Process for converting lignocellulosic material to organic liquefaction products

Through the hydrogenation liquefaction method of amorphous unsupported molybdenum sulfide catalyst and lignocellulose, the stability and oxygen content of bio-oil are solved, low-temperature conversion and efficient upgrade are achieved, and are suitable for use in refineries.

CN118922516APending Publication Date: 2024-11-08NESTE OYJ
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202380028429.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-17
Filing Date
2023-03-17
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

When the existing thermochemical methods convert solid lignocellulose into bio-oil, there are problems such as high oxygen content, spontaneous reactivity, carbon formation, loss of volatile organic components and high moisture content, resulting in unstable products and difficult to upgrade to Hydrocarbon fuels affect storage and heating safety.

Method used

Amorphous and unsupported molybdenum sulfide catalyst is used to mix with lignocellulose starting material, subject to hydrogen, elevated pressure and temperature conditions of 270°C to 450°C, to produce organic liquefied products with low oxygen content, avoiding the use of hydrogen donor solvents For example, tetrahydronaphthalene, co-feeds such as alkanes are used to improve conversion and stability.

Benefits of technology

It realizes the conversion of lignocellulose into organic liquefied products at low temperatures, reducing energy consumption, improving product stability and reducing oxygen content, which is suitable for further upgrading to hydrocarbon fuel, reducing the corrosion risk to refinery equipment, and improving the Thermal stability of intermediate products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922516A_ABST
    Figure CN118922516A_ABST
Patent Text Reader

Abstract

Lignocellulosic starting material can be converted into one or more liquid and / or aqueous phases and hydrocarbon phases in a process by subjecting a mixture of lignocellulosic starting material, an amorphous and unsupported molybdenum sulfide catalyst, and a co-feed to not less than a stoichiometric amount of hydrogen, the catalyst comprises an amorphous and unsupported molybdenum sulfide catalyst comprising one or more of the following elements: iron (Fe), tungsten (W), cobalt (Co), vanadium (V), and ruthenium (Ru), an elevated pressure, and a temperature in the range of 270 DEG C to 450 DEG C. Also disclosed are novel catalysts for use in the process and methods of making the same.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to novel processes for converting solid lignocellulosic feedstocks into organic liquefied products, novel molybdenum sulfide catalysts for use in the processes, and methods for producing the catalysts. Background Art

[0002] It is well known that thermochemical processes, such as pyrolysis and hydrothermal liquefaction (HTL), can depolymerize whole lignocellulosic biomass as well as lignocellulosic biomass fractions, such as kraft lignin and other renewable side streams, from agriculture, forestry and the paper and pulp industry, typically producing liquefied products collectively referred to as “bio-oil” or “bio-crude.” These liquefied products can then be further upgraded using hydrotreating and hydrocracking technologies, which are more or less similar to those used in refineries to upgrade fossil crude oils and their distillates to obtain hydrocarbon mixtures that can be used, for example, as components of transportation fuels.

[0003] Problems frequently encountered in the thermochemical liquefaction (pyrolysis or HTL) of biomass include, for example, relatively high oxygen contents and the spontaneously reactive nature of the resulting depolymerization product mixtures, wherein these depolymerization product mixtures contain, in particular, reactive phenolic derivatives in combination with aldehydes and ketones, other molecules of different structural classes, which together together give rise to more or less severe repolymerization during storage and / or heating. Other problems are, for example, char formation and losses of highly volatile organic components, ultimately leading to lower than desired carbon yields of hydrocarbon fuel components after upgrading.

[0004] An example of other problems is the high water content in the resulting product. In addition, due to the polar nature of many organic components in bio-oil, it is generally difficult or impossible to remove water by phase separation. Due to the above-mentioned repolymerization problem, during the heating process, water removal by distillation is excluded due to lack of stability. In addition, the high water content combined with the acidic nature of bio-oil leads to a situation where bio-oil is highly corrosive to standard construction materials used in refinery upgrading equipment. Using data as an example, the pyrolytic degradation of lignocellulosic materials results in an oxygen content in the condensable fraction in the range of 20%->40%. Due to the high content of carboxylic acids and water, the pH value of the aforementioned condensable fraction is generally about 2-3. Overall, this means that the total oxygen content and water content are not significantly lower than more stable undepolymerized, dried but not otherwise treated, and significantly lower acidic lignocellulosic biomass.

[0005] In summary, although the goal of obtaining pumpable liquid bio-oil is generally achieved, the bio-oil or bio-crude products produced by pyrolysis or HTL are corrosive and unstable to storage and heating due to problems of spontaneous repolymerization. In addition, these products show poor miscibility or immiscibility with fossil feedstocks or other renewable feedstocks of interest for easy and flexible co-processing in current standard refinery infrastructure. These properties are obviously problematic when developing practical and robust full-scale processes for upgrading pyrolysis and / or HTL bio-oils, either alone or by co-processing, to hydrocarbon transportation fuels and chemicals.

[0006] With regard to hydrocracking catalysts that can be used to upgrade fully and / or partially renewable feedstocks and feedstock mixtures, a large number of different base metal and noble metal catalysts are disclosed in the literature, which have been more or less successfully used to upgrade bio-oils or other materials derived from lignocellulose to hydrocarbon-rich product mixtures. These catalysts can be based on a single metal or a combination of different metals or metal compounds, which may or may not be supported on a chemically inert or reactive support material.

[0007] In short, a simple and robust process that is improved is needed, which can be applied to lignocellulosic raw materials and is suitable for upgrading. From the following description of the summary of the invention and the specific embodiments, these and other purposes will be more easily understood. It will be appreciated by those skilled in the art that one or more aspects can meet some purposes, while one or more other aspects can meet other purposes. Summary of the invention

[0008] The present disclosure provides a new hydroliquefaction method and a new catalyst for the method, as well as a method for preparing the catalyst. According to a first aspect, a method for converting a lignocellulosic starting material into an organic liquefied product is characterized in that a lignocellulosic starting material, optionally from a single source or from a mixture of related starting materials, an amorphous and unsupported molybdenum sulfide catalyst and a co-feed are mixed and subjected to a stoichiometric amount of hydrogen, an elevated pressure and a temperature in the range of 270°C to 450°C to produce an organic liquefied product.

[0009] The method according to the present disclosure is a hydroliquefaction method, which converts lignocellulosic biomass from a solid phase into an organic liquefied product, which can be subsequently converted into fuel or used in the production of chemicals. The method according to the present disclosure has the advantage that it can be carried out at surprisingly low temperatures, thus having advantages in reducing energy consumption, thereby generating potential cost benefits.

[0010] Another advantage is that the organic liquefied product, which may be an intermediate product intended for further conversion into one or more final products, has a low oxygen content, which makes the organic liquefied product a more thermally stable intermediate product and stable for storage.

[0011] In the prior art of lignocellulose hydroliquefaction, the typical carrier oil is a hydrogen donor solvent such as tetralin.

[0012] Compared to the prior art using CoMo catalysts to liquefy biomass (reference: Burton et al 1986, "Catalytic Hydroliquefaction of Lignocellulosic Biomass", International Journal of Solar Energy), the process of the present invention does not require the use of a hydrogen donor solvent, such as tetralin, as a co-feed, but the co-feed may be, for example, a paraffin. Another advantage of the present process compared to the prior art is that the process is carried out at a high solid lignocellulose content. Yet another advantage is that the organic liquefaction product has a better quality than, for example, the product of Burton et al. (whose process yields a large amount of asphaltenes).

[0013] Thus, the co-feed may include a co-feed other than tetralin.

[0014] The co-feed may alternatively be substantially free of tetralin, i.e. at least 99% of the co-feed is free of tetralin or at least 99.5% of the co-feed is free of tetralin. When the co-feed is substantially free of tetralin, this means that tetralin is not added as a co-feed during the method, but a small amount of tetralin residue may be formed during the method. Alternatively, the co-feed is free of tetralin. The fact that the method can be carried out with a co-feed substantially free of or free of tetralin enables the use of cheaper, conventional and easily available refinery feedstocks or the use of recycled products or fractions of products, thereby providing flexibility for the selection of the co-feed, because the co-feed does not need to have a strong hydrogen supply capacity to obtain a high conversion of the solid lignocellulose starting material.

[0015] The liquid phase additionally exhibits improved physical properties, providing process benefits in subsequent process steps, such as during pumping. In addition, due to its low oxygen content, the intermediate liquid product obtained can also be more easily integrated as a feedstock into conventional refineries.

[0016] Another advantage is that the low oxygen content in the organic liquefied product obtained by the process according to the present disclosure enables a reduced exotherm during complete hydrodeoxygenation to form hydrocarbon end products.

[0017] The term "elevated pressure" refers to pressure above atmospheric pressure.

[0018] The molar fraction of sulfur (S) relative to the molybdenum (Mo) content in the amorphous and unsupported molybdenum sulfide catalyst may range from 0.1 to 2.3. The present inventors have surprisingly found that the catalysts disclosed herein are capable of liquefying lignocellulosic starting materials with high yields.

[0019] The molar fraction of sulfur (S) in the amorphous and non-supported sulfided molybdenum catalyst relative to the molar fraction of molybdenum (Mo) may be in the range of 0.1 to 1.0. In an embodiment, the content of sulfur (S) is in the range of 0.3 to 0.99, for example, in the range of 0.5 to 0.95.

[0020] The molar fraction of the one or more elements: iron (Fe), tungsten (W), cobalt (Co), vanadium (V) and ruthenium (Ru) in the amorphous and non-supported molybdenum sulfide catalyst relative to the molar fraction of molybdenum (Mo) may be in the range of 0.1 to 0.3, optionally in the range of 0.1 to 0.2.

[0021] An important advantage of the catalyst being an unsupported catalyst without a carrier is that it can be added at different stages of the process, for example after the starting materials have been ground and thereby intimately mixed with the starting materials.

[0022] Preferably, the catalyst is introduced into the mixture of lignocellulosic starting material in the form of a slurry of catalyst particles in a liquid co-feed, optionally a pure liquid co-feed which is a pure liquid or a mixture of different liquid components.The liquid co-feed may be a hydrocarbon co-feed.

[0023] The co-feed may be selected from: vegetable oils and fats, such as tall oil and tall oil pitch; pyrolysis oils; HTL oils; animal fats; fatty acids; fossil or renewable liquid hydrocarbons; and / or recycled or recovered products or fractions of products obtained in the process.

[0024] In an exemplary embodiment, the co-feed is a mixture of vegetable oils and / or animal fats, and fossil or renewable hydrocarbons.

[0025] The total feed may consist of 5 to 90 wt % solid biomass, preferably 10 to 80 wt % solid biomass. The total feed may consist of 60 to 80 wt % solid biomass, or alternatively 10 to 35 wt % solid biomass. This means that the liquid content is 10 wt %, preferably up to 65 wt %, which may provide process advantages, such as a pumpable slurry.

[0026] The lignocellulosic starting material may have a dry content of greater than 50 wt%, preferably in the range of 70 to 95 wt%, most preferably in the range of 80 to 92 wt%.

[0027] The lignocellulosic starting material can be selected from wood chips and / or sawdust; forestry residues selected from bark and / or roots; wood that has undergone a drying or torrefaction process; lignocellulose from agriculture, for example straw from crops such as oats, wheat, barley and rye, corn stover, grasses and herbs, fodder crops, oat husks, rice husks, construction waste containing at least 50% by weight of lignocellulosic matter; and mixtures thereof.

[0028] According to another embodiment, which may also be freely combined with the above aspects and embodiments, the lignocellulosic starting material is not subjected to a thermochemical treatment, such as pyrolysis or hydrothermal liquefaction, before being subjected to the method. Thus, a more simplified method may be achieved.

[0029] The organic liquefaction product may have an oxygen content lower than the feed (including the co-feed), and optionally, the organic liquefaction product may have an oxygen content at least 5% by weight lower than the feed (including the co-feed), for example, at least 10% by weight lower than the lignocellulosic starting material. The feed here includes all starting materials.

[0030] According to yet another embodiment, which can also be freely combined with the above aspects and embodiments, the operating pressure is in the range of 50 bar to 300 bar. This can improve and accelerate the liquefaction process carried out in the temperature range of the present method.

[0031] The operating pressure may optionally be in the range of 60 bar to 300 bar.

[0032] The mixture may be subjected to a temperature in the range of 300° C. to 380° C. Operating temperatures within this preferred range provide improved liquid yields.

[0033] The process may or may not be divided into two or more hydrotreatment reactors with a flat or increasing temperature profile.Thus, the process may comprise at least a second conversion step after the first hydrotreatment step.

[0034] In the second hydroprocessing reactor, the operating temperature may be in the range of 270°C to 450°C. Alternatively, in the second hydroprocessing reactor, the operating temperature may be 350°C or higher, such as in the range of 350°C to 450°C.

[0035] In a preferred embodiment, the hydroprocessing is carried out in two or more reactors in series, wherein each subsequent reactor is operated at a higher temperature than the first reactor. Preferably, the process is carried out with three reactors in series, and the temperature of the first reactor is selected from the range of 270°C to 350°C, the temperature of the second reactor is selected from the range of 340°C to 400°C, and the temperature of the third reactor is selected from the range of 380°C to 400°C.

[0036] A second aspect of the present disclosure relates to a molybdenum sulfide catalyst comprising one or more elements (E) of the following: iron (Fe), tungsten (W), cobalt (Co), vanadium (V) and ruthenium (Ru), characterized in that the catalyst has an empirical formula for molybdenum (Mo), the one or more elements (E) and sulfur (S):

[0037] Mo x E y S z

[0038] Wherein, x=1, 0.1<y<0.3, and z≤2.3.

[0039] An important advantage of this innovative catalyst is that it is relatively cheap and easy to manufacture. In addition, since it can be used as is without being bound to a support, it can be added at different stages of the process.

[0040] For example, in the amorphous and unsupported molybdenum sulfide catalyst, the mole fraction of sulfur (S) relative to the mole fraction of molybdenum (Mo) is in the range of 0.1 to 2.3. In the amorphous and unsupported molybdenum sulfide catalyst, the mole fraction of sulfur (S) relative to the mole fraction of molybdenum (Mo) may be ≤1.0, optionally in the range of 0.1 to 1.0. In an embodiment, the content of sulfur (S) is in the range of 0.3 to 0.99, for example, in the range of 0.5 to 0.95.

[0041] The molar fraction of the one or more elements: iron (Fe), tungsten (W), cobalt (Co), vanadium (V) and ruthenium (Ru) in the amorphous and non-supported molybdenum sulfide catalyst relative to the molar fraction of molybdenum (Mo) can be in the range of 0.1 to 0.3, optionally in the range of 0.1 to 0.2.

[0042] Preferably, the catalyst is substantially amorphous as determined by X-ray powder diffraction analysis and optical microscopy using polarized light. Alternatively, the catalyst is amorphous as determined by X-ray powder diffraction analysis.

[0043] According to an embodiment of the second aspect, the catalyst has a particle size distribution in the range of 1 to 500 μm as measured by laser diffraction. Preferably, the catalyst has a particle size distribution in the range of 1 μm to 200 μm as measured by laser diffraction. The advantage of this particle size distribution is that it has improved dispersion in the feed slurry and is available throughout the reactor volume, while supported or larger catalyst particles are only available in the reaction zone. In addition, it makes the catalyst easy to contact with larger molecules and provides increased activity.

[0044] A third aspect of the present disclosure relates to a method for converting a lignocellulosic starting material into an organic liquefied product, characterized in that a mixture of the lignocellulosic starting material, a catalyst according to the second aspect and embodiments thereof, and a co-feed is subjected to a stoichiometric amount of hydrogen, an elevated pressure, and a temperature in the range of 270°C to 450°C, thereby producing an organic liquefied product.

[0045] A fourth aspect relates to a method for producing a molybdenum sulfide catalyst, the molybdenum sulfide catalyst comprising one or more elements (E) of iron (Fe), tungsten (W), cobalt (Co), vanadium (V) and ruthenium (Ru), the method comprising the following steps:

[0046] By mixing MoO 3 NH 4 ) 2 S and water form a first reaction mixture;

[0047] pressurizing the first mixture with hydrogen, heating and stirring the mixture;

[0048] forming a second mixture by adding a hydrocarbon fraction having a kinematic viscosity of 2.0 CSt@40°C and metal salts of Fe and / or W and / or Co and / or V and / or Ru, such as sulfates and / or nitrates of Fe, W, Co, V and Ru, to the first mixture at a suitable pressure and temperature;

[0049] Pressurizing the second mixture with hydrogen and heating it at a suitable heating rate;

[0050] depressurizing the second mixture and heating the residual hydrocarbons to a suitable temperature to remove water and part of the hydrocarbon fraction; and

[0051] The catalyst is recovered as a slurry containing residual hydrocarbons.

[0052] In the step of forming the second mixture, one or more of the following elements (E): iron (Fe), tungsten (W), cobalt (Co), vanadium (V) and ruthenium (Ru) may be added in an amount to provide a catalyst having an empirical formula with respect to molybdenum (Mo), the one or more elements (E) and sulfur (S):

[0053] Mo x E y S z

[0054] Wherein, x=1, 0.1<y<0.2, and z≤2.3.

[0055] For example, in the amorphous and unsupported molybdenum sulfide catalyst, the mole fraction of sulfur (S) relative to the mole fraction of molybdenum (Mo) is in the range of 0.1 to 2.3. In the amorphous and unsupported molybdenum sulfide catalyst, the mole fraction of sulfur (S) relative to the mole fraction of molybdenum (Mo) may be in the range of 0.1 to 1.0. In an embodiment, the content of sulfur (S) is in the range of 0.3 to 0.99, for example, in the range of 0.5 to 0.95.

[0056] In the amorphous and non-supported molybdenum sulfide catalyst, the molar fraction of the one or more elements: iron (Fe), tungsten (W), cobalt (Co), vanadium (V) and ruthenium (Ru) relative to the molar fraction of molybdenum (Mo) can be in the range of 0.1 to 0.3, optionally in the range of 0.1 to 0.2.

[0057] The fact that the hydrocarbon fraction has a kinematic viscosity of less than 2.0 CSt@40°C facilitates the removal of water by boiling and separation by distillation to obtain a catalyst free of water or at least substantially free of water.

[0058] Other aspects and embodiments will become apparent to those skilled in the art upon examination of the accompanying drawings and the following detailed description and examples. BRIEF DESCRIPTION OF THE DRAWINGS

[0059] Various aspects and embodiments will now be described by way of example with reference to the accompanying drawings, in which:

[0060] Figure 1 The XRPD diffraction pattern of the catalyst according to Example 1 is shown.

[0061] Figure 2 The particle size distribution of the catalyst according to Example 1 is shown.

[0062] Figure 3 TGA data for the organic liquid product phase of Example 2 is shown.

[0063] Figure 4 TGA data for the THF-soluble liquefied phase of Example 2 is shown.

[0064] Figure 5 TGA data for the organic liquid product phase of Example 4 is shown.

[0065] Figure 6TGA data for the THF-soluble liquefied phase of Example 4 is shown. DETAILED DESCRIPTION

[0066] When studying the specific embodiments, it should be understood that the terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting, since the scope of the aspects and embodiments of the present application will be limited only by the appended claims and their equivalents.

[0067] It should be noted that, as used in this specification and the appended claims, the singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise.

[0068] The terms "lignocellulosic material", "lignocellulosic starting material" and "lignocellulosic feedstock" are used herein to cover all integral non-fractionated lignocellulosic materials consisting essentially of cellulose, hemicellulose and lignin. Depending on the geographical location, there are different materials available, such as agricultural residues (e.g. corn stover, crop straw and bagasse), herbaceous crops (e.g. alfalfa, switchgrass), softwood and hardwood, short rotation woody plants, preheated and / or toasted wood, forestry residues (bark as well as branches, roots and tops) and other waste materials (e.g. urban and industrial waste containing whole lignocellulosic biomass, such as waste wood for the construction industry and / or cargo packaging). The inventors have tested pine sawdust with various dry matter contents, ground spruce roots and branches, fresh spruce needles, fresh pine bark and ground urban waste containing wood, plastic, sand, metal and paint residues.

[0069] The terms "unsupported" and "carrier-free" are used to define catalyst materials, such as sulfided Mo catalysts, that are not deposited on any solid support or carrier material.

[0070] The fact that the catalyst is "amorphous" means that it is substantially amorphous or amorphous as determined by X-ray powder diffraction analysis.

[0071] By X-ray powder diffraction analysis, The difference between amorphous and crystalline materials is that crystalline materials produce sharp peaks in the XRD pattern whereas amorphous materials No spikes will be generated Therefore, the amorphous catalyst determined by X-ray powder diffraction analysis has No spikes will be generated .

[0072] The terms "hydrocarbon fraction" and "hydrocarbon phase" herein refer to the liquid hydrocarbon fraction recoverable at room temperature according to the process disclosed herein, but this definition does not exclude that additional, more volatile hydrocarbons may be condensed at lower temperatures and included in the fraction.

[0073] The obtained organic liquefied product may be liquid at room temperature to at most 500° C. The organic liquefied product may include one or more organic liquid phases.

[0074] The term "solid residue" herein refers to the remaining solids separated from the organic liquefaction product after the hydroliquefaction of lignocellulose, as illustrated in the following experimental examples. According to a first aspect, a method for converting a lignocellulose starting material into an organic liquefaction product is characterized in that a lignocellulose starting material from a single source or from a mixture with related starting materials, an amorphous and non-supported molybdenum sulfide catalyst, and optionally a co-feed are mixed and subjected to not less than a stoichiometric amount of hydrogen, an elevated pressure, and a temperature in the range of 270°C to 450°C, thereby producing an organic liquefaction product, wherein the amorphous and non-supported molybdenum sulfide catalyst comprises one or more elements (E) of the following: iron (Fe), tungsten (W), cobalt (Co), vanadium (V), and ruthenium (Ru).

[0075] Preferably, the catalyst according to the present disclosure is an amorphous and unsupported sulfide cobalt-molybdenum catalyst.

[0076] Preferably, the catalyst is introduced to the mixture of lignocellulosic starting material in the form of a slurry of catalyst particles in a hydrocarbon co-feed.

[0077] In the process there is a co-feed which may be selected from: vegetable oils and fats, such as tall oil, tall oil pitch; pyrolysis oil; HTL oil; animal fats; fatty acids; fossil or renewable liquid hydrocarbons; and / or recycled or recovered products or fractions of products obtained in the process.

[0078] The lignocellulosic starting material may have a dry content of greater than 50 wt%, preferably in the range of 70 to 95 wt%, most preferably in the range of 80 to 92 wt%.

[0079] The lignocellulosic starting material can be selected from wood chips and / or sawdust; forestry residues selected from tree bark and / or tree roots; wood that has undergone a drying or torrefaction process; lignocellulose from agriculture, for example straw from crops such as oats, wheat, barley and rye, corn stover, grasses and herbs, fodder crops, oat husks, rice husks, construction waste containing at least 50% by weight of lignocellulosic matter; and mixtures thereof.

[0080] With regard to materials that have been subjected to a drying or baking process, it is emphasized that baking is considered herein only as a drying step, ie the removal of moisture, and not as a proper thermochemical process.

[0081] According to another embodiment, which may also be freely combined with the above-mentioned aspects and embodiments, the lignocellulosic starting material has not been subjected to a thermochemical treatment, such as pyrolysis or hydrothermal liquefaction, before being subjected to the method.

[0082] According to yet another embodiment, which can also be freely combined with the above aspects and embodiments, the operating pressure is in the range of 50 bar to 300 bar, for example in the range of 60 bar to 300 bar. When the method is operated in batch mode, the initial pressure is set according to the available head space volume and in a manner to ensure a stoichiometric excess of hydrogen, for example, the initial pressure at ambient temperature is set to 120 bar and allowed to increase and stabilized in the range of 150 bar to 300 bar, preferably 250 bar. When the method is operated in a continuous mode, the pressure is preferably set in the range of 70 bar to 180 bar, most preferably in the range of 90 bar to 160 bar.

[0083] The mixture may be subjected to a temperature in the range of 300° C. to 380° C. Operating temperatures within this preferred range provide improved liquid yields.

[0084] A second aspect of the present disclosure relates to a molybdenum sulfide catalyst comprising one or more elements (E) of: iron (Fe), tungsten (W), cobalt (Co), vanadium (V) and ruthenium (Ru), characterized in that the catalyst has an empirical formula for molybdenum (Mo), the one or more elements (E) and sulfur (S):

[0085] Mo x E y S z

[0086] Wherein, x=1, 0.1<y<0.3, and z≤2.3.

[0087] Preferably, the catalyst is substantially amorphous as determined by X-ray powder diffraction analysis.Alternatively, the catalyst is amorphous as determined by X-ray powder diffraction analysis.

[0088] Preferably, the catalyst according to the present disclosure is an amorphous and unsupported sulfide cobalt-molybdenum catalyst.

[0089] According to an embodiment of the second aspect, the catalyst has a particle size distribution with a median value in the range of 1 to 500 μm as measured by laser diffraction. Alternatively, the catalyst has a particle size distribution with a median value in the range of 1 to 200 μm as measured by laser diffraction.

[0090] A third aspect of the present disclosure relates to a method for converting a lignocellulosic starting material into an aqueous phase and a hydrocarbon phase, characterized in that a mixture of the lignocellulosic starting material, a catalyst according to the second aspect and embodiments thereof and a co-feed is subjected to a stoichiometric amount of hydrogen, elevated pressure and a temperature in the range of 270°C to 450°C, thereby producing one or more liquid phases and / or aqueous phases and hydrocarbon phases.

[0091] The fourth aspect relates to a method for preparing the catalyst according to the second aspect and embodiments thereof, comprising the following steps:

[0092] By mixing MoO 3 NH 4 ) 2 S and water form a first reaction mixture;

[0093] pressurizing the first mixture with hydrogen, heating and stirring the mixture;

[0094] forming a second mixture by adding a hydrocarbon fraction having a kinematic viscosity of less than 2.0 CSt@40°C and metal salts of Fe and / or W and / or Co and / or V and / or Ru, such as sulfates and / or nitrates of Fe, W, Co, V and Ru, to the first mixture at a suitable pressure and temperature;

[0095] Pressurizing the second mixture with hydrogen and heating it with a suitable heating rate;

[0096] depressurizing the second mixture and heating the residual hydrocarbons to a suitable temperature to remove water and part of the hydrocarbon fraction; and

[0097] The catalyst is recovered as a slurry containing residual hydrocarbons.

[0098] The lignocellulose starting material is subjected to mechanical pretreatment optionally to simplify material handling and increase area volume ratio (surface to volume ratio). Suitable pretreatment operation comprises milling, chip cutting and grinding.In the experiment carried out by the inventor so far, the starting material of various particle sizes has been tested, for example 10mm or less, such as in the scope of 0.5mm to 10mm, the particle size of the lignocellulose starting material is preferably 2mm or less.The result shows, the method can handle all these particle sizes, and particle size does not seem to be a key factor.

[0099] In the step of forming the second mixture, metal salts of Fe and / or W and / or Co and / or V and / or Ru, such as sulfates and / or nitrates of Fe, W, Co, V and Ru, may be added in an amount to provide a catalyst having an empirical formula with respect to molybdenum (Mo), the one or more elements (E) and sulfur (S):

[0100] Mo x E y S z

[0101] Wherein, x=1, 0.1<y<0.3, and z≤2.3.

[0102] In developing the present disclosure, the inventors constructed a laboratory-scale batch process, as described in more detail in the examples. The batch process enables testing of different lignocellulose starting materials, comparison of new catalysts with other known catalysts, and testing of different process parameters. And the process is also validated in semi-batch mode.

[0103] Example

[0104] Analytical methods

[0105] The hydroxyl number for analyzing the amount of hydroxyl groups belonging to fatty alcohols (aliphatic OH), phenols (aromatic OH) and OH-groups of carboxylic acids is determined by the method described, for example, in L. Akim et al. Holzforschung 2001, 55, 386-390 using a Bruker Avance 500 UltraShield NMR spectrometer. 31 P-NMR was used. 1 H-NMR is used to characterize the relative amounts of protons that are part of the aromatic, aliphatic, ether / alcohol, aldehyde, ketone, carboxylic acid, and olefin functional groups of the resulting product mixture.

[0106] The boiling point range was determined using thermogravimetric analysis on a Mettler-Toledo TGA / SDTA851e instrument.

[0107] The particle size distribution was determined using a Malvern Mastersizer 2000 laser diffractometer.

[0108] X-ray powder diffraction analysis (XRPD) was performed on a PANalytical X'Pert PRO spectrometer.

[0109] Example 1: Preparation of CoMo catalyst

[0110] Molybdenum trioxide (40g), ammonium sulfide (60mL, 20%w / w in water) and water (122g) are added to a 1.8L steel reactor. An inert nitrogen atmosphere is established by three vacuum-nitrogen cycles (nitrogen pressure 6 bar). The reactor is pressurized to 22 bar with hydrogen, and a paddle stirrer is used to stir the mixture at a tip speed of 2.4m / s. The jacket temperature is raised to 68°C, soaked for 4 hours, and then the temperature is reduced to 38°C. The reactor is decompressed, and an inert atmosphere is then established by vacuum-nitrogen cycles (nitrogen pressure 6 bar). A mixture of n-dodecane (400mL) and cobalt sulfate heptahydrate (45.9g, 28.4w / w% aqueous solution) is added to the reactor. The reactor is sealed, and an inert nitrogen atmosphere is established by three vacuum-nitrogen cycles (nitrogen pressure 6 bar), and then hydrogen is added to a pressure of 25 bar. The jacket temperature is raised to 210°C in 6 hours. After 1 hour at this temperature, the reactor contents were cooled to room temperature. The reactor was decompressed and an inert atmosphere was then established by vacuum-nitrogen circulation (nitrogen pressure 6 bar). After the condenser was applied to the reactor, water and half the amount of n-dodecane were distilled out using low flow ballast nitrogen gas at atmospheric pressure. After the distillation, the cooling reactor slurry contents were removed from the reactor and sieved by 280 μm stainless steel sieves when the catalyst was not affected by air, to remove larger particles. The catalyst was used and stored in the form of a slurry in dodecane, and its content was 26.1% w / w based on three repeated measurements.

[0111] Figure 1 The XRPD diffractogram of the catalyst according to Example 1 shown shows the absence of any XRPD peaks indicative of crystallinity, leading to the conclusion that the catalyst according to Example 1 is amorphous.

[0112] Figure 1 The XRPD diffraction pattern of the CoMoS catalyst according to Example 1 is shown, indicating that the catalyst is amorphous.

[0113] Figure 2 The particle size distribution of the CoMoS catalyst according to Example 1 is shown. To determine the particle size distribution, an aliquot of the catalyst prepared according to Example 1 was dispersed in pure dodecane and analyzed by laser diffraction after in situ ultrasound treatment on a Malvern Mastersizer 2000. The results show a median particle size of 1.6 μm.

[0114] Example 2: Using the CoMo catalyst according to Example 1 Sawdust Hydrodeoxygenation

[0115] Ground and sieved pine sawdust (30.01 g, dry matter content 91.5% w / w) and catalyst slurry prepared according to Example 1 (8.40 g, 26.1% w / w measured in dodecane) were added to a 300 mL stainless steel high pressure reactor. An inert nitrogen atmosphere was established using three vacuum-nitrogen cycles, and then the reactor was pressurized (120 bar) with hydrogen. The reactor contents were heated to 380° C. under stirring for 2 hours. After cooling, decompression and establishing an inert atmosphere by vacuum-nitrogen cycles, the reactor contents were poured into a centrifuge vial and centrifuged at 2.9×10-3G for 20 minutes. The organic liquid phase, aqueous phase and solid residue phase were separated. The solid residue, reactor, lid and agitator were washed continuously with two portions of n-pentane (2×45 mL) and three portions of 45 mL of tetrahydrofuran (THF). After each wash, the mixture was centrifuged and separated. The n-pentane wash phases were combined in a separate container and the THF wash phases were combined in another separate container before evaporating the solvents (n-pentane and THF). After completion of the work-up of the pentane and THF phases, including drying, the following products were isolated: an organic liquid phase, which combined the contents of the n-pentane wash phase (16.46 g of a light amber liquid, 45% w / w based on all feeds including dodecane); 8.45 g of an aqueous phase; 1.96 g of a THF-soluble liquefied phase; and 2.59 g of a solid residue. 1 H-NMR and 31 P-NMR data are shown in Tables 1 and 2 below, and TGA data are shown in Figure 3 . THF-soluble liquefied phase 1 H-NMR and 31 P-NMR data are shown below (Table 3 and Table 4), TGA data are shown in Figure 4 The NMR results indicated that the THF-soluble liquefied phase had a higher oxygen content, which was confirmed by the elemental analysis data below. The amount of isolated solid material calculated on dry biomass was 1.4% w / w. Considering the sawdust ash content of 0.6%, the amount of solid product was low.

[0116] Elemental analysis data of the organic liquid phase: C 84.1%, H 11.8%, N 0.34%, S 0.0%, O 3.1%, others 0.48%.

[0117] Elemental analysis data of the THF-soluble liquefied phase: C 81.9%, H 8.6%, N 0.56%, S 0.14%, O 8.32%, others 0.48%.

[0118] Table 1 shows the organic liquid phase of Example 2 1 H-NMR (CDCl 3 ) result (normalized integral).

[0119] <![CDATA[Example 2: 1 H-NMR signal]]> ppm integral Carboxylic acid H(COOH) and aldehyde H(CHO) 12-9 0 Aromatic H 9-6.2 6.1 Olefin H 6.2-4.5 0.1 Fatty alcohol H, -CHOH or aliphatic ether -CHOR 4.5-3.3 0.4 Aliphatic H 3.3-0 93.4

[0120] Table 2 shows the 31 The number of hydroxyl groups in the organic liquid phase of Example 2 measured by P-NMR.

[0121]

[0122] Figure 3 TGA data for the organic liquid product of Example 2 is shown, with the dashed line representing the boiling point range of diesel.

[0123] Table 3 shows the THF-soluble liquefied phase of Example 2. 1 H-NMR (DMSO-d6) results (normalized integration).

[0124] <![CDATA[Example 2: 1 H-NMR signal]]> ppm integral Carboxylic acids H(COOH), aldehydes H(CHO) and phenols (OH) 12-9 2.0 Aromatic H 9-6.2 14.6 Olefin H 6.2-4.5 1.0 Fatty alcohol H, -CHOH or aliphatic ether -CHOR 4.5-3.3 5.1 Aliphatic H 3.3-0 77.3

[0125] Table 4 shows the 31 The number of hydroxyl groups of the THF-soluble liquefied phase of Example 2 measured by P-NMR.

[0126]

[0127] Figure 4 TGA data for the THF-soluble liquefied phase of Example 2 is shown, where the dashed line represents the boiling point range of diesel.

[0128] Example 3: Preparation of CoMo Catalyst - Second Example

[0129] The catalyst slurry from Example 1 (23.24 g, 47 mmol) was added to a 300 mL Buchi batch autoclave followed by DMDS (6.7 mL, 76 mmol). The reactor was sealed and heated with N 2 (5 bar) for three inert treatments, followed by H 2 The reaction mixture was stirred at 800 rpm, heated to 300°C over a 1 hour ramp, and then held at that temperature for 12 hours. After cooling, the headspace was bubbled into a beaker containing an aqueous NaOH solution (30% w / w) to capture any H in the headspace gas mixture. 2 S. Then use H 2 O 2 The NaOH solution was quenched to oxidize the sulfide to sulfate. The black slurry mixture in the reactor was transferred to a vial. The reactor and agitator were rinsed with 20 mL of dodecane. Based on three independent samples, the dry catalyst content of the slurry was determined to reach 14.11% w / w.

[0130] Example 4: Using the CoMo catalyst according to Example 3 Sawdust Hydrodeoxygenation

[0131] Sawdust (30.0 g, dry matter content 91.5% w / w) with a particle size distribution <0.28 mm and a catalyst slurry prepared according to Example 3 (10.12 g, the catalyst content in dodecane was adjusted from 14.11% w / w to 28.03% w / w by centrifugation and removal of part of the dodecane using a pipette before use, dry catalyst weight 2.84 g) were mixed in a high pressure reactor at room temperature. An inert nitrogen atmosphere was established using a vacuum-nitrogen cycle, and the reactor was then pressurized with hydrogen (116 bar). The reaction mixture was heated to 320° C. and maintained at this temperature for 240 minutes. The maximum operating pressure during the reaction was 245 bar. After using the work-up procedure described in Example 2, 11.39 g of a dark brown organic liquid phase (28% w / w yield based on all feed), 5.99 g of an aqueous phase, 6.68 g of a THF-soluble liquefied phase (17% w / w yield based on all feed) and 3.17 g of a solid residue were isolated. 1 H-NMR and 31 The P-NMR data are shown in the table below, and the TGA data are shown in Figure 5 . THF-soluble liquefied phase 1 H-NMR and 31 The P-NMR data are shown in the table below and the TGA data are shown in Figure 6 The NMR results indicate that the THF-soluble liquefied phase has a high oxygen content, which is confirmed by the elemental analysis data below. Despite the low reaction temperature, the amount of solid material formed calculated on dry biomass is only 1.2% w / w. Considering the sawdust ash content of 0.6%, the amount of solid product is low.

[0132] Elemental analysis data of the organic liquid phase: C 84.0%, H 13.5%, N 0.06%, S 0.0%, O 2.2%, others 0.31%.

[0133] Elemental analysis data of the THF-soluble liquefied phase: C 79.8%, H 8.8%, N 0.55%, S 0.3%, O 9.5%, others 1.07%.

[0134] Table 5 shows the organic liquid phase of Example 4. 1 H-NMR (CDCl 3 ) result (normalized integral).

[0135] <![CDATA[Example 4: 1 H-NMR signal]]> ppm integral Carboxylic acid H(COOH) and aldehyde H(CHO) 12-9 0 Aromatic H 9-6.2 2.2 Olefin H 6.2-4.5 0.4 Fatty alcohol H, -CHOH or aliphatic ether -CHOR 4.5-3.3 0.03 Aliphatic H 3.3-0 97.4

[0136] Table 6 shows the 31 The number of hydroxyl groups in the organic liquid phase of Example 4 measured by P-NMR.

[0137]

[0138] Figure 5 TGA data for the organic liquid product phase of Example 4 is shown, where the dashed line represents the boiling point range of diesel.

[0139] Table 7 shows the THF-soluble liquefied phase of Example 4. 1 H-NMR (DMSO-d6) results (normalized integration).

[0140] <![CDATA[Example 4: 1 H-NMR signal]]> ppm integral Carboxylic acids H(COOH), aldehydes H(CHO) and phenols (OH) 12-9 1.3 Aromatic H 9-6.2 12.4 Olefin H 6.2-4.5 0.03 Fatty alcohol H, -CHOH or aliphatic ether -CHOR 4.5-3.3 2.7 Aliphatic H 3.3-0 83.6

[0141] Table 8 shows the 31 The number of hydroxyl groups of the THF-soluble liquefied phase of Example 4 measured by P-NMR.

[0142]

[0143] Figure 6 TGA data for the THF-soluble liquefied phase of Example 4 is shown, where the dashed line represents the boiling point range of diesel.

Claims

1. A method for converting a lignocellulosic starting material into an organic liquefied product, characterized in that In a first hydroprocessing step, a lignocellulosic starting material, an amorphous and unsupported molybdenum sulfide catalyst and a co-feed are mixed to obtain a mixture, wherein the amorphous and unsupported molybdenum sulfide catalyst includes one or more elements of the following items: iron (Fe), tungsten (W), cobalt (Co), vanadium (V) and ruthenium (Ru); and the mixture is subjected to not less than a stoichiometric amount of hydrogen at an elevated pressure and a temperature in the range of 270°C to 450°C to produce an organic liquefied product.

2. The method according to claim 1, wherein: In the amorphous and unsupported sulfide molybdenum catalyst, the mole fraction of sulfur (S) relative to the content of molybdenum (Mo) is in the range of 0.1 to 2.3, and optionally in the range of 0.1 to 1.

0.

3. The method according to claim 1 or 2, wherein: In the amorphous and non-supported molybdenum sulfide catalyst, the molar fraction of the one or more elements: iron (Fe), tungsten (W), cobalt (Co), vanadium (V) and ruthenium (Ru) relative to the molar fraction of molybdenum (Mo) is 0.1 to 0.3, optionally in the range of 0.1 to 0.

2.

4. A method according to any one of the preceding claims, wherein: The elevated pressure is a pressure in the range of 50 bar to 300 bar.

5. A method according to any one of the preceding claims, wherein: The catalyst is introduced into the mixture of lignocellulosic starting material in the form of a slurry of catalyst particles in a liquid co-feed.

6. A method according to any one of the preceding claims, wherein: The co-feed is selected from: vegetable oils and fats, such as tall oil and tall oil pitch; pyrolysis oil; HTL oil; Animal fats; fatty acids; fossil or renewable liquid hydrocarbons; and / or recycled or recovered products or fractions of products obtained in the process.

7. A method according to any one of the preceding claims, wherein: The co-feed is a mixture of vegetable oils and / or animal fats and fossil and / or renewable hydrocarbons.

8. A method according to any one of the preceding claims, wherein: The lignocellulosic starting material has a dry content of greater than 50 wt%, preferably in the range of 70 to 95 wt%, most preferably in the range of 80 to 92 wt%.

9. A method according to any one of the preceding claims, wherein: The lignocellulosic starting material is selected from: wood chips and / or sawdust; forestry residues selected from bark and / or roots and / or branches; wood that has undergone a drying or roasting process; lignocellulose from agriculture, for example straw from crops such as oats, wheat, barley and rye, corn straw, grasses and herbs, fodder crops, oat husks, rice husks, construction waste containing at least 50% by weight derived from lignocellulosic matter; and mixtures thereof.

10. A method according to any one of the preceding claims, wherein: Prior to being subjected to the process, the lignocellulosic starting material has not been subjected to thermochemical treatment, such as pyrolysis or hydrothermal liquefaction.

11. A method according to any one of the preceding claims, wherein: After the first hydrotreatment step, the process comprises at least a second conversion step, wherein the second conversion step may be a single step.

12. A method according to any one of the preceding claims, wherein: The mixture is subjected to a temperature in the range of 300°C to 380°C.

13. A molybdenum sulfide catalyst comprising one or more elements (E) of the following: iron (Fe), tungsten (W), cobalt (Co), vanadium (V) and ruthenium (Ru), characterized in that: The catalyst has an empirical formula with respect to molybdenum (Mo), the one or more elements (E) and sulfur (S): Mon x E y S z Wherein, x=1, 0.1<y<0.3, and z≤2.

3.

14. The catalyst according to claim 13, wherein The catalyst was substantially amorphous as determined by X-ray powder diffraction analysis and optical microscopy using polarized light.

15. The catalyst according to claim 13 or 14, wherein The catalyst has a particle size distribution determined by laser diffraction with a median value in the range of 1 μm to 500 μm, preferably in the range of 1 μm to 200 μm.

16. The catalyst according to any one of claims 13 to 15, wherein z≤1.0。 17. A method for converting a lignocellulosic starting material into one or more liquid and / or aqueous and hydrocarbon phases, characterized in that A mixture of lignocellulosic starting material, a catalyst according to any one of claims 13 to 16 and a co-feed is subjected to not less than a stoichiometric amount of hydrogen, elevated pressure and a temperature in the range of 270°C to 450°C to produce one or more liquid and / or aqueous phases and hydrocarbon phases.

18. A method for producing a molybdenum sulfide catalyst, the molybdenum sulfide catalyst comprising one or more elements (E) selected from the group consisting of iron (Fe), tungsten (W), cobalt (Co), vanadium (V) and ruthenium (Ru), the method comprising the following steps: forming a first reaction mixture by mixing MoO3, (NH4)2S and water; pressurizing the first mixture with hydrogen, heating and stirring the mixture; forming a second mixture by adding a hydrocarbon fraction having a kinematic viscosity of less than 2.0 CSt@40°C and metal salts of Fe and / or W and / or Co and / or V and / or Ru, such as sulfates and / or nitrates of Fe, W, Co, V and Ru, at a suitable pressure and temperature; Pressurizing the second mixture with hydrogen and heating it with a suitable heating rate; depressurizing the second mixture and heating the residual hydrocarbons to a suitable temperature to remove water and part of the hydrocarbon fraction; and The catalyst is recovered as a slurry containing residual hydrocarbons.

19. The method according to claim 18, wherein: In the step of forming the second mixture, metal salts of Fe and / or W and / or Co and / or V and / or Ru, such as sulfates and / or nitrates of Fe, W, Co, V and Ru are added in an amount to provide a catalyst having an empirical formula for molybdenum (Mo), the one or more elements (E) and sulfur (S): Mon x E y S z Wherein, x=1, 0.1<y<0.3, and z≤2.3.

Citation Information

Patent Citations

  • Conversion of solid biomass into a liquid hydrocarbon material

    IN201647041964A

  • Process for direct hydorliquefaction of biomass comprising two stages of ebullating bed hydroconversion

    US20110167713A1