A PAMAM / sodium alginate composite aerogel for adsorbing Au(III) and its preparation method and application
By preparing PAMAM/sodium alginate composite aerogel, using its functional groups to adsorb Au(III), the problem of small adsorption amount and poor selectivity in the prior art was solved, and efficient and selective Au was achieved (III) Recycling.
Patent Information
- Application Number
- CN202411419413.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-12
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-10-12
AI Technical Summary
When recovering Au(III) in water, existing adsorbents have problems such as small adsorption amount, poor selectivity and slow adsorption speed, especially in strong acid or strong alkaline complex solution systems containing lead, iron, copper, nickel and other interfering ions. Poor performance.
High-performance PAMAM/sodium alginate composite aerogel is prepared by crosslinking different algebras of PAMAM and sodium alginate by glutaraldehyde, using its rich functional groups such as OH, COO-, C=O, CONH, C-N The high-efficiency adsorption of Au(III) was carried out to achieve 100% selective adsorption.
High capacity and high selective adsorption of Au(III), can effectively remove Au(III) in complex solutions, and maintain excellent adsorption performance under different pH and temperature conditions.
Smart Images

Figure CN118925691B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of aerogel preparation and precious metal recovery, and specifically relates to a PAMAM / sodium alginate composite aerogel for adsorbing Au (III) and a preparation method and application thereof. Background Art
[0002] Gold, as a non-renewable resource, is widely used in electronics, medicine, catalysis and other fields due to its excellent ductility, conductivity and catalytic activity. The global annual consumption of gold for industrial processing has exceeded 300 tons, but part of the gold is discharged into the water environment in the form of Au(III), causing serious waste of resources. Therefore, it is urgent to develop a method that can efficiently recover Au(III) in water.
[0003] At present, the methods for recovering Au(III) from water bodies include electrochemical method, adsorption method, chemical precipitation method, ion exchange method, etc. Among them, the adsorption method is considered to be one of the most effective methods for recovering Au(III) from the aqueous phase because of its high efficiency, high selectivity and no secondary pollution. Among many adsorbents, aerogel, as a new type of material, has the advantages of high efficiency, low cost, and easy formability. At present, biomass aerogel has become a major trend in the field of adsorption and separation due to its advantages such as low environmental load, abundant resources, and good biocompatibility.
[0004] Sodium alginate (SA) is a biopolysaccharide extracted from seaweed, composed of β-D-mannuronic acid and α-L-guluronic acid, and is one of the most abundant polysaccharides in nature. SA has the advantages of abundant sources, good biocompatibility, low cost, and non-toxicity, making it an ideal choice for preparing aerogels. SA aerogels have abundant hydroxyl and carboxyl groups, are easy to functionalize, and can effectively chelate with metal ions to remove them efficiently. However, the mechanical properties and adsorption properties of pure SA aerogels are limited and need to be improved through physical / chemical modifications. Wang et al. designed elastic polyethyleneimine / SA aerogels for Cr 6+ and Cd 2+ Gao et al. used SA and KMnO4 modified cotton stalk biochar as raw materials and used the sol-gel method to prepare biochar with excellent adsorption of Pb 2+ Composite aerogel with high performance. Nitrogen-containing adsorbents have high separation efficiency and good selectivity for Au(Ⅲ), and show excellent performance in recovering gold from acid leaching solutions. Polyamide-amine dendrimers (PAMAM) are a class of highly branched polymers with the advantages of highly symmetrical structure, cavities within the molecules, rich N and O functional groups within the molecules, and hierarchical arrangement of functional groups. They are easy to combine with metal ions to achieve efficient adsorption and separation of pollutants such as metal ions. Kommu et al. synthesized PAMAM functionalized graphene and graphene oxide for efficient removal of Pb 2+Lang et al. synthesized a series of Schiff base modified PAMAM / silica adsorbents for selective removal of Hg from water using a homogeneous method. 2+ .
[0005] However, the concentration of Au(III) in gold-containing wastewater is low and the components are complex, usually a strong acid or strong alkaline complex solution system containing interfering ions such as lead, iron, copper, and nickel. Therefore, traditional adsorbents often face problems such as small adsorption capacity, poor selectivity, and slow adsorption rate in actual application, which become the key factors restricting their application.
[0006] Therefore, how to provide a composite aerogel that can achieve high capacity and high selectivity adsorption of Au(III) is a technical problem that needs to be solved urgently by those skilled in the art. Summary of the invention
[0007] In view of this, the present invention prepared high-performance PAMAM / sodium alginate composite aerogel by cross-linking PAMAM of different generations with sodium alginate through glutaraldehyde. The structure was characterized by FTIR, XPS, SEM and other means, and it was found that PAMAM / sodium alginate composite aerogel had excellent adsorption performance for Au(III).
[0008] In order to achieve the above object, the present invention adopts the following technical solution:
[0009] A method for preparing a PAMAM / sodium alginate composite aerogel for adsorbing Au(III) comprises the following steps:
[0010] 1) Dissolve sodium alginate in dilute sulfuric acid solution and stir to prepare a transparent solution A;
[0011] 2) PAMAM with ethylenediamine as the core and glutaraldehyde are slowly added dropwise into solution A in sequence and stirred to obtain a pink emulsion;
[0012] 3) ultrasonically dispersing CaCO3 powder into the pink emulsion, and then adding D-(+)-glucono delta-lactone under vigorous stirring to obtain a mixed emulsion;
[0013] 4) The mixed emulsion is quickly poured into a mold, allowed to stand, and then freeze-dried to obtain a PAMAM / sodium alginate composite aerogel.
[0014] Preferably, in the step 1), the mass concentration of sodium alginate in the transparent solution A is 2%, and the pH of the dilute sulfuric acid solution is 4.0.
[0015] Preferably, the PAMAM in step 2) is a 1.0, 2.0 or 3.0 generation PAMAM dendrimer G1.0, G2.0 or G3.0 with ethylenediamine as the core; More preferably, the PAMAM in step 2) is a 2.0 generation PAMAM dendrimer G2.0 with ethylenediamine as the core;
[0016] Preparation of G1.0: Under the protection of N2, methyl acrylate and ethylenediamine were dissolved in methanol, stirred and reacted at 25-50°C for 24-36 hours, and methanol and excess methyl acrylate were removed by distillation under reduced pressure after the reaction to obtain product G0.5; G0.5 and ethylenediamine were dissolved in methanol, stirred and reacted at 25-35°C for 48-60 hours under the protection of N2, and methanol and excess ethylenediamine were removed by distillation under reduced pressure after the reaction to obtain product G1.0;
[0017] Preparation of G2.0: Under the protection of N2, G1.0 and methyl acrylate were dissolved in methanol, stirred and reacted at 25-50°C for 36-48 hours, and methanol and excess methyl acrylate were removed by vacuum distillation after the reaction to obtain product G1.5; G1.5 and ethylenediamine were dissolved in methanol, stirred and reacted at 25-35°C for 72-84 hours under the protection of N2, and methanol and excess ethylenediamine were removed by vacuum distillation after the reaction to obtain product G2.0;
[0018] Preparation of G3.0: Under the protection of N2, G2.0 and methyl acrylate were dissolved in methanol, and the reaction was stirred at 25-50°C for 48-60 h. After the reaction, methanol and excess methyl acrylate were removed by distillation under reduced pressure to obtain product G2.5; G2.5 and ethylenediamine were dissolved in methanol, and the reaction was stirred at 25-35°C for 96-108 h under the protection of N2. After the reaction, methanol and excess ethylenediamine were removed by distillation under reduced pressure to obtain product G3.0.
[0019] Preferably, the volume ratio of methyl acrylate to ethylenediamine in the preparation of G1.0 is (65-80):10; the mass volume ratio of G0.5 to ethylenediamine is 20g:(16-20mL);
[0020] In the preparation of G2.0, the mass volume ratio of G1.0 to methyl acrylate is 20 g: (34-42 mL); the mass volume ratio of G1.5 to ethylenediamine is 20 g: (11-13 mL);
[0021] In the preparation of G3.0, the mass volume ratio of G2.0 to methyl acrylate is 20g:(24~30mL); the mass volume ratio of G2.5 to ethylenediamine is 20g:(11~15mL).
[0022] Preferably, the mass ratio of sodium alginate to PAMAM is 1:0.1-0.7, more preferably 1:0.3-0.7, and further preferably 1:0.7.
[0023] Preferably, the mass ratio of PAMAM to CaCO3 powder is 0.1~0.7:0.16; the mass ratio of PAMAM to D-(+)-glucono delta-lactone is 0.1~0.7:0.32.
[0024] Preferably, in step 2), a uniform pink emulsion is obtained after mechanical stirring at 25° C. for 3 h.
[0025] The invention also discloses a PAMAM / sodium alginate composite aerogel for adsorbing Au (III) prepared by the preparation method.
[0026] The invention also discloses the application of the PAMAM / sodium alginate composite aerogel prepared by the preparation method in adsorbing Au (III) in a solution.
[0027] Preferably, the PAMAM / sodium alginate composite aerogel can selectively adsorb Au(III) in a solution containing Au(III), Co(II), Cr(III), Ni(II), Cu(II) and Cd(II);
[0028] During adsorption, the pH of the solution is adjusted to -0.5 to 5.0, and the adsorption temperature is 288 to 308 K. More preferably, during adsorption, the pH of the solution is adjusted to -0.5 to 3.0.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] The aerogel prepared by the present invention contains abundant functional groups, such as OH, COO - , C=O, CONH, CN and other functional groups participated in the adsorption of Au(Ⅲ). Au(Ⅲ) in wastewater was mainly in the form of AuCl4 - The aerogel prepared by the present invention exists in the form of protonated amino groups, and 100% selective adsorption of Au (III) is achieved through electrostatic interaction. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is the synthetic route diagram of PAMAM of the present invention;
[0032] Figure 2 Schematic diagram of the synthesis of PAMAM / sodium alginate composite aerogel in Example 1 (taking G1.0 as an example);
[0033] Figure 3The infrared spectra of PAMAM and PAMAM / sodium alginate composite aerogels prepared in Examples 1-3, wherein (a) is the infrared spectrum of PAMAM, (b) is the infrared spectrum of PAMAM / sodium alginate composite aerogel prepared in Example 1, (c) is the infrared spectrum of PAMAM / sodium alginate composite aerogel prepared in Example 2, and (d) is the infrared spectrum of PAMAM / sodium alginate composite aerogel prepared in Example 3;
[0034] Figure 4 The XPS spectra and high-resolution spectra of the PAMAM / sodium alginate composite aerogels prepared in Examples 1-3, wherein (a) is the XPS spectra of SA / G1-7, SA / G2-7, and SA / G3-7, (b) is the high-resolution spectrum of C 1s of SA / G2-7, (c) is the high-resolution spectrum of N 1s of SA / G2-7, and (d) is the high-resolution spectrum of O 1s of SA / G2-7;
[0035] Figure 5 The nitrogen content of the PAMAM / sodium alginate composite aerogel prepared in Examples 1-3;
[0036] Figure 6 The scanning electron microscope images of the PAMAM / sodium alginate composite aerogels prepared in Examples 1-3, wherein (ac) are scanning electron microscope images of SA / G1-7 at different magnifications, (df) are scanning electron microscope images of SA / G2-7 at different magnifications, and (gi) are scanning electron microscope images of SA / G3-7 at different magnifications;
[0037] Figure 7 Thermogravimetric curves of SA / G1-7, SA / G2-7 and SA / G3-7 prepared in Examples 1-3;
[0038] Figure 8 The stress-strain curves of the PAMAM / sodium alginate composite aerogels prepared in Examples 1-3, wherein (a) is the stress-strain curves of SA / G2-1~7, and (b) is the stress-strain curves of SA / G1-7, SA / G2-7, and SA / G3-7;
[0039] Fig. 9 The static adsorption curves of Au(III) on the PAMAM / sodium alginate composite aerogels prepared in Examples 1-3 (C=100 ppm, T=298 K), wherein (a) is the static adsorption curve of the PAMAM / sodium alginate composite aerogel based on G1.0, (b) is the static adsorption curve of the PAMAM / sodium alginate composite aerogel based on G2.0, and (c) is the static adsorption curve of the PAMAM / sodium alginate composite aerogel based on G3.0;
[0040] Fig.10 The effect of solution pH on the adsorption of Au(Ⅲ) by SA / G1-7, SA / G2-7, and SA / G3-7, where (a) is the study of the adsorption performance of SA / G1-7, SA / G2-7, and SA / G3-7 for Au(Ⅲ) at different pH values (C=100 ppm, T=298 K), and (b) is the Zeta potential of the surface of SA / G1-7, SA / G2-7, and SA / G3-7 at different pH values;
[0041] Fig.11 Figure 2 shows the kinetic curves of Au(Ⅲ) adsorption on SA / G1-7, SA / G2-7 and SA / G3-7, where (a) is the kinetic curves of Au(Ⅲ) adsorption on SA / G1-7, SA / G2-7 and SA / G3-7 (pH=1.0, C=50 ppm, T=298 K), (b) is the kinetic curves of Au(Ⅲ) adsorption on SA / G1-7, SA / G2-7 and SA / G3-7 (pH=1.0, C=100 ppm, T=298 K), (c) is the kinetic curves of Au(Ⅲ) adsorption on SA / G1-7, SA / G2-7 and SA / G3-7 (pH=1.0, C=200 ppm, T=298 K), and (d) is the PSO kinetic fitting curves of Au(Ⅲ) adsorption on SA / G1-7, SA / G2-7 and SA / G3-7 (pH=1.0, C=100 ppm, T = 298 K);
[0042] Fig.12 The adsorption isotherms of SA / G1-7, SA / G2-7 and SA / G3-7 for Au(Ⅲ), where (a) is the adsorption isotherms of SA / G1-7, SA / G2-7 and SA / G3-7 for Au(Ⅲ) (C=50-900 ppm, T=298 K, pH=1.0), and (b) is the adsorption isotherm of SA / G2-7 for Au(Ⅲ) (C=50-900 ppm, T=288-308 K, pH=1.0);
[0043] Fig.13 is the adsorption selectivity of SA / G1-7, SA / G2-7, and SA / G3-7 for Au(Ⅲ), where (ac) are the adsorption selectivity of SA / G1-7, SA / G2-7, and SA / G3-7 for Au(Ⅲ) (pH=1.0, C=100 ppm, T=298 K), and (d) is the adsorption selectivity of SA / G1-7, SA / G2-7, and SA / G3-7 for Au(Ⅲ) in simulated wastewater (C=100 ppm, T=298 K);
[0044] Fig.14The fixed bed adsorption breakthrough curves of SA / G2-7 for Au(Ⅲ), where (a) is the fixed bed adsorption breakthrough curves of SA / G2-7 for Au(Ⅲ) at different filling column heights, (b) is the fixed bed adsorption breakthrough curves of SA / G2-7 for Au(Ⅲ) at different solution flow rates, and (c) is the fixed bed adsorption breakthrough curves of SA / G2-7 for Au(Ⅲ) at different solution concentrations;
[0045] Fig.15 The infrared spectra and XPS spectra of SA / G1-7, SA / G2-7 and SA / G3-7 before and after the adsorption of Au(Ⅲ), among which (a) is the infrared spectra of SA / G1-7, SA / G2-7 and SA / G3-7 before and after the adsorption of Au(Ⅲ), (b) is the XPS spectra of SA / G1-7, SA / G2-7 and SA / G3-7 before and after the adsorption of Au(Ⅲ), (c) is the high-resolution spectrum of Au 4f before and after the adsorption of Au(Ⅲ) by SA / G2-7, (d) is the high-resolution spectrum of C 1s before and after the adsorption of Au(Ⅲ) by SA / G2-7, (e) is the high-resolution spectrum of N 1s before and after the adsorption of Au(Ⅲ) by SA / G2-7, and (f) is the high-resolution spectrum of O 1s before and after the adsorption of Au(Ⅲ) by SA / G2-7. DETAILED DESCRIPTION
[0046] Examples of the present invention are described below. The examples are intended to explain the present invention but are not to be construed as limiting the present invention.
[0047] Experimental reagents
[0048] Sodium alginate (SA) and glutaraldehyde (GA) were purchased from Shanghai McLean Biochemical Co., Ltd.; hydrochloric acid, toluene, ethylenediamine (EDA), methyl acrylate (MA), methanol, calcium carbonate (CaCO3), D-(+)-gluconoδ-lactone (DGL), chloroauric acid (HAuCl4·4H2O), cupric chloride (CuCl2·2H2O), nickel nitrate (Ni(NO3)2·6H2O), cadmium chloride (CdCl2·2.5H2O), cobalt nitrate (Co(NO3)2·6H2O), and chromium nitrate (Cr(NO3)3·9H2O) were purchased from Sinopharm Chemical Reagent Co., Ltd. All reagents were of analytical grade.
[0049] Test Method
[0050] The infrared spectroscopy (FTIR) test was performed using a Nicolet Is50 infrared spectrometer from Nicolet Corporation of the United States, sampling 32 times and selecting a frequency collection range of 500-4000 cm -1The sample morphology was characterized by a SU8010 scanning electron microscope (SEM) from Hitachi, Japan. Zeta potential was tested using a Zetasizer Ultra particle size analyzer from Malvern Panalytical, UK. X-ray photoelectron spectroscopy (XPS) was performed using an ESCALAB XI from Thermo Fisher Scientific, USA. + The concentration of metal ions was determined by using an atomic absorption spectrophotometer (AAS) produced by Varian Corporation of the United States.
[0051] Example 1
[0052] Under the protection of N2, 75 mL of MA and 10 mL of EDA were dissolved in 130 mL of methanol and stirred at 50°C for 24 h. After the reaction, methanol and excess MA were removed by distillation under reduced pressure to obtain product G0.5. Subsequently, 20 g of G0.5 and 18 mL of EDA were dissolved in 100 mL of methanol and stirred at 25°C for 48 h under the protection of N2. After the reaction, methanol and excess EDA were removed by distillation under reduced pressure to obtain product G1.0.
[0053] 1g SA was dissolved in 49g dilute sulfuric acid solution (pH=4.0) and stirred vigorously for 30 minutes to prepare a transparent solution A. Subsequently, 0.7g G1.0 and 5mL GA were slowly added to the A solution, and a uniform pink emulsion was obtained after mechanical stirring at 25°C for 3h. 0.16g CaCO3 powder was ultrasonically dispersed into the emulsion, and then 0.32g DGL was added under vigorous stirring; finally, the mixed emulsion was quickly poured into a mold, and freeze-dried after standing for about 6h to obtain a PAMAM / sodium alginate composite aerogel, named SA / G1-7. Under the same conditions, the mass of G1.0 was adjusted to 0.1g, 0.2g, 0.3g, 0.4g, 0.5g, and 0.6g to obtain 1.0th generation PAMAM / sodium alginate composite aerogels with different compositions, which were named SA / G1-1, SA / G1-2, SA / G1-3, SA / G1-4, SA / G1-5, and SA / G1-6, respectively.
[0054] Example 2
[0055] Under the protection of N2, 20 g of G1.0 and 38 mL of MA were dissolved in 150 mL of methanol, and the mixture was stirred at 50 °C for 36 h. After the reaction, methanol and excess EDA were removed by distillation under reduced pressure to obtain product G1.5. Subsequently, 20 g of G1.5 and 13 mL of EDA were dissolved in 150 mL of methanol, and the mixture was stirred at 25 °C for 72 h under the protection of N2. After the reaction, methanol and excess EDA were removed by distillation under reduced pressure to obtain product G2.0.
[0056] 1 g SA was dissolved in 49 g dilute sulfuric acid solution (pH = 4.0) and stirred vigorously for 30 minutes to prepare a transparent solution A. Subsequently, 0.7 g G2.0 and 5 mL GA were slowly added dropwise to solution A at 25 °C. o C for 3 h to obtain a uniform pink emulsion. 0.16 g of CaCO3 powder was ultrasonically dispersed into the emulsion, and then a certain amount of 0.32 g of DGL was added under vigorous stirring; finally, the mixed emulsion was quickly poured into a mold, and freeze-dried after standing for about 6 h to obtain a PAMAM / sodium alginate composite aerogel, named SA / G2-7. Under the same conditions, the mass of G2.0 was adjusted to 0.1 g, 0.2 g, 0.3 g, 0.4 g, 0.5 g, and 0.6 g, and the 2.0th generation PAMAM / sodium alginate composite aerogels of different compositions were obtained, named SA / G2-1, SA / G2-2, SA / G2-3, SA / G2-4, SA / G2-5, and SA / G2-6, respectively.
[0057] Example 3
[0058] Under the protection of N2, 20 g of G2.0 and 29 mL of MA were dissolved in 180 mL of methanol and stirred at 25°C for 48 h. After the reaction, methanol and excess EDA were removed by distillation under reduced pressure to obtain product G2.5. Subsequently, 20 g of G2.5 and 12 mL of EDA were dissolved in 150 mL of methanol and stirred at 25°C for 96 h under the protection of N2. After the reaction, methanol and excess EDA were removed by distillation under reduced pressure to obtain product G3.0.
[0059] 1g SA was dissolved in 49g dilute sulfuric acid solution (pH=4.0) and stirred vigorously for 30 minutes to prepare a transparent solution A. Subsequently, 0.7g G3.0 and 5 mL GA were slowly added to solution A, and a uniform pink emulsion was obtained after mechanical stirring at 25°C for 3h. 0.16g CaCO3 powder was ultrasonically dispersed into the emulsion, and then a certain amount of 0.32g DGL was added under vigorous stirring; finally, the mixed emulsion was quickly poured into a mold, and freeze-dried after standing for about 6h to obtain a PAMAM / sodium alginate composite aerogel, named SA / G3-7. Under the same conditions, the mass of G3.0 was adjusted to 0.1g, 0.2g, 0.3g, 0.4g, 0.5g, and 0.6g to obtain 3.0th generation PAMAM / sodium alginate composite aerogels with different compositions, which were named SA / G3-1, SA / G3-2, SA / G3-3, SA / G3-4, SA / G3-5, and SA / G3-6, respectively.
[0060] Structural characterization of PAMAM / sodium alginate composite aerogels prepared in Example 1-3
[0061] 1 Infrared spectroscopy analysis
[0062] The structure of PAMAM G0.5~G3.0 was preliminarily characterized by FTIR. The results are as follows Figure 3 As shown in (a), Figure 3 (a) in the figure shows that G0.5~G3.0 were successfully synthesized by the divergent synthesis method.
[0063] The infrared spectra of the synthesized series of PAMAM / sodium alginate composite aerogels are shown in Figure 3 As shown in (bd). Figure 3 (bd) in the figure show that the series of PAMAM / sodium alginate composite aerogels were successfully synthesized.
[0064] 2 X-ray photoelectron spectroscopy analysis
[0065] XPS was used to further characterize the structure of the prepared series of PAMAM / sodium alginate composite aerogels. Figure 4 As shown. Figure 4 In (a), the characteristic peaks of C, N, O, Ca, and Na can be observed in the high-resolution spectra of all composite materials, indicating that the PAMAM / sodium alginate composite aerogel was successfully synthesized. Taking SA / G2-7 as an example, the spectra of the series of composite materials were further analyzed by high-resolution XPS spectra. Figure 4 In the high-resolution spectrum of C1s in (b), the characteristic peaks at 287.45, 285.86, 284.44 and 285.15 eV are attributed to C=O, CO, CC and CN. Figure 4 The two peaks centered at 399.90 and 398.80 eV in (c) indicate the presence of CN and CONH groups. Figure 4 (d) is the high-resolution spectrum of O1s, OH / COO - The characteristic peaks of CO and CONH appear at 532.52, 531.84 and 530.85 eV respectively. The XPS characterization results further prove the successful synthesis of PAMAM / sodium alginate composite aerogel.
[0066] 3 Element analysis
[0067] The nitrogen element in the synthesized series of composite aerogels was quantitatively analyzed by elemental analysis. The results are as follows Figure 5 As shown in the figure, the nitrogen content of the composite aerogel gradually increases with the increase of the dendrimer generation number. It is expected that the composite aerogel with 0.7g PAMAM added has better adsorption performance for metal ions. The nitrogen content in SA / G1-7, SA / G2-7 and SA / G3-7 is 0.38, 0.40 and 0.42 mmol·g, respectively.-1 .
[0068] 4 SEM analysis
[0069] Taking SA / G1-7, SA / G2-7 and SA / G3-7 as examples, the morphology of composite aerogels was studied by scanning electron microscopy (SEM). Figure 6 As shown. All samples showed a typical three-dimensional porous structure composed of interlinked sheets, proving that the aerogel was successfully synthesized. With the increase of PAMAM generation, the pores of the composite aerogel became more regular and dense, indicating that the cross-linking between the sheets became tighter and tighter. Its uniformly dispersed micron-scale pores and smooth internal and external channels are conducive to the adsorption of metal ions.
[0070] 5 Thermogravimetric analysis
[0071] TGA results show that the prepared PAMAM / sodium alginate composite aerogel has good thermal stability and can be used for adsorption in a wide temperature range below 200°C.
[0072] 6Compression performance test
[0073] The PAMAM / sodium alginate composite aerogels all exhibit a typical compression process. Under the condition of fixed PAMAM generation, as the amount of PAMAM added increases, the compressive capacity of the composite aerogel increases first and then decreases, such as Figure 8 As shown in (a) in the figure. The composite aerogel SA / G2-4 with 0.4 g of G2.0 added has the strongest compressive capacity, with a stress of 0.32 MPa at a strain of 50%. Under the condition of a fixed addition amount, the compressive capacity of the composite aerogel first increases and then decreases with the increase of PAMAM generation number, as shown in Figure 8 As shown in (b) in the figure. Under the condition of 60% strain, the maximum stress that SA / G2-7 can withstand is 0.22MPa, which is 2.56 times that of SA / G1-7. The results show that the cross-linking between PAMAM and sodium alginate enhances the compressive strength and mechanical properties of the composite aerogel to a certain extent.
[0074] Test example
[0075] 1. Test Method
[0076] 1 Static adsorption
[0077] Weigh 10 mg of a series of PAMAM / sodium alginate composite aerogels into a 100 mL iodine volumetric flask, add 20 mL of 100 ppm Au(Ⅲ) solution to each aerogel, and place it in a constant temperature oscillator at 25°C for 12 hours. Subsequently, the concentration of residual Au(Ⅲ) was determined by AAS. The adsorption amount q (mg·g) of different metal ions was calculated according to formula (2-1): -1 ):
[0078] (2-1)
[0079] Where C0 is the initial concentration (ppm); C is the concentration after adsorption (ppm); V represents the volume of the solution (L); and W represents the mass of the adsorbent (g).
[0080] 2 Effect of solution pH on Au(Ⅲ) adsorption performance
[0081] Taking SA / G1-7, SA / G2-7 and SA / G3-7 as representatives, a batch experiment method was adopted to study the effect of solution pH of -0.5~5.0 on the adsorption of Au(Ⅲ) according to the same steps as the study of the static adsorption performance of Au(Ⅲ). The concentration after adsorption was determined and the adsorption amount of Au(Ⅲ) at different pH values was calculated.
[0082] 3 Adsorption kinetics of Au(Ⅲ)
[0083] The adsorption kinetics of Au(Ⅲ) on a series of composite aerogels was also studied using SA / G1-7, SA / G2-7, and SA / G3-7 as representatives. The batch experiment method was used, and similar steps were followed for the static adsorption capacity determination. The solution pH was fixed at 1.0, and samples were taken at different time intervals. The concentration of adsorbed Au(Ⅲ) at different times was determined and the adsorption amount was calculated.
[0084] 4 Isothermal adsorption of Au(Ⅲ)
[0085] The isothermal adsorption of Au(Ⅲ) by a series of composite aerogels was also studied using SA / G1-7, SA / G2-7, and SA / G3-7 as representatives. The batch experiment method was used, and the pH of the solution was fixed at 1.0. The concentration of Au(Ⅲ) after composite aerogel adsorption was measured at different Au(Ⅲ) concentrations (50-700 ppm) at different adsorption temperatures (288, 298, and 308K), and the adsorption amount was calculated.
[0086] 5 Study on the adsorption selectivity of Au(Ⅲ)
[0087] Taking SA / G1-7, SA / G2-7, and SA / G3-7 as representatives, the solution pH was fixed at 1.0, and the adsorption solution was replaced with binary ion solutions of Au(Ⅲ)-Ni(Ⅱ), Au(Ⅲ)-Cu(Ⅱ), Au(Ⅲ)-Cd(Ⅱ), Au(Ⅲ)-Co(Ⅱ), and Au(Ⅲ)-Cr(Ⅲ), where the concentrations of Au(Ⅲ), Co(Ⅱ), Cr(Ⅲ), Ni(Ⅱ), Cu(Ⅱ), and Cd(Ⅱ) were 100 ppm respectively. After adsorption, the concentrations of different ions were measured and the adsorption amount of all ions was calculated to study the adsorption selectivity of the series of composite aerogels for Au(Ⅲ).
[0088] 2. Test Results
[0089] 1 Static adsorption
[0090] The adsorption performance of the series of PAMAM / sodium alginate composite aerogels prepared in Examples 1-3 of the present invention for Au(III) is shown in the following table: Fig. 9 As shown in (ac) in the figure. With the increase of the content of dendrimers, the adsorption performance of composite aerogels at the same generation for Au(Ⅲ) gradually improves. Under the condition of the same addition amount, with the increase of the generation of dendrimers, the adsorption capacity for Au(Ⅲ) first increases and then decreases. The adsorption performance of SA / G1-7, SA / G2-7, and SA / G3-7 for Au(Ⅲ) is higher than that of other proportions of dendrimers with the same generation. Subsequent experiments will be studied using SA / G1-7, SA / G2-7, and SA / G3-7 as examples.
[0091] 2 Effect of solution pH on the adsorption of Au(Ⅲ)
[0092] Solution pH is a key factor affecting the adsorption capacity of the adsorbent. Under different pH conditions, the adsorption performance of composite aerogels for Au(Ⅲ) first increases and then decreases. Fig.10 The surface charge state of the adsorbent was investigated by Zeta potential, and the results are shown in Fig.10 As shown in (b) in the figure, as the pH value increases, the surface charge of the adsorbent gradually changes from positive to negative. It can be inferred that the smaller the pH value, the stronger the adsorption capacity of the composite aerogel for Au(Ⅲ). However, under the condition of pH < 1, the excess Cl in the solution - Will react with AuCl4 - Strongly compete for adsorption sites on the composite aerogel; as the pH value increases, Cl - As the concentration of AuCl4 decreases, the competition between the two decreases, and the adsorption capacity of the composite aerogel for Au(Ⅲ) increases. - Hydrolysis occurs to form a chloride-hydroxide complex of Au(III), resulting in a decrease in the adsorption efficiency of Au(III).
[0093] 3 Adsorption kinetics of Au(Ⅲ)
[0094] Taking SA / G1-7, SA / G2-7 and SA / G3-7 as examples, the adsorption kinetics of Au(Ⅲ) at different concentrations were investigated. Fig.11As shown in (ac) in the figure. The adsorption rate of Au(Ⅲ) at different concentrations by the composite aerogels was fast in the first 100 min, then the adsorption rate gradually decreased and finally reached equilibrium. For example, at an initial concentration of 100 ppm, the adsorption amounts of Au(Ⅲ) by SA / G1-7, SA / G2-7, and SA / G3-7 in the first 100 min were 169.76, 179.22, and 150.07 mg·g, respectively. -1 , and can reach 84.88%, 89.61%, and 75.04% of the equilibrium. After reaching adsorption equilibrium at 360 min, the adsorption amount can reach 191.92, 199.08, and 180.61 mg·g -1 The removal rates can reach 95.96%, 99.67% and 90.30% respectively. Under the condition of Au(Ⅲ) initial concentration of 200 ppm, the adsorption of Au(Ⅲ) by SA / G1-7, SA / G2-7 and SA / G3-7 reached equilibrium within 360 min, and the adsorption amount reached 274.62, 285.83 and 260.35 mg·g -1 The removal rates can reach 61.50%, 62.34% and 58.31% respectively. When the initial concentration of Au(Ⅲ) is 50 ppm, SA / G1-7, SA / G2-7 and SA / G3-7 can completely adsorb 100% of Au(Ⅲ) in the solution within 300 min.
[0095] The adsorption kinetic data were fitted using pseudo-first-order (PFO) and pseudo-second-order kinetic models (PSO), and the results are shown in Table 1. The fitting parameter R2 of the pseudo-second-order kinetic model 2 R1 2 is closer to 1, and the equilibrium adsorption capacity (q e,cal ) and the experimental value (q e,exp ), which shows that the adsorption process of Au(Ⅲ) on composite aerogels is more consistent with the PSO kinetic model. The results show that the adsorption process of Au(Ⅲ) on composite aerogels is mainly driven by chemical adsorption and is a heterogeneous adsorption process.
[0096] Table 1 PFO and PSO model fitting parameters
[0097]
[0098] 4 Isothermal adsorption of Au(Ⅲ)
[0099] Isothermal adsorption studies were conducted by varying concentration and temperature. Fig.12 As shown. Fig.12 As shown in (a), the increase in initial concentration is conducive to the improvement of adsorption amount, but at the same time the removal rate will decrease. Fig.12 (b) in the figure shows that increasing the system temperature can increase the adsorption capacity of the adsorbent for Au(III).
[0100] The isothermal adsorption data were fitted by the Langmuir and Freundlich models, and the results are shown in Table 2. The correlation coefficient R obtained by fitting the Langmuir model L 2 are greater than the corresponding correlation coefficient R obtained by fitting the Freundlich model. F 2 The values indicate that the adsorption behavior of Au(Ⅲ) on the composite aerogel is more consistent with the Langmuir model and is a monolayer adsorption.
[0101] Table 2 Langmuir and Freundlich model parameters
[0102]
[0103] 5. Selectivity
[0104] The high selectivity of the adsorbent is the key to recovering high-purity Au from practical metallurgical solutions. 2+ Cr 3+ 、Ni 2+ , Cu 2+ and Cd 2+ The selectivity in the solution and simulated wastewater is shown in Fig.13 As shown. Under the condition of pH=1.0, SA / G1-7, SA / G2-7, and SA / G3-7 can 100% selectively adsorb Au(Ⅲ), and in the presence of Cu 2+ The Au(Ⅲ) can be selectively adsorbed 100% in simulated wastewater with metal ions much higher than Au(Ⅲ), and the adsorption amounts are 169.55, 189.93 and 183.53 mg·g -1 According to the hard-soft acid-base theory, Au(III) as a soft acid has a stronger affinity with CN, and its affinity is much higher than that of the critical acid (Co 2+ 、Ni 2+ , Cu 2+ ); and under the condition of pH=1.0, Au(Ⅲ) is mainly in the form of AuCl4 - The amine groups in the adsorbent were protonated, and 100% selective adsorption of Au(III) was achieved through electrostatic interaction.
[0105] 6 Fixed bed adsorption
[0106] The dynamic adsorption performance of the material to Au(Ⅲ) was studied through fixed bed adsorption experiments. The penetration time of the breakthrough curve has a very important influence on the operation performance and dynamic response of dynamic column adsorption. Taking SA / G2-7 as an example, Fig.14 (a), (b), and (c) are the effects of the filling column height, solution flow rate, and solution concentration on the dynamic adsorption of Au(Ⅲ). When the filling height of the adsorption column increases from 0.5 cm to 1.5 cm, the breakthrough point of Au(Ⅲ) increases from 38 min to 66 min; when the flow rate increases from 0.8 to 1.6 mL·min -1 When the concentration increased from 350 to 500 ppm, the breakthrough point of Au(Ⅲ) was shortened from 48 min to 20 min; when the concentration increased from 350 to 500 ppm, the breakthrough point was shortened from 72 min to 46 min. The results show that the breakthrough point of dynamic adsorption of Au(Ⅲ) on SA / G2-7 is delayed with the increase of the filling column height; it is advanced with the increase of initial concentration and flow rate, which leads to the deterioration of dynamic removal efficiency.
[0107] 7 Adsorption mechanism
[0108] Firstly, the adsorption mechanism of Au(Ⅲ) on composite aerogel was investigated by FTIR. The results are as follows Fig.15 For example, in the infrared spectrum of SA / G2-7, OH is at 3284 cm -1 The absorption peak near the Au(Ⅲ) was significantly weakened after the adsorption of Au(Ⅲ), which indicated that OH participated in the adsorption process of Au(Ⅲ); COO - At 1598 and 1402 cm -1 The peaks of antisymmetric and symmetric stretching vibrations are also weakened, indicating that COO - It also participates in the adsorption process of Au(Ⅲ).
[0109] The adsorption mechanism was further confirmed by XPS. Fig.15 The characteristic peaks of Au 4f and Cl 2p appeared in the XPS spectrum after adsorption, indicating that Au(Ⅲ) was successfully captured by the composite aerogel. After the adsorption of Au(Ⅲ), the high-resolution spectrum of OH / COO in O 1s - The characteristic peaks of OH, CO and CONH moved from 532.52, 531.84 and 530.85 eV to 533.19, 532.71 and 532.09 eV. The characteristic peaks of CN and CONH in the high-resolution spectrum of N 1s moved from 399.90 and 398.80 eV to 401.95 and 400.25 eV. XPS results show that OH, COO - , CONH, CN and other functional groups participate in the adsorption of Au(Ⅲ).
[0110] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a PAMAM / sodium alginate composite aerogel for adsorbing Au(III), characterized in that: The following steps are involved: 1) Dissolve sodium alginate in dilute sulfuric acid solution and stir to prepare a transparent solution A; 2) PAMAM with ethylenediamine as the core and glutaraldehyde are slowly added dropwise into solution A in sequence and stirred to obtain a pink emulsion; 3) ultrasonically dispersing CaCO3 powder into the pink emulsion, and then adding D-(+)-glucono delta-lactone under vigorous stirring to obtain a mixed emulsion; 4) Pour the mixed emulsion into a mold, let it stand and then freeze-dry to obtain the PAMAM / sodium alginate composite aerogel; In step 2), the PAMAM is a 1.0, 2.0 or 3.0 generation PAMAM dendrimer G1.0, G2.0 or G3.0 with ethylenediamine as the central core; Preparation of G1.0: Under the protection of N2, methyl acrylate and ethylenediamine were dissolved in methanol, stirred and reacted at 25-50°C for 24-36 hours, and methanol and excess methyl acrylate were removed by distillation under reduced pressure after the reaction to obtain product G0.5; G0.5 and ethylenediamine were dissolved in methanol, stirred and reacted at 25-35°C for 48-60 hours under the protection of N2, and methanol and excess ethylenediamine were removed by distillation under reduced pressure after the reaction to obtain product G1.0; Preparation of G2.0: Under the protection of N2, G1.0 and methyl acrylate were dissolved in methanol, stirred and reacted at 25-50°C for 36-48 hours, and methanol and excess methyl acrylate were removed by vacuum distillation after the reaction to obtain product G1.5; G1.5 and ethylenediamine were dissolved in methanol, stirred and reacted at 25-35°C for 72-84 hours under the protection of N2, and methanol and excess ethylenediamine were removed by vacuum distillation after the reaction to obtain product G2.0; Preparation of G3.0: Under the protection of N2, G2.0 and methyl acrylate were dissolved in methanol, and the reaction was stirred at 25-50°C for 48-60 h. After the reaction, methanol and excess methyl acrylate were removed by distillation under reduced pressure to obtain product G2.5; G2.5 and ethylenediamine were dissolved in methanol, and the reaction was stirred at 25-35°C for 96-108 h under the protection of N2. After the reaction, methanol and excess ethylenediamine were removed by distillation under reduced pressure to obtain product G3.
0.
2. The method for preparing a PAMAM / sodium alginate composite aerogel for adsorbing Au(III) according to claim 1, characterized in that: In the step 1), the mass concentration of sodium alginate in the transparent solution A is 2%, and the pH of the dilute sulfuric acid solution is 4.
0.
3. The method for preparing a PAMAM / sodium alginate composite aerogel for adsorbing Au(III) according to claim 1, characterized in that: The volume ratio of methyl acrylate to ethylenediamine in the preparation of G1.0 is (65-80):10; the mass volume ratio of G0.5 to ethylenediamine is 20g:(16-20mL); In the preparation of G2.0, the mass volume ratio of G1.0 to methyl acrylate is 20 g: (34-42 mL); the mass volume ratio of G1.5 to ethylenediamine is 20 g: (11-13 mL); In the preparation of G3.0, the mass volume ratio of G2.0 to methyl acrylate is 20g:(24~30mL); the mass volume ratio of G2.5 to ethylenediamine is 20g:(11~15mL).
4. The method for preparing a PAMAM / sodium alginate composite aerogel for adsorbing Au(III) according to claim 1, characterized in that: The mass ratio of sodium alginate to PAMAM is 1: 0.1~0.
7.
5. The method for preparing a PAMAM / sodium alginate composite aerogel for adsorbing Au(III) according to claim 1, characterized in that: The mass ratio of PAMAM to CaCO3 powder is 0.1~0.7: 0.16; the mass ratio of PAMAM to D-(+)-glucono delta-lactone is 0.1~0.7: 0.
32.
6. The method for preparing a PAMAM / sodium alginate composite aerogel for adsorbing Au(III) according to claim 1, characterized in that: Step 2) After mechanical stirring at 25°C for 3 to 5 h, a uniform pink emulsion was obtained.
7. PAMAM / sodium alginate composite aerogel for adsorbing Au(III) prepared according to the preparation method according to any one of claims 1 to 6.
8. Use of the PAMAM / sodium alginate composite aerogel prepared according to the method according to any one of claims 1 to 6 in adsorbing Au (III) in a solution.
9. The use according to claim 8, characterized in that: The PAMAM / sodium alginate composite aerogel can selectively adsorb Au(Ⅲ) from solutions containing Au(Ⅲ), Co(Ⅱ), Cr(Ⅲ), Ni(Ⅱ), Cu(Ⅱ) and Cd(Ⅱ); During adsorption, the pH of the solution was adjusted to 1~5.0 and the adsorption temperature was 288~308K.
Citation Information
Patent Citations
Micro-nano gel particle, controllable preparation method and application thereof
CN104128136A