Use of nickel-iron-chromium alloy with high resistance in highly corrosive environments and simultaneously good processability and strength
By preparing nickel-iron-chromium alloy powder with specific composition, the problems of corrosion resistance and processing difficulty of existing nickel-iron-chromium alloys in highly corrosive environments have been solved. Good corrosion resistance and machinability in highly corrosive environments have been achieved, making it suitable for additive manufacturing and traditional processing methods.
Patent Information
- Application Number
- CN202380029908.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-28
- Filing Date
- 2023-04-20
- Publication Date
- 2024-11-08
AI Technical Summary
Existing nickel-iron-chromium alloys have insufficient resistance to high-temperature corrosion in highly corrosive environments such as carburizing, sulfidation, and chlorination environments, and also present problems of processing difficulty and welding difficulty.
A nickel-iron-chromium alloy powder with a specific composition range is used, containing 35.0% to 38% nickel, 26.0% to 30.0% chromium, 0.7% to 1.50% silicon, and 0.40% to 1.30% aluminum. Spherical powder particles are prepared by vacuum induction inert gas atomization device to satisfy the relationship Fc=-1.2+0.29*Ni-4.6*Si-4.4*Al≤2.5. Oxyphilic elements such as cerium, lanthanum, yttrium, zirconium, and hafnium are added to improve corrosion resistance.
It exhibits good resistance to high-temperature corrosion in highly corrosive environments, possesses sufficient machinability and weldability, and has similar high-temperature strength at 500°C, making it suitable for additive manufacturing and conventional processing methods.
Smart Images

Figure CN118922575A_ABST
Abstract
Description
[0001] The present invention relates to the use of a nickel-iron-chromium alloy having good high temperature corrosion resistance in a highly corrosive environment and at the same time good machinability and strength.
[0002] Austenitic nickel-iron-chromium alloys with different nickel, chromium and iron contents have long been used in furnace construction and in the chemical and petrochemical industries. For this application, good high-temperature corrosion resistance, even in highly corrosive environments, such as carburizing, sulfiding and chlorination, as well as good high-temperature strength are required.
[0003] In general, it should be noted that the high-temperature corrosion resistance of the alloys listed in Table 1 increases with increasing chromium content. All these alloys form a chromium oxide layer (Cr2O3) with a more or less closed silicon oxide layer underneath. Trace additions of strongly oxygen-affinity elements such as yttrium or cerium improve the corrosion resistance. During use in the application area, the chromium content is slowly consumed for the construction of the protective layer. The service life of the material is therefore extended by a higher chromium content, since a higher content of elemental chromium forming the protective layer delays the time when the chromium content falls below a critical limit and forms other oxides besides Cr2O3, which are, for example, iron-containing and nickel-containing oxides. The high-temperature corrosion resistance can be further increased by adding silicon or aluminum. Starting from a certain minimum content, these elements form a closed layer under the chromium oxide layer and in this way reduce the consumption of chromium.
[0004] In carburizing environments (CO, H2, CH4, CO2, H2O mixtures), carbon can penetrate into the material and thus lead to the formation of internal carbides. This leads to a loss of notched impact strength. Transformation processes may occur due to the loss of chromium in the matrix.
[0005] High carburization resistance is obtained by materials with low carbon solubility and low carbon diffusion rate. Therefore, nickel alloys are generally more resistant to carburization than iron-based alloys, because the carbon diffusion and carbon solubility in nickel are lower than those in iron. An increase in the chromium content brings higher carburization resistance by forming a protective chromium oxide layer, unless the oxygen partial pressure in the gas is insufficient for the formation of this protective chromium oxide layer. Under very low oxygen partial pressures, materials that form a silicon oxide layer or even a more stable aluminum oxide layer can be used, both of which can form a protective oxide layer even at much lower oxygen contents.
[0006] In carburizing and sulfiding environments with low oxygen partial pressure (mixtures of CO, H2, H2O, CO2, H2S), sulfur may penetrate into the material, resulting in the formation of sulfides. The melting point may also drop to very low values (635°C for Ni-Ni3S2 eutectic and 988°C for Fe-FeS eutectic). In sulfiding environments, nickel-iron-chromium alloys with high nickel content are generally more sensitive than nickel-iron-chromium alloys with high iron content. Here, further improvement of high temperature corrosion resistance can also be achieved by adding silicon or aluminum.
[0007] In a chlorinated environment with low oxygen partial pressure, volatile metal chlorides with high vapor pressure and / or low melting point may form, resulting in high corrosion rates. High levels of chromium and / or nickel improve corrosion resistance.
[0008] In DE 41 30 139 C1, a heat-resistant, hot-formable austenitic nickel alloy is described, which consists of (in mass %) 0.05% to 0.15% carbon, 2.5% to 3.0% silicon, 0.2% to 0.5% manganese, up to 0.015% phosphorus, up to 0.005% sulfur, 25% to 30% chromium, 20% to 27% iron, 0.05% to 0.15% aluminum, 0.001% to 0.005% calcium, 0.05% to 0.15% rare earth elements, 0.05% to 0.20% nitrogen, the remainder being nickel and impurities usually associated with melting.
[0009] The alloy described in DE 41 30 139 C1 is known by the designation “NiCr28FeSiCe”, alloy 45TM, Nicrofer45TM or by the material number 2.4889 and will be referred to as “45TM” hereinafter.
[0010] Alloy 45TM is very resistant in carburizing and sulfiding media, which is why it is suitable for use in waste incineration plants or coal gasification plants. Figure 1 The metallographically measured corrosion attack depths in various alloys as a function of the temperature of the various alloys after exposure to H2S-containing gases for 2100 hours in the PRENFLO coal gasification pilot plant in Fürstenhausen are shown. Table 1 shows the composition of the investigated alloys according to the prior art. High chromium and high silicon contents significantly reduce the corrosion attack depth. A silicon oxide layer which imparts a high corrosion resistance to the material can be formed under the protective chromium oxide layer by means of a high silicon content ≥ 2.5%. 45TM with 26% to 29% chromium and 2.5% to 3% silicon shows the smallest corrosion attack depth at all temperatures, followed by AC66 with 26% to 28% chromium and up to 0.3% silicon.
[0011] However, the alloy 45TM is extremely difficult to process. This can be shown, for example, by crack formation during hot forming. 45TM is also prone to crack formation during welding, which makes the same type of welding (using welding fillers within the composition range of the materials to be welded) impossible for corrosion protection reasons and makes the practical use of the material more difficult. As reasons for the increased formation of hot cracks, it is mentioned that for austenitic FeCrNi weld metals with primary austenite solidification, there is the formation of low-melting phases due to silicon enrichment at the austenite grain boundaries (Fe-Fe2Si eutectic: 1212°C; NNiSi-Ni3Si2 eutectic: 964°C and NiSi eutectic: 996°C) and an extended solidification range.
[0012] In contrast, alloy AC66 (composition see Table 1) has adequate weldability and machinability, but is not very corrosion resistant in coal gasification units, such as Figure 1 shown.
[0013] The demands on the material are further increased when chlorine attack is added to the carburizing and sulfiding conditions, as occurs in coal gasification plants, waste incineration plants, etc.
[0014] For materials used in carburizing, sulfiding and chlorinated environments (especially atmospheres), a compromise must be reached in terms of composition.
[0015] The high temperature strength is improved in particular by a high carbon content. However, high contents of mixed crystal solidifying elements such as chromium, aluminum, silicon, molybdenum and tungsten can also improve the high temperature strength.
[0016] US 6,623,869 B1 describes a metal material containing the following components in mass %: no more than 0.2% carbon, 0.01-4% silicon, 0.05-2% manganese, no more than 0.04% phosphorus, no more than 0.015% sulfur, 10-35% chromium, 30-78% nickel, not less than 0.005% but less than 4.5% aluminum, 0.005-0.2% nitrogen, and one or two of 0.015-3% copper and 0.015-3% cobalt, wherein the balance is mainly iron. The value of 40Si+Ni+5Al+40N+10(Cu+Co) is not less than 50, wherein the symbol of the element represents the alloy content of each element. The metal material has excellent corrosion resistance in an environment where metal dusting may occur, and can therefore be used in furnace tubes, piping systems, heat exchange tubes, etc. in oil refining devices or petrochemical devices. The durability and safety of the device can be significantly improved.
[0017] US 3,833,358 A describes an iron-based fireproof alloy which provides high resistance to creep, thermal shock, thermal fatigue and intergranular oxidation, as well as good weldability, and consists essentially of the following elements (in parts by weight):
[0018]
[0019]
[0020] In this case, the weight percentages of the above elements satisfy the following formula: 30*C%+Ni%+0.5*Mn%+16*N%=
[0021] Cr%+0.5*(Nb+1 / 2Ta)%+3.5*Ti%+1.5*Si%+Mo%+(11+ / -2)%
[0022] A=B+ / -20%
[0023] Wherein A=30*C%B=2*Ti%+6*(Nb+1 / 2Ta)%.
[0024] US 3,865,581 A describes a heat-resistant alloy having hot formability, which contains 0.01% to 0.5% C, 0.01% to 2.0% Si, 0.01% to 3.0% Mn, 22% to 80% Ni and 10% to 40% Cr as main components, and one or two of 0.0005% to 0.20% B and 0.001% to 6.0% Zr, and in addition one or more of 0.001% to 0.5% Ce, 0.001% to 0.2% Mg and 0.001% to 1.0% Be, the balance being iron and unavoidable impurities. It is suitable for furnace construction (burner nozzle, protective shell, thermocouple protection tube, etc.).
[0025] DE 1024719 A describes a method for adding cerium and / or lanthanum to nickel-iron alloys. It relates to a hot workable alloy characterized by the following composition: 0% to 0.5% carbon, 10% to 60% of one or more of the elements chromium, molybdenum and tungsten (wherein the amount of each of these elements does not exceed 30%), 0% to 73% iron, 0.02% to 1.10% of cerium or lanthanum or both, the remainder being 4% to 70% nickel including impurities, provided that the content of rare earth metals is matched to the nickel content in the following manner:
[0026]
[0027] In EP 0 812 926 A1, a nickel-based alloy is described, the strength of which increases during use and which consists of 0.06%-0.14% carbon, 35%-46% nickel, 22.5%-26.5% chromium, 0%-1.5% manganese, 0.5%-2% silicon, 0.1%-1% titanium, 0.05%-2% aluminum, 1%-3% molybdenum, 0.2% niobium, 0.1%-1% tantalum, 0-0.3% tungsten, 0-0.008% boron, 0%-0.05% zirconium, the remainder iron and incidental impurities.
[0028] WO 2007 / 124996 A1 describes a reaction vessel for producing hydrogen sulfide by reaction between sulfur and hydrogen, wherein the reaction vessel and optionally the connecting lines and fittings and measuring and control elements consist partly or completely of an aluminum-containing material that is resistant to the reaction mixture. In particular, the material comprises the following components: 0%-0.3% C, 0%-2.5% Si, 0%-2.5% Mn, 0%-0.1% P, 0%-0.3% S, 15.0%-28.0% Cr, 0%-1.0% Cu, 0%-balance % Fe, 1.0%-5.0% Al, 0%-2.5% Co, 0%-1.5% Ti, 0%-0.4% Y and up to 70% Ni (in wt %).
[0029] DE 10 2007 005 605 A1 describes an iron-nickel-chromium-silicon alloy having (in wt. %) 34% to 42% nickel, 18% to 26% chromium, 1.0% to 2.5% silicon with additions of 0.05% to 1% Al, 0.01% to 1% Mn, 0.01% to 0.26% lanthanum, 0.0005% to 0.05% magnesium, 0.01% to 0.14% carbon, 0.01% to 0.14% nitrogen, maximum 0.01% sulfur, maximum 0.005% boron, the remainder iron and customary process-related impurities. This alloy is used for heating elements.
[0030] US 5,021,215 A discloses a high-strength heat-resistant steel having improved formability and consisting essentially of the following components (weight %):
[0031]
[0032] (Mo+1 / 2W=3.0% or less)
[0033] The balance is Fe and unexpected impurities, wherein the impurities oxygen and nitrogen are limited to 50 ppm or less and 200 ppm or less, respectively, and wherein the austenite grain size number is limited to No. 4 or coarser.
[0034] JPS 56163244 A describes improving the hot workability and oxidation resistance of austenitic steels by adding specific amounts of C, Si, Mn, Ni, Cr, Al, B, rare earth elements and Ca to the steel. This is achieved by an austenitic steel containing the following composition in weight %: <0.2% C, 1.5%-3.5% Si, <2% Mn, 8%-35% Ni, 15%-30% Cr, <2% Al, 0.0005%-0.005% B, 0.005%-0.1% rare earth elements and 0.0005%-0.02% Ca, or, if necessary, additionally introducing 0.0005%-0.03% Mg. The austenitic steel obtained in this way is refined in a standard steelmaking furnace and the molten steel is formed into billets, which are then hot rolled.
[0035] US 7,118,636 B2 describes a nickel-iron-chromium alloy containing strengthening phases which is able to maintain a fine grain structure during forging and during processing of the alloy at high temperatures. The alloy contains sufficient amounts of titanium, zirconium, carbon and nitrogen to form fine titanium and zirconium nitrides, even if these nitrides are close to their solubility limits in the molten state of the alloy. During the manufacture of articles from this alloy by thermomechanical processing, a dispersion of fine titanium carbonitride and zirconium carbonitride precipitates is formed during solidification of the melt and is retained in the alloy during subsequent processing steps (at high temperatures), thereby inhibiting austenite grain growth. The nickel-iron-chromium alloy contains less than 0.05 weight percent niobium, at least 0.05 weight percent zirconium, at least 0.05 weight percent carbon, at least 0.05 weight percent nitrogen, a carbon-nitrogen weight ratio of at least 1:2 to less than 1:1, sufficient titanium, zirconium and / or aluminum (so as to be free of chromium carbides), and sufficient amounts of titanium, zirconium, carbon and nitrogen (so as to form a uniform dispersion of finely divided titanium and zirconium carbonitrides, in sufficient amounts to obtain [(Ti)] carbonitride precipitates in the molten state of the alloy) x Zr 1-x )(C y N 1-y )]). In addition, this nickel-iron-chromium alloy is composed of: about 32% to about 38% by weight iron, about 22% to 28% by weight chromium, about 0.10% to about 0.60% titanium, about 0.05% to about 0.30% zirconium, about 0.05% to about 0.30% carbon, about 0.05% to about 0.30% nitrogen, about 0.05% to about 0.5% aluminum, up to 0.99% molybdenum, up to about 0.01% boron, up to about 1% silicon, up to about 1% manganese, the balance nickel and unexpected impurities.
[0036] JPS 57134544 A describes improving the stress corrosion cracking resistance of oil drill pipes by adding a specific amount of Mo, W, etc. to high chromium-nickel steel as a pipe material. For this purpose, an alloy steel having the following composition: <0.10% C, <1.0% Si, <2.0% Mn, <0.030% P, <0.005% S, <0.5% Al, 22.5%-30% Cr, 25%-60% Ni and Mo and / or W, and satisfying the following formula is used:
[0037] Cr(%)+10*Mo(%)+5*W(%)≥70%
[0038] 4%≤Mo(%)+1 / 2W(%)<8%.
[0039] This steel is used for pipes for oil drilling used in highly corrosive and harsh environments such as oil sources, natural gas sources, etc. <1% Cu and / or <2% Co and / or <0.10% of one or more rare earth elements, <0.20% Y, <0.10% Mg, <0.10% Ca and <0.5% Ti can be added to the alloy. Oil drilling pipes with excellent resistance to stress corrosion cracking in highly corrosive environments of oil sources containing H2S, CO2 and Cl can be manufactured.
[0040] The basic object of the present invention is therefore to devise a use for a nickel-iron-chromium alloy which
[0041] a) In highly corrosive environments, such as carburizing, sulfiding and chlorination environments, it has good high temperature corrosion resistance comparable to Alloy 45TM,
[0042] b) have adequate machinability, in particular weldability, comparable as closely as possible to that of alloy AC66, and
[0043] c) Having sufficient high temperature strength at 500°C similar to that of alloy AC66.
[0044] The basic task of the present invention is achieved by using a nickel-iron-chromium alloy as a powder, which has excellent high-temperature corrosion resistance, wherein the powder consists of spherical particles with a size of 5 to 250 μm and wherein the alloy contains (in mass %):
[0045] 35.0% to 38% nickel,
[0046] 26.0% to 30.0% chromium,
[0047] >0.7% to 1.50% silicon,
[0048] 0.40% to 1.30% aluminum,
[0049] 0.00% to 1.0% manganese,
[0050] 0.0001% to 0.05% magnesium and / or calcium, respectively,
[0051] 0.015% to 0.12% carbon,
[0052] 0.001% to 0.150% nitrogen,
[0053] 0.001% to 0.030% phosphorus,
[0054] 0.0001% to 0.100% oxygen,
[0055] Maximum 0.010% sulfur,
[0056] Less than 1.0% molybdenum,
[0057] Less than 1.0% cobalt,
[0058] Less than 0.5% copper,
[0059] Less than 1.0% tungsten,
[0060] The balance is iron and usually process-related impurities, where the following relationship must be satisfied:
[0061] Fc=-1.2+0.29*Ni-4.6*Si-4.4*Al≤2.5(1a),
[0062] Herein, Ni, Si and Al are the concentrations of the elements in mass %.
[0063] Advantageous further developments of the subject matter of the invention can be inferred from the associated dependent claims.
[0064] The nickel content is between 35.0% and 38.0%, wherein the preferred content can be adjusted within the following numerical ranges:
[0065] -35 or >35.0 to <38.0%
[0066] -35 or >35.0 to 37 or <37.0%.
[0067] The value of the element chromium ranges between 26.0% and 30.0%, wherein the preferred range can be adjusted as follows:
[0068] ->26.0 to <30.0%
[0069] -27.0 or >27.0 to 30.0 or <30.0%
[0070] -28.0 or >28.0 to 30.0 or <30.0%
[0071] The silicon content is between >0.70% and 1.50%. Preferably, silicon can be adjusted in the alloy within the following value range:
[0072] ->0.70 to <1.50%.
[0073] -0.80 or >0.80 to 1.50 or <1.50%
[0074] -0.90 or >0.90 to 1.50 or <1.50%
[0075] -0.80 or >0.80 to 1.50 or <1.50%
[0076] -0.80 or >0.80 to 1.45 or <1.45%.
[0077] The aluminum content is between 0.40% and 1.30%, wherein the preferred aluminum content can also be adjusted as follows:
[0078] ->0.40 to <1.30%
[0079] -0.50 or >0.50 to 1.30 or <1.30%
[0080] -0.50 or >0.50 to 1.20 or <1.20%
[0081] -0.50 or >0.50 to 1.10 or <1.10%
[0082] -0.60 or >0.60 to 1.10 or <1.10%.
[0083] The same is true for manganese, which is present in the alloy in a content of 0.0% to 1.0%. Alternatively, the following ranges of values are also contemplated:
[0084] -> 0.0 to <1.00%
[0085] ->0.0 to 0.50 or <0.50%
[0086] ->0.0 to 0.05 or <0.05%
[0087] -0.005 or >0.005 to 0.20 or <0.20%
[0088] -0.005 or >0.005 to 0.10 or <0.10%.
[0089] Magnesium and / or calcium are also present in a content of 0.0001% to 0.05%. Preferably, there is the possibility of adjusting these elements in the alloy as follows:
[0090] -0.0001% to 0.030%
[0091] -0.0001% to 0.020%
[0092] -0.0002% to 0.015%
[0093] -0.0010% to 0.010%.
[0094] The alloy contains 0.015% to 0.12% carbon. Preferably, this can be adjusted in the alloy within the following value range:
[0095] ->0.015 to <0.12%.
[0096] -0.03 or >0.03 to 0.10 or <0.10%
[0097] -0.04 or >0.04 to 0.10 or <0.10%
[0098] -0.05 or >0.05 to 0.10 or <0.10%
[0099] -0.05 or >0.05 to 0.09 or <0.09%.
[0100] The same is true for the element nitrogen, which is present in a content between 0.001% and 0.150%. The preferred content can be specified as follows:
[0101] ->0.001 to <0.150%
[0102] -0.010 or >0.010 to 0.140 or <0.140%
[0103] -0.020 or >0.020 to 0.140 or <0.140%
[0104] -0.050 or >0.050 to 0.140 or <0.140%.
[0105] The alloy also contains phosphorus in an amount between 0.001% and 0.030%. The preferred amounts may be specified as follows:
[0106] -0.001% to 0.015%.
[0107] The alloy also contains oxygen in an amount between 0.0001% and 0.100%.
[0108] Elemental sulfur may be present in the alloy in an amount up to 0.010%. Preferred contents may be specified as follows:
[0109] - Sulfur 0.008% max.
[0110] Molybdenum is contained in the alloy in an amount of less than 1.0%. The molybdenum content may also be limited as follows:
[0111] -Mo up to 0.50% or <0.50%
[0112] -Mo up to 0.20% or <0.20%
[0113] -Mo up to 0.10% or <0.10%
[0114] -Mo up to 0.05% or <0.05%
[0115] -Mo up to 0.02% or <0.02%
[0116] Furthermore, the alloy contains less than 1.0% cobalt. The cobalt content may also be limited as follows:
[0117] -Co max 0.50% or <0.50%
[0118] -Co max 0.20% or <0.20%
[0119] -Co max 0.10% or <0.10%
[0120] -Co max 0.05% or <0.05%
[0121] -Co max 0.015% or <0.015%.
[0122] Furthermore, the alloy may contain less than 0.5% copper. The copper content may also be limited as follows:
[0123] -Cu max 0.30% or <0.30%
[0124] -Cu max 0.10% or <0.10%
[0125] -Cu max 0.05% or <0.05%
[0126] -Cu max 0.015% or <0.015%
[0127] Tungsten is contained in the alloy in a content of up to 1.0%. The tungsten content may also be limited as follows:
[0128] -W < 1.0%
[0129] -W up to 0.50% or < 0.50%
[0130] -W up to 0.20% or < 0.20%
[0131] -W up to 0.10% or < 0.10%
[0132] -W 0.05% max or <0.05%
[0133] -W 0.02% max or <0.02%
[0134] The remainder of the alloy consists of iron and customary manufacturing-related impurities. The iron content can also be limited as follows:
[0135] -28.0 or >28.0 to 38.0%
[0136] -29.0 or >29.0 to 38.0%
[0137] -30.0 or >30.0 to 38.0 or <38.0%.
[0138] The following relationships between nickel, silicon and aluminum must be met to ensure adequate resistance in carburizing, sulfiding and chlorinated environments.
[0139] Fc=-1.2+0.29*Ni-4.6*Si-4.4*Al≤2.5(1a),
[0140] Herein, Ni, Si, Al and Si are the concentrations of the elements in mass %.
[0141] The preferred range can be adjusted as follows:
[0142] Fc=-1.2+0.29*Ni-4.6*Si-4.4*Al≤1.5(1b) Fc=-1.2+0.29*Ni-4.6*Si-4.4*Al≤1.0(1c)
[0143] Additions of oxygen-philic elements such as cerium, lanthanum, yttrium, zirconium and hafnium improve corrosion resistance. They do this by being built into the oxide layer, where they block the diffusion paths of oxygen at the grain boundaries.
[0144] If necessary, the alloy may contain 0.001% to 0.20% of one or more of the elements cerium, lanthanum, yttrium, zirconium and hafnium, respectively, wherein the following formula must be satisfied:
[0145] FRE=0.714*Ce+0.720*La+1.124*Y+1.096*Zr+0.560*Hf≤0.10(2a)
[0146] wherein Ce, La, Y, Zr and Hf are the concentrations of the elements in mass %.
[0147] Preferably, in the presence of at least one of the elements cerium, lanthanum, yttrium, zirconium and hafnium, the FRE may be adjusted as follows
[0148] FRE=0.714*Ce+0.720*La+1.124*Y+1.096*Zr+0.560*Hf≤0.075(2b)
[0149] FRE=0.714*Ce+0.720*La+1.124*Y+1.096*Zr+0.560*Hf≤0.065(2c)
[0150] Alternatively, in the presence of cerium and lanthanum, cerium mixed metal (abbreviated as CeMM) can also be used in a content of 0.001% to 0.20%, wherein the FRE must be modified as follows:
[0151] FRE=0.716*CeMM+1.124*Y+1.096*Zr+0.560*Hf≤0.10(3a)
[0152] wherein CeMM, Y, Zr and Hf are the concentrations of the elements in mass %.
[0153] Preferably, in case of adding cerium mixed metal, the FRE can be adjusted as follows:
[0154] FRE=0.716*CeMM+1.124*Y+1.096*Zr+0.560*Hf≤0.075(3b)
[0155] FRE=0.716*CeMM+1.124*Y+1.096*Zr+0.560*Hf≤0.065(3c)
[0156] Preferably, cerium, lanthanum, cerium mixed metal, zirconium and hafnium may be included in the alloy within the following value ranges:
[0157] ->0.001 to <0.20%
[0158] -0.001 or >0.001 to 0.15 or <0.15%
[0159] -0.001 or >0.001 to 0.10 or <0.10%
[0160] -0.001 or >0.001 to 0.08 or <0.08%
[0161] -0.001 or >0.001 to 0.05 or <0.05%
[0162] -0.001 or >0.001 to 0.04 or <0.04%.
[0163] -0.01 or >0.01 to 0.04 or <0.04%
[0164] Preferably, yttrium may be included in the alloy within the following value ranges:
[0165] ->0.001 to <0.20%
[0166] -0.001 or >0.001 to 0.15 or <0.15%
[0167] -0.001 or >0.001 to 0.10 or <0.10%
[0168] -0.001 or >0.001 to 0.08 or <0.08%
[0169] -0.01 or >0.01 to 0.08 or <0.08%
[0170] -0.01 or >0.01 to <0.045%.
[0171] Optionally, elemental titanium may be included in the alloy in an amount of 0.0% to 0.50%. Preferably, titanium may be included in the alloy in the range of the following values:
[0172] -> 0.0 to < 0.50%
[0173] ->0.0 to 0.50 or <0.50%
[0174] -0.001 or >0.001 to 0.20 or <0.20%
[0175] -0.001 or >0.001 to 0.15 or <0.15%
[0176] -0.001 or >0.001 to 0.10 or <0.10%
[0177] -0.001 or >0.001 to 0.05 or <0.05%
[0178] -0.001 or >0.001 to 0.04 or <0.04%.
[0179] -0.005 or >0.005 to 0.20 or <0.20%.
[0180] -0.010 or >0.010 to 0.20 or <0.20%.
[0181] Optionally, the niobium element may be adjusted to a content of 0.0% to 0.2% in the alloy. Preferably, niobium may be present in the alloy within the following value range:
[0182] -> 0.0 to < 0.20%
[0183] ->0.0 to 0.15 or <0.15%
[0184] ->0.0 to 0.10 or <0.10%
[0185] ->0.0 to 0.05 or <0.05%
[0186] ->0.0 to 0.02 or <0.02%
[0187] -0.001 or >0.001 to 0.20 or <0.20%
[0188] -0.010 or >0.010 to 0.20 or <0.20%.
[0189] Optionally, 0.0% to 0.20% tantalum may be included in the alloy. Preferred contents may be specified as follows:
[0190] -> 0.0 to < 0.20%
[0191] ->0.0 to 0.10 or <0.10%
[0192] ->0.0 to 0.05 or <0.05%.
[0193] Optionally, the element boron may be included in the alloy in an amount of 0.0001% to 0.008%. Preferred amounts may be specified as follows:
[0194] - Boron 0.0005% to 0.008%
[0195] - Boron 0.0005% to 0.005%
[0196] - Boron 0.0005% to 0.004%.
[0197] Furthermore, up to 0.50% vanadium may be included in the alloy.
[0198] -V<0.50%
[0199] -V up to 0.40% or < 0.50%
[0200] -V up to 0.20% or <0.20%
[0201] -V up to 0.08% or <0.10%
[0202] -V up to 0.05% or <0.05%
[0203] Finally, as impurities, the contents of the elements lead, zinc and tin may also be specified as follows:
[0204] Pb 0.002% max., Zn 0.002% max., Sn 0.002% max.
[0205] The element beryllium can then be specified as follows:
[0206] Be is less than 0.001%,
[0207] The powder according to the invention is preferably produced in a vacuum induction inert gas atomization device (VIGA). For this purpose, the alloy is first melted, optionally in an open state or in a vacuum, and optionally subsequently remelted with ESU and / or VAR. The powder is then produced by atomization of the alloy melt in a vacuum induction inert gas atomization device (VIGA). In this device, the alloy is melted in a vacuum induction melting furnace (VIM) and introduced into a casting funnel leading to a gas nozzle, where the molten metal is atomized into metal particles with an inert gas at a high pressure of 5 to 100 bar. The melt is heated in a melting crucible to 5 to 400° C. above the melting point. The metal flow rate during the atomization process is 0.5 to 80 kg / min and the gas flow rate is 2-150 m 3 / min. By rapid cooling, the metal particles are solidified in a spherical shape (spherical particles). The inert gas used in the atomization process may contain 0.01% to 100% nitrogen as needed. The gas phase is then separated from the powder in one cycle, and the powder is then packaged.
[0208] In this process, the particles have a particle size of 5 to 250 μm, a pore area of 0.0% to 4% of the total area of the object being evaluated (pores > 1 μm), an entrained gas of 2 to up to about 8.5 g / cm 3 The alloy density is the bulk density of the alloy and is airtightly packaged under a protective atmosphere containing argon.
[0209] The particle size values of the powder range between 5 and 250 μm, with a preferred range between 5 and 150 μm, or between 10 and 150 μm. The preferred range is achieved by separating too fine and too coarse particles through sieving and screening processes. These processes are carried out under a protective gas atmosphere and can be carried out once or several times.
[0210] The powder has a gas inclusion of pore area (pores>1 μm) of 0.0% to 4% relative to the total area of the object being evaluated, wherein the preferred range is
[0211] 0.0% to 2%
[0212] 0.0% to 0.5%
[0213] 0.0% to 0.2%
[0214] 0.0% to 0.1%
[0215] 0.0% to 0.05%
[0216] The bulk density of the powder is 2, and the maximum can reach about 8.5g / cm 3The density of the alloy, the preferred range of which can be the following values
[0217] 4 to 5 g / cm 3
[0218] 2 to 8 g / cm 3
[0219] 2 to 7 g / cm 3
[0220] 3 to 6 g / cm 3
[0221] The amount of gas entrained in the powder is such that the manufactured components have an extremely low residual porosity.
[0222] The inert gas used for powder production may optionally be argon or a mixture of argon with 0.01% to <100% nitrogen. Possible limits for the nitrogen content may be
[0223] 0.01% to 80%
[0224] 0.01% to 50%
[0225] 0.01% to 30%
[0226] 0.01% to 20%
[0227] 0.01% to 10%
[0228] 0.01% to 10%
[0229] 0.1% to 5%
[0230] 0.5% to 10%
[0231] 1% to 5%
[0232] 2% to 3%
[0233] Alternatively, the inert gas may optionally be helium.
[0234] The inert gas should preferably have a purity of at least 99.996% by volume. In particular, the nitrogen content should be 0.0 to 10 ppmv, the oxygen content 0.0 to 4 ppmv, and the H2O content ≤ 5 ppmv.
[0235] In particular, the inert gas may preferably have a purity of at least 99.999% by volume. In particular, the nitrogen content should be 0.0 to 5 ppmv, the oxygen content 0.0 to 2 ppmv, and the H2O content ≤ 3 ppmv.
[0236] The dew point in the device is in the range of -10°C to -120°C. It is preferably in the range of -30°C to -100°C.
[0237] The pressure during powder atomization is preferably between 10 and 80 bar.
[0238] The powder produced from the alloy in this way can be used in any desired manufacturing process using powders for the production of components or layers on components.
[0239] The powder produced in this way can be used for the additive manufacturing of components or layers on components.
[0240] For additive manufacturing, terms such as generative manufacturing, rapid technology, rapid machining, rapid prototyping, etc. are also understood.
[0241] In general, the distinction here is:
[0242] 3D printing with powder,
[0243] Selective Laser Sintering and
[0244] Selective Laser Melting
[0245] Electron beam melting
[0246] Adhesive Jetting
[0247] Laser cladding
[0248] High-speed laser cladding
[0249] Ultra-high speed laser cladding
[0250] Selective electron beam welding, etc.
[0251] Components or layers on components produced by additive manufacturing accumulate to a layer thickness of 5 to 600 μm and have a texture immediately after production containing grains with an average grain size of 2 to 1000 μm extending in the stacking direction. The preferred range is between 5 and 600 μm.
[0252] The powders produced from this alloy can use spraying methods for the binder. In these methods, the components are built up in layers. However, in contrast to the laser melting method, an organic binder is used locally, which ensures that the powder particles are bonded together. After the binder has solidified, the so-called green body is separated from the unbound powder, which is then debindered and sintered.
[0253] For powders produced from alloys, methods and additional devices for preheating and postheating can be advantageous. For example, the EBM method (electron beam melting) can be considered. The powder bed is selectively melted layer by layer by an electron beam. This process is carried out under high vacuum. Therefore, the method is particularly suitable for hard materials with low ductility and / or for reactive materials. The preheating and / or postheating device can also be implemented in laser-based methods.
[0254] In addition, if desired, the powder produced from the alloy can be used to manufacture components by HIP (hot isostatic pressing) or conventional sintering-pressing and extrusion-pressing processes. In addition, a combined method including additive manufacturing and subsequent HIP treatment is possible. If desired, hot forming can also be performed subsequently and / or if desired, cold forming or alternation of hot forming and cold forming can be performed. For hot forming, the component can be optionally annealed at a temperature between 800°C and 1290°C for 0.1 hour to 70 hours, followed by hot forming, optionally with intermediate annealing between 800°C and 1290°C for 0.05 hour to 70 hours. The surface of the material can be optionally (even multiple times) subjected to chemical and / or mechanical scouring for cleaning during this period and / or at the end of hot forming. For cold forming, cold forming with deformation up to 98% can be carried out, optionally with an intermediate annealing between 800°C and 1250°C for a duration of 0.05 minutes to 70 hours, optionally under a protective gas such as argon or hydrogen, followed by cooling in air, in an agitated annealing atmosphere or in a water bath.
[0255] The components or layers on the components produced by the various methods from the powder can optionally be solution annealed in a temperature range of 700° C. to 1250° C. for 0.1 minutes to 70 hours, optionally under a protective gas such as argon or hydrogen, followed by cooling in air, in a stirred annealing atmosphere or in a water bath. Afterwards, the surface can optionally be cleaned or processed by pickling, sandblasting, grinding, turning, peeling, milling. Even as early as before annealing, this processing can optionally be carried out partially or completely.
[0256] The components or layers on the components produced from this powder have an average grain size of 2 μm to 2000 μm after annealing. The preferred range is between 20 and 600 μm.
[0257] Components or layers on components produced from the powders according to the invention are preferably used in areas where highly corrosive conditions prevail, such as carburizing or sulfiding or chlorinating environments, or carburizing and chlorinating environments, or carburizing and chlorinating environments, or carburizing and sulfiding and chlorinating environments, especially atmospheric air. Such environments are found, for example, in components in waste incineration plants, pyrolysis plants, refineries, the chemical industry, coal gasification plants and industrial furnace construction, for activated carbon filters, waste pyrolysis and precious metal recovery.
[0258] Specific implementation form:
[0259] Determinations performed
[0260] Evaluation of the resistance to high temperature corrosion in highly corrosive conditions, exemplified by carburizing and sulfiding as well as chlorinated environments, is carried out by testing the material's resistance at high temperatures in a flowing forming gas atmosphere having these characteristics (at Dechema).
[0261] For this purpose, cut pieces with the dimensions 20x8x4 mm from the semi-finished product of the corresponding alloy. 3 The samples are then provided with a 3 mm hole and thereafter wet ground with SiC paper to 1200 grit (grain size about 15 μm). The samples are degreased and cleaned in an ultrasonic bath containing isopropanol. Through the hole, each sample is suspended in a reaction vessel above a ceramic crucible in order to capture any flaked corrosion products, and the mass of the flaked material can be determined by weighing the crucible containing the corrosion products. The sum of the mass of the flaked material and the change in the mass of the sample is the total change in the mass of the sample. The specific mass change is the mass change relative to the surface area of the sample. These are described below. netto Expresses specific net mass change, m brutto Expresses the change in total mass, m spall Indicates the specific mass change of the exfoliated oxide.
[0262] A gas mixture of 60% CO, 30% H2, 4% CO2, 1% H2S, 0.05% HCl and 3.95% H2O was passed through the space of the reaction vessel. This mixture has carburizing (60% CO), sulfiding (1% H2S) and chlorinating (0.05% HCl) effects. The test was carried out at 500°C. The test duration was 1056 hours, divided into 11 cycles of 96 hours each. Two specimens of each alloy were used in each test. The indicated value is the average of these two specimens.
[0263] In the following study, after 1056 hours,
[0264] -≤2.0mg / cm 2 Total mass increase (4)
[0265] The alloy is considered resistant in carburizing, sulfiding and chloriding environments.
[0266] This is the case when the following relationship is satisfied between nickel, silicon and aluminum:
[0267] Fc=-1.2+0.29*Ni-4.6*Si-4.4*Al≤2.5(1a),
[0268] Herein, Ni, Si, Al and Si are the concentrations of the elements in mass %.
[0269] Weldability is assessed by the extent of hot crack formation during welding. The greater the risk of hot crack formation, the worse the weldability of the material.
[0270] In order to quantify the lack of resistance to hot cracks, various alloys were tested at the BAM (Bundesanstalt für Materialforschung und-prüfung) using the MVT (Modifizierten Varestraint Transvarestraint) test. For this purpose, test specimens with the dimensions of 100 mm x 40 mm x 10 mm were produced from the alloy. In the MVT test, WIG welding (WIG: tungsten inert gas) is carried out completely mechanically on the upper side of the test specimen in the longitudinal direction at a constant feed rate. When the arc passes through the middle of the test specimen, a defined bending strain is applied to the test specimen. The test specimen is thereby bent longitudinally in the welding direction (Varestraint mode). During this phase of bending, hot cracks are formed in a locally limited test area of the MVT test specimen.
[0271] The tests were conducted under pure argon gas at 4.8, with a bending strain of 4%, a die speed of 2 mm / s, and an energy per unit length of 7.5 kJ / cm.
[0272] For the evaluation, the lengths of all solidification cracks and remelting cracks visible on the sample were measured and summed in an optical microscope at a magnification of 25 times. Based on these results, the material can be classified into the categories of "safe for hot cracking" (range 1), "increased tendency to hot cracking" (range 2) and "at risk of hot cracking" (range 3), as shown in Table 2.
[0273] In the following studies, alloys in the MVT test in range 1 "safe for hot cracking" and range 2 "extended tendency to hot cracking" are considered to be acceptably weldable, since the alloy AC66, which is weldable according to the prior art, is in range 2. Alloys with a risk of hot cracking (range 3) are generally difficult to weld. In particular, welding with intrinsic welding fillers (having a composition comparable to that of the materials to be welded) is more difficult or impossible.
[0274] Thermal Strength Evaluation Passed the hot tensile test This is determined in a tension test according to DIN EN ISO 6892-2 at the desired temperature. In the process, the yield strength R p0.2 , tensile strength R m and elongation at break A. The test was performed on a circular specimen with a measuring area diameter of 6 mm and an initial gauge length L0 of 30 mm. Yield strength R at 500 °C p0.2 Or tensile strength R m At least the minimum values for alloy AC66 according to the prior art should be achieved:
[0275] -500℃: Rp 0.2≥95MPa or Rm≥115MPa (5a, 5b) It is expected that they are better than the minimum values of alloy 45TM according to the prior art.
[0276] -500℃: Rp 0.2 ≥150MPa or Rm≥500MPa.(6a,6b)
[0277] Grain size was determined by the linear intercept method.
[0278] manufacture
[0279] To determine the properties of components manufactured from the powders, alloys melted on a laboratory scale in a vacuum furnace were used.
[0280] Tables 3a and 3b show the analysis of some batches of AC66 (1.4877) and 45TM (2.4889) melted on laboratory scale and, for comparison, melted on industrial scale according to the prior art. Batches according to the prior art are marked with T, batches according to the invention are marked with E. Batches melted on laboratory scale are marked with L, batches melted on industrial scale are marked with G.
[0281] The alloy ingots in Table 3a and Table 3b melted on a laboratory scale in vacuum were annealed between 900° C. and 1270° C. for 8 hours and hot rolled to a final thickness of 13 mm and 6 mm by hot rolling and further intermediate annealing between 900° C. and 1270° C. for 0.1 to 1 hour. The sheets prepared in this way were solution annealed between 800° C. and 1250° C. for 1 hour. The test specimens required for the measurements were made from these sheets.
[0282] For alloys melted on an industrial scale, samples were obtained from industrial-scale production of commercially manufactured sheets of appropriate thickness. Test specimens required for the measurements were made from these sheets.
[0283] All alloy variants typically have a grain size of 50 to 190 μm.
[0284] For the exemplary batches in Table 3a) and Table 3b), the following properties were compared:
[0285] -High temperature corrosion resistance in carburizing, sulfiding and chlorinated environments (as examples of high corrosion resistance in highly corrosive environments)
[0286] - Solderability determined by MVT test
[0287] - Creep resistance determined by hot tensile testing
[0288] The results are summarized in Table 4.
[0289] Table 4 shows the results of the corrosion tests in the form of total weight change and exfoliation at 500°C after 1056 hours in an atmosphere of 60% CO, 30% H2, 4% CO2, 1% H2S, 0.05% HCl and 3.95% H2O. The chromium content of all tested alloys is about 27% to 28%. The alloy AC66 according to the prior art, which contains only 0.2% silicon, shows 10.92 mg / cm 2 The 45TM alloy according to the prior art with 2.6% silicon, as well as all test batches melted on a laboratory scale and with silicon contents above 1.0%, showed less than or equal to 2.0 mg / cm 2 In addition, if the aluminum content is greater than 0.40%, the total mass change of the batch with a silicon content less than or equal to 1.0% may also be less than or equal to 2.0 mg / cm if the formula (1a) Fc≤2.5 is satisfied at the same time. 2 This is the case for batches 250084 (Si=0.59% and Al=0.95%), 250085 (Si=0.90% and Al 0.98%), 250106 (Si=0.98% and Al 0.80%) and 250108 (Si=0.70% and Al=0.86%).
[0290] Batches 250084, 250106, 250105, 250108 and 250107 are in accordance with the invention, whereas batch 2209 with a silicon content of more than 1.50% and batch 250098 with a nickel content of 44.0% are not in accordance with the invention. Despite a significant increase in silicon content of 1.2%, batch 250098 (Si=1.20% and Al=0.85%) shows a comparable or greater total mass increase compared to batches 250106 (Si=0.98% and Al=0.80%) and 250101 (Si=1.01% and Al=0.75%). The nickel content of batch 250098 (Ni=44.0%) is significantly increased compared to batches 250106 (Ni=35.6%) and 250101 (Ni=38.2%). This indicates that a higher nickel content can exacerbate corrosion. Therefore, the upper limit of nickel is set to a maximum of 40%.
[0291] In batch 250100 (Ni=38.2%, Si=0.99% and Al=0.43%), the aluminum content is slightly too low compared to batch 250101 (Ni=38.2%, Si=1.01% and Al=0.75%), so formula (1a) is not satisfied, batch 250100 does not conform to the present invention, and the total mass increases (3.43 mg / cm 2) is significantly greater than 2.0 mg / cm 2 In batch 250103 (Ni=38.2, Si=0.36% and Al=0.82%) and batch 250099 (Ni=38.4%, Si=1.00% and Al=0.20%) (which do not conform to the invention and also have a significantly greater than 2.0 mg / cm 2 The total mass increase (8.01 mg / cm 2 and 5.35mg / cm 2 )), the silicon and aluminum contents are outside the required limits and otherwise do not satisfy formula (1a).
[0292] Alloys 250084 and 250106 according to the invention also exhibit spalling. Furthermore, if the formula (1c) Fc≤1.0 is satisfied, these alloys no longer exhibit any spalling (250107) and surprisingly have a significantly lower Si content of less than 1.0 mg / cm 2 A very low total mass variation of the order of magnitude of 45TM having 2.6% silicon and 0.16% aluminum.
[0293] Table 4 shows the classification of the weldability of the alloys by the MVT test. The weldable alloy AC66 according to the prior art is in range 2. Alloy 45TM is classified in range 3 (risk of hot cracking) and is therefore strongly prone to crack formation, which makes welding difficult and welding using intrinsic welding fillers more difficult or impossible.
[0294] The batches not in accordance with the invention with a silicon content higher than or equal to 1.50% (45TM, batches 2091, 2099, 2100, 2200, 2203, 2207, 2208, 2209) are all in range 3. Of the batches with a silicon content of about 1.4%, the batches with an aluminum content lower than 0.1% are in range 2 (batches 2093, 2101), while the batches with a higher aluminum content are already in range 3 (batches 2103, 2096, 2097, 2098). The batches with a silicon content lower than 1.3% are all in range 1 or 2 (AC66, batches 2095, 2102, 250084 to 250108). All laboratory batches according to the invention are in range 1 (batches 250084, 250106, 250105, 250108 and 250107) or in range 2 (batch 250102).
[0295] The results of hot tensile tests at 500 °C in the table show that the yield strength R p0.2153 MPa or more, so they clearly exceed the minimum value of 95 MPa for AC66. They also even exceed the minimum value of 150 MPa for 45TM, although not significantly (see equations 5a and 6a). Similarly, the tensile strength R of all alloys according to the invention is m Greater than or equal to 192 MPa, thus also significantly greater than the minimum value of 115 MPa for AC66 (see formula 5b). All hot tensile tests at 500°C have an elongation greater than 35%.
[0296] Therefore, it can be proved separately as follows The claimed scope of the alloy "E" as powder according to the present invention :
[0297] A relatively low nickel content (with a relatively high iron content (the rest)) is conducive to lower corrosion in highly corrosive environments, such as carburizing, sulfiding and chlorination atmospheres. Therefore, a content of 40% is the upper limit of nickel. Too low a nickel content (with too high an iron content (the rest)) is conducive to the formation of σ phase, especially in the case of high chromium and silicon contents. Therefore, a nickel content of 35% is the lower limit.
[0298] Chromium improves corrosion resistance in highly corrosive environments, such as in carburizing, sulfiding and chloriding atmospheres. Too low a chromium content means that during use of the alloy in a highly corrosive environment, the chromium concentration drops very quickly below a critical limit, so that closed chromium oxide is no longer formed. Therefore, 26% chromium is the lower limit of chromium in the case of use in carburizing, sulfiding and chloriding environments. Too high a chromium content promotes the formation of the sigma phase of the alloy, especially at high chromium contents. Therefore, 30% chromium is considered an upper limit.
[0299] Silicon improves corrosion resistance in highly corrosive environments, such as in carburizing, sulfiding and chlorinated atmospheres. Therefore, a minimum content of 0.40% is necessary. Excessively high contents in turn impair weldability and promote the formation of sigma phases, especially at high chromium contents. Therefore, the silicon content is limited to 1.50%.
[0300] A certain content of aluminum improves the corrosion resistance in highly corrosive environments, such as in carburizing, sulfiding and chloriding atmospheres. Therefore, a minimum content of 0.40% is necessary. Too high a content in turn impairs weldability, especially in the case of high chromium and silicon contents. Therefore the aluminum content is limited to 1.30%.
[0301] Manganese is used to improve machinability. Manganese is limited to 1.0% because this element reduces high temperature corrosion resistance.
[0302] Even very low magnesium and / or calcium contents improve processing by incorporation of sulfur, thereby avoiding the appearance of low-melting NiS eutectics. Therefore, a minimum content of 0.0001% is necessary for magnesium and / or calcium. At too high a content, intermetallic Ni-Mg phases or Ni-Ca phases may occur, which in turn greatly deteriorate the machinability. Therefore, the content of magnesium and / or calcium is limited to at most 0.05%.
[0303] A minimum carbon content of 0.015% is necessary for good creep resistance. Carbon is limited to at most 0.12% because above this level the element reduces machinability due to excessive formation of primary carbides.
[0304] A minimum nitrogen content of 0.001% is necessary, thereby improving the machinability and high temperature strength of the material. Nitrogen is limited to a maximum of 0.150% since this element reduces machinability by forming coarse carbonitrides.
[0305] The phosphorus content should be less than or equal to 0.030%, because this surface active element will weaken the high temperature corrosion resistance. Too low a phosphorus content will increase the cost. Therefore, the phosphorus content is ≥ 0.001%.
[0306] The oxygen content must be less than or equal to 0.100% to ensure the manufacturability of the alloy. Too low an oxygen content will increase the cost. Therefore, the oxygen content is ≥ 0.0001%.
[0307] The sulfur content should be adjusted to be as low as possible, since this surface-active element impairs the high-temperature corrosion resistance. Therefore, a maximum sulfur content of 0.010% is specified.
[0308] Molybdenum is limited to less than 1.0% because this element reduces high temperature corrosion resistance.
[0309] Tungsten is limited to less than 1.0% since this element also reduces high temperature corrosion resistance.
[0310] Cobalt may be present in the alloy in amounts less than 1.0%. Higher amounts may reduce high temperature corrosion resistance.
[0311] Copper is limited to less than 0.5% because this element reduces high temperature corrosion resistance.
[0312] The following relationship between nickel, silicon and aluminum must be met to ensure that there is sufficient resistance in highly corrosive environments, such as in carburizing, sulfiding and chlorinated atmospheres.
[0313] Fc=-1.2+0.29*Ni-4.6*Si-4.4*Al≤2.5(1a),
[0314] wherein Ni, Si and Al and Si are the concentrations of the elements in mass %. The limitation of Fc has been demonstrated in detail above.
[0315] If necessary, the high temperature corrosion resistance can be further improved by adding oxygen-philic elements. They do this by being incorporated into the oxide layer, where they block the diffusion path of oxygen to the grain boundaries.
[0316] For one or more of the elements cerium, lanthanum, cerium mixed metal, yttrium, zirconium and hafnium, a minimum content of 0.001% is necessary to achieve the effect of improving high temperature corrosion resistance. For cost reasons, the upper limit of each element is set at 0.20%. In this case, the following formula must be satisfied:
[0317] FRE=0.714*Ce+0.720*La+1.124*Y+1.096*Zr+0.560*Hf≤0.10(2a)
[0318] Where Ce, La, Y, Zr and Hf are the concentrations of the elements in percentage. The total content of the elements Ce, Lanthanum, Yttrium, Zirconium and Hafnium is limited by this formula. Contents of FRE>1.0 will again increase the corrosion rate and impair machinability.
[0319] Titanium can be added if desired. Titanium enhances high temperature strength. At 0.50% and above, high temperature corrosion behavior may be impaired, which is why 0.50% is the maximum.
[0320] Niobium can be added if desired, as it also increases high temperature strength. Higher levels increase cost significantly. Therefore, the upper limit is set at 0.20%.
[0321] If desired, the alloy may also contain tantalum, as it also increases high temperature strength. Higher contents greatly increase the cost. Therefore, the upper limit is set at 0.20%. A minimum content of 0.001% is necessary to achieve the effect.
[0322] Boron can be added to the alloy if necessary, as it improves creep resistance. Therefore, it should be present in a content of at least 0.0001%. At the same time, this surface-active element deteriorates high temperature corrosion resistance. Therefore, a boron content of at most 0.008% is specified.
[0323] If necessary, vanadium is limited to at most 0.50% since this element reduces the resistance to high temperature corrosion.
[0324] If necessary, limit lead to a maximum of 0.002% as this element reduces resistance to high temperature corrosion. The same is true for zinc and tin.
[0325] Too small a particle size of less than 5 μm will impair flow properties and should be avoided, while too large a particle size of more than 250 μm will impair performance during additive manufacturing.
[0326] Too low 2g / cm 3 The bulk density will impair performance during additive manufacturing. Up to about 8g / cm 3 The possible bulk density is determined by the density of the alloy.
[0327]
[0328]
[0329]
[0330] BRIEF DESCRIPTION OF THE DRAWINGS
[0331] Figure 1 : Corrosion depth of various alloys as a function of temperature after exposure to H2S-containing gases for 2100 h in the Prenflo pilot plant.
Claims
1. Use of a nickel-iron-chromium alloy having excellent high temperature corrosion resistance as a powder, wherein the powder consists of spherical particles having a size of 5 to 250 μm, and wherein the alloy comprises, in mass %,: 35.0% to 38% nickel, 26.0% to 30.0% chromium, >0.7% to 1.50% silicon, 0.40% to 1.30% aluminum, 0.00% to 1.0% manganese, 0.0001% to 0.05% magnesium and / or calcium, respectively, 0.015% to 0.12% carbon, 0.001% to 0.150% nitrogen, 0.001% to 0.030% phosphorus, 0.0001% to 0.100% oxygen, Maximum 0.010% sulfur, Less than 1.0% molybdenum, Less than 1.0% cobalt, Less than 0.5% copper, Less than 1.0% tungsten, The balance is iron and usually process-related impurities, where the following relationship must be satisfied: Fc=-1.2+0.29*Ni-4.6*Si-4.4*Al≤2.5(1a), Wherein Ni, Si and Al are the concentrations of the elements in mass %.
2. Use according to claim 1, wherein the nickel content is >35.0 to <38.0%.
3. The method according to claim 1, wherein the chromium content is >26.0 to 30.0%.
4. The method according to claim 1, wherein the aluminum content is ≥ 0.50% or > 0.50% to < 1.30%.
5. The method according to claim 1, wherein the residual iron content is 28.0% or >28.0% to 38.0%.
6. The method according to claim 1, wherein the metal contains 0.001% to 0.20% of one or more of the elements cerium, lanthanum, yttrium, zirconium and hafnium, wherein the following formula must be satisfied: FRE = 0.714*Ce + 0.720*La + 1.124*Y + 1.096*Zr + 0.560*Hf ≤ 0.10 (2a) wherein Ce, La, Y, Zr and Hf are the concentrations of the elements in mass %.
7. The method according to claim 1, wherein in the presence of cerium and lanthanum, a cerium mixed metal (abbreviated as CeMM) in an amount of 0.001% to 0.20% is also used, wherein the FRE must be modified as follows: FRE = 0.716*CeMM + 1.124*Y + 1.096*Zr + 0.560*Hf ≤ 0.10 (3a) wherein CeMM, Y, Zr and Hf are the concentrations of the elements in mass %.
8. Use according to any one of claims 1 to 7, optionally wherein the titanium content is from 0.0% to 0.50%.
9. The method according to claim 1, wherein the niobium and / or tantalum content is 0.0% to 0.50%, respectively.
10. Use according to any one of claims 1 to 9, optionally wherein the boron content is from 0.0001% to 0.008%.
11. The method according to claim 1, further comprising optionally up to 0.50% vanadium.
12. The method according to claim 1, wherein the impurity content is adjusted to a maximum of 0.002% lead, a maximum of 0.002% tin, a maximum of 0.002% zinc.
13. The method according to claim 1, wherein the powder is produced by vacuum induction inert gas atomization (VIGA).
14. Use according to one of claims 1 to 13 in any desired production process using powders for producing components or layers on components.
15. Use according to one of claims 1 to 14 for additive manufacturing.
16. Use according to one of claims 1 to 15 as a component or in a component in the chemical industry.
17. Use according to any one of claims 1 to 15 as a component or in a component in a waste incineration plant or a waste pyrolysis plant.
Citation Information
Patent Citations
iron-nickel-chromium-silicon alloy
DE102007005605A1
Heat-resistant, thermoformable austenitic nickel alloy
DE4130139C1
Nickel-base alloys used for ethylene pyrolysis applications
EP0812926A1
Refractory iron-base alloy resisting to high temperatures
US3833358A
Heat resistant alloy having excellent hot workabilities
US3865581A
Cited By
Iron-chromium-nickel-aluminum high-temperature alloy material and application method thereof
CN119710371A