at a temperature of 80°C to 190°C, or 100°C to 180°C, or 100°C to 170°C, or 110°C to 170°C, or 110°C to 160°C.

[0199] The curing of the hydrosilylation-curable silicone rubber composition on the inorganic substrate can be carried out in any suitable manner, which may depend on the manner in which the hydrosilylation-curable silicone rubber composition is applied in step (c). For example, curing can be carried out in a mold to form a molded composite part / wherein the silicone elastomer produced by the curing process adheres to the inorganic substrate. In the case of such an inorganic substrate, the hydrosilylation-curable silicone rubber composition used herein can be injection molded to form an article adhered to the inorganic material, for example, after coating the inorganic material with the adhesion modifier composition, or the composition can be overmolded by injection molding around such an inorganic substrate or article or on an inorganic substrate after coating the inorganic material with the adhesion modifier composition.

[0200] When cured in the presence of a heat-sensitive inorganic substrate, the hydrosilylation-curable silicone rubber composition as described above can be cured under such conditions as to form a mechanical bond with the heat-sensitive inorganic substrate or the like, and more specifically, by using a temperature and a curing time at which the heat-sensitive inorganic substrate does not deform, melt or denature.

[0201] Also provided is an article or a composite part of an article obtained or obtainable by the above method.

[0202] In one embodiment herein, there is provided an article or composite part comprised of a silicone elastomer cured from a hydrosilylation-curable silicone rubber composition on a rigid or flexible inorganic substrate (e.g., of the type described above), provided that the rigid or flexible substrate is coated with a layer of an adhesion modifier composition in step (b) of the method prior to applying the hydrosilylation-curable silicone rubber composition in step (c) of the method.

[0203] In all of the above cases, examples of such articles or composite parts can be found in a variety of industries, including but not limited to automotive applications, industrial applications, electronic applications, and consumer applications, such as packaging, storage, handling, production, preparation, processing, consumption, and molding of food and beverage products for human consumption, provided that they meet the necessary regulations, such as for use in household products, food contact, dishwasher compatibility, or beverage / fluid compliance (e.g., hot water, coffee, tea contact in machines). In automotive applications, this may include housings, plugs and connectors with silicone seals or gaskets, parts of various sensors, membranes, diaphragms, climate vent parts, etc. Electronic applications may include mobile phone cover seals, mobile phone accessories, precision electronic devices, electronic switches and switch covers, watches and wristbands, wearable devices (e.g., masks), wearable electronic devices, etc.

[0204] The composite parts can also be selected from the following parts: mobile phones, mobile communication devices, game consoles, clocks, image receivers, DVD devices, MD (Mini Disk) devices, CD devices, and other precision electronic devices, thin displays of TV, LCD TV and plasma TV, various household appliances, copiers, printers, fax machines and other office equipment, connector seals, spark plug caps, various sensor parts, and other automotive parts.

[0205] Composite articles and / or parts containing or consisting of silicone rubber and inorganic materials used in the transportation, packaging, storage, handling, production, preparation, processing, consumption and molding of household products and / or food and beverage products for human consumption may include machine parts for the production, preparation, forming and processing of food, baking utensils such as baking molds, kitchen equipment and / or food and beverage processing equipment such as beverage makers, kettles, tableware, crockery, cooking utensils, drinking containers (including bottles for babies), other types of containers, trays, food molds, and parts in ovens (including microwave ovens), refrigerators, bread machines, rice cookers and / or dishwashers, as well as containers for transportation and materials that come into contact with water intended for human consumption, etc. Example

[0206] In the following examples, unless otherwise stated, all viscosities are at 25°C using a Brookfield 1000 with an RV-4 spindle (for viscosities less than 10,000 mPa.s). TM The rotational viscometer measures at a speed of 20 rpm in each case.

[0207] Each cleaned and / or activated substrate was coated with a layer of the adhesion regulator composition as described above or the comparative coating composition as indicated in the corresponding table using a pipette to apply the adhesion regulator composition or the comparative coating composition as indicated in the corresponding table and then wiping the composition on the substrate surface to provide a continuous layer of the composition on the substrate. The substrate coated with the adhesion regulator (Example 1-1 composition) was then coated with a 2-3 mm layer of liquid silicone rubber (LSR) and cured at 120° C. for 15 minutes.

[0208] Several examples of adhesion modifiers useful herein were prepared and their compositions are disclosed in Tables 1a and 1b below:

[0209] Table 1a: Adhesion regulator compositions of Ex. 1-1 to 1-4 (wt.%)

[0210] Ex.1-1 Ex.1-2 Ex.1-3 Ex.1-4 Vinyltriethoxysilane 32.18 0 0 32.27 Allyltriethoxysilane 0 32.18 0 0 Hexenyltriethoxysilane 0 0 31.70 0 Karstedt Catalyst 0.65 0.65 0.65 0.65 Tetra-tert-butyl titanate 5.33 5.33 5.37 5.35 Tetraethoxysilane 11.17 11.17 11.25 0 Tetrapropoxysilane 0 0 0 10.91 Polymer 1 50.67 50.67 51.04 50.82

[0211] Polymer 1 is a vinyl dimethyl terminated polydimethylsiloxane having a viscosity of about 450 mPa.s at 25°C and a vinyl content of 0.46 wt.% vinyl (Vi) content.

[0212] The Karstedt catalyst was provided in a polymer 1 masterbatch.

[0213] Table 1b: Adhesion regulator compositions of Ex. 1-5 to 1-9 (wt.%)

[0214] Ex.1-5 Ex.1-6 Ex.1-7 Ex.1-8 Ex.1-9 Vinyltriethoxysilane 32.18 32.18 32.18 32.18 32.01 Karstedt Catalyst 0.32 0.16 0.32 0.32 0.65 Tetra-tert-butyl titanate 5.33 5.33 5.33 5.33 0 Tetrabutyl titanate 0 0 0 0 5.85 Tetraethoxysilane 11.17 11.17 11.17 11.17 11.11 Polymer 1 51.00 51.16 0 0 50.39 Polymer 2 0 0 51.00 0 0 Polymer 3 0 0 0 51.00 0

[0215] In Table 1b, in Ex. 1-7 and 1-8:

[0216] Polymer 2 is a 1:1 ratio (by weight) mixture of two vinyl dimethyl terminated polydimethylsiloxanes having viscosities of approximately 450 mPa.s and 2000 mPa.s at 25°C, respectively, and an average vinyl content of 0.34 wt.% vinyl (Vi). The viscosity of the mixture is 1190 mPa.s;

[0217] Polymer 3 is a 1:1 mixture of two vinyl dimethyl terminated polydimethylsiloxanes having viscosities of approximately 450 mPa.s and 9000 mPa.s at 25°C, respectively, and an average vinyl content of 0.28 wt.% Vi. ​​The viscosity of the mixture is 2440 mPa.s; and

[0218] When polymer 2 replaces polymer 1, the Karstedt catalyst is provided in the polymer 2 masterbatch, and likewise when polymer 3 replaces polymer 1, the Karstedt catalyst is provided in the polymer 3 masterbatch.

[0219] Work Example

[0220] In the working examples, adhesion modifiers as described in Ex. 1-9 in Table 1b were used to evaluate their ability to help LSR1 (Silastic TM 3D 3335 LSR) has the ability to bond to a range of inorganic substrates. TM 3D 3335 LS is commercially available from Dow Silicones Corporation (Midland, Michigan, USA).

[0221] The substrates used were several commercial test panels purchased from Rocholl GmbH of Eschelbronn, Germany.

[0222] The test plate substrates used, including their dimensions, were glass (60×25×4 mm 3 ); 6061T6 aluminum alloy (60×25×2mm 3 ); SF-Cu F24 copper (60×25×1mm 3 );DX51 D+Z275 hot dip galvanized steel (60×25×1mm 3 ) and DC04 steel (60×25×1mm 3 )

[0223] The different inorganic substrates were first cleaned with isopropyl alcohol. Usually, the isopropyl alcohol evaporates immediately, but the substrates were left at room temperature for about 10 minutes to dry before use.

[0224] Then use two test plates of each substrate.Use pipette to coat the first test plate of each test plate with adhesion regulator composition (e.g., 2-1 composition), and then wipe the composition on the substrate surface to provide a continuous layer thereon.Each of the second test plate is not coated with adhesion regulator.Then coat both the first and second test plates with a 2-3mm LSR layer, and then cure at 120°C for 15 minutes to form a test plate composite.The resulting test plate composite is stored for at least 24 hours before testing adhesion.Each composite test plate is qualitatively tested by trying to pull LSR off the test plate by hand.

[0225] Table 2: Adhesion modifier composition applied and not applied to the surface of the test plate. Adhesion of inorganic test panels .

[0226] Test Board Adhesion after application of adhesion modifier Bonding without application of adhesion modifier Glass good Difference aluminum good Difference copper good Difference Galvanized Steel good Difference steel good Difference

[0227] In each case, it was found that in the case where the adhesion regulator was applied to the surface of the test plate (marked as "good" in Table 2), the silicone rubber layer was inseparable from the test plate, and in each case where the silicone rubber was applied to the surface of the test plate without prior treatment with the adhesion regulator, the adhesion was proved to be "poor", which means that the silicone rubber layer was easily peeled off from the surface of the test plate.

Claims

1. A method for preparing a composite material of a silicone elastomer and an inorganic substrate, the method The following steps are involved: (a) optionally cleaning and / or activating the surface of an inorganic substrate; (b) treating the optionally cleaned and / or activated inorganic substrate surface with an adhesion regulator composition; (c) applying a hydrosilylation-curable silicone rubber composition to the treated surface obtained in step (b); (d) curing the hydrosilylation-curable silicone rubber composition, It is characterized in that the adhesion regulator composition comprises: (i) Formula Si(OR) 3 R 1 Trialkoxysilane, wherein each R may be the same or different and is an alkyl group having at least two carbon atoms per radical, and each R 1 The unsaturated The trialkoxysilane is present in an amount of 20 wt.% to 45 wt.% of the adhesion regulator composition; (ii) a platinum group metal-based hydrosilylation catalyst, wherein the platinum group metal is present in the form of The adhesion regulator composition is present in an amount of 0.1wt.%-1.5wt.%; (iii) an alkoxy titanium compound having 2 to 4 alkoxy groups The amount of the alkoxy titanium compound is the adhesion regulator combination 1wt.% to 10wt.% of the substance; (iv) Formula Si(OR 2 ) 4 A tetraalkoxysilane, wherein each R 2 Can be the same or different and is an alkyl group having at least two carbon atoms per group, the tetraalkoxy The amount of the silane is 5 wt.% to 20 wt.% of the adhesion regulator composition; and (v) any of the following: (a') a polyorganosiloxane containing at least two unsaturated groups selected from alkenyl groups and alkynyl groups per molecule and prepared using a Brookfield having an RV-4 spindle TM The viscometer has a viscosity in the range of 50 mPa.s to 9000 mPa.s at 25°C at 20 rpm; or (b') a mixture of two or more polyorganosiloxanes containing at least two unsaturated groups selected from alkenyl groups and alkynyl groups per molecule, the mixture being prepared using a Brookfield 1000 having an RV-4 spindle TM The viscometer has a viscosity in the range of 50 mPa.s to 9000 mPa.s at 25°C at 20 rpm; Wherein the component (v) is present in an amount of 25 wt.% to 60 wt.% of the adhesion regulator composition.

2. The method for preparing a composite material of a silicone elastomer and an inorganic substrate according to claim 1, wherein the surface of the inorganic substrate is cleaned and / or activated by one of plasma treatment, corona discharge treatment, UV-C / ozone or vacuum-UV irradiation, flame pyrolytic deposition of amorphous silica or flame treatment.

3. The method for preparing a composite material of a silicone elastomer and an inorganic substrate according to claim 1, wherein steps (c) and / or (d) involve injection molding or 3-D printing.

4. A process for preparing a composite material of a silicone elastomer and an inorganic substrate according to any preceding claim, wherein the inorganic substrate is selected from a metal, a metal alloy, a glass or a ceramic material.

5. A process for preparing a composite material of a silicone elastomer and an inorganic substrate according to any preceding claim, wherein component (i) of the adhesion modifier composition has the formula Si(OR) 3 R 1 , wherein each R may be the same or different and is selected from ethyl, propyl, n-butyl, isobutyl or tert-butyl, and each R 1 are alkenyl groups which may be identical or different and are selected from ethenyl, propenyl, n-butenyl, pentenyl or hexenyl.

6. A process for preparing a composite of a silicone elastomer and an inorganic substrate according to any preceding claim, wherein component (ii) of the adhesion regulator composition is one or more coordination compounds of platinum.

7. A process for preparing a composite material of a silicone elastomer and an inorganic substrate according to any preceding claim, wherein component (iii) is one or more of the formula Ti(OR 3 ) 4 、Ti(OR 3 ) 3 R 4 、Ti(OR 3 ) 2 R 4 2 Alkoxytitanium compounds or chelated alkoxytitanium molecules, wherein R 3 is a straight or branched chain alkyl group having 1 to 20 carbons, and when present, R 4 is an organic group such as an alkyl group having 1 to 10 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an alkynyl group having 2 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms or an aromatic group having 6 to 20 carbon atoms, or a mixture thereof.

8. The method for preparing a composite material of a silicone elastomer and an inorganic substrate according to claim 7, wherein component (iii) is selected from the group consisting of Ti(OR 3 ) 4 、Ti(OR 3 ) 3 R 4 、Ti(OR 3 ) 2 R 4 2 titanate, wherein each R 3 is an isobutyl group, a tert-butyl group or an n-butyl group, or component (iii) is an ester of an enolate of titanic acid and acetoacetate.

9. A process for preparing a composite material of a silicone elastomer and an inorganic substrate according to any preceding claim, wherein component (iv) is of the formula Si(OR 2 ) 4 A tetraalkoxysilane, wherein each R 2 Selected from ethyl, propyl, isopropyl, n-butyl, isobutyl, tert-butyl, pentyl or hexyl.

10. A method for preparing a composite of a silicone elastomer and an inorganic substrate according to any preceding claim, wherein the hydrosilylation-curable silicone rubber composition is applied in step (c) before the adhesion regulator layer applied in step (b) is cured or solidified.

11. A composite article or component obtained or obtainable by the method according to any one of claims 1 to 10.

12. The composite product or component according to claim 11, wherein the composite product or component has a weight of 100 g / kg. Contains up to 50 mg platinum.

13. A composite article or part according to claim 11 or 12, wherein the silicone elastomer and inorganic composite material is used for transportation, packaging, storage, handling, production, preparation, processing and consumption applications and / or molding of household products and / or food and beverage products for human consumption.

14. Use of an adhesion regulator composition in a method for preparing a composite material of a silicone elastomer and an inorganic substrate according to any one of claims 1 to 10, the adhesion regulator composition comprising: (i) Formula Si(OR) 3 R 1 A trialkoxysilane wherein each R may be the same or different and is an alkyl group having at least two carbon atoms, and each R 1 may be the same or different and are unsaturated groups selected from alkenyl groups or alkynyl groups; the trialkoxysilane is present in an amount of 20 wt.% to 45 wt.% of the adhesion regulator composition; (ii) a platinum group metal-based hydrosilylation catalyst, wherein the platinum group metal is present in an amount of 0.1 wt.% to 1.5 wt.% of the adhesion modifier composition; (iii) an alkoxy titanium compound having 2 to 4 alkoxy groups, the alkoxy titanium compound being present in an amount of 1 wt.% to 10 wt.% of the adhesion regulator composition; (iv) Formula Si(OR 2 ) 4 A tetraalkoxysilane, wherein each R 2 may be the same or different and are alkyl groups having at least two carbons per group, the tetraalkoxysilane being present in an amount of 5 wt.% to 20 wt.% of the adhesion modifier composition; and (v) any of the following: (a') a polyorganosiloxane containing at least two unsaturated groups selected from alkenyl groups and alkynyl groups per molecule and prepared using a Brookfield having an RV-4 spindle TM The viscometer has a viscosity in the range of 50 mPa.s to 9000 mPa.s at 25°C at 20 rpm; or (b') a mixture of two or more polyorganosiloxanes containing at least two unsaturated groups selected from alkenyl groups and alkynyl groups per molecule, the mixture being prepared using a Brookfield 1000 having an RV-4 spindle TM The viscometer has a viscosity in the range of 50 mPa.s to 9000 mPa.s at 25°C at 20 rpm; Wherein the component (v) is present in an amount of 25 wt.% to 60 wt.% of the adhesion regulator composition.

15. Use according to claim 14, wherein the silicone elastomer and inorganic composite material is used for transportation, packaging, storage, handling, production, preparation, processing, consumption and molding of household products and / or food and beverage products for human consumption.

Citation Information

Patent Citations

  • Self-adhesive silicone elastomers

    CN103068926A

  • Binding agent composition, useful in the production of metal silicon elastomer groups, comprises a metallic compound, a hydroxylation catalyst and an organic solvent

    DE102004024696A1

  • Low temperature cure silicone elastomer

    US20190040204A1

  • Primer compositions

    US5985371A