Doping type titanium adsorbent with high adsorption rate and preparation method thereof
By preparing titanium-based adsorbents with high adsorption rates through doping treatment, the problem of low adsorption rates of titanium-based lithium-ion adsorbents is solved, and the adsorption rate and capacity are improved, simplifying the preparation process and maintaining environmental friendliness.
Patent Information
- Application Number
- CN202410957778.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-12
AI Technical Summary
The existing titanium-based lithium-ion adsorbents have low adsorption rates, which affects their industrial application.
A lithium titanium oxide precursor was formed by mixing lithium carbonate, titanium oxide, and anhydrous ethanol, and then subjected to heat treatment and elution to prepare a doped titanium-based adsorbent with a high adsorption rate.
This method improves the adsorption rate and capacity of titanium-based adsorbents, enhances their kinetic properties, simplifies the preparation process, and is environmentally friendly.
Smart Images

Figure CN118925655A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion adsorption, and in particular relates to a doped titanium-based adsorbent with a high adsorption rate and a preparation method thereof. Background Art
[0002] Due to the continuous depletion of solid lithium ore resources, scientists have begun to seek methods to extract lithium from salt lake brine and seawater, which has become the main direction of lithium salt production in countries around the world. Currently, there are many methods such as adsorption, membrane, extraction, calcination, and electrodialysis that are being studied for lithium extraction from salt lakes. Among them, the adsorption method has high selectivity, low pollution, simple process, and low energy consumption. It is a very promising lithium extraction method.
[0003] Titanium-based lithium ion adsorbents have attracted much attention due to their high adsorption capacity and strong cycle stability. However, due to the compact internal structure and narrow mass transfer channels of titanium-based lithium ion adsorbents, their adsorption rate is low and the adsorption equilibrium time is too long, which seriously affects their industrial application. Therefore, how to further improve the adsorption performance of titanium-based lithium ion adsorbents is a technical problem that needs to be solved urgently. Summary of the invention
[0004] In order to solve the technical problems existing in the above-mentioned prior art, an embodiment of the present invention provides a doped titanium-based adsorbent with a high adsorption rate and a preparation method thereof.
[0005] According to the first aspect of an embodiment of the present invention, a method for preparing a doped titanium-based adsorbent with a high adsorption rate includes: step one, mixing lithium carbonate and titanium oxide with anhydrous ethanol to obtain a mixture; step two, heat-treating the mixture to form a lithium titanium oxide precursor; step three, eluting the lithium titanium oxide precursor to form a doped titanium-based adsorbent with a high adsorption rate.
[0006] In an example of the method for preparing a doped titanium-based adsorbent with a high adsorption rate provided in the first aspect above, the lithium titanium oxide precursor is a Li2TiO3 precursor.
[0007] In an example of the method for preparing a doped titanium-based adsorbent with a high adsorption rate provided in the first aspect above, the doped titanium-based adsorbent with a high adsorption rate is a H2TiO3 adsorbent.
[0008] According to the second aspect of an embodiment of the present invention, a method for preparing a doped titanium-based adsorbent with a high adsorption rate includes: step one, mixing lithium carbonate, titanium oxide and cerium nitrate hexahydrate with anhydrous ethanol to obtain a mixture; step two, heat-treating the mixture to obtain a cerium-doped lithium titanium oxide precursor; step three, eluting the cerium-doped lithium titanium oxide precursor to form a cerium-doped doped titanium-based adsorbent with a high adsorption rate.
[0009] In an example of the method for preparing a doped titanium-based adsorbent with a high adsorption rate provided in the second aspect above, the cerium-doped lithium titanium oxide precursor is a cerium-doped Li2TiO3 precursor.
[0010] In an example of the method for preparing a doped titanium-based adsorbent with a high adsorption rate provided in the second aspect, the cerium-doped doped titanium-based adsorbent with a high adsorption rate is a cerium-doped H2TiO3 adsorbent.
[0011] According to the third aspect of an embodiment of the present invention, a method for preparing a doped titanium-based adsorbent with a high adsorption rate includes: step one, mixing lithium carbonate, titanium oxide and aluminum chloride hexahydrate with anhydrous ethanol to obtain a mixture; step two, heat-treating the mixture to obtain an aluminum-doped lithium titanium oxide precursor; step three, eluting the aluminum-doped lithium titanium oxide precursor to form an aluminum-doped doped titanium-based adsorbent with a high adsorption rate.
[0012] In an example of the method for preparing a doped titanium-based adsorbent with a high adsorption rate provided in the third aspect above, the aluminum-doped lithium titanium oxide precursor is an aluminum-doped Li2TiO3 precursor.
[0013] In an example of the method for preparing a doped titanium-based adsorbent with a high adsorption rate provided in the third aspect above, the aluminum-doped doped titanium-based adsorbent with a high adsorption rate is an aluminum-doped H2TiO3 adsorbent.
[0014] The doped titanium-based adsorbent with a high adsorption rate provided in accordance with the fourth aspect of an embodiment of the present invention is prepared by the above-mentioned preparation method.
[0015] Beneficial effects: The preparation method of the doped titanium-based adsorbent with a high adsorption rate of the present invention is simple to operate, green and environmentally friendly, and the prepared doped titanium-based adsorbent with a high adsorption rate has excellent adsorption performance. In this preparation method, by controlling the type of doped metal elements and determining the optimal doping amount, the interlayer spacing of the doped titanium-based adsorbent with a high adsorption rate can be effectively regulated to affect its adsorption performance, and the doping of metal ions is conducive to expanding the internal lithium ion diffusion channel and increasing the diffusion rate of the doped titanium-based adsorbent, thereby enhancing the adsorption capacity and kinetic characteristics of the doped titanium-based adsorbent with a high adsorption rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] The above and other aspects, features and advantages of the embodiments of the present invention will become more apparent through the following description in conjunction with the accompanying drawings, in which:
[0017] Figure 1 is a flow chart of a method for preparing a doped titanium-based adsorbent with a high adsorption rate according to an embodiment of the present invention;
[0018] Figure 2 is a graph showing the variation of adsorption capacity over time of an undoped doped titanium-based adsorbent with a high adsorption rate and an aluminum-doped doped titanium-based adsorbent with a high adsorption rate according to a specific embodiment of the present invention;
[0019] Figure 3 is a graph showing the variation of adsorption capacity over time of an undoped high-adsorption-rate doped titanium-based adsorbent and a cerium-doped high-adsorption-rate doped titanium-based adsorbent with different cerium doping amounts according to a specific embodiment of the present invention;
[0020] Figure 4 It is the XRD diagram of an undoped high-adsorption-rate doped titanium-based adsorbent precursor, an aluminum-doped high-adsorption-rate doped titanium-based adsorbent precursor, and a cerium-doped high-adsorption-rate doped titanium-based adsorbent precursor with different cerium doping amounts according to a specific embodiment of the present invention. DETAILED DESCRIPTION
[0021] Hereinafter, specific embodiments of the present invention will be described in detail with reference to the accompanying drawings. However, the present invention may be implemented in many different forms, and the present invention should not be construed as being limited to the specific embodiments set forth herein. On the contrary, these embodiments are provided to explain the principles of the present invention and their practical applications, so that other persons skilled in the art can understand the various embodiments of the present invention and various modifications suitable for specific intended applications.
[0022] As used herein, the term "including" and its variations represent open terms, meaning "including but not limited to". The terms "based on", "according to", etc. mean "based at least in part on", "based at least in part on". The terms "one embodiment" and "an embodiment" mean "at least one embodiment". The term "another embodiment" means "at least one other embodiment". The terms "first", "second", etc. may refer to different or the same objects. Other definitions may be included below, whether explicit or implicit. Unless the context clearly indicates otherwise, the definition of a term is consistent throughout the specification.
[0023] Figure 1 The flowchart is a method for preparing a doped titanium-based adsorbent with a high adsorption rate according to an embodiment of the present invention.
[0024] Reference Figure 1 According to an embodiment of the present invention, a method for preparing a doped titanium-based adsorbent with a high adsorption rate comprises:
[0025] Step S110: mixing lithium carbonate, titanium oxide and doping material with anhydrous ethanol to obtain a mixture;
[0026] Step S120: heat-treating the mixture to form a doped lithium titanium oxide precursor;
[0027] Step S130: performing an elution treatment on the doped lithium titanium oxide precursor to form a doped titanium-based adsorbent with a high adsorption rate.
[0028] As an example, the titanium oxide is titanium dioxide, but the present invention is not limited thereto.
[0029] As an example, the lithium titanium oxide precursor is a Li2TiO3 precursor.
[0030] As an example, the doped titanium-based adsorbent with a high adsorption rate is a H2TiO3 adsorbent.
[0031] The following describes a specific implementation of preparing a doped titanium-based adsorbent with a high adsorption rate using the method for preparing a doped titanium-based adsorbent with a high adsorption rate according to an embodiment of the present invention.
[0032] <Specific implementation method one>
[0033] First, 3.362 g Li2CO3 and 3.634 g TiO2 were mixed with 50 mL anhydrous ethanol, and then ultrasonically treated at 50 °C for 30 min. After being taken out, they were placed in a 60 °C oven and dried for 24 h.
[0034] Secondly, after the above drying, the mixture was taken out, fully ground and put into a crucible, and calcined in a muffle furnace at 900°C for 4h to obtain a white powder Li2TiO3 precursor;
[0035] Finally, the above-mentioned Li2TiO3 precursor was acid-leached with 0.15 mol / L HCl at 60°C for 24 hours, and the titanium dissolution rate was 1.08%. After washing with deionized water, an undoped high-adsorption-rate doped titanium-based adsorbent, namely H2TiO3 adsorbent, was obtained.
[0036] In addition, 0.25 g of the H2TiO3 adsorbent prepared above was placed in 50 mL of 0.1 mol / L LiOH solution at 60 °C for adsorption. The adsorption data curve is as follows: Figure 2 and Figure 3 As shown, the adsorption capacity is about 51.25 mg / g. Figure 2 is a graph showing the adsorption capacity variation over time of an undoped doped titanium-based adsorbent with a high adsorption rate and an aluminum-doped doped titanium-based adsorbent with a high adsorption rate according to the present invention; Figure 3 The adsorption capacity of the undoped high-adsorption-rate doped titanium-based adsorbent and the cerium-doped high-adsorption-rate doped titanium-based adsorbent with different cerium doping amounts according to the present invention varies with time. Figure 2 In the above, HTO represents an undoped titanium-based adsorbent with a high adsorption rate, and Al 0.025 -HTO means aluminum-doped titanium-based adsorbent with high adsorption rate. Figure 3 In the above, HTO represents an undoped titanium-based adsorbent with a high adsorption rate, and Ce 0.025 -HTO、Ce 0.05 -HTO、Ce 0.1 -HTO represent different cerium doping amounts of cerium doped high adsorption rate doped titanium adsorbents; among them, Ce 0.1 -HTO contains more Ce than Ce 0.05 -Cerium doping amount in HTO, Ce 0.05 -HTO contains more Ce than Ce 0.025 - Ce doping level in HTO.
[0037] <Specific implementation method two>
[0038] First, 1.319 g Li2CO3, 1.390 g TiO2, and 0.189 g Ce(NO3)3·6H2O were mixed with 50 mL anhydrous ethanol, and then ultrasonically treated at 50 °C for 30 min, and then taken out and dried in a 60 °C oven for 24 h;
[0039] Secondly, after the above drying, the mixture was taken out, fully ground and put into a crucible, and calcined in a muffle furnace at 900°C for 4h to obtain Ce-doped Ce 0.025 -LTO precursor (i.e. Ce-doped Li2TiO3 precursor), please refer to its XRD pattern Figure 4 Compared with the first embodiment, the CeO2 phase appears in the Ce-doped Li2TiO3 precursor synthesized in the second embodiment.
[0040] Finally, the above Ce 0.025 -LTO precursor was acid-leached with 0.15 mol / L HCl at 60 °C, and the titanium dissolution rate was 0.61%. Ce-doped Ce was obtained by washing with deionized water. 0.025 -HTO adsorbent, i.e. Ce-doped H2TiO3 adsorbent.
[0041] In addition, 0.25 g of the Ce-doped H2TiO3 adsorbent prepared above was placed in 50 mL of a 0.1 mol / L LiOH solution for adsorption. Figure 3 As shown, its adsorption capacity is 61.08 mg / g. Compared with the first embodiment, the titanium dissolution rate of the second embodiment is lower, its adsorption capacity is higher, and the adsorption rate is significantly improved.
[0042] In addition, it should be noted that Figure 4 The XRD diagrams of an undoped high-adsorption-rate doped titanium-based adsorbent precursor, an aluminum-doped high-adsorption-rate doped titanium-based adsorbent precursor, and a cerium-doped high-adsorption-rate doped titanium-based adsorbent precursor with different cerium doping amounts according to a specific embodiment of the present invention are shown in FIG. Figure 4 In the above, LTO represents an undoped titanium-based adsorbent precursor with a high adsorption rate, and Al 0.025 -LTO represents an aluminum-doped titanium-based adsorbent precursor with a high adsorption rate, Ce 0.025 -LTO, Ce 0.05 -LTO, Ce 0.1 -LTO represent different cerium doping amounts of cerium doped high adsorption rate doped titanium-based adsorbent precursors; 0.1 -The Ce doping amount in LTO is greater than Ce 0.05 -Cerium doping amount in LTO, Ce 0.05 -The Ce doping amount in LTO is greater than Ce 0.025 - Ce doping level in LTO.
[0043] <Specific implementation method three>
[0044] First, 3.399 g Li2CO3, 3.582 g TiO2, and 0.278 g AlCl3·6H2O were mixed with 50 mL anhydrous ethanol, and then ultrasonically treated at 50 °C for 30 min, and then taken out and dried in a 60 °C oven for 24 h;
[0045] Secondly, after the above drying, the obtained product was taken out, fully ground and put into a crucible, and calcined in a muffle furnace at 900°C for 4 hours to obtain Al-doped Al 0.025 -LTO precursor (i.e. Al-doped Li2TiO3 precursor). Figure 4 It can be seen that the Al-doped Li2TiO3 precursor does not show any impurity phase, indicating that Al is successfully incorporated into the LTO precursor.
[0046] Finally, the above Al 0.025 -LTO precursor was acid-leached with 0.15 mol / L HCl at 60°C, and the titanium dissolution rate was 0.72%. After washing with deionized water, Al-doped Al 0.025 -HTO adsorbent, i.e. Al-doped H2TiO3 adsorbent.
[0047] In addition, 0.25 g of the Al-doped H2TiO3 adsorbent prepared above was placed in 50 mL of 0.1 mol / L LiOH solution at 60 °C for adsorption. The adsorption data curve is shown in Figure 2 As shown, its adsorption capacity is about 59.03 mg / g.
[0048] <Specific implementation method four>
[0049] First, 1.293 g Li2CO3, 1.328 g TiO2, and 0.380 g Ce(NO3)3·6H2O were mixed with 50 mL anhydrous ethanol, and then ultrasonically treated at 50 °C for 30 min, and then taken out and dried in a 60 °C oven for 24 h;
[0050] Secondly, after the above drying, the mixture was taken out and fully ground and put into a crucible, and calcined in a muffle furnace at 900°C for 4h. 0.05 -LTO precursor (i.e. Ce-doped Li2TiO3 precursor), please refer to its XRD pattern Figure 4 .
[0051] Finally, the above Ce 0.05 -LTO precursor was acid-leached with 0.15 mol / L HCl at 60 °C, and the titanium dissolution rate was 1.29%. Ce-doped Ce was obtained by washing with deionized water. 0.05 -HTO adsorbent, i.e. Ce-doped H2TiO3 adsorbent.
[0052] In addition, 0.25 g of Ce 0.05 -HTO adsorbent was placed in 50mL of 0.1mol / L LiOH solution for adsorption. Figure 3 As shown, its adsorption capacity is 53.45 mg / g. Compared with the second embodiment, the titanium dissolution rate of the fourth embodiment is higher and the adsorption capacity is lower, but its adsorption equilibrium time is 6 hours, and the adsorption rate is significantly improved.
[0053] <Specific Implementation Method Five>
[0054] First, 1.242 g Li2CO3, 1.208 g TiO2, and 0.730 g Ce(NO3)3·6H2O were mixed with 50 mL anhydrous ethanol, and then ultrasonically treated at 50 °C for 30 min, and then taken out and dried in a 60 °C oven for 24 h;
[0055] Secondly, after the above drying, the mixture was taken out and fully ground and put into a crucible, and calcined in a muffle furnace at 900°C for 4h. 0.1 -LTO precursor (i.e. Ce-doped Li2TiO3 precursor), please refer to its XRD pattern Figure 4 .Depend on Figure 4 It can be seen that the higher the Ce doping amount, the stronger the peak signal of CeO2, which means that the more Ce doping amount, the more Ce cannot be effectively incorporated into the LTO precursor.
[0056] Finally, the above Ce 0.1 -LTO precursor was acid-leached with 0.15 mol / L HCl at 60 °C, and the titanium dissolution rate was 2.03%. Ce-doped Ce was obtained by washing with deionized water. 0.1 -HTO adsorbent, i.e. Ce-doped H2TiO3 adsorbent.
[0057] In addition, 0.25 g of Ce 0.1 -HTO adsorbent was placed in 50mL of 0.1mol / L LiOH solution for adsorption. Figure 3 As shown, its adsorption capacity is 59.71 mg / g. Compared with the fourth embodiment, the fifth embodiment has a higher titanium dissolution rate and a higher adsorption capacity.
[0058] In summary, the preparation method of the doped titanium-based adsorbent with a high adsorption rate according to the embodiment of the present invention is simple to operate, green and environmentally friendly, and the prepared titanium-based adsorbent has excellent adsorption performance. In this preparation process, by controlling the type of doped metal elements and determining the optimal doping amount, the interlayer spacing of the doped titanium-based adsorbent with a high adsorption rate can be effectively regulated to affect its adsorption performance, and the doping of metal ions is conducive to expanding the internal lithium ion diffusion channel and increasing the diffusion rate of the doped titanium-based adsorbent with a high adsorption rate, thereby enhancing the adsorption capacity and kinetic characteristics of the doped titanium-based adsorbent with a high adsorption rate.
[0059] The terms "exemplary," "example," and the like used throughout this specification mean "used as an example, instance, or illustration" and do not mean "preferred" or "advantageous" over other embodiments. The detailed description includes specific details for the purpose of providing an understanding of the described techniques. However, these techniques can be implemented without these specific details. In some instances, in order to avoid obscuring the concepts of the described embodiments, well-known structures and devices are shown in block diagram form.
[0060] The optional implementation modes of the embodiments of the present invention are described in detail above in conjunction with the accompanying drawings. However, the embodiments of the present invention are not limited to the specific details in the above implementation modes. Within the technical concept of the embodiments of the present invention, various simple modifications can be made to the technical solutions of the embodiments of the present invention, and these simple modifications all belong to the protection scope of the embodiments of the present invention.
[0061] The above description of the contents of this specification is provided to enable any person of ordinary skill in the art to implement or use the contents of this specification. Various modifications to the contents of this specification will be apparent to those of ordinary skill in the art, and the general principles defined herein may be applied to other variations without departing from the scope of protection of the contents of this specification. Therefore, the contents of this specification are not limited to the examples and designs described herein, but are consistent with the widest range of principles and novel features disclosed herein.
Claims
1. A method for preparing a doped titanium-based adsorbent with a high adsorption rate, characterized in that: The preparation method comprises: Step 1: mixing lithium carbonate and titanium oxide with anhydrous ethanol to obtain a mixture; Step 2: heat-treating the mixture to form a lithium titanium oxide precursor; Step 3: performing an elution treatment on the lithium titanium oxide precursor to form a doped titanium-based adsorbent with a high adsorption rate.
2. The preparation method according to claim 1, characterized in that: The lithium titanium oxide precursor is a Li2TiO3 precursor.
3. The preparation method according to claim 1 or 2, characterized in that: The doped titanium-based adsorbent with high adsorption rate is H2TiO3 adsorbent.
4. A method for preparing a doped titanium-based adsorbent with a high adsorption rate, characterized in that: The preparation method comprises: Step 1: mixing lithium carbonate, titanium oxide, cerium nitrate hexahydrate and anhydrous ethanol to obtain a mixture; Step 2: heat-treating the mixture to obtain a cerium-doped lithium titanium oxide precursor; Step 3: performing an elution treatment on the cerium-doped lithium titanium oxide precursor to form a cerium-doped doped titanium-based adsorbent with a high adsorption rate.
5. The preparation method according to claim 4, characterized in that: The cerium-doped lithium titanium oxide precursor is a cerium-doped Li2TiO3 precursor.
6. The preparation method according to claim 4 or 5, characterized in that: The cerium-doped titanium-based adsorbent with a high adsorption rate is a cerium-doped H2TiO3 adsorbent.
7. A method for preparing a doped titanium-based adsorbent with a high adsorption rate, characterized in that: The preparation method comprises: Step 1: mixing lithium carbonate, titanium oxide and aluminum chloride hexahydrate with anhydrous ethanol to obtain a mixture; Step 2: heat-treating the mixture to obtain an aluminum-doped lithium titanium oxide precursor; Step 3: performing an elution treatment on the aluminum-doped lithium titanium oxide precursor to form an aluminum-doped doped titanium-based adsorbent with a high adsorption rate.
8. The preparation method according to claim 7, characterized in that: The aluminum-doped lithium titanium oxide precursor is an aluminum-doped Li2TiO3 precursor.
9. The preparation method according to claim 7 or 8, characterized in that: The aluminum-doped doped titanium-based adsorbent with a high adsorption rate is an aluminum-doped H2TiO3 adsorbent.
10. A doped titanium-based adsorbent with a high adsorption rate, characterized in that: The doped titanium-based adsorbent with a high adsorption rate is prepared by the preparation method described in any one of claims 1 to 9.