Lithium ion adsorbent and preparation method thereof

By configuring the solution and controlling the reaction conditions, an efficient Li/Al-LDHs adsorbent was prepared, which solved the problems of low dynamic adsorption capacity and serious pulverization of aluminum-based adsorbents, and significantly improved the adsorption performance and stability.

CN118925657APending Publication Date: 2024-11-12QINGHAI CITIC GUOAN SCI & TECH DEV CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410957684.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

When aluminium-based lithium-ion adsorbent is used on a large scale, the dynamic adsorption capacity is extremely low and the powdering is severe, resulting in insufficient adsorption performance.

Method used

The first solution is arranged using soluble aluminum salt and lithium salt, the second solution is arranged in alkali, and the third solution is arranged in sodium alginate. The Li/Al-LDHs precursor is formed through reaction, and the elution process is carried out to obtain Li/Al-LDHs adsorption. The reaction conditions such as temperature, pH and drop acceleration are controlled to improve adsorption performance.

Benefits of technology

It effectively improves the dynamic adsorption capacity of aluminum-based adsorbents, reduces the phenomenon of powdering, and improves the adsorption performance and cycle stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925657A_ABST
    Figure CN118925657A_ABST
Patent Text Reader

Abstract

The invention provides a lithium ion adsorbent preparation method, which comprises: 1, preparing a first solution by using a soluble aluminum salt and a soluble lithium salt, preparing a second solution by using a soluble alkali, and preparing a third solution by using sodium alginate; 2, adding the second solution into a mixed solution formed by mixing the first solution and the third solution, and reacting to obtain a solid-liquid mixture; step 3, carrying out solid-liquid separation on the solid-liquid mixture so as to obtain a Li / Al-LDHs precursor; and step 4, carrying out elution treatment on the Li / Al-LDHs precursor, so as to obtain the Li / Al-LDHs adsorbent. The invention also provides the lithium ion adsorbent prepared by the preparation method. The preparation method provided by the invention effectively solves the problems of sudden drop of dynamic adsorption capacity, serious pulverization and the like of the aluminum adsorbent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of new chemical materials, and in particular, relates to a lithium ion adsorbent and a preparation method thereof. Background Art

[0002] Due to the continuous depletion of solid lithium ore resources, scientists have begun to seek methods to extract lithium from salt lake brine and seawater, which has become the main direction of lithium salt production in countries around the world. Currently, there are many methods such as adsorption, membrane, extraction, calcination, and electrodialysis that are being studied for lithium extraction from salt lakes. Among them, the adsorption method has high selectivity, low pollution, simple process, and low energy consumption. It is a very promising lithium extraction method.

[0003] Aluminum-based lithium ion adsorbents have attracted much attention due to their green, efficient and recyclable properties. Aluminum-based lithium ion adsorbent powders need to be formed and granulated before being used in industrial production. When used on a large scale, they still have problems such as extremely low dynamic adsorption capacity and severe pulverization. Therefore, how to further improve the adsorption performance of aluminum-based lithium ion adsorbents is a technical problem that needs to be solved urgently. Summary of the invention

[0004] In order to solve the technical problems existing in the above-mentioned prior art, a lithium ion adsorbent and a preparation method thereof are provided according to an embodiment of the present invention.

[0005] According to one aspect of an embodiment of the present invention, a method for preparing a lithium ion adsorbent is provided, comprising: step 1, preparing a first solution using a soluble aluminum salt and a soluble lithium salt, preparing a second solution using a soluble base, and preparing a third solution using sodium alginate; step 2, adding the second solution to a mixed solution formed by mixing the first solution and the third solution to react to obtain a solid-liquid mixture; step 3, performing solid-liquid separation on the solid-liquid mixture to obtain a Li / Al-LDHs precursor; step 4, eluting the Li / Al-LDHs precursor to obtain a Li / Al-LDHs adsorbent.

[0006] In an example of the preparation method of the lithium ion adsorbent provided in the above aspect, the soluble aluminum salt includes at least one of anhydrous aluminum chloride, hydrated aluminum chloride, aluminum sulfate, hydrated aluminum sulfate, aluminum nitrate, hydrated aluminum nitrate, aluminum silicate, and aluminum sulfide; wherein the aluminum ion concentration in the first solution is 0.1-10 mol / L.

[0007] In an example of the method for preparing a lithium ion adsorbent provided in the above aspect, the soluble lithium salt includes at least one of anhydrous lithium chloride, hydrated lithium chloride, anhydrous lithium hydroxide, hydrated lithium hydroxide, lithium carbonate, lithium acetate and lithium nitrate; wherein the lithium ion concentration in the first solution is 0.1-10 mol / L.

[0008] In an example of the method for preparing a lithium ion adsorbent provided in the above aspect, the soluble alkali includes at least one of sodium hydroxide, potassium hydroxide, lithium hydroxide, calcium hydroxide, ammonia water, and urea; wherein the alkali concentration in the second solution is 0.5-20.0 mol / L.

[0009] In an example of the method for preparing the lithium ion adsorbent provided in the above aspect, the amount of sodium alginate added to prepare the third solution is selected to be 0.1%-15%.

[0010] In an example of the method for preparing the lithium ion adsorbent provided in the above aspect, the step 2 specifically comprises: uniformly dropping the second solution into the mixed solution formed by the first solution and the third solution and stirring at a constant temperature; wherein the flow rate during the dropping is 5-60 mL·min -1 , the reaction time is 0-24h, the reaction temperature is 10-90℃; the pH value of the mixed solution after the dropwise addition is adjusted to prepare gibbsite by reaction; wherein the pH value of the mixed solution after the pH value adjustment is greater than 3 and less than 12.

[0011] In an example of the method for preparing the lithium ion adsorbent provided in the above aspect, the solid-liquid separation in step three includes at least one of centrifugal filtration, mechanical filter press and vacuum filtration.

[0012] In an example of the method for preparing the lithium ion adsorbent provided in the above aspect, the molar ratio of lithium ions to aluminum ions in the first solution is 0.2-5.

[0013] In an example of the preparation method of the lithium ion adsorbent provided in the above aspect, the step three specifically includes: performing solid-liquid separation on the solid-liquid mixture to obtain a solid; washing the solid with water, and drying the washed solid to obtain a Li / Al-LDHs precursor; wherein the drying temperature during the drying treatment is 50-150°C, and the drying treatment method includes at least one of freeze drying, vacuum drying or oven drying.

[0014] According to another aspect of an embodiment of the present invention, a lithium ion adsorbent is prepared by the above-mentioned preparation method.

[0015] Beneficial effects: The method for preparing the lithium ion adsorbent according to the embodiment of the present invention effectively solves the problems of sudden drop in dynamic adsorption capacity and severe pulverization of aluminum-based adsorbents. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] The above and other aspects, features and advantages of the embodiments of the present invention will become more apparent through the following description in conjunction with the accompanying drawings, in which:

[0017] Figure 1 is a flow chart of a method for preparing a lithium ion adsorbent according to an embodiment of the present invention;

[0018] Figure 2 is a schematic diagram of the relationship between the adsorption capacity and the adsorption time of the lithium ion adsorbent according to the comparative example, the first embodiment and the second embodiment of the present invention;

[0019] Figure 3 is an XRD diagram of an adsorbent precursor according to a comparative example, specific embodiment 1 and specific embodiment 2 of the present invention;

[0020] Figure 4 It is a schematic diagram of the adsorption capacity of the lithium ion adsorbent according to the first and second specific embodiments of the present invention in multiple adsorption and desorption cycles. DETAILED DESCRIPTION

[0021] Hereinafter, specific embodiments of the present invention will be described in detail with reference to the accompanying drawings. However, the present invention may be implemented in many different forms, and the present invention should not be construed as being limited to the specific embodiments set forth herein. On the contrary, these embodiments are provided to explain the principles of the present invention and their practical applications, so that other persons skilled in the art can understand the various embodiments of the present invention and various modifications suitable for specific intended applications.

[0022] As used herein, the term "including" and its variations represent open terms, meaning "including but not limited to". The terms "based on", "according to", etc. mean "based at least in part on", "based at least in part on". The terms "one embodiment" and "an embodiment" mean "at least one embodiment". The term "another embodiment" means "at least one other embodiment". The terms "first", "second", etc. may refer to different or the same objects. Other definitions may be included below, whether explicit or implicit. Unless the context clearly indicates otherwise, the definition of a term is consistent throughout the specification.

[0023] Figure 1 is a flow chart of a method for preparing a lithium ion adsorbent according to an embodiment of the present invention.

[0024] Reference Figure 1 According to an embodiment of the present invention, the preparation method of the lithium ion adsorbent includes:

[0025] Step S110: preparing a first solution using a soluble aluminum salt and a soluble lithium salt, preparing a second solution using a soluble base, and preparing a third solution using sodium alginate;

[0026] Step S120: adding the second solution to a mixed solution formed by mixing the first solution and the third solution to react, so as to obtain a solid-liquid mixture;

[0027] Step S130: performing solid-liquid separation on the solid-liquid mixture to obtain a Li / Al-LDHs precursor; wherein LDHs (Layered Double Hydroxides, LDHs for short) is called double-layer hydroxide, also known as layered double metal oxide;

[0028] Step S140: performing an elution treatment on the Li / Al-LDHs precursor to obtain a Li / Al-LDHs adsorbent, wherein the elution treatment on the Li / Al-LDHs precursor is to remove part of the lithium ions in the Li / Al-LDHs precursor, thereby forming lithium vacancies.

[0029] As an example, in step S110, soluble aluminum salt and soluble lithium salt are dissolved in pure water to obtain a first solution, soluble alkali is dissolved in pure water to obtain a second solution, and sodium alginate is dissolved in pure water to obtain a third solution.

[0030] As an example, the soluble aluminum salt includes at least one of anhydrous aluminum chloride, hydrated aluminum chloride, aluminum sulfate, hydrated aluminum sulfate, aluminum nitrate, hydrated aluminum nitrate, aluminum silicate, and aluminum sulfide; wherein the aluminum ion concentration in the first solution is 0.1-10 mol / L.

[0031] As an example, the soluble lithium salt includes at least one of anhydrous lithium chloride, hydrated lithium chloride, anhydrous lithium hydroxide, hydrated lithium hydroxide, lithium carbonate, lithium acetate and lithium nitrate; wherein the lithium ion concentration in the first solution is 0.1-10 mol / L.

[0032] As an example, the soluble alkali includes at least one of sodium hydroxide, potassium hydroxide, lithium hydroxide, calcium hydroxide, ammonia water, and urea; wherein the alkali concentration in the second solution is 0.5-20.0 mol / L.

[0033] As an example, the amount of sodium alginate used to prepare the third solution is selected to be 0.1%-15%.

[0034] Furthermore, the step S120 specifically includes: uniformly dropping the second solution into the mixed solution formed by the first solution and the third solution and stirring at a constant temperature; wherein the flow rate during the dropping is 5-60 mL·min -1, the reaction time is 0-24h, the reaction temperature is 10-90℃; the pH value of the mixed solution after the dropwise addition is adjusted to prepare gibbsite by reaction; wherein the pH value of the mixed solution after the pH value adjustment is greater than 3 and less than 12.

[0035] As an example, the method of performing solid-liquid separation in step S130 includes at least one of centrifugal filtration, mechanical filter press and vacuum filtration.

[0036] As an example, the molar ratio of lithium ions to aluminum ions in the first solution is 0.2-5.

[0037] Furthermore, the step S130 specifically includes: performing solid-liquid separation on the solid-liquid mixture to obtain a solid; washing the solid with water, and drying the washed solid to obtain a Li / Al-LDHs precursor; wherein the drying temperature during the drying treatment is 50-150°C, and the drying treatment method includes at least one of freeze drying, vacuum drying or oven drying.

[0038] In addition, after step S130, the supernatant after solid-liquid separation is taken and tested to obtain a lithium ion intercalation rate of >80%. In addition, after step S140, a small amount of Li / Al-LDHs precursor and Li / Al-LDHs adsorbent is taken, dissolved in nitric acid and centrifuged, and the supernatant is taken to test the lithium ion content, and the lithium ion elution rate in Li / Al-LDHs is calculated to be >80%, thereby generating more active sites for lithium ions, reaching adsorption saturation faster, and improving the adsorption capacity.

[0039] The specific implementation of preparing the lithium ion adsorbent by using the preparation method of the lithium ion adsorbent according to the embodiment of the present invention is described below.

[0040] <Comparative Example>

[0041] Sodium hydroxide, aluminum chloride hexahydrate and lithium chloride are weighed according to the molar ratio of Na:Al:Li of 3:1:0.5, and sodium alginate is added at 0%. Pure water and sodium hydroxide are mixed to form a sodium hydroxide solution, and pure water, aluminum chloride hexahydrate and lithium chloride are mixed to form a lithium aluminum mixed solution; sodium hydroxide solution is added dropwise to the lithium aluminum mixed solution of aluminum chloride and lithium chloride at a uniform speed, and the mixture is stirred at a constant temperature for a period of time and then allowed to stand until the solid-liquid separation is achieved. The lower layer of white colloid is washed with water, centrifuged and dried, and then ground to obtain an adsorbent precursor. Take a small amount of the adsorbent precursor and mix it with pure water. After oscillation and deintercalation on a constant temperature shaker for 1 hour, wash and dry to obtain an aluminum-based adsorbent; take a small amount of the aluminum-based adsorbent and mix it with the initial lithium ion solution, oscillate and adsorb on a constant temperature shaker for 1.5 hours, the adsorption saturation time is <30 minutes, and the adsorption capacity is >5.0 mg / g. Figure 2The curve SA-LDHs-A is shown in FIG. Figure 2 It is a schematic diagram of the relationship between the adsorption capacity and the adsorption time of the lithium ion adsorbent according to the comparative example, the first embodiment and the second embodiment of the present invention.

[0042] <Specific implementation method one>

[0043] Sodium hydroxide, aluminum chloride hexahydrate and lithium chloride are weighed in a ratio of 3:1:0.5 for the molar ratio of Na:Al:Li, and 5% sodium alginate is added. Pure water and sodium hydroxide are mixed to form a sodium hydroxide solution, and pure water, aluminum chloride hexahydrate and lithium chloride are mixed to form a lithium aluminum mixed solution, and sodium alginate and pure water are mixed to form a sodium alginate solution. The sodium hydroxide solution is uniformly added dropwise to the mixed solution formed by the lithium aluminum mixed solution and the sodium alginate solution, and the mixture is stirred at a constant temperature for a period of time and then allowed to stand until the solid-liquid separation of the mixture is completed. The lower layer of white colloid is washed with water, centrifuged and dried, and then ground to obtain an adsorbent precursor. Take a small amount of the adsorbent precursor and mix it with pure water, shake and deintercalate on a constant temperature shaker for 1 hour, then wash and dry to obtain an aluminum-based adsorbent; take a small amount of the aluminum-based adsorbent and mix it with the initial lithium ion solution, shake and adsorb on a constant temperature shaker for 1 hour, the adsorption saturation time is <30min, and the adsorption capacity is >6.0mg / g. Figure 2 As shown in curve SA-LDHS-B.

[0044] <Specific implementation method two>

[0045] Sodium hydroxide, aluminum chloride hexahydrate and lithium chloride are weighed in a ratio of 3:1:0.5 for the molar ratio of Na:Al:Li, and sodium alginate is added at 10%. Pure water and sodium hydroxide are mixed to form a sodium hydroxide solution, and pure water, aluminum chloride hexahydrate and lithium chloride are mixed to form a lithium aluminum mixed solution, and sodium alginate and pure water are mixed to form a sodium alginate solution. The sodium hydroxide solution is uniformly added dropwise to the mixed solution formed by the lithium aluminum mixed solution and the sodium alginate solution, and the mixture is stirred at a constant temperature for a period of time and then allowed to stand until the solid-liquid separation of the mixture is completed. The lower layer of white colloid is washed with water, centrifuged and dried, and then ground to obtain an adsorbent precursor. A small amount of the adsorbent precursor is mixed with pure water, and after oscillation and deintercalation on a constant temperature shaker for 1 hour, the aluminum adsorbent is washed and dried to obtain a aluminum adsorbent; a small amount of the aluminum adsorbent is mixed with the initial lithium ion solution, and adsorbed on a constant temperature shaker for 1 hour. The adsorption saturation time is <30min, and the adsorption capacity is >7.0mg / g. Figure 2 The curve in is shown as SA-LDHs-C.

[0046] Figure 3 1 is an XRD diagram of an adsorbent precursor according to a comparative example, a specific embodiment 1 and a specific embodiment 2 of the present invention. Figure 3In the figure, curve SA-LDHs-A corresponds to the ratio, curve SA-LDHs-B corresponds to the first embodiment, curve SA-LDHs-C corresponds to the second embodiment, and Gibbsite represents gibbsite. Figure 3 The characteristic peaks of gibbsite almost disappeared, and the prepared Li / Al-LDHs precursor had a high degree of crystallinity and could overlap with the corresponding LiAl·LDHs standard card 31-0700 at 11.4°, 20.3°, 22.9°, 35.8°, 39.6° and 46.8°, indicating that Li / Al-LDHs were successfully formed.

[0047] Figure 4 Schematic diagram of the adsorption capacity of multiple adsorption and desorption cycles of the lithium ion adsorbent according to the first and second specific embodiments of the present invention. Figure 4 Column SA-LDHs-B corresponds to the first embodiment, and column SA-LDHs-C corresponds to the second embodiment. Figure 4 According to the lithium ion adsorbent of the first and second embodiments of the present invention, after 8 adsorption and desorption cycles, the adsorption capacity is greater than 6 mg / g, and the adsorption rate is maintained at 85%, which effectively solves the problem of the sudden drop in the dynamic adsorption capacity of the aluminum adsorbent. Analysis shows that since the cross-linked structure of sodium alginate supports and protects the powder, the porous sodium alginate-based material can provide a channel for the solution to enter and exit, thereby solving the problem of the sudden drop in the adsorption capacity of the aluminum adsorbent after granulation.

[0048] In summary, the method for preparing the lithium ion adsorbent according to the embodiment of the present invention effectively solves the problems of sudden drop in dynamic adsorption capacity and severe pulverization of aluminum-based adsorbents.

[0049] The terms "exemplary," "example," and the like used throughout this specification mean "used as an example, instance, or illustration" and do not mean "preferred" or "advantageous" over other embodiments. The detailed description includes specific details for the purpose of providing an understanding of the described techniques. However, these techniques can be implemented without these specific details. In some instances, in order to avoid obscuring the concepts of the described embodiments, well-known structures and devices are shown in block diagram form.

[0050] The optional implementation modes of the embodiments of the present invention are described in detail above in conjunction with the accompanying drawings. However, the embodiments of the present invention are not limited to the specific details in the above implementation modes. Within the technical concept of the embodiments of the present invention, various simple modifications can be made to the technical solutions of the embodiments of the present invention, and these simple modifications all belong to the protection scope of the embodiments of the present invention.

[0051] The above description of the contents of this specification is provided to enable any person of ordinary skill in the art to implement or use the contents of this specification. Various modifications to the contents of this specification will be apparent to those of ordinary skill in the art, and the general principles defined herein may be applied to other variations without departing from the scope of protection of the contents of this specification. Therefore, the contents of this specification are not limited to the examples and designs described herein, but are consistent with the widest range of principles and novel features disclosed herein.

Claims

1. A method for preparing a lithium ion adsorbent, characterized in that: The preparation method comprises: Step 1: preparing a first solution using a soluble aluminum salt and a soluble lithium salt, preparing a second solution using a soluble base, and preparing a third solution using sodium alginate; Step 2: adding the second solution into a mixed solution formed by mixing the first solution and the third solution to react, so as to obtain a solid-liquid mixture; Step 3, performing solid-liquid separation on the solid-liquid mixture to obtain a Li / Al-LDHs precursor; Step 4: Eluting the Li / Al-LDHs precursor to obtain a Li / Al-LDHs adsorbent.

2. The preparation method according to claim 1, characterized in that: The soluble aluminum salt includes at least one of anhydrous aluminum chloride, hydrated aluminum chloride, aluminum sulfate, hydrated aluminum sulfate, aluminum nitrate, hydrated aluminum nitrate, aluminum silicate, and aluminum sulfide; wherein the aluminum ion concentration in the first solution is 0.1-10 mol / L.

3. The preparation method according to claim 1, characterized in that: The soluble lithium salt includes at least one of anhydrous lithium chloride, hydrated lithium chloride, anhydrous lithium hydroxide, hydrated lithium hydroxide, lithium carbonate, lithium acetate and lithium nitrate; wherein the lithium ion concentration in the first solution is 0.1-10 mol / L.

4. The preparation method according to claim 1, characterized in that: The soluble alkali includes at least one of sodium hydroxide, potassium hydroxide, lithium hydroxide, calcium hydroxide, ammonia water, and urea; wherein the alkali concentration in the second solution is 0.5-20.0 mol / L.

5. The preparation method according to claim 1, characterized in that: The amount of sodium alginate used to prepare the third solution is selected to be 0.1%-15%.

6. The preparation method according to claim 1, characterized in that: The step 2 specifically includes: The second solution is uniformly added to the mixed solution formed by the first solution and the third solution and stirred at a constant temperature; wherein the flow rate during the addition is 5-60 mL·min -1 , the reaction time is 0-24h, and the reaction temperature is 10-90℃; The pH value of the mixed solution after the dropwise addition is regulated to prepare gibbsite by reaction; wherein the pH value of the mixed solution after the pH value is regulated is greater than 3 and less than 12.

7. The preparation method according to claim 1, characterized in that: The solid-liquid separation method in step three includes at least one of centrifugal filtration, mechanical filter press and vacuum filtration.

8. The preparation method according to claim 1, characterized in that: The molar ratio of lithium ions to aluminum ions in the first solution is 0.2-5.

9. The preparation method according to claim 1, characterized in that: The step three specifically includes: Performing solid-liquid separation on the solid-liquid mixture to obtain a solid; The solid matter is washed with water, and the washed solid matter is dried to obtain a Li / Al-LDHs precursor; The drying temperature during the drying process is 50-150° C., and the drying process includes at least one of freeze drying, vacuum drying or oven drying.

10. A lithium ion adsorbent prepared by the method for preparing a lithium ion adsorbent according to any one of claims 1 to 9.