Method for eluting aluminum ions and / or zinc ions

By using alkali metal hydroxide and ammonium hydroxide as eluents, the pollution and cost problems of eluting aluminum ions and zinc ions in the prior art are solved, and a high selectivity and environmentally friendly elution effect is achieved.

CN118922567APending Publication Date: 2024-11-08LANXESS DEUTSCHLAND GMBH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202380029224.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-22
Filing Date
2023-03-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art methods for eluting aluminum and zinc ions on polymers containing aminomethylphosphonic acid groups require the use of complexing agents, resulting in contamination of wastewater and increased costs.

Method used

Alkaline metal hydroxide and ammonium hydroxide or mixtures thereof are used as eluents to remove aluminum ions and zinc ions from the polymer containing aminomethylphosphonic acid groups with high selectivity.

Benefits of technology

Highly selective eluting of aluminum and zinc ions is achieved, avoiding the use of complexing agents, and reducing contamination and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005052634990000051
    Figure BDA0005052634990000051
  • Figure BDA0005052634990000081
    Figure BDA0005052634990000081
  • Figure FDA0005052634980000021
    Figure FDA0005052634980000021
Patent Text Reader

Abstract

The invention relates to a method for eluting aluminum ions and / or zinc ions of a polymer containing aminomethylphosphonic acid groups.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for eluting aluminum ions and / or zinc ions from a polymer containing aminomethylphosphonic acid groups. Background Art

[0002] The recycling of lithium-ion batteries is a key technology in order to enable the transition to more sustainable electromobility. Ion exchangers represent a promising technology for removing impurities such as copper, aluminum and zinc from the electrolyte concentrate produced by recycled lithium-ion batteries. For example, it is known from WO-A 2012 / 113657 that the use of polymers containing phosphonate groups is particularly suitable for removing divalent and trivalent metal ions. It is also known from WO-A 2012 / 113657 that polymers containing phosphonate groups can be regenerated by using alkaline solutions containing tartrate, citrate, oxalate or EDTA ions, and in doing so remove metal ions from the polymer.

[0003] Virolainen et al. (S. Virolainen, T. Vesselborg, A. Kaukinen, T. Sainio, Hydrometallurgy 2021, 202, 105602, pp. 1-9) describe polymers containing aminomethylphosphonic acid groups such as The MDS TP 260 is particularly suitable for removing aluminum and iron from a mixture of aluminum, copper, manganese, iron, lithium, nickel and cobalt concentrates. For this purpose, Virolainen et al. developed a two-stage process in which the metal ions are first bound to a polymer containing aminomethylphosphonic acid groups and then in a first step the copper, manganese and cobalt are eluted with sulfuric acid, the cobalt solution is adsorbed again and in a second step the aluminum is complexed and eluted with an alkaline potassium oxalate solution.

[0004] The stripping methods known from the prior art for stripping aluminum and / or zinc ions from polymers containing aminomethylphosphonic acid groups provide for the use of complexing agents, since the binding affinity of aluminum and zinc ions to phosphonic acid groups is very high. However, complexing agents are wastewater-polluting compounds, i.e., have ecological disadvantages, and therefore must be removed from them again. This in turn increases the costs of the process.

[0005] There is therefore still a need for a process by which aluminium ions and / or zinc ions can be eluted with high selectivity from polymers containing aminomethylphosphonic acid groups. Summary of the invention

[0006] It has now surprisingly been found that aluminium and / or zinc ions can be eluted with high selectivity from polymers containing aminomethylphosphonic acid groups if the base used for elution is a base selected from the group of alkali metal hydroxides and ammonium hydroxide or a mixture of these bases.

[0007] Therefore, the present invention provides a method for eluting aluminum ions and / or zinc ions, wherein an aminomethylphosphonic acid group-containing polymer or a salt thereof which is at least partially loaded with aluminum ions and / or zinc ions is mixed with a base selected from the group consisting of alkali metal hydroxides and ammonium hydroxide or a mixture of these bases, and the aluminum ions and / or zinc ions are eluted.

[0008] The scope of the present invention encompasses all the above and below detailed radical definitions, parameters and illustrations mentioned in general terms or in preferred ranges, together with one another (ie including any combination between the corresponding range and the preferred range).

[0009] The polymer containing aminomethylphosphonic acid groups is preferably a polystyrene copolymer containing aminomethylphosphonic acid groups. Even further preferred is a polymer containing aminomethylphosphonic acid groups a polystyrene-divinylbenzene copolymer containing aminomethylphosphonic acid groups.

[0010] The polymer containing aminomethylphosphonic acid group includes the polymer containing aminomethyl monophosphonic acid group, the polymer containing aminomethyl diphosphonic acid group and its salt. The salt of the polymer containing aminomethylphosphonic acid group is preferably the metal salt of alkali metal salt, alkaline earth metal salt and the periodic table III group to XII group. The salt of the polymer containing aminomethylphosphonic acid group is preferably sodium salt, potassium salt, lithium salt, magnesium salt, calcium salt, iron salt, copper salt, manganese salt, cobalt salt and nickel salt. The salt of the polymer containing aminomethylphosphonic acid group can be particularly preferably its sodium salt, potassium salt, lithium salt, cobalt salt and nickel salt. It is particularly preferred to use sodium salt, potassium salt or nickel salt as the salt of the polymer containing aminomethylphosphonic acid group.

[0011] The polystyrene copolymers used are preferably copolymers of monovinylaromatic monomers selected from the group of styrene, vinyltoluene, ethylstyrene, α-methylstyrene, chlorostyrene or chloromethylstyrene and mixtures of these monomers, and polyvinylaromatic compounds (crosslinkers) selected from the group of divinylbenzene, divinyltoluene, trivinylbenzene, divinylnaphthalene and / or trivinylnaphthalene.

[0012] The polystyrene copolymer backbone used is particularly preferably a styrene / divinylbenzene copolymer. Styrene / divinylbenzene copolymers are copolymers crosslinked with divinylbenzene. It is preferred to use technical-grade divinylbenzene, which may contain up to 30% by weight of ethylvinylbenzene. Therefore, styrene / divinylbenzene copolymers also include copolymers which additionally contain ethylvinylbenzene as a monomer.

[0013] The polymer preferably has a spherical form.

[0014] The polymer containing aminomethylphosphonic acid groups preferably has a macroporous structure.

[0015] The terms "microporous" or "in gel form" / "macroporous" have been described in detail in the technical literature, for example in Seidl, Malinsky, Dusek, Heitz, Adv. Polymer Sci. [Advances in Polymer Science], 1967, Vol. 5, pp. 113 to 213. Possible methods for measuring macroporosity, such as mercury porosimetry and BET determination, are also described in the literature. The pores of the macroporous polymers of the polymers containing aminomethylphosphonic acid groups generally and preferably have a diameter of 20 nm to 100 nm.

[0016] The polymer containing aminomethylphosphonic acid groups preferably has a monodisperse distribution.

[0017] In the present application, monodisperse materials are those in which at least 90% by volume or 90% by mass of the particles have a diameter within + / - 10% of the most common diameter.

[0018] For example, in the case of a material having a most common diameter of 0.5 mm, at least 90% by volume or 90% by mass is within the size interval between 0.45 mm and 0.55 mm; in the case of a material having a most common diameter of 0.7 mm, at least 90% by volume or 90% by mass is within the size interval between 0.77 mm and 0.63 mm.

[0019] The polymer containing aminomethylphosphonic acid groups preferably has a diameter (d 50 ).

[0020] Very particularly preferably, it has a diameter (d 50 ).

[0021] Polymers containing aminomethylphosphonic acid groups can be produced according to known methods, for example by phthalamidomethylation of styrene-divinylbenzene copolymers and functionalization of the resulting amino groups by reaction of pH-acidic compounds with formalin in a suspension containing sulfuric acid. They are also commercially available, for example from LANXESS Deutschland GmbH as MDS TP 260.

[0022] The average degree of substitution indicates the statistical ratio between unsubstituted, monosubstituted and disubstituted aminomethyl groups in the polymer containing aminomethylphosphonic acid groups. Thus, the average degree of substitution may be between 0 and 2. At a degree of substitution of 0, no substitution will occur and the aminomethyl groups will be present as primary amino groups. At a degree of substitution of 2, all aminomethyl groups in the resin will be present as disubstituted phosphonic acid groups. At a degree of substitution of 1, from a statistical point of view, all aminomethyl groups in the resin will be present as monosubstituted forms.

[0023] The average degree of substitution of the aminomethyl groups by phosphonic acid groups in the polymer containing aminomethylphosphonic acid groups is preferably from 1.4 to 2.0.

[0024] Preferably, the polymer containing aminomethylphosphonic acid groups has a total hydrogen capacity of 2.5 mol / L to 7.0 mol / L of resin. Very particularly preferably, the polymer containing aminomethylphosphonic acid groups has a total hydrogen capacity of 3.0 to 3.4 mol / L of resin.

[0025] The total capacity of the polymers containing aminomethylphosphonic acid groups is determined in accordance with DIN 54403 (Testing of ionexchangers—Determination of the total capacity of cation exchangers).

[0026] Preferably, the polymer containing aminomethylphosphonic acid groups is a chelating resin containing a functional group of structural unit (I)

[0027]

[0028] in is a polystyrene copolymer backbone, and

[0029] R 1 and R 2 may be the same or different and are independently -CH2PO(OX 1 )2 and -CH2PO(OH)OX 2 or hydrogen, where R 1 and R 2 cannot be both hydrogen and X 1 and X 2 is independently hydrogen, sodium, potassium or lithium.

[0030] Preferably, R 1 and R 2 independently -CH2PO(OX 1 )2 and -CH2PO(OH)OX 2 Preferably, X 1 and X 2 =H.

[0031] In the polystyrene copolymer backbone, -CH2-NR 1 R 2 The group is bonded to the phenyl group.

[0032] The polymer containing aminomethylphosphonic acid groups is preferably a macroporous, monodisperse chelating resin containing the functional groups of structural unit (I).

[0033] The polymers containing aminomethylphosphonic acid groups can be partially or completely loaded with aluminum ions and / or zinc ions.

[0034] Preferably, the polymer containing aminomethylphosphonic acid groups is loaded with aluminum ions and / or zinc ions to an extent of 10 mol % to 90 mol % based on the total capacity of the polymer.

[0035] The alkali metal hydroxides used are preferably sodium hydroxide and potassium hydroxide. The alkali metal hydroxide is preferably present in an aqueous solution.

[0036] The alkali metal hydroxide solution preferably contains between 5% and 20% by weight of alkali metal hydroxide. Particularly preferably, the alkali metal hydroxide solution contains 6% to 12% by weight of alkali metal hydroxide.

[0037] In a further preferred embodiment, the alkali metal hydroxide solution contains 5 to 20% by weight of alkali metal hydroxide and 79 to 94% by weight of water and up to 1% by weight of organic solvents or other impurities such as alkaline earth metal hydroxide or potassium oxalate. If potassium oxalate is present, the proportion is in each case <0.1% by weight.

[0038] In a further preferred embodiment, the alkali metal hydroxide solution contains 6 to 12% by weight of alkali metal hydroxide and 87 to 93% by weight of water, and up to 1% by weight of organic solvents or other impurities (such as alkaline earth metal hydroxide or potassium oxalate) may be present. If potassium oxalate is present, the proportion is in each case <0.1% by weight.

[0039] In a further preferred embodiment, the alkali metal hydroxide solution consists of 5 to 20% by weight of alkali metal hydroxide and 80 to 95% by weight of water, and the sum of these compounds totals 100% by weight.

[0040] Preference is given to using as ammonium hydroxide a solution of ammonia in water with a concentration of between 15% and 35% by weight.

[0041] In a further preferred embodiment, the ammonium hydroxide solution contains 15 to 35% by weight of alkali metal hydroxide and 84 to 64% by weight of water, and up to 1% by weight of organic solvents or other impurities (such as alkaline earth metal hydroxide or potassium oxalate) may be present. If potassium oxalate is present, the proportion is in each case <0.1% by weight.

[0042] In a further preferred embodiment, the base used does not contain any complexing agent. In the context of the present invention, the complexing agent is preferably a solution containing tartrate, citrate, oxalate or EDTA ions. Even further preferably, the base does not contain oxalate ions, in particular does not contain potassium oxalate.

[0043] The elution can be carried out in a batch process or by application to a column. The amount of base which must be applied for the elution is preferably 1 to 10 bed volumes of polymer, particularly preferably 3 to 7 bed volumes of polymer.

[0044] In the elution, the pH of the eluent is preferably 10 to 14.

[0045] Elution is preferably carried out at a temperature of 60 to 90° C. To achieve this temperature, the base can be heated or the polymer containing aminomethylphosphonic acid groups can be heated during the column (for example and preferably by means of a heating coil).

[0046] After the wash-out, the polymer containing aminomethylphosphonic acid groups can be regenerated again by contacting with acid. In this step, impurities are removed on the one hand, but the polymer containing aminomethylphosphonic acid groups is also converted back to H form on the other hand. This allows the resin to be loaded with metal ions again. Preferably, mineral acid is used as the acid for regenerating the polymer containing aminomethylphosphonic acid groups. The mineral acid used is preferably sulfuric acid, hydrochloric acid and nitric acid. Particularly preferably, sulfuric acid is used to regenerate the polymer containing aminomethylphosphonic acid groups.

[0047] Preferably, sulfuric acid is used in a concentration of 5% to 20% by weight for regenerating the polymer containing aminomethylphosphonic acid groups.

[0048] In a further preferred embodiment, the present invention encompasses a method for eluting aluminum ions and / or zinc ions, wherein in step a.) at least one chelating resin containing a functional group of structural unit (I) is reacted with

[0049]

[0050] in is a polystyrene copolymer backbone, and

[0051] R 1 and R 2 may be the same or different and are independently -CH2PO(OX 1 )2 and -CH2PO(OH)OX 2 or hydrogen, where R 1 and R 2 cannot be both hydrogen and X 1 and X 2 independently hydrogen, sodium, potassium and lithium,

[0052] contacting the chelating resin with an aqueous metal ion solution containing aluminum ions and / or zinc ions and optionally additional metal ions, and

[0053] In step b.), the aluminum and / or zinc ions are eluted with an aqueous alkali metal hydroxide solution or an aqueous ammonium hydroxide solution or a mixture of these bases.

[0054] Step a.)

[0055] Metal ion and / or aluminum ion and / or zinc ion are contacted with a chelating resin containing the functional group of structural unit (I) in a metal ion aqueous solution. Metal adsorption can be carried out in a batch process or by being applied to a post. Adsorption is preferably carried out in a post process.

[0056] In step a.), aluminum ions and / or zinc ions in a concentration of 10 μg / L to 5g / L can be used. Preferably, aluminum ions and / or zinc ions in a concentration of 1mg / L to 1g / L are used. The chelating resin containing the functional group of the structural unit (I) can be contacted with other metal ions and thus loaded with these other metal ions. Ions of metallic iron, copper, manganese, cobalt, nickel and lithium can be preferably used as metal ions. Preferably divalent or trivalent iron ions are used. Preferably divalent copper, manganese, cobalt and / or nickel ions are used. Preferably trivalent aluminum ions are used. Preferably divalent zinc ions are used. Lithium, nickel and cobalt ions can be particularly preferably used. Even further preferably, nickel and cobalt ions are used.

[0057] Preferably, in step a.) an aqueous metal ion solution of aluminum ions, nickel ions and cobalt ions is applied to the chelate resin.

[0058] Preferably, the molar ratio of aluminum ions to nickel ions and / or cobalt ions in the application in step a.) is from 0.5 to 1.5.

[0059] The ratio of the weight concentration of metal ions to aluminum ions and / or zinc ions in the chelating resin in step a.) is preferably from 100:1 to 2:1.

[0060] The ratio of the weight concentration of lithium ions to aluminum ions and / or zinc ions in the chelating resin in step a.) is preferably from 100:1 to 2:1.

[0061] The ratio of the weight concentration of cobalt ions to aluminum ions and / or zinc ions in the chelating resin in step a.) is preferably from 100:1 to 2:1.

[0062] The ratio of the weight concentration of manganese ions to aluminum ions and / or zinc ions in the chelating resin in step a.) is preferably from 100:1 to 2:1.

[0063] The ratio of the weight concentration of copper ions to aluminum ions and / or zinc ions in the chelating resin in step a.) is preferably from 100:1 to 2:1.

[0064] The ratio of the weight concentration of iron ions to aluminum ions and / or zinc ions in the chelating resin in step a.) is preferably from 100:1 to 2:1.

[0065] The ratio of the weight concentration of nickel ions to aluminum ions and / or zinc ions in the chelating resin in step a.) is preferably from 100:1 to 2:1.

[0066] Preferably, an inorganic metal salt solution is used as the aqueous metal ion solution in step a.). The inorganic metal salt used is particularly preferably a nitrate, chloride or sulfate. Very particular preference is given to using metal sulfates. Cobalt(II) sulfate, nickel(II) sulfate and aluminum(III) sulfate are preferably used.

[0067] In another preferred embodiment, in step a.), the chelating resin containing the functional groups of the structural unit (I) is loaded with aluminum ions, which may contain other metal ions, but no zinc ions are present.

[0068] In step a.) preferably a chelating resin containing functional groups of structural unit (I) is used at a specific flow rate of 2 to 10 bed volumes / hour (BV / h).

[0069] Preferably, in step a.), 0.5 to 1.5 equivalents (Eq) of the chelating resin containing the functional groups of the structural unit (I) are used per equivalent (Eq) of the aluminum ions and / or zinc ions.

[0070] In step a.), preferably the chelating resin containing the functional group of structural unit (I) is loaded with metal ions at a pH of 1.5 to 6.0. Because the metal ions used constitute Lewis acids, this pH is often already present in the aqueous solution used. If there is no such pH, ​​then an acid, preferably an inorganic acid, can be used to adjust the pH. For this purpose, preferably sulfuric acid, hydrochloric acid or nitric acid is used. Particularly preferably sulfuric acid is used.

[0071] Step b.)

[0072] In step b.), aluminum ions and / or zinc ions are eluted from the chelating resin containing the functional groups of the structural unit (I). In step a.), trivalent aluminum ions are preferably used and eluted in step b.). In step a.), divalent zinc ions are preferably used and eluted in step b.). Elution is preferably carried out using an alkali metal hydroxide solution. Preferably, aluminum ions are eluted in step b.).

[0073] The process according to the invention, in which an alkali metal hydroxide solution and / or an ammonium hydroxide solution is used to selectively remove aluminum ions and / or zinc ions from a polymer containing aminomethylphosphonic acid groups and / or a chelating resin containing a functional group of structural unit (I), has created a method for selectively treating metallic lithium-containing waste from spent batteries. DETAILED DESCRIPTION

[0074] method

[0075] ICP

[0076] The ion concentration can be determined by methods known to the person skilled in the art from the prior art.The ion concentration is preferably determined in the method according to the invention by inductively coupled plasma spectroscopy (ICP).

[0077] In this case the mobile phase from the ion exchanger column was divided into 10 ml portions and analyzed by ICP and the ion concentration was determined.

[0078] Determination of total capacity

[0079] The total capacity of the chelating resin containing the functional groups of the structural unit (I) is determined according to DIN 54403 (Testing of ion exchangers—Determination of the total capacity of cation exchangers).

[0080] Determination of polymer diameter

[0081] The diameter of the polymer is determined in accordance with DIN 54407: Testing of ion exchange resins-Determination of bead size distribution. The diameter d50 is the diameter of the polymer or polymer particles at which 50% of the polymer falls through a sieve with a mesh size of 0.5 mm and 50% is retained.

[0082] Examples

[0083] Example 1

[0084] A. Loading the macroporous, monodisperse chelating resin containing the functional group of structural unit (I) with aluminum, nickel and cobalt

[0085] 200 ml of a chelating resin containing a functional group of structural unit (I) in the form of H (where R1 and R 2 independently -CH2PO(OX 1 )2 and -CH2PO(OH)OX 2 , where X 1 and X 2 =H( MDS TP 260, degree of substitution of aminomethyl groups by phosphonic acid groups = 2.0, total capacity 3.2 mol / L, H form, d 50 0.385 mm, monodisperse and macroporous)) were dispersed in deionized water and adjusted to pH = 4 with H2SO4 in a beaker under stirring. This was followed by the gradual addition of 250 ml of Co 2 + / Ni 2+ / Al 3+ Sulphate solution, this sulphate solution has 6.95g (0.118mol / 0.027g / L) cobalt, 6.93g (0.118mol) nickel and 3.20g (0.118mol) aluminium.During the intercalation of solution, the pH in the supernatant of ion exchanger drops to 1.9 from 4.0.Then supernatant is decanted out completely and volume measurement is carried out.Resin is washed with deionized water several times and suction is carried out to remove attached Co, Ni, Al (850ml washing water).The load capacity of the resin of the functional group that contains structural unit (I) is calculated by the minimization of Al, Ni and Co in the supernatant, and is 10.9g / L (0.4mol / L) for Al, 0.8g / L (0.0135mol / L) for Ni and 1.1g / L (0.0135mol / L) for Co.37.8% of the total capacity of resin is loaded with aluminium ion.

[0086] B. Selective aluminum elution with NaOH and regeneration by dilute sulfuric acid

[0087] In the next step, under stirring at 80 ℃ through 3 hours time period with 100ml of 9 % by weight of NaOH aqueous solution elution 20ml from the functional group containing structural unit (I) of A. Then decant alkaline solution. After this, some fully regenerated resins are dried and digested in microwave. Aluminum, nickel and cobalt concentrations are determined by ICP (inductively coupled plasma spectrometer). Aluminum concentration is lower than detection limit. Nickel and cobalt concentrations on the functional group containing structural unit (I) remain unchanged within the scope of detection limit. Remaining chelating resin is fully washed and under stirring at room temperature through 1 hour time period with 100ml of 15 % by weight H SO Regeneration. After carrying out washing steps with 80mL deionized water, remove supernatant NaOH. By adding 15 % by weight H SO The nickel and cobalt retained on the ion exchanger are eluted to almost 100 % by weight within the scope of detection limit.

Claims

1. A method for eluting aluminum ions and / or zinc ions, It is characterized in that The aminomethylphosphonic acid group-containing polymer or its salt at least partially loaded with aluminum ions and / or zinc ions is mixed with a base selected from the group consisting of alkali metal hydroxides and ammonium hydroxide and mixtures of these bases, and the aluminum ions and / or zinc ions are eluted.

2. The method according to claim 1, It is characterized in that An aminomethylphosphonic acid group-containing polystyrene-divinylbenzene copolymer was used as the aminomethylphosphonic acid group-containing polymer.

3. The method according to claim 1 or 2, It is characterized in that The average degree of substitution of aminomethyl groups by phosphonic acid groups in the polymer containing aminomethylphosphonic acid groups is from 1.4 to 2.

0.

4. The method according to at least one of claims 1 to 3, It is characterized in that The base does not contain any potassium oxalate.

5. The method according to at least one of claims 1 to 4, It is characterized in that The polymer has a diameter (d 50 ).

6. The method according to claim 5, It is characterized in that At least 90% by volume or 90% by mass of the particles have a diameter within + / - 10% of the most common diameter.

7. The method according to at least one of claims 1 to 6, It is characterized in that A 6% to 12% by weight aqueous solution of an alkali metal hydroxide is used.

8. The method according to at least one of claims 1 to 7, It is characterized in that The method involves the elution of aluminum ions.

9. The method according to at least one of claims 1 to 8, It is characterized in that The polymer containing aminomethylphosphonic acid groups is a chelating resin containing a functional group of structural unit (I). in is a polystyrene copolymer backbone, and R 1 and R 2 may be the same or different and are independently -CH 2 PO(OX 1 ) 2 and -CH 2 PO(OH)OX 2 or hydrogen, where R 1 and R 2 cannot be both hydrogen and X 1 and X 2 is independently hydrogen, sodium, potassium or lithium.

10. A method for eluting aluminum ions and / or zinc ions, It is characterized in that In step a.), at least one chelating resin containing a functional group of structural unit (I) is reacted with in is a polystyrene copolymer backbone, and Where R 1 and R 2 , X 1 and X 2 With the definitions given above, contacting the chelating resin with an aqueous metal ion solution containing aluminum ions and / or zinc ions and optionally additional metal ions, and In step b.), the aluminum ions and / or zinc ions are eluted with an aqueous alkali metal hydroxide solution and / or an aqueous ammonium hydroxide solution.

11. The method according to claim 10, It is characterized in that R 1 and R 2 may be the same or different and are independently -CH 2 PO(OX 1 ) 2 and -CH 2 PO(OH)OX 2 .

12. The method according to claim 11, It is characterized in that X 1 and X 2 =H.

13. The method according to at least one of claims 10 to 12, It is characterized in that In step a.) an aqueous metal ion solution of aluminum ions, nickel ions and cobalt ions is applied to the chelate resin.

14. The method according to claim 13, It is characterized in that The molar ratio of aluminum ions to the nickel ions and / or the cobalt ions in step a.) is from 0.5 to 1.

5.

15. The method according to at least one of claims 10 to 14, It is characterized in that The aqueous metal ion solution containing aluminum ions, nickel ions and cobalt ions applied to the chelate resin in step a.) has a pH of 1.5 to 6.0.

Citation Information

Cited By

  • Purification method for reducing aluminum ion residues in leucine

    CN120058543A