Efficient chlorinated paraffin compound stabilizer and preparation method thereof
The MOF stabilizer, formed by the self-assembly of adamantane disulfonic acid derivatives and rare earth metal ions, solves the stability problem of chlorinated paraffin caused by factors such as light, heat and oxygen during processing, and achieves a highly efficient thermal stabilization effect.
Patent Information
- Application Number
- CN202411116654.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
AI Technical Summary
Existing chlorinated paraffin composite stabilizers are easily affected by factors such as light, heat, and oxygen during processing, molding, transportation, and use, resulting in darkening of color or reduction in quality. The thermal stabilization effect of rare earth stabilizers is not efficient enough.
Metal-organic framework (MOF) materials with a three-dimensional network structure are used as stabilizers. Through the bimetallic ion self-assembly reaction of adamantane disulfonic acid derivatives and rare earth metal elements, a bimetallic MOF stabilizer with regular porous channels and high specific surface area is formed. Combined with phosphite, organotin, antioxidants and ultraviolet absorbers, the stability is improved.
It effectively prevents chlorinated paraffin from being affected by factors such as light, heat, and oxygen during processing, molding, transportation, and use, thereby improving thermal stability and maintaining good physical and chemical properties.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of chlorinated paraffin, and in particular to a chlorinated paraffin high-efficiency composite stabilizer and a preparation method thereof. Background Art
[0002] Chlorinated paraffin, also known as chlorinated wax or chlorocarbon, is a chlorinated derivative of paraffin. According to its chlorine content, it can be mainly divided into three types: chlorinated paraffin-42, chlorinated paraffin-52, and chlorinated paraffin-70. This substance has the advantages of low volatility, flame retardancy, good electrical insulation, and low price. Chlorinated paraffin has a low freezing point, is insoluble in water, soluble in phenyl ether, and slightly soluble in alcohol. It is widely used as a flame retardant and auxiliary plasticizer for polyvinyl chloride, and is used in the production of cable materials, floor materials, hoses, artificial leather, rubber and other products. In addition, it can also be used as an additive for polyurethane waterproof coatings, polyurethane plastic tracks, lubricating oils, etc. During the production and use of chlorinated paraffin, due to the characteristics of its chemical properties, it is easily affected by external conditions and discolors or deteriorates. Therefore, in order to maintain the stability of chlorinated paraffin and extend its service life, stabilizers need to be added. The addition of stabilizers also helps the long-term storage of chlorinated paraffin, reduces its acid value, and forms good compatibility and compatibility with other additives, thereby exerting better effects.
[0003] Prior art Chinese patent CN201610715887.1 discloses a chlorinated paraffin composite stabilizer, which is made by mixing ethylene glycol diglycidyl ether, composite rare earth stabilizer, phosphite, composite antioxidant, p-methoxyphenol, and ethylene bisstearamide. All raw materials can be mixed during production; the weight ratio of ethylene glycol diglycidyl ether, composite rare earth stabilizer, and phosphite is 42-60:10:5-6. It can be seen that the stabilization effect of chlorinated paraffin in this prior art mainly relies on ethylene glycol diglycidyl ether, and the addition of rare earth stabilizer mainly plays a synergistic effect with ethylene glycol diglycidyl ether, thereby improving the thermal stability efficiency and reducing the amount of stabilizer. Summary of the invention
[0004] In view of the above background technology, one aspect of the present invention is to provide a high-efficiency composite stabilizer for chlorinated paraffin to solve the problem that the existing chlorinated paraffin composite stabilizer containing rare earth stabilizers cannot efficiently exert its thermal stabilization effect, thereby effectively preventing the chlorinated paraffin from being affected by factors such as light, heat, oxygen, etc. during processing, molding, transportation and use.
[0005] The inventors of this application found in the long-term experimental research process of chlorinated paraffin stabilizers that different types of compounded added stabilizers, either the raw materials of each component in the stabilizer composition are difficult to disperse evenly when initially added, or the subsequent addition and use are affected by factors such as segregation or migration of small molecules, resulting in problems such as color deepening or quality reduction of chlorinated paraffin. Further, the inventors also found that rare earth stabilizers can play a certain stabilizing effect, but there is still a large room for technical improvement to further cooperate with other stabilizers so that the compounded stabilizer can exert an efficient thermal stabilization effect. The inventors of this application innovatively synthesized metal organic framework MOF materials with unique structural characteristics, using MOF materials with porous channel mesh structures, and further combined with the synergistic effect of bimetallic ions and organic ligands containing rare earth metal elements, thereby effectively preventing chlorinated paraffin from being affected by factors such as light, heat, and oxygen during processing, molding, transportation, and use, improving the stability of chlorinated paraffin, and ultimately maintaining good physical and chemical properties.
[0006] In order to achieve the above purpose, the technical solution adopted by the present invention is:
[0007] A high-efficiency composite stabilizer for chlorinated paraffin, the composite stabilizer comprises at least one bimetallic MOF stabilizer, the bimetal in the bimetallic MOF stabilizer comprises at least one rare earth metal element, and the organic ligand of the bimetallic MOF stabilizer is an adamantane disulfonic acid derivative.
[0008] The bimetallic MOF stabilizer described in this application has significant innovation and practicality in the field of chemical industry. It uses adamantane disulfonic acid derivative as an organic ligand, and reacts with bimetallic ions containing rare earth metal elements through molecular self-assembly to generate a metal organic framework material with a three-dimensional network structure. This unique structural design makes the stabilizer excellent in thermal stability and is particularly suitable for the stabilization treatment of materials such as chlorinated paraffin.
[0009] First, the choice of adamantane disulfonic acid derivatives was carefully considered. The adamantane structure has a high degree of symmetry and stability, which makes it stable under high temperature and high pressure. At the same time, the introduction of sulfonic acid groups gives the organic ligand good water solubility and ion exchange capacity, thereby enhancing the ability of the stabilizer to bind metal ions.
[0010] Secondly, the introduction of rare earth metal elements brings unique properties to the bimetallic MOF stabilizer. Rare earth metal elements have rich electronic configurations and special physical and chemical properties. Their combination with adamantane disulfonic acid derivatives not only enhances the stability of the stabilizer, but also improves its adsorption capacity and selectivity for HCl. This adsorption capacity enables the stabilizer to effectively capture the HCl produced by chlorinated paraffin during heating, thereby delaying its thermal decomposition process.
[0011] In addition, the three-dimensional network structure of the bimetallic MOF stabilizer gives it an ultra-high specific surface area. This structure enables the stabilizer to provide more active sites, thereby accelerating the adsorption rate of HCl. At the same time, the regular porous channel structure allows HCl molecules to more easily enter the interior of the stabilizer, further improving its adsorption efficiency.
[0012] Finally, the stabilizer also has the advantage of high temperature resistance. Under high temperature conditions, the bimetallic MOF stabilizer can still maintain good structural stability and adsorption performance, which enables it to play a long-term stabilizing role in the processing and use of chlorinated paraffin.
[0013] In summary, the bimetallic MOF stabilizer of the present application provides a new solution for the stabilization treatment of materials such as chlorinated paraffin with its unique structural design and excellent performance characteristics. Its successful application is expected to promote technological progress and product upgrades in related industries.
[0014] As a preferred technical solution, the bimetal in the bimetallic MOF stabilizer includes only one rare earth metal element, and the other metal element is calcium or zinc.
[0015] As a preferred technical solution, the rare earth metal element is at least one of yttrium, lanthanum, cerium, praseodymium and neodymium.
[0016] As a preferred technical solution, the adamantane disulfonic acid derivative is obtained by an addition reaction of adamantane diacrylate and olefin sulfonic acid through an unsaturated double bond. The specific synthesis path of the adamantane disulfonic acid derivative is: dissolving adamantane diacrylate in an organic solvent, then dropping olefin sulfonic acid, stirring evenly with a magnetic force, and performing an addition reaction under light conditions to obtain the adamantane disulfonic acid derivative.
[0017] As a preferred technical solution, the adamantane diacrylate is 1,3-adamantanediol dimethacrylate and / or 1,3-adamantanediol diacrylate.
[0018] As a preferred technical solution, the olefin sulfonic acid is vinyl sulfonic acid and / or vinylbenzene sulfonic acid.
[0019] As a preferred technical solution, the composite stabilizer also includes at least one of phosphite, organic tin, antioxidant, and ultraviolet absorber.
[0020] Another aspect of the present invention is to provide a method for preparing the above-mentioned chlorinated paraffin high-efficiency composite stabilizer, the preparation method comprising the following steps:
[0021] S1: dissolving the organic ligand of adamantane disulfonic acid derivative in a mixed solvent, then adding an aqueous solution of a bimetallic salt, transferring to an autoclave, heating and pressurizing for a solvent thermal reaction, and obtaining a bimetallic MOF stabilizer;
[0022] S2: compounding the bimetallic MOF stabilizer obtained in step S1 with phosphite, organotin, antioxidant and ultraviolet absorber to obtain the chlorinated paraffin high-efficiency composite stabilizer.
[0023] As a preferred technical solution, the mixed solvent is a mixed solvent of dimethyl sulfoxide, toluene and deionized water.
[0024] As a preferred technical solution, the reaction temperature of the solvent thermal reaction is 80-120° C., and the reaction pressure is 15-22 MPa.
[0025] Beneficial effects of the present invention:
[0026] The present invention discloses a highly efficient composite stabilizer for chlorinated paraffin, which uses adamantane disulfonic acid derivative as an organic ligand, and reacts with bimetallic ions including rare earth metal elements through molecular self-assembly reaction to form a metal organic framework material with a three-dimensional network structure; by utilizing its regular porous channel structure characteristics and ultra-high specific surface area, it has the advantages of large HCl adsorption capacity, fast adsorption rate, high selectivity, and high temperature resistance; it effectively improves the thermal stability of chlorinated paraffin; further, it is compatible with phosphites, organotin, antioxidants, and ultraviolet absorbers to effectively prevent chlorinated paraffin from being affected by factors such as light, heat, and oxygen during processing, molding, transportation, and use, thereby improving the stability of chlorinated paraffin and ultimately maintaining good physical and chemical properties. DETAILED DESCRIPTION
[0027] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art may think of other obvious variations.
[0028] Example 1
[0029] The chlorinated paraffin high-efficiency composite stabilizer of the present embodiment is composed of a bimetallic MOF stabilizer, a phosphite, an organic tin, an antioxidant and an ultraviolet absorber; the bimetallic MOF stabilizer of the present embodiment uses a disulfonic acid derivative of adamantane as an organic ligand, which reacts with calcium ions and yttrium ions through molecular self-assembly to form a metal organic framework material with a three-dimensional network structure.
[0030] The specific preparation method of the chlorinated paraffin high-efficiency composite stabilizer of this embodiment comprises the following steps:
[0031] Step S1: dissolving 1,3-adamantanediol dimethacrylate (1 mol) in an organic solvent ethyl acetate (1000 mL), and then slowly adding vinyl sulfonic acid, wherein the molar ratio of the 1,3-adamantanediol dimethacrylate to the vinyl sulfonic acid is 1:2.2, stirring evenly with a magnetic force, and performing an addition reaction under illumination conditions, wherein the addition reaction uses a high-pressure mercury lamp as a light source, wherein the power range of the high-pressure mercury lamp is 1000 W, and the illumination is performed for 10 minutes to obtain an organic ligand of an adamantane disulfonic acid derivative.
[0032] Step S2: The organic ligand (0.6 mol) of the adamantane disulfonic acid derivative prepared in step S1 is dissolved in a mixed solvent (500 mL) of dimethyl sulfoxide, toluene and deionized water in a volume ratio of 2:1:2, and then a calcium nitrate aqueous solution with a mass concentration of 30% and a yttrium nitrate aqueous solution with a mass concentration of 20% are added respectively (the molar ratio of calcium nitrate, yttrium nitrate and adamantane disulfonic acid derivative is 3:2:2), and then transferred to an autoclave, heated and pressurized for hydrothermal reaction, the reaction temperature of the hydrothermal reaction is 80°C, and the reaction pressure is 22 MPa; the reaction time is flexibly adjusted according to the degree of reaction. In this embodiment, the reaction time is controlled at 45 min. After the reaction is completed, heating and pressurization are stopped, and the reaction mixture is allowed to cool naturally to room temperature. The bimetallic MOF stabilizer is obtained by filtering, washing and drying.
[0033] Step S3: Compound the bimetallic MOF stabilizer (50 g) obtained in step S2 with triphenyl phosphite (37 g), methyltin mercaptan (18 g), antioxidant 1010 (2.5 g) and ultraviolet absorber UV-326 (1.8 g), and stir and mix evenly to obtain the chlorinated paraffin high-efficiency composite stabilizer.
[0034] Example 2
[0035] The present embodiment is a high-efficiency composite stabilizer for chlorinated paraffin, which is composed of a bimetallic MOF stabilizer, a phosphite, an organic tin, an antioxidant and an ultraviolet absorber; the bimetallic MOF stabilizer of the present embodiment uses a disulfonic acid derivative of adamantane as an organic ligand, which reacts with zinc ions and lanthanum ions through molecular self-assembly to form a metal organic framework material with a three-dimensional network structure.
[0036] The specific preparation method of the chlorinated paraffin high-efficiency composite stabilizer of this embodiment comprises the following steps:
[0037] Step S1: dissolving 1,3-adamantanediol diacrylate (1 mol) in an organic solvent ethyl acetate (1000 mL), and then dropping vinylbenzenesulfonic acid, wherein the molar ratio of the 1,3-adamantanediol diacrylate to the vinylbenzenesulfonic acid is 1:2.1, stirring evenly with a magnetic force, and performing an addition reaction under illumination conditions, wherein a high-pressure mercury lamp is used as a light source for the addition reaction, wherein the power range of the high-pressure mercury lamp is 1000 W, and the illumination is performed for 10 minutes to obtain an organic ligand of an adamantane disulfonic acid derivative.
[0038] Step S2: The organic ligand (0.6 mol) of the adamantane disulfonic acid derivative prepared in step S1 is dissolved in a mixed solvent (500 mL) of dimethyl sulfoxide, toluene and deionized water in a volume ratio of 2:1:2, and then a zinc nitrate aqueous solution with a mass concentration of 30% and a lanthanum nitrate aqueous solution with a mass concentration of 20% are added respectively (the molar ratio of calcium nitrate, lanthanum nitrate and adamantane disulfonic acid derivative is 2:1:1), and the mixture is transferred to an autoclave, heated and pressurized for a hydrothermal reaction. The reaction temperature of the hydrothermal reaction is 105° C. and the reaction pressure is 18 MPa. The reaction time is flexibly adjusted according to the degree of reaction. In this embodiment, the reaction time is controlled at 40 min. After the reaction is completed, heating and pressurization are stopped, and the reaction mixture is allowed to cool naturally to room temperature. The bimetallic MOF stabilizer is obtained by filtering, washing and drying.
[0039] Step S3: Compound the bimetallic MOF stabilizer (50 g) obtained in step S2 with triphenyl phosphite (37 g), methyltin mercaptan (18 g), antioxidant 1010 (2.5 g) and ultraviolet absorber UV-326 (1.8 g), and stir and mix evenly to obtain the chlorinated paraffin high-efficiency composite stabilizer.
[0040] Example 3
[0041] The present embodiment is a high-efficiency composite stabilizer for chlorinated paraffin, which is composed of a bimetallic MOF stabilizer, a phosphite, an organic tin, an antioxidant and an ultraviolet absorber; the bimetallic MOF stabilizer of the present embodiment uses a disulfonic acid derivative of adamantane as an organic ligand, which reacts with calcium ions and cerium ions through molecular self-assembly to form a metal organic framework material with a three-dimensional network structure.
[0042] The specific preparation method of the chlorinated paraffin high-efficiency composite stabilizer of this embodiment comprises the following steps:
[0043] Step S1: dissolving 1,3-adamantanediol dimethacrylate (1 mol) in an organic solvent ethyl acetate (1000 mL), and then dropping vinylbenzenesulfonic acid, wherein the molar ratio of the 1,3-adamantanediol dimethacrylate to the vinylbenzenesulfonic acid is 1:2.3, stirring evenly with a magnetic force, and performing an addition reaction under illumination conditions, wherein a high-pressure mercury lamp is used as a light source for the addition reaction, wherein the power range of the high-pressure mercury lamp is 1000 W, and the illumination is performed for 10 minutes to obtain an organic ligand of an adamantane disulfonic acid derivative.
[0044] Step S2: The organic ligand (0.6 mol) of the adamantane disulfonic acid derivative prepared in step S1 is dissolved in a mixed solvent (500 mL) of dimethyl sulfoxide, toluene and deionized water in a volume ratio of 2:1:2, and then a calcium nitrate aqueous solution with a mass concentration of 30% and a cerium nitrate aqueous solution with a mass concentration of 20% are added respectively (the molar ratio of calcium nitrate, cerium nitrate and adamantane disulfonic acid derivative is 2:3:2), and the mixture is transferred to an autoclave, heated and pressurized for a hydrothermal reaction. The reaction temperature of the hydrothermal reaction is 120°C and the reaction pressure is 15 MPa. The reaction time is flexibly adjusted according to the degree of reaction. In this embodiment, the reaction time is controlled at 35 min. After the reaction is completed, heating and pressurization are stopped, and the reaction mixture is allowed to cool naturally to room temperature. The bimetallic MOF stabilizer is obtained by filtering, washing and drying.
[0045] Step S3: Compound the bimetallic MOF stabilizer (50 g) obtained in step S2 with triphenyl phosphite (37 g), methyltin mercaptan (18 g), antioxidant 1010 (2.5 g) and ultraviolet absorber UV-326 (1.8 g), and stir and mix evenly to obtain the chlorinated paraffin high-efficiency composite stabilizer.
[0046] Example 4
[0047] The present embodiment is a high-efficiency composite stabilizer for chlorinated paraffin, which is composed of a bimetallic MOF stabilizer, a phosphite, an organic tin, an antioxidant and an ultraviolet absorber; the bimetallic MOF stabilizer of the present embodiment uses a disulfonic acid derivative of adamantane as an organic ligand, which reacts with zinc ions and cerium ions through molecular self-assembly to form a metal organic framework material with a three-dimensional network structure.
[0048] The specific preparation method of the chlorinated paraffin high-efficiency composite stabilizer of this embodiment comprises the following steps:
[0049] Step S1: dissolving 1,3-adamantanediol diacrylate (1 mol) in an organic solvent ethyl acetate (1000 mL), and then slowly adding vinyl sulfonic acid, wherein the molar ratio of the 1,3-adamantanediol diacrylate to the vinyl sulfonic acid is 1:2.3, stirring evenly with a magnetic force, and performing an addition reaction under illumination conditions, wherein the addition reaction uses a high-pressure mercury lamp as a light source, wherein the power range of the high-pressure mercury lamp is 1000 W, and the illumination is performed for 10 minutes to obtain an organic ligand of an adamantane disulfonic acid derivative.
[0050] Step S2: The organic ligand (0.6 mol) of the adamantane disulfonic acid derivative prepared in step S1 is dissolved in a mixed solvent (500 mL) of dimethyl sulfoxide, toluene and deionized water in a volume ratio of 2:1:2, and then a zinc nitrate aqueous solution with a mass concentration of 30% and a cerium nitrate aqueous solution with a mass concentration of 20% are added respectively (the molar ratio of zinc nitrate, cerium nitrate and adamantane disulfonic acid derivative is 2:1:1), and the mixture is transferred to an autoclave, heated and pressurized for a hydrothermal reaction. The reaction temperature of the hydrothermal reaction is 120° C. and the reaction pressure is 15 MPa. The reaction time is flexibly adjusted according to the degree of reaction. In this embodiment, the reaction time is controlled at 35 min. After the reaction is completed, heating and pressurization are stopped, and the reaction mixture is allowed to cool naturally to room temperature. The bimetallic MOF stabilizer is obtained by filtering, washing and drying.
[0051] Step S3: Compound the bimetallic MOF stabilizer (50 g) obtained in step S2 with triphenyl phosphite (37 g), methyltin mercaptan (18 g), antioxidant 1010 (2.5 g) and ultraviolet absorber UV-326 (1.8 g), and stir and mix evenly to obtain the chlorinated paraffin high-efficiency composite stabilizer.
[0052] Comparative Example 1
[0053] The raw material composition of the chlorinated paraffin stabilizer in this comparative example is substantially the same as that in Example 1, except that this comparative example does not contain a bimetallic MOF stabilizer.
[0054] Comparative Example 2
[0055] The raw material composition of the chlorinated paraffin stabilizer in this comparative example is basically the same as that in Example 1, except that, during the preparation process of the MOF stabilizer in this comparative example, no yttrium nitrate aqueous solution is added to participate in the reaction to obtain the Ca-MOF metal organic framework material.
[0056] Comparative Example 3
[0057] The raw material composition of the chlorinated paraffin stabilizer in this comparative example is basically the same as that in Example 1, except that during the preparation process of the MOF stabilizer in this comparative example, no calcium nitrate aqueous solution is added to participate in the reaction to obtain the Y-MOF metal organic framework material.
[0058] The chlorinated paraffin stabilizers prepared in Examples 1 to 4 and Comparative Examples 1 to 3 were subjected to performance tests (the weight of the stabilizer was added at a ratio of 0.8% of the weight of chlorinated paraffin-52, and after uniform mixing, 30 g of the sample was placed in a 25 mm × 125 mm test tube for testing), and the performance results are shown in Table 1: Table 1 Thermal stability temperature, °C 180℃ thermal stability time, min Light stabilization time, min Example 1 182 66 270 Example 2 178 63 280 Example 3 181 69 270 Example 4 182 63 280 Comparative Example 1 115 33 230 Comparative Example 2 136 42 240 Comparative Example 3 151 45 230
[0059] The thermal stability temperature of the sample is tested with reference to the method for determining the thermal decomposition temperature of chlorinated paraffin in GB1680-81.
[0060] The determination of the thermal stability time of chlorinated paraffin at 180°C and the determination of the light stability time of chlorinated paraffin are carried out with reference to the determination method disclosed in the embodiment of the specification of the prior art Chinese patent CN201610715887.1 (the test conditions are the same). That is, for the determination of the thermal stability time of chlorinated paraffin at 180°C, the sample is observed in the aging box for 30 minutes, and then observed once every 3 minutes, and the time when the color starts to change is recorded. The temperature of the aging box is 180°C ± 2°C. For the determination of the light stability time of chlorinated paraffin, the sample is observed in the aging box equipped with ultraviolet lamp for 1 hour, and then observed once every 10 minutes, and the time when the color starts to change is recorded. The temperature of the aging box is 50°C ± 2°C, and the speed is 3r / min.
[0061] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions only describe the principles of the present invention. The present invention may be subject to various changes and improvements without departing from the spirit and scope of the present invention, and these changes and improvements fall within the scope of the present invention claimed.
Claims
1. A chlorinated paraffin high-efficiency composite stabilizer, characterized in that: The composite stabilizer comprises at least one bimetallic MOF stabilizer, the bimetal in the bimetallic MOF stabilizer comprises at least one rare earth metal element, and the organic ligand of the bimetallic MOF stabilizer is an adamantane disulfonic acid derivative.
2. The chlorinated paraffin high-efficiency composite stabilizer according to claim 1, characterized in that: The bimetal in the bimetallic MOF stabilizer includes only one rare earth metal element, and the other metal element is calcium or zinc.
3. The chlorinated paraffin high-efficiency composite stabilizer according to claim 1 or 2, characterized in that: The rare earth metal element is at least one of yttrium, lanthanum, cerium, praseodymium and neodymium.
4. The chlorinated paraffin high-efficiency composite stabilizer according to claim 1, characterized in that: The adamantane disulfonic acid derivative is obtained by an addition reaction of adamantane diacrylate and olefin sulfonic acid through an unsaturated double bond. The specific synthesis route of the adamantane disulfonic acid derivative is: dissolving adamantane diacrylate in an organic solvent, then dropping olefin sulfonic acid, stirring evenly with a magnetic force, and performing an addition reaction under light conditions to obtain the adamantane disulfonic acid derivative.
5. The chlorinated paraffin high-efficiency composite stabilizer according to claim 1, characterized in that: The adamantane diacrylate is 1,3-adamantanediol dimethacrylate and / or 1,3-adamantanediol diacrylate.
6. The chlorinated paraffin high-efficiency composite stabilizer according to claim 1, characterized in that: The olefin sulfonic acid is vinyl sulfonic acid and / or vinylbenzene sulfonic acid.
7. The chlorinated paraffin high-efficiency composite stabilizer according to claim 1, characterized in that: The composite stabilizer also includes at least one of phosphite, organic tin, antioxidant and ultraviolet absorber.
8. A method for preparing the chlorinated paraffin high-efficiency composite stabilizer according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: S1: dissolving the organic ligand of adamantane disulfonic acid derivative in a mixed solvent, then adding an aqueous solution of a bimetallic salt, transferring to an autoclave, heating and pressurizing for a solvent thermal reaction, and obtaining a bimetallic MOF stabilizer; S2: compounding the bimetallic MOF stabilizer obtained in step S1 with phosphite, organotin, antioxidant and ultraviolet absorber to obtain the chlorinated paraffin high-efficiency composite stabilizer.
9. The method for preparing the chlorinated paraffin high-efficiency composite stabilizer according to claim 8, characterized in that: The mixed solvent is a mixed solvent of dimethyl sulfoxide, toluene and deionized water.
10. The method for preparing the chlorinated paraffin high-efficiency composite stabilizer according to claim 8, characterized in that: The reaction temperature of the solvent thermal reaction is 80-120° C., and the reaction pressure is 15-22 MPa.
Citation Information