Solid electrolyte material with increased moisture content

By introducing appropriate amount of water into the synthesis of lithium-based solid electrolyte materials, the problem of high reactivity between lithium-based electrolyte and nickel cathode is solved, and the performance of electrochemical batteries is improved, including discharge capacity and charging efficiency.

CN118922952APending Publication Date: 2024-11-08SOLID POWER OPERATING INC
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202280090398.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2021-12-20
Filing Date
2022-12-20
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing lithium-based solid electrolyte materials are prone to react when in contact with the nickel cathode, resulting in deterioration of the cathode surface and reduced electrochemical properties, and it is difficult to maintain high ionic conductivity and low reactivity.

Method used

By introducing an appropriate amount of water during the synthesis of solid electrolyte materials, oxygen-containing electrolyte materials are formed, oxygen is used to replace part of sulfur atoms, reactivity with the nickel cathode, and ionic conductivity of the electrolyte material is improved.

Benefits of technology

It is achieved to reduce the reactivity of the cathode material while maintaining high ionic conductivity, improve the discharge capacity, first cycle efficiency and reduce the charging resistance of the electrochemical battery, significantly improve the overall performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922952A_ABST
    Figure CN118922952A_ABST
Patent Text Reader

Abstract

Solid electrolyte materials having high moisture content are described herein. The electrolyte material may include Li, T, X, A, O, and optionally Y, wherein T is at least one element selected from the group consisting of P, As, Si, Ge, Al, and B; x and Y, when present, are halogen, pseudo-halogen or superhalogen; and A is at least one element selected from the group consisting of S, Se and N. The electrolyte material is generally prepared by exposing an electrolyte precursor to a predetermined amount of water during manufacture. Also described herein are methods of making the solid state electrolyte materials, processes for making the solid state electrolyte materials, and electrochemical cells comprising the solid state electrolyte materials.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This Patent Cooperation Treaty (PCT) application is related to and claims priority to U.S. Provisional Application No. 63 / 291,835, filed on December 20, 2021, entitled “Solid-State Electrolyte Materials Having Increased Water Content,” the entire contents of which are incorporated herein by reference for all purposes. Technical Field

[0003] The present disclosure relates to solid electrolyte materials. Therefore, the present disclosure relates to the fields of electronics, chemistry and materials science. Background Art

[0004] Based on the known shortcomings of liquid electrolyte-based batteries and at the same time due to the explosive growth of battery-powered devices, the development of solid-state battery technology is being pursued. Lithium-based solid electrolytes including argyrodite materials (such as Li6PS5Cl) have been widely studied due to their high ionic conductivity. However, argyrodite materials and other electrolytes are also highly reactive to cathode materials. Typically, when placed near a nickel cathode, the sulfur in the electrolyte will react with the nickel to form nickel sulfide and degrade the surface of the cathode. This can lead to reduced ion / electronic isolation of the cathode material and reduced electrochemical performance.

[0005] For electrolyte precursors, the presence of water is avoided during the synthesis of the electrolyte material. Therefore, it has been sought to produce electrolyte materials without the presence of water to reduce degradation of the electrolyte precursor and thereby maximize ionic conductivity.

[0006] What is needed is a solid electrolyte material with high ionic conductivity and low reactivity with the cathode material.It is with these observations, and others, in mind that various aspects of the present disclosure were conceived. Summary of the invention

[0007] A solid electrolyte material is described herein, comprising Li, T, X, A, O, and optionally Y, wherein: T is at least one element selected from the group consisting of: P, As, Si, Ge, Al, and B; X and Y, when present, are halogens or pseudohalogens; A is at least one element selected from the group consisting of S, Se, and N; and the electrolyte material has a relative humidity of about 975 cm -1 ±25cm -1 、690cm -1 ±25cm -1 and 525cm -1 ±25cm-1 has an FT-IR peak. In some embodiments, T is P. In some embodiments, X is Cl. In some embodiments, A is S. In some embodiments, the solid electrolyte material is represented by the formula Li 7-w-z PS 6-w-z-v O v X w Y z . In some aspects, 0 < v ≤ 1. In some embodiments, the solid electrolyte material may have an FT-IR spectrum as depicted by Figure 2 . In some embodiments, the amount of oxygen present in the solid electrolyte material is based on exposure to 40 ppm to 1000 ppm water. In some embodiments, the electrochemical cell comprising the electrolyte material has a higher discharge capacity compared to an electrochemical cell comprising the same electrolyte material synthesized with 0 ppm H2O and lacking an oxygen component. In some embodiments, the electrochemical cell comprising the electrolyte material has a higher first cycle efficiency (FCE) compared to an electrochemical cell comprising the same electrolyte material exposed to 0 ppm H2O and lacking an oxygen component. In some embodiments, the electrochemical cell comprising the electrolyte material has a lower resistance rise compared to an electrochemical cell comprising the same electrolyte material exposed to 0 ppm H2O and lacking an oxygen component.

[0008] Also described herein is a method of preparing a solid electrolyte material, the method comprising mixing reactants according to the following reaction to produce a solid electrolyte material of the formula Li6PS 5-E O E Cl: XLi2S (A ppm H2O) + YP2S 5(B ppm H2O) + ZLi x(C ppm H2O) + W solvent (D ppm H2O) → Li6P S5-E O E Cl + W solvent; where E = (X*A) + (Y*B) + (Z*C) + (W*D), A, B, C, and D = ppm per unit mass of H2O, and Z, Y, Z, and W = unit mass; and controlling the ppm of water in each precursor and solvent to produce an electrolyte material having high ionic conductivity while having low reactivity towards a high nickel content cathode.

[0009] This document further describes an electrochemical cell that includes a positive electrode and an electrolyte material disposed between the positive electrode and a negative electrode, where the electrolyte material has the general structure Li 7-w-z PS 6-w-z-v O v X w Y z , and where X and Y are each one or more of a halogen or pseudohalogen, 0 ≤ w ≤ 2, 0 ≤ z ≤ 2, and 0 < v ≤ 1. In some embodiments, X and Y are each selected from the group consisting of F, Cl, Br, I, BF4, BH4, NO2, and NO3 and mixtures thereof. In some embodiments, the electrolyte material has an FT-IR spectrum with absorption peaks at approximately 975 ± 25 cm -1 , 690 ± 25 cm -1 , and 525 ± 25 cm -1 . In some embodiments, compared to a material having the general formula Li 7-w-z PS 6-w-z X w Y z , the electrochemical cell has a higher discharge capacity. In some embodiments, compared to a material having the general formula Li 7-w-z PS 6-w-z X w Y z , the electrochemical cell has a higher first-cycle efficiency. In some embodiments, the first-cycle efficiency of the electrochemical cell is at least about 88%. In some embodiments, compared to a material having the general formula Li 7-w-z PS 6-w-z X w Y z , the electrochemical cell has a lower charge resistance. In some embodiments, the ionic conductivity of the electrolyte material can be at least 1 x 10 -4 mS / cm 2 .

[0010] This document further includes an electrochemical cell that includes a positive electrode and an electrolyte material disposed between the positive electrode and a negative electrode, where the electrolyte material includes Li, S, and P. In some embodiments, the electrolyte material further includes at least one of a halogen or pseudohalogen.

[0011] Further described herein is a method for making an electrolyte material, the method comprising grinding a mixture, the mixture comprising: a plurality of electrolyte precursors, the electrolyte precursors comprising one or more lithium (Li)-containing materials; and one or more phosphorus (P)-containing materials; halides or pseudohalides; one or more solvents; and water. In some embodiments, the electrolyte precursor further comprises a sulfur (S)-containing material. In some embodiments, the electrolyte precursor further comprises one or more of a halide-containing material or a pseudohalide-containing material. In some embodiments, the method further comprises heating the mixture after the grinding. In some aspects, the heating may cause the mixture to crystallize to form the electrolyte material. In some embodiments, the mixture may contain at least 100 ppm water, about 250 ppm water, about 500 ppm water, about 1000 ppm water, or about 100,000 ppm water. In some embodiments, the water is added to the solvent prior to the grinding. In some embodiments, at least one of the plurality of electrolyte precursors is anhydrous. In some embodiments, the amount of water added is predetermined based on the amount of water contained in the plurality of electrolyte precursors and the amount of water contained in the solvent. In some embodiments, the solvent is a low polar aprotic solvent. In some aspects, the solvent can be selected from the group consisting of: xylene, benzene, toluene, heptane and combinations thereof. In some other aspects, the solvent can comprise ether, ester, nitrile, ketone or alcohol.

[0012] Further described herein is an electrochemical cell comprising a positive electrode, an electrolyte material, and a negative electrode, wherein the electrolyte material is disposed between the positive electrode and the negative electrode, and wherein the electrolyte material is prepared by a method comprising grinding a mixture comprising: a plurality of electrolyte precursors, the electrolyte precursors comprising one or more lithium (Li)-containing materials; and one or more phosphorus (P)-containing materials; a halide or pseudohalide; one or more solvents; and water. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 A flow chart of a method for preparing a solid electrolyte material of the present disclosure is shown.

[0014] Figure 2 FT-IR graphs of the electrolyte material of the present disclosure having water contents of 0 ppm, 100 ppm, 250 ppm, 500 ppm, and 1000 ppm are shown.

[0015] Figures 3A-3C A graph depicting the performance characteristics of the disclosed electrolyte material having a water content of 0 ppm, 100 ppm, 250 ppm, 500 ppm, and 1000 ppm is shown.

[0016] Figure 4 Shown is a graph of an X-ray diffraction measurement of a solid electrolyte material produced by the method of the present disclosure.

[0017] Figure 5 Shown is a graph of an X-ray diffraction measurement of a solid electrolyte material produced by the method of the present disclosure. DETAILED DESCRIPTION

[0018] Before disclosing and describing the present invention, it should be understood that the present invention is not limited to the specific methods, compositions or materials disclosed herein, but extends to equivalents thereof that will be recognized by those of ordinary skill in the relevant art. It should also be understood that the terminology employed herein is only for the purpose of describing specific embodiments and is not intended to be limiting.

[0019] Concentrations, amounts, and other numerical data may be expressed or presented in a range format herein. It should be understood that such range formats are used only for convenience and brevity, and should be flexibly interpreted as including not only the values ​​explicitly stated as the limits of the range, but also all individual values ​​or subranges within the range, as if each value and subrange were explicitly stated. As an illustration, a numerical range of "about 2 to about 50" should be interpreted as including not only the values ​​of 2 to 50 explicitly stated, but also all individual values ​​and subranges within the indicated range. Thus, included in this numerical range are individual values, such as 2, 2.4, 3, 3.7, 4, 5.5, 10, 10.1, 14, 15, 15.98, 20, 20.13, 23, 25.06, 30, 35.1, 38.0, 40, 44, 44.6, 45, 48, and sub-ranges, such as 1-3, 2-4, 5-10, 5-20, 5-25, 5-30, 5-35, 5-40, 5-50, 2-10, 2-20, 2-30, 2-40, 2-50, etc. This same principle applies to ranges that recite only one value as a minimum or maximum value. Furthermore, this interpretation should apply regardless of the breadth of the range or the characteristics described.

[0020] As used herein, the term "about" is used to provide flexibility to numerical range endpoints by specifying that a given value may be "slightly above" or "slightly below" the endpoint. For example, the endpoint may be within 10%, 8%, 5%, 3%, 2%, or 1% of the listed value. In addition, for convenience and brevity, a numerical range of "about 50 mg / mL to about 80 mg / mL" should also be understood to support a "range of 50 mg / mL to 80 mg / mL". Endpoints can also be based on variability allowed by appropriate regulatory agencies (such as FDA, USP, etc.).

[0021] In this disclosure, the terms "including," "containing," and / or "having" are understood to mean inclusive, and are open-ended terms.

[0022] As used herein, "pseudohalogen" and "pseudohalide" refer to compounds that are chemically similar to halogen elements and halide ions. The terms "pseudohalogen" and "pseudohalide" may be used interchangeably with "superhalogen" or "superhalide", respectively.

[0023] Solid electrolyte materials synthesized with a predetermined amount of water are described herein, and the electrolyte materials have better performance characteristics than similar electrolyte materials synthesized under exposure to small amounts of water or no water. In some preferred embodiments, the electrolyte materials described herein exhibit better performance in terms of discharge capacity, efficiency, and charge resistance.

[0024] The solid electrolyte material of the present disclosure may be a lithium argyrodite-like material or a hydrate or solvate thereof. Lithium argyrodite-like materials are generally known and described in the art and have a general structure Li + (12-n-y) T n+ A 2- (6-y )X - (y) In some embodiments, the solid electrolyte material may include Li3PS4, Li7PS6, Li7P3S 11 , Li4PS4X and Li7P2S8X, wherein X is a halogen or a pseudohalogen.

[0025] Typically, it is desirable to synthesize electrolyte materials, including argyrodite-like materials, in the presence of small amounts of water to the absence of water. Exposure to water during the manufacturing process introduces oxygen into the electrolyte material, which can replace atoms (such as sulfur and / or phosphorus) in the electrolyte material and / or form bridging oxygen bonds with sulfur (e.g., SOS) or phosphorus (e.g., POP). The ionic conductivity of the resulting oxygen-containing electrolyte material is greatly reduced, sometimes one or more orders of magnitude lower (e.g., 1000 times lower) than that of an oxygen-free electrolyte material. Therefore, electrolyte materials are typically manufactured in a dry, oxygen-free environment where the humidity and gas content are highly controlled.

[0026] In addition, the presence of oxygen also reduces reactivity with certain cathode materials (such as nickel and cobalt), which are highly reactive with sulfur. In an electrochemical cell containing a sulfur-containing electrolyte and a nickel-containing cathode, nickel reacts with sulfur to form nickel sulfide. If the reaction continues, the nickel sulfide and other byproducts may ionically sequester the cathode material and reduce the performance of the battery cell.

[0027] However, it was unexpectedly and surprisingly found that synthesizing the electrolyte material with a predetermined amount of water can improve one or more aspects of the performance of the electrochemical cell containing the electrolyte material. Water is present during the milling of the solid electrolyte precursor and is converted into lithium-oxygen species and H2S during the synthesis of the electrolyte. Therefore, the synthesized electrolyte material contains a negligible amount of water or is anhydrous. Specifically, the inventors found that although the critical current density is initially greatly reduced, the further increase in the oxygen content of the electrolyte material will increase the ionic conductivity to a level closer to that of the oxygen-free electrolyte material. Additionally, it was surprisingly found that the electrochemical cell made using the electrolyte material of the present disclosure has a better first cycle efficiency than the electrochemical cell made with the oxygen-free electrolyte material. Without wishing to be bound by any particular theory, the improvement in performance may be caused by improved interfacial contact between the cathode material and the electrolyte material; additionally, the solid electrolyte material can form a more stable interface between itself and the cathode material, thereby reducing the degradation of the cathode material. When the electrolyte material itself contains a certain amount of oxygen, especially near the surface where an interface can be formed with the oxygen-containing cathode material, the driving force for the reaction is reduced and therefore less interfacial reaction occurs.

[0028] Thus, the electrolyte materials of the present disclosure achieve a surprising and unexpected balance between maintaining high ionic conductivity and reducing the activity of cathode materials such as nickel.

[0029] I. Electrolyte Materials

[0030] The solid electrolyte material of the present disclosure comprises lithium (Li), T, X, A and oxygen (O). In some embodiments, the solid electrolyte material may further comprise Y. In some embodiments, the solid electrolyte material may be of the formula Li 7-w-z TA 6-w-z-v O v X w Y z represents, where 0≤w≤2, 0≤z≤2 and 0 <v≤2。

[0031] In some embodiments, T may be selected from the group consisting of phosphorus (P), arsenic (As), silicon (Si), germanium (Ge), aluminum (Al), boron (B), and mixtures thereof. In a non-limiting example, T is phosphorus.

[0032] In some embodiments, X and Y, when present, may be halogens or pseudohalogens. In some embodiments, when X and / or Y are halogens, the halogens may be selected from the group consisting of fluorine (F), chlorine (Cl), bromine (Br), iodine (I), or combinations thereof. In some embodiments, when X and / or Y are pseudohalogens, the pseudohalogens may comprise borohydrides (BH4 - ), fluoroborate (BF4- ), azide (NH2 - ), nitrogen trioxide (NO3 - ), cyanide (CN - ), hydroxide (OH - ), thiocyanate (SCN - ), Hydrogen sulfide (SH - ) and other pseudohalogens known in the art and combinations thereof. In a non-limiting example, X is chlorine.

[0033] In some embodiments, A may be at least one element selected from the group consisting of sulfur (S), selenium (Se) and nitrogen (N). In a non-limiting example, A is sulfur.

[0034] The solid electrolyte materials of the present disclosure may have unique FT-IR signatures due to the presence of oxygen in the electrolyte material (see, e.g., Figure 2 In some embodiments, the FT-IR spectrum of the electrolyte material of the present disclosure may be at about 975 cm -1 ±25cm -1 、About 690cm -1 ±25cm -1 and about 525cm -1 ±25cm -1 In some non-limiting examples, the solid electrolyte material may have a peak as follows: Figure 2 FT-IR spectra depicted.

[0035] The solid electrolyte material of the present disclosure may have a unique x-ray diffraction pattern (XRD). For example, Li 5.5 PS 4.5 The solid electrolyte material of the present disclosure including LiCl may have a peak at 2θ=15.6°±0.5°, 18.0°±0.5°, 25.5°±0.5°, 29.9°±0.5°, and 31.5°±0.5°. As another example, the solid electrolyte material of the present disclosure including LiCl may have a peak at 2θ=34.8°±0.5°. As yet another example, the solid electrolyte material of the present disclosure including Li2S may have a peak at 2θ=27.2°±0.5°.

[0036] As described above, oxygen is incorporated into the electrolyte material during the synthesis process by the presence of water. In some embodiments, the amount of oxygen incorporated into the solid electrolyte material and the amount of water present during the synthesis process may be predetermined.

[0037] In some aspects, the amount of oxygen present in the solid electrolyte material can be based on being exposed to 40ppm to 5000ppm water during the synthesis process. Therefore, the amount of oxygen present in the solid electrolyte material can be based on being exposed to about 40ppm water to 100ppm water, about 100ppm water to about 200ppm water, about 200ppm water to about 300ppm water, about 300ppm water to about 400ppm water, about 400ppm water to about 500ppm water, about 500ppm water to about 600ppm water, about 600ppm water to about 700ppm water, about 700ppm water to about 800ppm water, about 800ppm water to about 900ppm water, about 900ppm water to about 1000ppm water, about 1000ppm water to about 2000ppm water, about 2000ppm water to about 3000ppm water, about 3000ppm water to about 4000ppm water or about 4000ppm water to about 5000ppm water. In some aspects, the amount of oxygen present in the solid electrolyte material can be based on exposure to about 40 ppm water to about 200 ppm water, about 40 ppm water to about 300 ppm water, about 40 ppm water to about 400 ppm water, about 40 ppm water to about 500 ppm water, about 40 ppm water to about 600 ppm water, about 40 ppm water to about 700 ppm water, about 40 ppm water to about 800 ppm water, about 40 ppm water to about 900 ppm water, about 40 ppm water to about 1000 ppm water, about 40 ppm water to about 2000 ppm water, about 40 ppm water to about 3000 ppm water, about 40 ppm water to about 4000 ppm water, ppm water to about 5000 ppm water, about 400 ppm water to about 5000 ppm water, about 3000 ppm water to about 5000 ppm water, about 2000 ppm water to about 5000 ppm water, about 1000 ppm water to about 5000 ppm water, about 900 ppm water to about 5000 ppm water, about 800 ppm water to about 5000 ppm water, about 700 ppm water to about 5000 ppm water, about 600 ppm water to about 5000 ppm water, about 500 ppm water to about 5000 ppm water, about 400 ppm water to about 5000 ppm water, about 300 ppm water to about 5000 ppm water, about 200 ppm water to about 5000 ppm water, or about 100 ppm water to about 5000 ppm water. In still other aspects, the amount of oxygen present in the solid electrolyte material can be based on exposure to about 40ppm water, 100ppm water, 200ppm water, 300ppm water, 400ppm water, 500ppm water, 600ppm water, 700ppm water, 800ppm water, 900ppm water, 1000ppm water, 2000ppm water, 3000ppm water, 4000ppm water or about 5000ppm water. In some embodiments, the amount of oxygen present in the solid electrolyte material can be based on exposure to greater than about 5000ppm water.In some non-limiting examples, the amount of oxygen present in the solid electrolyte material can be based on exposure to about 100ppm water, about 250ppm water, about 500ppm water or about 1000ppm water. In still other embodiments, the amount of oxygen present in the solid electrolyte material can be based on exposure to at least about 40ppm water, at least about 100ppm water, at least about 200ppm water, at least about 300ppm water, at least about 400ppm water, at least about 500ppm water, at least about 600ppm water, at least about 700ppm water, at least about 800ppm water, at least about 900ppm water, at least about 1000ppm water, at least about 2000ppm water, at least about 3000ppm water, at least about 4000ppm water or at least about 5000ppm water.

[0038] In some other aspects, the amount of oxygen present in the solid electrolyte material can be based on exposure to about 40ppm to about 100,000ppm water during the synthesis process. The amount of oxygen present in the solid electrolyte material can be based on exposure to about 40ppm to about 100ppm, about 100ppm to about 500ppm, about 500ppm to about 1,000ppm, about 1,000ppm to about 5,000ppm, about 5,000ppm to about 10,000ppm, about 10,000ppm to about 25,000ppm, about 25,000ppm to about 50,000ppm, about 50,000ppm to about 75,000ppm or about 75,000ppm to about 100,000ppm. In further aspects, the amount of oxygen present in the solid electrolyte material can be based on about 100 ppm to about 500 ppm, about 100 ppm to about 1,000 ppm, about 100 ppm to about 5,000 ppm, about 100 ppm to about 10,000 ppm, about 100 ppm to about 25,000 ppm, about 100 ppm to about 50,000 ppm, about 100 ppm to about 75,000 ppm, about 100 ppm to about 100,000 ppm, about 500 ppm to about 100,000 ppm, about 1,000 ppm to about 100,000 ppm, about 5,000 ppm to about 100,000 ppm, about 10,000 ppm to about 100,000 ppm, about 25,000 ppm to about 100,000 ppm, about 50,000 ppm to about 100,000 ppm, or about 75,000 ppm to about 100,000 ppm. In some examples, the amount of oxygen present in the solid electrolyte material can be based on about 40 ppm, about 100 ppm, about 500 ppm, about 1,000 ppm, about 5,000 ppm, about 10,000 ppm, about 25,000 ppm, about 50,000 ppm, about 75,000 ppm, or about 100,000 ppm exposure.

[0039] In some embodiments, with a general formula Li (7-w-z) PS (6-w-z) X w Y z The solid electrolyte material of the present disclosure may have improved performance compared to a solid electrolyte material of , wherein X and Y are each a halogen or a pseudohalogen, wherein 0≤w≤2, 0≤z≤2, and w+z=2. In some further embodiments, the solid electrolyte material of the present disclosure may have improved performance compared to the same electrolyte material synthesized with 0ppm H2O and / or lacking an oxygen component. The improved performance metrics may include discharge capacity, first cycle efficiency, and lower charge resistance.

[0040] In some embodiments, with a general formula Li (7-w-z) PS (6-w-z) X w Y z The solid electrolyte materials of the present disclosure generally have lower ionic conductivity than solid electrolyte materials of the present disclosure, wherein X and Y are each a halogen or a pseudohalogen, wherein 0≤w≤2, 0≤z≤2, and w+z=2. In some further embodiments, the solid electrolyte materials of the present disclosure may have lower ionic conductivity than the same electrolyte material synthesized with 0ppm H2O and lacking an oxygen component. However, for many applications, the improvements in the other metrics described above outweigh this loss in ionic conductivity. In some embodiments, the ionic conductivity of the solid electrolyte of the present disclosure may be at least about 1x 10 -6 mS / cm 2 In some aspects, the ionic conductivity of the solid electrolyte of the present disclosure can be at least about 1 x 10 -5 mS / cm 2 , at least about 1x 10 -4 mS / cm 2 or at least about 1x 10 -3 mS / cm 2 .

[0041] II. Method for producing solid electrolyte material

[0042] The solid electrolyte materials described in Section I can be synthesized by mixing the reactants according to the following reaction. (a ppm水) +βT2A 5(b ppm水) +γLiX (c ppm水) +δLiY (d ppm水) +ε solvent (e ppm水) Li 7-w-z TA 6-w-z-v O v X w Y z +ε solvent

[0043] where v=(α*a)+(β*b)+(γ*c)+(δ*d)+(ε*e),

[0044] a, b, c, d and e = ppm per mol of water, and

[0045] α, β, γ, δ and ε = mol.

[0046] The species of reactants A, T, X and Y can be the species described in Section 1 above. In some preferred embodiments, the reactant species can be anhydrous, i.e., the reactant species can have a water content of 0ppm each or together. In other embodiments, the reactant species can have a water content greater than 0ppm each or together. The water content of the reactant can be considered to determine how much water to add during the reaction to achieve the desired oxygen content of the electrolyte material. As used herein, the terms "reactant" and "reactant species" can be used interchangeably with the terms "precursor" or "electrolyte precursor".

[0047] Solvent can be any aprotic solvent with low polarity. In certain embodiments, solvent can include one or more of the following: aromatic hydrocarbons (e.g., benzene, toluene, xylene), alkanes (e.g., pentane, hexane, heptane, octane, nonane, decane), cycloalkanes (e.g., cyclopentane, cyclohexane, cycloheptane, cyclooctane, cyclononane, cyclodecane), chloroform, ether and combinations thereof. In some aspects, solvent can have a low tendency to produce hydrogen sulfide gas when contacting with electrolyte material precursor or final electrolyte material. Preferably, solvent can keep liquid state (see Section III below) during at least part of the grinding process or during the whole grinding process. The water content of solvent can be 0ppm or higher. In certain embodiments, water can be added to solvent to achieve the desired oxygen content of electrolyte material. In some other embodiments, reaction can include using one or more cosolvents selected from the above-mentioned solvents.

[0048] The solvent may comprise an ether. Examples of ethers suitable for use in the methods described herein include tetrahydrofuran, diethyl ether, dibutyl ether, diamyl ether, dimethoxyethane (DME), dioxane, anisole, and combinations thereof, as well as other ethers known in the art.

[0049] The solvent may comprise an ester. Examples of esters suitable for use in the methods described herein include ethyl acetate, ethyl butyrate, isobutyl acetate, butyl acetate, butyl butyrate, and butyl propionate, and combinations thereof, as well as other esters known in the art.

[0050] The solvent may comprise a nitrile. Examples of nitriles suitable for use in the methods described herein include acetonitrile, propionitrile, butyronitrile, isobutyronitrile, and combinations thereof, as well as other nitriles known in the art.

[0051] The solvent may comprise an alcohol. Examples of alcohols suitable for use in the methods described herein include methanol, ethanol, propanol, butanol, isopropanol, isobutanol, and combinations thereof, as well as other alcohols known in the art.

[0052] The solvent may comprise a ketone. Examples of ketones suitable for use in the methods described herein include acetone, cyclohexanone, diacetone, methyl ethyl ketone, methyl isobutyl ketone, and combinations thereof, as well as other ketones known in the art.

[0053] The ppm of water of each reactant and solvent can be controlled to produce an electrolyte material with high ionic conductivity and low reactivity to cathodes (such as cathodes with high nickel content).

[0054] In some respects, the total water content of mixture (that is, reactant and solvent) can be 40ppm to 5000ppm water.Therefore, the total water content of mixture can be about 40ppm water to 100ppm water, about 100ppm water to about 200ppm water, about 200ppm water to about 300ppm water, about 300ppm water to about 400ppm water, about 400ppm water to about 500ppm water, about 500ppm water to about 600ppm water, about 600ppm water to about 700ppm water, about 700ppm water to about 800ppm water, about 800ppm water to about 900ppm water, about 900ppm water to about 1000ppm water, about 1000ppm water to about 2000ppm water, about 2000ppm water to about 3000ppm water, about 3000ppm water to about 4000ppm water or about 4000ppm water to about 5000ppm water. In some aspects, the total water content of the mixture can be from about 40 ppm water to about 200 ppm water, from about 40 ppm water to about 300 ppm water, from about 40 ppm water to about 400 ppm water, from about 40 ppm water to about 500 ppm water, from about 40 ppm water to about 600 ppm water, from about 40 ppm water to about 700 ppm water, from about 40 ppm water to about 800 ppm water, from about 40 ppm water to about 900 ppm water, from about 40 ppm water to about 1000 ppm water, from about 40 ppm water to about 2000 ppm water, from about 40 ppm water to about 3000 ppm water, from about 40 ppm water to about 4000 ppm water, from about 30 ppm water to about 5000 ppm water, about 400 ppm water to about 5000 ppm water, about 300 ppm water to about 5000 ppm water, about 200 ppm water to about 5000 ppm water, about 1000 ppm water to about 5000 ppm water, about 900 ppm water to about 5000 ppm water, about 800 ppm water to about 5000 ppm water, about 700 ppm water to about 5000 ppm water, about 600 ppm water to about 5000 ppm water, about 500 ppm water to about 5000 ppm water, about 400 ppm water to about 5000 ppm water, about 300 ppm water to about 5000 ppm water, about 200 ppm water to about 5000 ppm water, or about 100 ppm water to about 5000 ppm water. In still other aspects, the total water content of the mixture can be about 40ppm water, 100ppm water, 200ppm water, 300ppm water, 400ppm water, 500ppm water, 600ppm water, 700ppm water, 800ppm water, 900ppm water, 1000ppm water, 2000ppm water, 3000ppm water, 4000ppm water or about 5000ppm water. In some embodiments, the total water content of the mixture can be greater than about 5000ppm water.In some non-limiting examples, the total water content of the mixture can be about 100ppm water, about 250ppm water, about 500ppm water or about 1000ppm water. In still other embodiments, the total water content of the mixture can be at least about 40ppm water, at least about 100ppm water, at least about 200ppm water, at least about 300ppm water, at least about 400ppm water, at least about 500ppm water, at least about 600ppm water, at least about 700ppm water, at least about 800ppm water, at least about 900ppm water, at least about 1000ppm water, at least about 2000ppm water, at least about 3000ppm water, at least about 4000ppm water or at least about 5000ppm water.

[0055] In some other aspects, the total water content of the mixture can be about 40ppm to about 100,000ppm water. The total water content of the mixture can be about 40ppm to about 100ppm, about 100ppm to about 500ppm, about 500ppm to about 1,000ppm, about 1,000ppm to about 5,000ppm, about 5,000ppm to about 10,000ppm, about 10,000ppm to about 25,000ppm, about 25,000ppm to about 50,000ppm, about 50,000ppm to about 75,000ppm or about 75,000ppm to about 100,000ppm. In further aspects, the total water content of the mixture can be from about 100 ppm to about 500 ppm, from about 100 ppm to about 1,000 ppm, from about 100 ppm to about 5,000 ppm, from about 100 ppm to about 10,000 ppm, from about 100 ppm to about 25,000 ppm, from about 100 ppm to about 50,000 ppm, from about 100 ppm to about 75,000 ppm, from about 100 ppm to about 100,000 ppm, from about 500 ppm to about 100,000 ppm, from about 1,000 ppm to about 100,000 ppm, from about 5,000 ppm to about 100,000 ppm, from about 10,000 ppm to about 100,000 ppm, from about 25,000 ppm to about 100,000 ppm, from about 50,000 ppm to about 100,000 ppm, or from about 75,000 ppm to about 100,000 ppm. In some examples, the total water content of the mixture can be about 40 ppm, about 100 ppm, about 500 ppm, about 1,000 ppm, about 5,000 ppm, about 10,000 ppm, about 25,000 ppm, about 50,000 ppm, about 75,000 ppm, or about 100,000 ppm.

[0056] The reaction is usually carried out in an inert atmosphere, which includes or consists of argon (Ar) or nitrogen (N2) gas. In some embodiments, the water content of the inert atmosphere can be 0ppm. This helps to control the amount of water added to the solid electrolyte material and prevents excessive water from reacting with the solid electrolyte material. In other embodiments, the water content of the atmosphere can be greater than 0ppm.

[0057] The reaction can be carried out in about 6 seconds to about 200 hours. In some embodiments, the reaction can be carried out in 6 seconds, 15 seconds, 30 seconds, 1 minute, 5 minutes, 15 minutes, 30 minutes, 1 hour, 2 hours, 4 hours, 12 hours, 24 hours, 48 ​​hours, 100 hours, 200 hours or more. One of ordinary skill in the art will appreciate that the duration of the reaction may be affected by several variables, including energy input, temperature, particle size of the reactants, solvent species, etc.

[0058] The final electrolyte material may contain impurities. In some embodiments, the impurities may include reactants that are not fully incorporated into the solid electrolyte material. In some examples, the impurities may include LiX (wherein X is a halogen or pseudohalogen), Li2S or other reactants.

[0059] Typically, electrolyte materials synthesized under dry conditions will react with water and / or air in the environment, causing the phosphorus and sulfur species in the electrolyte to combine with oxygen and release sulfur in the form of H2S. This reaction degrades the electrolyte material. Surprisingly, it was found that by incorporating oxygen in the form of water into the synthesis of the solid electrolyte material and replacing some of the sulfur atoms with oxygen, the reaction between the electrolyte and water / air can be slowed down.

[0060] In addition, the presence of oxygen in the solid electrolyte material slows down the reaction between the electrolyte and the high nickel content cathode. When the electrolyte contacts the surface of the cathode with a high concentration of nickel, the sulfur in the electrolyte reacts with the nickel to form nickel sulfide (NiS). This reaction deteriorates both the electrolyte and the cathode. Surprisingly, it was found that by replacing the sulfur atoms in the solid electrolyte material with oxygen, the reactivity of the electrolyte material and the cathode was reduced, thereby slowing down the degradation of both the electrolyte and the cathode.

[0061] In some embodiments, the degradation rate of the solid electrolyte and / or cathode can be determined by measuring the capacity of the electrochemical cell when charged and discharged over time. In some other embodiments, the degradation rate of the solid electrolyte and / or cathode can be determined by measuring the first cycle efficiency of the electrochemical cell.

[0062] III. Methods for preparing electrolyte materials

[0063] Figure 1A flow chart of a method for producing a solid electrolyte composition of the present disclosure is shown. Process 100 begins with a preparation step 110, in which any preparation actions such as precursor synthesis, purification, and equipment preparation may be performed. After any initial preparation, process 100 proceeds to step 120, in which materials including lithium, materials including phosphorus, materials including sulfur, materials including selenium, materials including nitrogen, and mixtures thereof (such as those described in Sections I and II) may be combined with one or more solvents and / or other liquids. Some materials may fall into multiple categories; for example, lithium sulfide (Li2S) may be considered to be a material including lithium and a material including sulfur. In some embodiments, each of the materials may be provided in a powder, granule, pellet, block, flake, or other dry or solid form known in the art. In some instances in the examples, each of the materials may be provided in powder form. When the material is provided in powder form, the material may be provided in a crystalline powder, an amorphous powder, or both. The one or more solvents may be one or more low-polarity aprotic solvents as described in Section II.

[0064] In some embodiments, the material including lithium may include lithium metal, lithium sulfide (Li2S), lithium chloride (LiCl), lithium nitride (Li3N), lithium borohydride (LiBH4), lithium fluoroborate (LiBF4), lithium amide (LiNH2), lithium nitrate (LiNO3), and mixtures thereof.

[0065] In some embodiments, the material including sulfur may include elemental sulfur, phosphosulfides including phosphorus pentasulfide (P2S5), and phosphorus sulfides having the general chemical formula P4S x (where 3≤x≤10), lithium sulfide (Li2S), alkali metal sulfide, alkaline metal sulfide, boron sulfide (B2S3), aluminum sulfide (Al2S3), antimony trisulfide (Sb2S3), antimony pentasulfide (Sb2S5), germanium sulfide (Ge2S3), silicon trisulfide (Si2S3), copper sulfide (CuS), copper disulfide (CuS2), zinc sulfide (ZnS), iron sulfide (FeS2), tin sulfide (SnS), and mixtures thereof. In some examples, the general chemical formula P4S x (where 3≤x≤10) phosphosulfides include P4S3, P4S4, P4S5, P4S6, P4S7, P4S8, P4S9, P4S 10or a combination thereof. In another example, the alkali metal sulfide comprises sodium sulfide (Na2S), potassium sulfide (K2S), rubidium sulfide (Rb2S), and cesium sulfide (Cs2S). In still another example, the alkali metal sulfide comprises beryllium sulfide (BeS), calcium sulfide (CaS), magnesium sulfide (MgS), strontium sulfide (SrS), and barium sulfide (BaS). In some embodiments, the material including phosphorus may include elemental phosphorus, phosphorus sulfides including phosphorus pentasulfide (P2S5), phosphorus oxides including phosphorus pentoxide (P2S5), and phosphorus oxides having the general chemical formula P4S x Phosphosulfides (where 3≤x≤10), phosphochlorides including phosphorus trichloride (PCl3) and phosphorus pentachloride (PCl5), phosphorus oxychloride (POCl3) and mixtures thereof.

[0066] In some embodiments, the material including selenium may include selenium sulfide (Se2S), selenium disulfide (SeS2), and mixtures thereof.

[0067] The ratio and amount of the reactant compound may not be particularly limited, as long as the water content of the reactant compound and the one or more solvents is predetermined to achieve the desired oxygen content of the solid electrolyte material. The amount of the added solvent may be predetermined based on the water content of each reactant compound in the reactant compound and based on the water content of the solvent. Therefore, the amount of the added solvent may be adjusted to achieve the desired oxygen content in the final electrolyte material. In addition, water may be added to the solvent or the mixture of the reactant compound and the solvent to achieve the desired oxygen content of the electrolyte material. During this step 120, additional materials may be added, including cosolvents and polymers.

[0068] Next, in step 130, the composition can be mixed and / or ground within a predetermined time period and at a predetermined temperature to produce a solid electrolyte as described in Sections I and II. Mixing can be accomplished by methods known to those skilled in the art. In some non-limiting examples, mixing can be accomplished using a planetary ball mill or a grinding mill. The mixing time is not particularly limited, as long as the mixing time allows for proper homogenization and reaction of the precursors to produce a solid electrolyte material. The mixing temperature is not particularly limited, as long as the mixing temperature allows for proper mixing and is not too high so that the precursors enter a gaseous state.

[0069] In some embodiments, at a temperature of about -20°C to about 200°C, appropriate mixing can be accomplished within about 6 seconds to about 200 hours. Those skilled in the art will appreciate that the amount of time required for adequate mixing may be affected by various factors, including energy input, temperature, particle size of the precursor, solvent species, etc. In some aspects, appropriate mixing can be accomplished within about 6 seconds, 30 seconds, 1 minute, 5 minutes, 10 minutes, 30 minutes, 1 hour, 2 hours, 3 hours, 6 hours, 12 hours, 24 hours, 36 hours, 48 ​​hours, 100 hours, 200 hours, or more than 200 hours. In some instances, appropriate mixing can be accomplished after about 10 minutes to about 48 hours. In some additional aspects, suitable mixing can be accomplished at temperatures of about -20°C to about 0°C, about 0°C to about 25°C, about 25°C to about 50°C, about 50°C to about 75°C, about 75°C to about 100°C, about 100°C to about 125°C, about 125°C to about 150°C, about 150°C to about 175°C, or about 175°C to about 200°C.

[0070] By introducing water prior to step 130 and milling / mixing the composition with greater than 0 ppm water, the resulting electrolyte material contains oxygen uniformly distributed throughout the composition, as opposed to a composition containing only surface oxygen.

[0071] Next, in step 140, the composition can be dried in an inert atmosphere (such as argon or nitrogen) or under vacuum for a predetermined time period and at a predetermined temperature. Drying can be performed in a static drying operation or preferably a stirring drying operation. After drying, heat treatment can be performed during optional step 150. The temperature of the heat treatment is not particularly limited, as long as the temperature is equal to or higher than the temperature required for the crystalline phase of the solid electrolyte material disclosed herein or the temperature required for enhancing ionic conductivity or lithium metal compatibility. The material produced by the heat treatment step 150 can be single-phase and can also contain other crystalline phases, glass phases and a small portion of precursor phases.

[0072] Usually, heat treatment time is unrestricted, as long as heat treatment time allows to produce desired composition and phase.Described time can be in the scope of for example about 1 minute to about 24 hours.In some respects, heat treatment can be carried out in about 1 minute, 10 minutes, 30 minutes, 1 hour, 2 hours, 4 hours, 6 hours, about 12 hours, about 18 hours or about 24 hours.In addition, heat treatment can be carried out in inert gas atmosphere (for example, argon or nitrogen), reducing atmosphere (for example, hydrogen) or under vacuum.If desired composition and phase are obtained during earlier mixing and drying step, then heat treatment step 150 can be skipped completely.

[0073] IV. Electrochemical Cells

[0074] Solid electrolyte materials described herein can be used in solid electrochemical cells. Solid electrolyte materials can be placed between the positive electrode and the negative electrode in the solid electrolyte material layer. The solid electrolyte material layer can include a solid electrolyte material of the present disclosure having a concentration of about 10 volume % to about 100 volume %. In certain embodiments, the concentration of the solid electrolyte material of the present disclosure in the solid electrolyte material layer can be about 10 volume % to about 20 volume %, about 20 volume % to about 30 volume %, about 30 volume % to about 40 volume %, about 40 volume % to about 50 volume %, about 50 volume % to about 60 volume %, about 60 volume % to about 70 volume %, about 70 volume % to about 80 volume %, about 80 volume % to about 90 volume % or about 90 volume % to about 100 volume %. In some further embodiments, the concentration of the solid-state electrolyte material of the present disclosure in the solid-state electrolyte material layer can be about 10 vol% to about 30 vol%, about 10 vol% to about 40 vol%, about 10 vol% to about 50 vol%, about 10 vol% to about 60 vol%, about 10 vol% to about 70 vol%, about 10 vol% to about 80 vol%, about 10 vol% to about 90 vol%, about 20 vol% to about 100 vol%, about 30 vol% to about 10 vol%, about 40 vol% to about 100 vol%, about 50 vol% to about 100 vol%, about 60 vol% to about 100 vol%, about 70 vol% to about 100 vol%, or about 80 vol% to about 100 vol%. In still other embodiments, the concentration of the solid-state electrolyte material of the present disclosure in the solid-state electrolyte material layer may be about 10 volume %, 20 volume %, 30 volume %, 40 volume %, 50 volume %, 60 volume %, 70 volume %, 80 volume %, 90 volume %, or about 100 volume %.

[0075] In some embodiments, the solid electrolyte material layer may include an adhesive or other modifier. In some aspects, the adhesive may include polyvinyl chloride, polyaniline, poly(methyl methacrylate), nitrile rubber, styrene-butadiene rubber, polystyrene, polyvinylidene fluoride, self-healing polymers, polyethylene oxide, or other adhesives known in the art and combinations thereof.

[0076] The thickness of the solid electrolyte material layer may be between about 1 μm and about 1000 μm. In some embodiments, the thickness of the solid electrolyte material layer can be about 1 μm to about 5 μm, about 5 μm to about 10 μm, about 10 μm to about 15 μm, about 15 μm to about 20 μm, about 20 μm to about 25 μm, about 25 μm to about 30 μm, about 30 μm to about 35 μm, about 35 μm to about 40 μm, about 40 μm to about 45 μm, about 45 μm to about 50 μm, about 50 μm to about 100 μm, about 100 μm to about 200 μm, about 200 μm to about 300 μm, about 300 μm to about 400 μm, about 400 μm to about 500 μm, about 500 μm to about 600 μm, about 600 μm to about 700 μm, about 700 μm to about 800 μm, about 800 μm to about 900 μm, or about 900 μm to about 1000 μm. In some further embodiments, the thickness of the solid electrolyte material layer may be from about 1 μm to about 10 μm, from about 1 μm to about 15 μm, from about 1 μm to about 20 μm, from about 1 μm to about 25 μm, from about 1 μm to about 30 μm, from about 1 μm to about 35 μm, from about 1 μm to about 40 μm, from about 1 μm to about 45 μm, from about 1 μm to about 50 μm, from about 1 μm to about 100 μm, from about 1 μm to about 200 μm, from about 1 μm to about 300 μm, from about 1 μm to about 400 μm, from about 1 μm to about 500 μm, from about 1 μm to about 600 μm, from about 1 μm to about 700 μm, from about 1 μm to about 800 μm, from about 1 μm to about 900 μm, from about 5 μm to about 1000 μm, from about 10μm to about 1000μm, about 15μm to about 1000μm, about 20μm to about 1000μm, about 25μm to about 1000μm, about 30μm to about 1000μm, about 35μm to about 1000μm, about 40μm to about 1000μm, about 45μm to about 1000μm, about 50μm to about 1000μm, about 100μm to about 1000μm, about 200μm to about 1000μm, about 300μm to about 1000μm, about 400μm to about 1000μm, about 500μm to about 1000μm, about 600μm to about 1000μm, about 700μm to about 1000μm or about 800μm to about 1000μm. In still other embodiments, the thickness of the solid electrolyte material layer can be 1μm, 5μm, 10μm, 15μm, 20μm, 25μm, 30μm, 35μm, 40μm, 45μm, 50μm, 100μm, 200μm, 300μm, 400μm, 500μm, 600μm, 700μm, 800μm, 900μm or about 1000μm.

[0077] The electrochemical cell may include a positive electrode. The positive electrode may be formed of materials including aluminum, nickel, titanium, stainless steel and carbon. In some embodiments, the positive electrode may include a positive electrode current collector and a positive electrode composite material. The positive electrode composite material may include a positive electrode active material, a binder and a conductive additive. In some aspects, the positive electrode active material may include a metal oxide, a metal phosphate, a metal sulfide, sulfur, lithium sulfide, oxygen, air or other materials known in the art. The thickness of the positive electrode active material may be from about 1 μm to about 1000 μm. The positive electrode active material may further include a solid electrolyte material of the present disclosure having a concentration of about 5% by volume to about 80% by volume. In some other aspects, the positive electrode binder may include polyvinyl chloride, polyaniline, poly(methyl methacrylate), nitrile rubber, styrene-butadiene rubber, polystyrene, polyvinylidene fluoride or other binders known in the art and combinations thereof. In still further aspects, the conductive additive can comprise carbon (eg, carbon black, graphite, carbon nanotubes, carbon fibers, graphene, etc.), metal particles, filaments or other structures, or other conductive additives known in the art, and combinations thereof.

[0078] The electrochemical cell may include a negative electrode. The negative electrode may be formed of a material including copper, nickel, stainless steel or carbon. The negative electrode may include a negative electrode active material, a binder and a conductive additive. In some embodiments, the negative electrode active material may include lithium metal, lithium alloy, silicon, tin (Sn), graphite carbon, hard carbon, and may further include a solid electrolyte composition, such as the solid electrolyte composition described herein. The negative electrode active material may include a solid electrolyte material of the present disclosure at a concentration of about 5% by volume to about 80% by volume. The thickness of the negative electrode active material may be about 1 μm to about 1000 μm. Examples of binders used in the negative electrode may include those used in the positive electrode. Examples of conductive additives used in the negative electrode may include those used in the positive electrode.

[0079] The discharge capacity of an electrochemical cell refers to the amount of electricity that is discharged from the cell during a discharge cycle. (7-w-z) PS (6-w-z) X w Y zCompared with an electrochemical cell of a solid electrolyte material of the present invention, an electrochemical cell including the solid electrolyte material of the present invention can have a higher discharge capacity, wherein X and Y are each a halogen or a pseudo-halogen, wherein 0≤w≤2, 0≤z≤2 and w+z=2. In some other embodiments, compared with an electrochemical cell including an electrochemical cell of the same electrolyte material synthesized with 0ppm H2O and lacking an oxygen component, an electrochemical cell including the solid electrolyte material of the present invention has a higher discharge capacity. In still other embodiments, the discharge capacity of an electrochemical cell including the solid electrolyte material of the present invention can be about at least about 100mAh / g. In some aspects, the discharge capacity can be at least about 110mAh / g, at least about 120mAh / g, or at least about 130mAh / g. In some additional aspects, the discharge capacity can be about 100 mAh / g to about 105 mAh / g, about 105 mAh / g to about 110 mAh / g, about 110 mAh / g to about 115 mAh / g, about 115 mAh / g to about 120 mAh / g, about 120 mAh / g to about 125 mAh / g, about 125 mAh / g to about 130 mAh / g, or greater than about 130 mAh / g.

[0080] The first cycle efficiency of an electrochemical cell is defined as the ratio of the first discharge capacity to the first charge capacity. In some embodiments, an electrochemical cell comprising a solid electrolyte material of the present disclosure may have a higher first cycle efficiency than an electrochemical cell comprising a solid electrolyte material having the general formula Li6PS5Cl. In some other embodiments, an electrochemical cell comprising a solid electrolyte material of the present disclosure may have a higher first cycle efficiency than an electrochemical cell comprising an electrochemical cell synthesized with 0ppm H2O and lacking an oxygen component. In still other embodiments, the first cycle efficiency may be greater than about 85%, greater than about 86%, greater than about 87%, greater than about 88%, greater than about 89%, greater than about 90%, greater than about 91%, greater than about 92%, greater than about 93%, greater than about 94%, greater than about 95%, greater than about 96%, greater than about 97%, greater than about 98% or greater than about 99%. In some aspects, the first cycle efficiency can be about 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, or about 99%. In an exemplary embodiment, the first cycle efficiency of the electrochemical cell including the solid electrolyte material of the present disclosure is greater than 88%.

[0081] In some embodiments, the (7-w-z) PS (6-w-z) X w Y zCompared to an electrochemical cell of a solid electrolyte material of the present invention, an electrochemical cell including the solid electrolyte material of the present invention may have a higher charging resistance, wherein X and Y are each a halogen or a pseudo-halogen, wherein 0≤w≤2, 0≤z≤2 and w+z=2. In some other embodiments, an electrochemical cell including the solid electrolyte material of the present invention may have a higher charging resistance than the same electrolyte material synthesized with 0ppm H2O and lacking an oxygen component. In still other embodiments, the charging resistance of an electrochemical cell including a solid electrolyte material may be from about 4 minutes to about 6 minutes. In some aspects, the charging resistance of an electrochemical cell including a solid electrolyte material may be from about 4 ohms to about 4.5 ohms, from about 4.5 ohms to about 5 ohms, from about 5 ohms to about 5.5 ohms, or from about 5.5 ohms to about 6 ohms. In some other aspects, the charging resistance may be about 4 ohms, 4.25 ohms, 4.5 ohms, 4.75 ohms, 5 ohms, 5.25 ohms, 5.5 ohms, 5.75 ohms, or about 6 ohms.

[0082] Exemplary Embodiments

[0083] Embodiment 1: An electrochemical cell comprising: a positive electrode; and an electrolyte material disposed between the positive electrode and the negative electrode, wherein the electrolyte material has a general structure Li 7-w-z PS 6-w-z-v O v X w Y z ; wherein X and Y are each one or more of halogen and pseudohalogen; 0≤w≤2; 0≤z≤2; and 0 <v≤1。

[0084] Embodiment 2: The electrochemical cell of Embodiment 1, wherein X and Y are each selected from the group consisting of F, Cl, Br, I, BF4, BH4, NO2, and NO3.

[0085] Embodiment 3: The electrochemical cell according to Embodiment 1 or Embodiment 2, wherein the electrolyte material has a -1 、690±25cm -1 and 525±25cm -1 FT-IR spectrum with absorption peak at .

[0086] Embodiment 4: The electrochemical cell according to any one of Embodiments 1 to 3, wherein the 7-w-z PS 6-w-z X w Y z Compared with an electrochemical cell having an electrolyte material, the electrochemical cell has a higher discharge capacity.

[0087] Embodiment 5: The electrochemical cell according to any one of Embodiments 1 to 4, wherein the 7-w-z PS 6-w-z X w Y z The electrochemical cell has a higher first cycle efficiency than an electrochemical cell having an electrolyte material.

[0088] Embodiment 6: The electrochemical cell of any one of Embodiments 1 to 5, wherein the first cycle efficiency of the electrochemical cell is at least about 88%.

[0089] Embodiment 7: The electrochemical cell according to any one of Embodiments 1 to 6, wherein the 7-w-z PS 6-w-z X w Y z Compared with an electrochemical cell having an electrolyte material, the electrochemical cell has a lower charging resistance.

[0090] Example 8: A method for manufacturing an electrolyte material, the method comprising: grinding a mixture, the mixture comprising: a plurality of electrolyte precursors, the electrolyte precursors comprising one or more lithium (Li)-containing materials; and one or more phosphorus (P)-containing materials; a halide or pseudohalide; one or more solvents; and water.

[0091] Embodiment 9: The method according to embodiment 8, wherein the electrolyte precursor further comprises a sulfur (S)-containing material.

[0092] Embodiment 10: The method according to embodiment 8 or embodiment 9, wherein the electrolyte precursor further comprises one or more of a halide-containing material or a pseudo-halide-containing material.

[0093] Embodiment 11: The method of any one of embodiments 8 to 10, further comprising heating the mixture after the grinding.

[0094] Embodiment 12: The method of Embodiment 11, wherein the heating causes the mixture to crystallize to form the electrolyte material.

[0095] Embodiment 13: The method of any one of embodiments 8 to 12, wherein the mixture comprises at least 100 ppm water.

[0096] Embodiment 14: The method of embodiment 13, wherein the mixture comprises about 250 ppm water.

[0097] Embodiment 15: The method of embodiment 13, wherein the mixture comprises about 500 ppm water.

[0098] Embodiment 16: The method of embodiment 13, wherein the mixture comprises 1000 ppm water.

[0099] Embodiment 17: The method of Embodiment 13, wherein the mixture comprises about 100,000 ppm water.

[0100] Embodiment 18: The method of any one of embodiments 8 to 17, wherein the water is added to the solvent prior to the grinding.

[0101] Embodiment 19: The method of any one of Embodiments 8 to 18, wherein at least one electrolyte precursor of the plurality of electrolyte precursors is anhydrous.

[0102] Embodiment 20: The method according to any one of embodiments 8 to 19, wherein the amount of water added is predetermined based on the amount of water contained in the plurality of electrolyte precursors and the amount of water contained in the solvent.

[0103] Embodiment 21: The method according to any one of embodiments 8 to 20, wherein the solvent is a low polarity aprotic solvent.

[0104] Embodiment 22: The method of embodiment 21, wherein the solvent is selected from the group consisting of xylene, toluene, benzene, heptane, and combinations thereof.

[0105] Embodiment 23: The method of any one of Embodiments 8 to 20, wherein the solvent comprises an ether, an ester, a nitrile, or an alcohol.

[0106] Embodiment 24: An electrochemical cell comprising a positive electrode; an electrolyte material; and a negative electrode; wherein the electrolyte material is disposed between the positive electrode and the negative electrode, and the electrolyte material is prepared by the method according to any one of Embodiments 8 to 23.

[0107] Embodiment 25: A solid electrolyte material comprising: Li, T, X, A, O, and optionally Y, wherein T is at least one element selected from the group consisting of: P, As, Si, Ge, Al, and B; X and Y when present are halogens or pseudohalogens; A is at least one element selected from the group consisting of S, Se, and N; and the electrolyte material has a relative humidity of about 975 cm -1 ±25cm -1 、690cm -1 ±25cm -1 and 525cm -1 ±25cm -1 There is a FT-IR peak at .

[0108] Embodiment 26: A solid electrolyte material according to Embodiment 25, wherein T is P.

[0109] Embodiment 27: The solid electrolyte material according to Embodiment 25 or Embodiment 26, wherein X is Cl.

[0110] Embodiment 28: A solid electrolyte material according to any one of Embodiments 25 to 27, wherein A is S.

[0111] Embodiment 29: A solid electrolyte material according to any one of Embodiments 25 to 28, wherein the material is composed of the formula Li 7-w-z PS 6-w-z-v O v X w Y z express.

[0112] Embodiment 30: The solid electrolyte material according to embodiment 29, wherein 0 <v≤1。

[0113] Embodiment 31: The solid electrolyte material according to Embodiment 29 or Embodiment 30, wherein the solid electrolyte material has Figure 2 Depicted FT-IR.

[0114] Embodiment 32: The solid electrolyte material of any one of Embodiments 29 to 31, wherein the amount of oxygen present is based on exposure to 40 ppm to 1000 ppm water.

[0115] Embodiment 33: The solid electrolyte material of any one of Embodiments 29 to 32, wherein an electrochemical cell comprising the electrolyte material has a higher discharge capacity than an electrochemical cell comprising the same electrolyte material synthesized with 0 ppm H2O and lacking an oxygen component.

[0116] Embodiment 34: A solid electrolyte material according to any one of Embodiments 29 to 33, wherein an electrochemical cell comprising the electrolyte material has a higher first cycle efficiency (FCE) compared to an electrochemical cell comprising the same electrolyte material exposed to 0 ppm H2O and lacking an oxygen component.

[0117] Embodiment 35: The solid electrolyte material of any one of Embodiments 29 to 34, wherein an electrochemical cell comprising the electrolyte material has a lower resistance rise compared to an electrochemical cell comprising the same electrolyte material exposed to 0 ppm H2O and lacking an oxygen component.

[0118] Embodiment 36: The solid electrolyte material according to any one of Embodiments 25 to 35, wherein the ionic conductivity of the electrolyte material is at least 1 x 10 -4mS / cm 2 .

[0119] Embodiment 37: A method for preparing a solid electrolyte material, the method comprising: mixing reactants according to the following reaction to produce a solid electrolyte material of the following formula:

[0120] Li6PS 5-E O E Cl:XLi2S (A ppm H2O) +YP2S 5(B ppm H2O) +ZLi X(C ppm H2O) +W solvent (D ppm H2O) →Li6P S5-E O E Cl+W solvent;

[0121] Where E = (X*A) + (Y*B) + (Z*C) + (W*D), A, B, C and D = ppm of H2O per unit mass, and Z, Y, Z and W = unit mass; and the ppm of water of each precursor and solvent is controlled to produce an electrolyte material with high ionic conductivity while having low reactivity to high nickel content cathodes.

[0122] Examples

[0123] Example 1: Characterization of electrolyte materials

[0124] Solid electrolyte materials were prepared according to the methods described herein. The electrolyte materials contained phosphorus and sulfur in the electrolyte precursor. The electrolyte materials were synthesized using precursors having water contents of 0 ppm, 100 ppm, 250 ppm, 500 ppm, and 1000 ppm. Fourier transform-infrared spectroscopy (FT-IR) was performed to characterize each of these samples (see Figure 2 ).like Figure 2 As can be seen in Figure 2, as the water content of the electrolyte material increases, the -1 、690cm -1 and 525cm -1 Although the identity of the peak is unknown, the peak is characteristic of the materials described herein.

[0125] like Figure 2 As shown, as the water content of the electrolyte material increases, the amplitude of the peaks corresponding to SO and PO bonds also increases. As the water content of the electrolyte material increases, the presence of oxygen in the material increases.

[0126] Example 2: Performance of electrolyte materials

[0127] The electrolyte material of Example 1 was subjected to performance tests. Figures 3A-3C The results of the performance test are shown in FIG.

[0128] Figure 3A The discharge capacity (in mAh / g) of the electrolyte material after charge cycles 1-12 is shown. The electrolyte material with 100 ppm, 250 ppm and 500 ppm water has a higher discharge capacity than the same electrolyte material with 0 ppm or 1000 ppm water.

[0129] Figure 3B The efficiency of the electrolyte materials after charge cycles 1-5 is shown. The electrolyte materials with 500 ppm and 1000 ppm water have higher first cycle efficiency (FCE) compared to the electrolyte material with 0 ppm water. The FCE of all electrolyte materials tested was above at least 88%.

[0130] Figure 3C The charge resistance of the electrolyte material after charge cycles 1 - 15 is shown. The electrolyte material with 1000 ppm water has a slightly lower resistance increase compared to the material with 0 ppm water.

[0131] Figure 4 The XRD pattern of the electrolyte material synthesized with the precursor having 1000 ppm water is shown. Figure 4 In the XRD pattern shown, it can be observed that the electrolyte material contains Li 5.5 PS 4.5-x O x Composite materials of electrolyte phases of Cl and LiCl. 5.5 PS 4.5-x O x Cl has peaks at 15.4°, 17.9°, 25.4°, 29.9°, and 31.4°. LiCl has a peak at 34.7°.

[0132] Example 3: Electrolyte material with 100,000 ppm water

[0133] Electrolyte materials synthesized using precursors and solvents having 100,000 ppm of water were prepared according to the method of the present disclosure. Figure 5 In the XRD pattern shown, it can be observed that the electrolyte material contains Li 5.5 PS 4.5-x O x Composite materials of electrolyte phases of Cl, Li2S and LiCl. 5.5 PS 4.5-x Ox Cl has peaks at 15.7°, 18.1°, 25.6°, 29.8°, and 31.6°. Li2S has a peak at 27.2°. LiCl has a peak at 34.9°.

Claims

1. An electrochemical cell comprising a positive electrode; and an electrolyte material disposed between the positive electrode and the negative electrode, in, The electrolyte material has the general formula Li 7-w-z PS 6-w-z-v O v X w Y z ;in X and Y are each one or more of halogen and pseudohalogen; 0≤w≤2; 0≤z≤2; and 0<v≤1。 2. The electrochemical cell of claim 1, wherein X and Y are each selected from the group consisting of: F, Cl, Br, I, BF 4 , BH 4 、NO 2 and NO 3 .

3. The electrochemical cell according to claim 1 or claim 2, wherein the electrolyte material has a relative humidity of 975 ± 25 cm -1 、690±25cm -1 and 525±25cm -1 FT-IR spectrum with absorption peak at .

4. The electrochemical cell according to any one of claims 1 to 3, wherein the 7-w-z PS 6-w- z X w Y z Compared with an electrochemical cell having an electrolyte material, the electrochemical cell has a higher discharge capacity.

5. The electrochemical cell according to any one of claims 1 to 4, wherein the 7-w-z PS 6-w- z X w Y z The electrochemical cell has a higher first cycle efficiency than an electrochemical cell having an electrolyte material.

6. The electrochemical cell of any one of claims 1 to 5, wherein the first cycle efficiency of the electrochemical cell is at least about 88%.

7. The electrochemical cell according to any one of claims 1 to 6, wherein the 7-w-z PS 6-w- z X w Y z Compared with an electrochemical cell having an electrolyte material, the electrochemical cell has a lower charging resistance.

8. A method for making an electrolyte material, the method comprising grinding a mixture comprising: a plurality of electrolyte precursors, the electrolyte precursors comprising one or more lithium (Li) containing materials; One or more phosphorus (P) containing materials; Halides or pseudohalides; one or more solvents; and water. 9 . The method according to claim 8 , wherein the electrolyte precursor further comprises a sulfur (S)-containing material.

10. The method of claim 8 or claim 9, wherein the electrolyte precursor further comprises one or more of a halide-containing material or a pseudo-halide-containing material.

11. The method of any one of claims 8 to 10, further comprising heating the mixture after the grinding.

12. The method of claim 11, wherein the heating causes the mixture to crystallize to form the electrolyte material.

13. The method of any one of claims 8 to 12, wherein the mixture comprises at least 100 ppm water.

14. The method of claim 13, wherein the mixture comprises about 250 ppm water.

15. The method of claim 13, wherein the mixture comprises about 500 ppm water.

16. The method of claim 13, wherein the mixture comprises about 1000 ppm water.

17. The method of claim 13, wherein the mixture comprises about 100,000 ppm water.

18. The method according to any one of claims 8 to 17, wherein the water is added to the solvent prior to the grinding.

19. The method of any one of claims 8 to 18, wherein at least one electrolyte precursor of the plurality of electrolyte precursors is anhydrous.

20. The method according to any one of claims 8 to 19, wherein the amount of water added is predetermined based on the amount of water contained in the plurality of electrolyte precursors and the amount of water contained in the solvent.

21. The method according to any one of claims 8 to 20, wherein the solvent is a low polarity aprotic solvent.

22. The method of claim 21, wherein the solvent is selected from the group consisting of xylene, toluene, benzene, heptane, and combinations thereof.

23. The method of any one of claims 8 to 20, wherein the solvent comprises an ether, an ester, a nitrile or an alcohol.

24. An electrochemical cell comprising Positive electrode; Electrolyte materials; and Negative electrode; in, The electrolyte material is disposed between the positive electrode and the negative electrode, and The electrolyte material is prepared by the method according to any one of claims 8 to 23.

25. A solid electrolyte material, include: Li, T, X, A, O and optionally Y, wherein, T is at least one element selected from the group consisting of P, As, Si, Ge, Al and B; X and Y, when present, are halogen or pseudohalogen; A is at least one element selected from the group consisting of S, Se and N; and The electrolyte material is at about 975 cm -1 ±25cm -1 、690cm -1 ±25cm -1 and 525cm -1 ±25cm -1 There is a FT-IR peak at .

26. The solid electrolyte material according to claim 25, wherein T is P.

27. A solid electrolyte material according to claim 25 or claim 26, wherein X is Cl.

28. The solid electrolyte material according to any one of claims 25 to 27, wherein A is S.

29. The solid electrolyte material according to any one of claims 25 to 27, wherein the material is of the formula Li 7-w- z PS 6-w-z-v O v X w Y z express.

30. The solid electrolyte material according to claim 29, wherein <v≤1。 31. The solid electrolyte material of claim 29, wherein the solid electrolyte material has FT-IR as depicted in FIG.

2.

32. The solid electrolyte material of claim 29, wherein the amount of oxygen present is based on exposure to 40 ppm to 1000 ppm water.

33. A solid electrolyte material according to any one of claims 29 to 32, wherein the 2 An electrochemical cell comprising the electrolyte material has a higher discharge capacity than an electrochemical cell of the same electrolyte material having O synthesis and lacking an oxygen component.

34. A solid electrolyte material according to any one of claims 29 to 33, wherein the 2 An electrochemical cell comprising the electrolyte material has a higher first cycle efficiency (FCE) than an electrochemical cell of the same electrolyte material having no oxygen component and lacking oxygen.

35. A solid electrolyte material according to any one of claims 29 to 34, wherein the 2 An electrochemical cell including the electrolyte material has a lower resistance rise than an electrochemical cell of the same electrolyte material having no oxygen component and lacking an oxygen component.

36. The solid electrolyte material according to any one of claims 25 to 35, wherein the ionic conductivity of the electrolyte material is at least 1 x 10 -4 mS / cm 2 .

37. A method for preparing a solid electrolyte material, the method comprising The reactants are mixed according to the following reaction to produce the formula Li 6 PS 5-E O E Solid electrolyte materials for Cl: XLi 2 S (AppmH2O) +YP 2 S 5(BppmH2O) +ZLi X(CppmH2O) +W solvent (DppmH2O) →Li 6 P S5-E O E Cl+W solvent; Where E=(X*A)+(Y*B)+(Z*C)+(W*D) A, B, C and D = mass per unit H 2 O ppm, and Z, Y, Z, and W = unit mass; and, The ppm of water of each precursor and solvent is controlled to produce an electrolyte material with high ionic conductivity while having low reactivity towards high nickel content cathodes.

Citation Information