PEI / g-C3N4 composite material capable of efficiently adsorbing humic acid as well as preparation method and application of PEI / g-C3N4 composite material
Through the preparation of PEI/g-C3N4 composite material, the composite of PEI and secondary calcined g-C3N4 is used to solve the problem of low adsorption efficiency of existing adsorption materials on humic acid, and the effect of efficient adsorption of humic acid is achieved. The rate reached 157.1 mg/g.
Patent Information
- Application Number
- CN202411176806.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-12
AI Technical Summary
The adsorption efficiency of existing adsorption materials on humic acid is low, making it difficult to meet the demand for its removal in water treatment.
Using PEI/g-C3N4 composite material, by mixing polyethyleneimine with secondary calcined g-C3N4, stirring, separation and washing, an adsorbent that is highly effective in adsorbing humic acid is prepared, and the composite of PEI and g-C3N4 is used. Increase adsorption rate.
Highly efficient adsorption of humic acid is achieved, with an adsorption rate of more than 145 mg/g, which significantly improves the adsorption effect in the prior art.
Smart Images

Figure CN118925688A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of water treatment, and in particular to a PEI / g-C3N4 composite material for efficiently adsorbing humic acid, a preparation method and an application thereof. Background Art
[0002] Humic acids (HAs) are naturally occurring molecules commonly found in wastewater that react with widely used chlorine disinfectants to form carcinogenic byproducts such as trihalomethanes, haloacetic acids, and haloketones. In addition, studies have shown that a large amount of natural organic matter found in wastewater, including HAs, can be toxic to aquatic organisms, thereby destabilizing the food chain and affecting human health. At the same time, HAs interfere with the removal of heavy metals and other toxic pollutants from contaminated water through complex physicochemical interactions. For these reasons, multiple government agencies have implemented strict restrictions to limit the amount of natural organic matter, such as HAs, in water.
[0003] Over the past few decades, technologies for removing HAs from wastewater include coagulation / sedimentation, ion exchange resins, membrane filtration, biofiltration, advanced oxidation processes, and adsorption. HAs adsorption treatment is generally considered to be the simplest and most cost-effective method for removing organic pollutants from water. Many different types of adsorbents have been developed, such as carbonaceous materials, metal oxides, low-cost agricultural materials, clays, zeolites, biopolymers, composite materials, etc. However, the adsorption efficiency of current adsorbent materials for humic acid is not high enough and needs to be improved. Summary of the invention
[0004] The purpose of the present invention is to overcome the above technical deficiencies, provide a PEI / g-C3N4 composite material for efficiently adsorbing humic acid, and a preparation method and application thereof, so as to solve the technical problem of low adsorption efficiency of humic acid in the prior art.
[0005] In order to achieve the above technical purpose, the technical solution provided by the present invention is: In a first aspect, the present invention provides a method for preparing a PEI / g-C3N4 composite material for efficiently adsorbing humic acid, comprising the following steps: mixing polyethyleneimine, secondary calcined g-C3N4 and water, stirring for more than 10 hours, and then separating and washing to obtain a PEI / g-C3N4 composite material.
[0006] Preferably, the step of mixing polyethyleneimine, secondary calcined g-C3N4 and water is specifically as follows: dissolving polyethyleneimine in deionized water, and then adding secondary calcined g-C3N4.
[0007] Preferably, the ratio of polyethyleneimine to water is 1 g: (10-50) mL.
[0008] Preferably, the mass ratio of polyethyleneimine to secondary calcined g-C3N4 is (0.5-4):1.
[0009] Preferably, the stirring time is 12 to 48 hours.
[0010] Preferably, the preparation steps of the secondary calcined g-C3N4 include: adding a nitric acid solution dropwise to a melamine solution at 50 to 80°C to obtain a mixed solution; the mixed solution is naturally cooled to obtain a precipitate, the precipitate is separated and washed and dried; the dried precipitate is calcined at 500 to 600°C, and then cooled to room temperature to obtain tubular g-C3N4; the tubular g-C3N4 is calcined at 510 to 550°C, and then cooled to room temperature to obtain secondary calcined g-C3N4.
[0011] Further preferably, the melamine solution is obtained by dissolving melamine in an alcohol solvent at 50-80° C.; the alcohol solvent includes ethylene glycol; the ratio of melamine to the alcohol solvent is (1-4) g:120 mL; the concentration of the nitric acid solution is 0.15 mol / L; and the ratio of melamine to nitric acid is 1 g:(8-12) mmol.
[0012] Further preferably, the dried precipitate is calcined at 500-600°C for 2-4 h; and the tubular g-C3N4 is calcined at 510-550°C for 1.5-4 h.
[0013] In a second aspect, the present invention provides a PEI / g-C3N4 composite material for efficiently adsorbing humic acid obtained by the above preparation method.
[0014] In a third aspect, the present invention provides an application of the above-mentioned PEI / g-C3N4 composite material as an adsorbent in the efficient adsorption of humic acid.
[0015] Compared with the prior art, the beneficial effects of the present invention include: The present invention uses secondary calcined g-C3N4 as a raw material, which has a large specific surface area; and then composites it with PEI, and increases the adsorption rate of humic acid through PEI, thereby achieving efficient adsorption of humic acid. According to tests, the PEI / g-C3N4 composite material prepared by the present invention is used as an adsorbent, and the adsorption rate of humic acid is above 145 mg / g, up to 157.1 mg / g. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 The SEM images of the tubular g-C3N4 (TCN) and the secondary calcined g-C3N4 (TCN-550) prepared in Example 1 of the present invention, wherein (A) TCN, (B) TCN-550; Figure 21 is the XRD pattern of the tubular g-C3N4 (TCN) and the secondary calcined g-C3N4 (TCN-550) prepared in Example 1 of the present invention; Figure 3 is the XRD pattern of PEI / TCN-550 prepared in Example 1 of the present invention; Figure 4 It is the adsorption rate result in Application Example 1 of the present invention. DETAILED DESCRIPTION
[0017] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0018] In view of the problem that the adsorption efficiency of current adsorption materials for humic acid in water is not high enough, the present invention provides a PEI / g-C3N4 composite material for efficiently adsorbing humic acid, a preparation method and an application thereof. The PEI / g-C3N4 composite material obtained by compounding polyethyleneimine (PEI) with g-C3N4 adsorbs Has. The composite material is environmentally friendly, simple to prepare, and has a good adsorption effect. It can solve practical problems in the field of water treatment and promote the development of the field of environmental science and engineering.
[0019] In a first aspect, the present invention provides a method for preparing a PEI / g-C3N4 composite material for efficiently adsorbing humic acid, comprising the following steps: The polyethyleneimine, the secondary calcined g-C3N4 and water are mixed, stirred for more than 10 hours, and then separated and washed to obtain a PEI / g-C3N4 composite material.
[0020] Preferably, the step of mixing polyethyleneimine, secondary calcined g-C3N4 and water is specifically as follows: dissolving polyethyleneimine in deionized water, and then adding secondary calcined g-C3N4.
[0021] Preferably, the ratio of polyethyleneimine to water is 1g: (10-50) mL. Specifically, the ratio of polyethyleneimine to water can be selected from 1g: 10mL, 1g: 15mL, 1g: 20mL, 1g: 25mL, 1g: 30mL, 1g: 35mL, 1g: 40mL, 1g: 45mL, 1g: 50mL or any value between 1g: (10-50) mL. If the solution is too dense, that is, the solute concentration is too high, some solutes may no longer continue to dissolve in the solvent, resulting in precipitation or crystallization. Solutions with high concentrations tend to have higher viscosities, that is, the fluidity becomes worse. On the one hand, higher concentrations mean that more reactant molecules have an increased chance of meeting, which may promote the reaction; but on the other hand, high concentrations may also result in limited mass transfer rates, thereby affecting the reaction efficiency. Too low a concentration will reduce the chance of reactant molecules meeting, thereby reducing the reaction rate.
[0022] Preferably, the mass ratio of polyethyleneimine to secondary calcined g-C3N4 is (0.5-4):1. Specifically, the mass ratio of polyethyleneimine to secondary calcined g-C3N4 can be selected from 0.5:1, 1:1, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1, 4:1 or any value between (0.5-4):1. If the mass ratio of polyethyleneimine to secondary calcined g-C3N4 is too low, the effect is not obvious; if it is too high, the role of secondary calcined g-C3N4 will be hindered, and the effect is also poor.
[0023] Preferably, the stirring time is 12 to 48 h. Specifically, the stirring time can be selected from 12 h, 13 h, 15 h, 18 h, 20 h, 22 h, 24 h, 25 h, 26 h, 28 h, 30 h, 32 h, 35 h, 38 h, 40 h, 45 h, 48 h or any value between 12 to 48 h. If the stirring time is too short, the contact between the reactants is insufficient, the reaction rate is limited, and the expected reaction effect cannot be achieved. If the stirring time is too long, it not only wastes precious energy resources, but also may cause non-target side reactions in the system due to slight changes in the environment (such as temperature fluctuations, impurity introduction), thereby affecting the purity and yield of the product.
[0024] Preferably, the preparation steps of the secondary calcined g-C3N4 include: adding a nitric acid solution dropwise to a melamine solution at 50 to 80°C to obtain a mixed solution; the mixed solution is naturally cooled to obtain a precipitate, the precipitate is separated and washed and dried; the dried precipitate is calcined at 500 to 600°C, and then cooled to room temperature to obtain tubular g-C3N4; the tubular g-C3N4 is calcined at 510 to 550°C, and then cooled to room temperature to obtain secondary calcined g-C3N4. Specifically, the calcination temperature of the dried precipitate can be selected from 510°C, 520°C, 530°C, 540°C, 550°C, 560°C, 570°C, 580°C, 590°C, 600°C or any value between 500 and 600°C; the calcination temperature of tubular g-C3N4 can be selected from 510°C, 520°C, 530°C, 540°C, 550°C or any value between 510 and 550°C.
[0025] Further preferably, the melamine solution is obtained by dissolving melamine in an alcohol solvent at 50 to 80°C; the alcohol solvent includes ethylene glycol; and the ratio of melamine to the alcohol solvent is (1 to 4) g: 120 mL. Specifically, the preparation temperature of the melamine solution can be selected from 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C or any value between 50 and 80°C. If the heating temperature is too low, the dissolution is insufficient, and if the heating temperature is too high, energy is wasted on the one hand, and some side reactions may occur on the other hand. The ratio of melamine to the alcohol solvent can be selected from 1 g: 120 mL, 1.5 g: 120 mL, 2 g: 120 mL, 2.5 g: 120 mL, 3 g: 120 mL, 3.5 g: 120 mL, 4 g: 120 mL or any value between (1 to 4) g: 120 mL.
[0026] More preferably, the concentration of the nitric acid solution is 0.15 mol / L, and the ratio of melamine to nitric acid is 1 g: (8-12) mmol. Specifically, the ratio of melamine to nitric acid can be selected from any value between 1 g: 8 mmol, 1 g: 9 mmol, 1 g: 10 mmol, 1 g: 11 mmol, 1 g: 12 mmol, or 1 g: (6-12) mmol.
[0027] More preferably, the precipitate is washed with ethanol 2 to 4 times.
[0028] Further preferably, the dried precipitate is calcined at 500-600°C for 2-4 h; the tubular g-C3N4 is calcined at 510-550°C for 1.5-4 h. Specifically, the calcination time of the dried precipitate is 2h, 2.5h, 3h, 3.5h, 4h or any value between 2 and 4 h; the calcination time of the tubular g-C3N4 is 1.5h, 2h, 2.5h, 3h, 3.5h, 4h or any value between 1.5 and 4 h. If the temperature is too low or the time is too short, the precursor molecules will not be fully cross-linked, the reaction will not be complete, and the purity and crystallinity of the product will be affected. On the contrary, if the temperature is too high or the time is too long, it may trigger side reactions, destroy the product structure, or even lead to no product generation at all, such as excessive oxidation or carbonization.
[0029] In a second aspect, the present invention provides a PEI / g-C3N4 composite material for efficiently adsorbing humic acid obtained by the above preparation method.
[0030] In a third aspect, the present invention provides an application of the above-mentioned PEI / g-C3N4 composite material as an adsorbent in the efficient adsorption of humic acid.
[0031] In the present invention, g-C3N4 can be made thinner and have a larger specific surface area by secondary calcination, and the adsorption effect is better after being compounded with PEI; and if the temperature of the secondary calcination is too low, it will not have any effect, and if the temperature is too high, the material will decompose or even disappear during the secondary calcination. The present invention mainly utilizes secondary calcined g-C3N4 to adsorb humic acid, and increases the adsorption rate of humic acid by compounding g-C3N4 with PEI, thereby achieving efficient adsorption of humic acid.
[0032] The present invention is further described in detail below through specific examples.
[0033] Example 1 A method for preparing a PEI / g-C3N4 composite material for efficiently adsorbing humic acid comprises the following steps: S1, the preparation process of secondary calcined g-C3N4 is as follows: (1) Dissolve 4 g of melamine in 120 ml of ethylene glycol at 60 °C and stir to obtain a transparent solution; (2) Prepare 240 mL of 0.15 mol / L nitric acid aqueous solution and add it dropwise to the above melamine solution; (3) After the above solution is naturally cooled to room temperature, a white precipitate appears. The white precipitate is washed three times with ethanol and then dried in an oven at 55°C. (4) The white precipitate was placed in a crucible, calcined at 600 °C for 2 h, and then naturally cooled to room temperature to obtain tubular g-C3N4, denoted as TCN; (5) The tubular g-C3N4 was calcined again at 550 °C in air atmosphere for 3 h to obtain a secondary calcined g-C3N4, which was recorded as TCN-550; The SEM image of TCN is as follows Figure 1 As shown in A, the SEM image of TCN-550 is as follows Figure 1 As shown in B, it can be seen that after secondary calcination, the morphology of TCN-550 relative to TCN changes.
[0034] The XRD patterns of TCN and TCN-550 are shown in Figure 2 As shown, it is shown that all synthesized materials are g-C3N4.
[0035] S2, preparation of PEI / TCN-550 composite material: 1 g of PEI was dissolved in 20 mL of deionized water, TCN-550 was added at a mass ratio of PEI:TCN-550=2:1, stirred for 24 h, and finally washed three times with deionized water to obtain a PEI / TCN-550 composite material, recorded as 2PEI / TCN-550.
[0036] The XRD pattern of 2PEI / TCN-550 is as follows: Figure 3 As shown, it can be seen that the addition of PEI does not change the crystal phase of g-C3N4.
[0037] Example 2 The only difference from Example 1 is that in the adjustment step S2, PEI:TCN-550=1:1, and the other steps and conditions are the same as Example 1. The obtained PEI / TCN-550 composite material is recorded as 1PEI / TCN-550.
[0038] Example 3 The only difference from Example 1 is that in the adjustment step S2, PEI:TCN-550=3:1, and the other steps and conditions are the same as Example 1. The obtained PEI / TCN-550 composite material is recorded as 3PEI / TCN-550.
[0039] Comparative Example 1 The only difference from Example 1 is that the secondary calcination temperature in step (5) of step S1 is adjusted to 500°C, and the other steps and conditions are the same as Example 1. The obtained secondary calcined g-C3N4 is recorded as TCN-500.
[0040] Comparative Example 2 The only difference from Example 1 is that the preparation process of the secondary calcination of g-C3N4 in step S1 is adjusted, and melamine is directly calcined twice as a raw material, and the other steps and conditions are the same as those in Example 1; the difference is that: S1, the preparation process of secondary calcined g-C3N4 is as follows: (1) 4 g of melamine was placed directly in a crucible and calcined at 600 °C for 2 h to obtain bulk g-C3N4, denoted as BCN; (2) The bulk g-C3N4 was calcined at 550°C in air atmosphere for 3 h to obtain flake g-C3N4, which was recorded as BCN-550.
[0041] Application Example 1 20 mg of the adsorbent was added to 50 mL of 100 mg / L humic acid solution at pH=3, stirred at room temperature for 2 h, 3 mL of the solution was centrifuged at 1000 rpm for 5 min, and the supernatant was tested for absorbance at 254 nm using a UV-visible spectrophotometer. The adsorbents were BCN, BCN-550, TCN, TCN-500, TCN-550, 1PEI / TCN-550, 2PEI / TCN-550, and 3PEI / TCN-550 prepared in the above Examples 1-3 and Comparative Examples 1-2.
[0042] The adsorption rate was obtained according to the absorbance. Figure 4 As shown in A and B.
[0043] from Figure 4 A It can be seen that the adsorption rate of humic acid by tubular g-C3N4 (TCN) is higher than that of bulk g-C3N4 (BCN). After secondary calcination (TCN-500, TCN-550 and BCN-550), the adsorption rate of humic acid by both can be further improved. Moreover, the adsorption rate of humic acid by g-C3N4 (TCN-550) calcined twice at 550 °C is the highest, which is 114.3 mg / g, which is 1.3 times that of the secondary calcined bulk g-C3N4 (BCN-550), 4.3 times that of the tubular g-C3N4 (TCN), and 8.9 times that of the bulk g-C3N4 (BCN).
[0044] from Figure 4 B It can be seen that after the secondary calcination of g-C3N4 composite PEI, the obtained 1PEI / TCN-550, 2PEI / TCN-550 and 3PEI / TCN-550 can further enhance their adsorption of humic acid, and the mass ratio of PEI to secondary calcined g-C3N4 is 2, which is the highest, that is, 157.1 mg / g. Taking all factors into consideration, the preferred mass ratio of polyethyleneimine to secondary calcined g-C3N4 in the present invention is (1~2):1.
[0045] In summary, the present invention uses secondary calcined g-C3N4 as raw material, which has a large specific surface area; and then composites it with PEI, and increases the adsorption rate of humic acid through PEI, thereby achieving efficient adsorption of humic acid. According to tests, under the same conditions, the PEI / g-C3N4 composite material prepared by the present invention is used as an adsorbent, and the adsorption rate of humic acid is above 145 mg / g, up to 157.1 mg / g.
[0046] The specific implementation of the present invention described above does not constitute a limitation on the protection scope of the present invention. Any other corresponding changes and modifications made based on the technical concept of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A method for preparing a PEI / g-C3N4 composite material for efficient adsorption of humic acid, characterized in that: The following steps are involved: The polyethyleneimine, the secondary calcined g-C3N4 and water are mixed, stirred for more than 10 hours, and then separated and washed to obtain a PEI / g-C3N4 composite material.
2. The method for preparing the PEI / g-C3N4 composite material for efficient adsorption of humic acid according to claim 1, characterized in that: The step of mixing polyethyleneimine, secondary calcined g-C3N4 and water is specifically as follows: dissolving polyethyleneimine in deionized water, and then adding secondary calcined g-C3N4.
3. The method for preparing the PEI / g-C3N4 composite material for efficient adsorption of humic acid according to claim 1, characterized in that: The ratio of the polyethyleneimine to water is 1 g: (10-50) mL.
4. The method for preparing the PEI / g-C3N4 composite material for efficient adsorption of humic acid according to claim 1, characterized in that: The mass ratio of the polyethyleneimine to the secondary calcined g-C3N4 is (0.5-4):
1.
5. The method for preparing the PEI / g-C3N4 composite material for efficient adsorption of humic acid according to claim 1, characterized in that: The stirring time is 12 to 48 hours.
6. The method for preparing the PEI / g-C3N4 composite material for efficient adsorption of humic acid according to claim 1, characterized in that: The preparation steps of the secondary calcined g-C3N4 include: Adding nitric acid solution dropwise into melamine solution at 50-80°C to obtain a mixed solution; The mixed solution is naturally cooled to obtain a precipitate, and the precipitate is separated, washed and dried; The dried precipitate is calcined at 500-600° C., and then cooled to room temperature to obtain tubular g-C3N4; The tubular g-C3N4 is calcined at 510-550°C and then cooled to room temperature to obtain secondary calcined g-C3N4.
7. The method for preparing the PEI / g-C3N4 composite material for efficient adsorption of humic acid according to claim 6, characterized in that: The melamine solution is obtained by dissolving melamine in an alcohol solvent at 50 to 80° C.; the alcohol solvent includes ethylene glycol; the ratio of melamine to the alcohol solvent is (1 to 4) g: 120 mL; The concentration of the nitric acid solution is 0.15 mol / L; the ratio of melamine to nitric acid is 1g: (8-12)mmol.
8. The method for preparing the PEI / g-C3N4 composite material for efficient adsorption of humic acid according to claim 6, characterized in that: The dried precipitate is calcined at 500-600°C for 2-4 h; the tubular g-C3N4 is calcined at 510-550°C for 1.5-4 h.
9. A PEI / g-C3N4 composite material with high efficiency in adsorbing humic acid obtained by the preparation method according to any one of claims 1 to 8.
10. Use of the PEI / g-C3N4 composite material as claimed in claim 9 as an adsorbent for efficient adsorption of humic acid.