Catalytic converter without activated aluminum oxide and preparation method thereof
By using cerium-zirconium solid solution and additives with low degradation coefficient in the three-way catalyst to replace activated alumina, the problem of Rh inactivation in the lean-ignition state is solved, the catalytic effect and stability are improved, and the catalyst is significantly enhanced Anti-aging properties and catalytic utilization.
Patent Information
- Application Number
- CN202411418688.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-12
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The reaction of activated alumina with precious metal Rh in the existing three-way catalyst in a lean state leads to the loss of catalytic effect, and the alumina itself does not have catalytic capacity, resulting in limited catalytic effect and utilization.
Using a catalyst without activated alumina, the activated alumina is replaced by a cerium-zirconium solid solution with low deterioration coefficient, combined with additives such as barium acetate, neodymium nitrate and precious metals Pd, Pt, and Rh, to optimize the composition and coating composition of the cerium-zirconium solid solution. Improve catalytic performance and stability.
It effectively avoids the inactivation of Rh, improves the catalytic effect and coating stability, significantly enhances the anti-aging performance and catalytic utilization of the catalyst, and extends the service life.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of tail gas catalyst manufacturing, in particular to a catalyst containing no activated alumina and a preparation method thereof. Background Art
[0002] The three-way catalytic converter is an indispensable part of modern internal combustion engine vehicles. The three-way catalytic converter is a purification device installed at the tail end of the automobile exhaust pipe and used to purify automobile exhaust. Its main purpose is to convert harmful gases such as carbon monoxide, hydrocarbons and nitrogen oxides contained in automobile exhaust into harmless carbon dioxide, water and nitrogen through oxidation and reduction, and then discharge them into the atmosphere.
[0003] The three-way catalytic converters on the market are generally composed of activated alumina, cerium-zirconium solid solution, additives, precious metals, etc. For example, a Chinese patent with publication number CN102003254A discloses a natural gas automobile exhaust purification catalytic converter, the front and rear catalysts of which include a carrier, a coating coated on the carrier, and a catalyst active component coated on the coating; wherein the carrier is a cordierite honeycomb ceramic material with a pore density of 300~600cpsi; the coating is a mixture of high thermal stability activated alumina, cerium-zirconium solid solution, rare earth oxide, alkaline earth metal oxide and binder; the catalytic active component is a platinum group metal and at least one transition metal composite oxide or transition metal-rare earth composite oxide. In the above catalyst, the activated alumina has a large specific surface, pore volume and stability, which can stabilize the catalyst and slow down degradation, and because of its relatively large particle size, the catalyst coating is not easy to fall off, which plays a role in supporting the catalyst. However, it was found in actual use that when λ>1, that is, in a lean combustion state, and the temperature is greater than 650°C, the precious metal Rh in the coating will react with alumina, causing Rh to lose its catalytic effect and be unable to catalyze pollutants such as nitrogen oxides, hydrocarbons, and carbon monoxide. At the same time, alumina itself does not have catalytic ability, so the catalytic effect and catalytic utilization rate are relatively limited. Summary of the invention
[0004] The technical problem to be solved by the present invention is to overcome the above-mentioned problems and provide a catalyst that does not contain activated alumina and a preparation method thereof, using a cerium-zirconium solid solution with a low degradation coefficient to replace the activated alumina, while ensuring that the coating shedding rate does not increase and having good coating firmness, while better improving the catalytic effect and coating stability.
[0005] On the one hand, the present invention provides a catalyst without activated alumina, comprising a catalyst carrier and a coating coated on the surface of the catalyst carrier, characterized in that the coating comprises the following components based on the total weight of the oxides: 80-90% cerium-zirconium solid solution, 5.5-15% oxide of an additive, 3-5% oxide of a binder, and 0-3% oxide of a noble metal; the cerium-zirconium solid solution is Cex Zr y M z O2, wherein 0.05≤x≤0.5, 0.5≤y≤0.8, 0≤z≤0.2, x+y+z=1, and M is at least one of the rare elements La, Y, Nd, and Pr; the degradation coefficient of the cerium-zirconium solid solution is defined as the ratio of the difference between its fresh specific surface area and the specific surface area after the aging test to the fresh specific surface area, and the degradation coefficient of the cerium-zirconium solid solution is ≤40%; the additives include at least barium acetate and neodymium nitrate; the precious metals include at least one of Pd and Pt and Rh.
[0006] In the present invention, the degradation coefficient of the cerium-zirconium solid solution is obtained under an aging test environment of 1000°C and 4 hours of calcination. In the above-mentioned catalyst coating, the cerium-zirconium solid solution is used to replace the original activated alumina, which effectively avoids the reaction of the activated alumina with the precious metal Rh under the lean combustion state and causes Rh to lose its catalytic effect; at the same time, by reasonably proportioning the various components, the content of the cerium-zirconium solid solution is increased, and the redox activity and oxygen storage capacity of the cerium-zirconium solid solution itself are fully utilized to enhance the catalytic performance. At the same time, the cerium-zirconium solid solution components are reasonably selected, the zirconium content is increased, and the degradation coefficient is reduced, effectively ensuring a larger pore volume and specific surface area, enhancing the material stability, and significantly improving the catalytic performance of the catalyst after aging.
[0007] As a preferred technical solution of the present invention, the mass ratio of the sum of the oxides of the noble metals Pd and Pt to the oxide of Rh is 1:1-20:1, which has low cost and good catalytic activity.
[0008] As a preferred technical solution of the present invention, the degradation coefficient is ≤20%.
[0009] As a preferred technical solution of the present invention, the auxiliary agent also includes at least one of cerium acetate and lanthanum acetate. The addition of cerium acetate and lanthanum acetate can improve the stability of the catalyst and reduce the ignition temperature of the catalyst.
[0010] As a preferred technical solution of the present invention, the oxide content of the barium acetate is 5-10%, and the oxide content of the neodymium nitrate is 0.5-5%. These two additives are easy to dissolve and can adjust the pH and viscosity.
[0011] As a preferred technical solution of the present invention, the adhesive is aluminum glue, silica gel or zirconium glue.
[0012] On the other hand, the present invention also provides a method for preparing the above-mentioned catalyst without activated alumina, comprising the following steps: (1) Selecting cerium-zirconium solid solution: Selecting a suitable cerium-zirconium solid solution according to the degradation coefficient of the cerium-zirconium solid solution, wherein the pore size of the cerium-zirconium solid solution is ≥7 nm and the D50 particle size is ≥20 μm; (2) Weighing raw materials: Calculate and weigh the cerium-zirconium solid solution, additive, binder, and noble metal salt solution according to the content of each component of the catalyst coating; (3) Step-by-step mixing: Add additives other than neodymium nitrate and pure water in a ratio of 1:5-1:10 into a ball mill and stir with a stirrer to dissolve; add cerium-zirconium solid solution, stir for 5-10 minutes and let stand for 0.5-1 hour; then add precious metal salt solutions in the order of precious metals Pd, Pt, and Rh, stir for 5-10 minutes after each addition and then let stand, with an interval of at least 0.5 hour between different precious metal salt solutions; finally, add neodymium nitrate and binder, stir for 5-10 minutes and let stand for 0.5-1 hour; control the solid content to 38-42%; (4) Adjusting pH value and particle size: Measure pH value and particle size, add nitric acid or tetraethylammonium hydroxide to adjust pH value to 3-5; add ball milling beads for ball milling to adjust particle size to 15-60 μm; filter out ball milling beads to obtain coating slurry; (5) Preparation of catalyst: The coating slurry is evenly coated on the catalyst carrier at a coating amount of 80-100 g / L, and then dried and calcined to form a catalyst.
[0013] The above preparation method has the characteristics of simple process, easy preparation and use. It utilizes cerium-zirconium solid solution to replace activated alumina to improve the catalytic effect and coating stability. At the same time, the pH value and particle size of the slurry are precisely controlled during the preparation process to ensure that the coating still has good firmness after the activated alumina is removed.
[0014] As a preferred technical solution of the present invention, in step (4), nitric acid or tetraethylammonium hydroxide is added by a gradual dripping method, and the pH value is measured after each dripping, and the operation is repeated until the pH reaches 3-5, and the amount of each dripping is 0.5-1% of the total mass of the coating. By the above-mentioned gradual dripping method, the purpose of accurately controlling the pH value of the slurry is achieved.
[0015] As a preferred technical solution of the present invention, the ball milling fine beads are made of zirconium oxide with a diameter of 2-3 mm, and the addition amount thereof is 10-20% of the total mass of the coating, and the ball milling time is 3-5 minutes.
[0016] The beneficial effects of the present invention are: 1. The catalyst prepared by the present invention uses cerium-zirconium solid solution to replace the original activated alumina, which effectively avoids the activated alumina from reacting with the precious metal Rh under lean combustion conditions and losing its activity, thereby improving the catalytic utilization rate of the precious metal Rh, and can better catalyze nitrogen oxides and carbon monoxide under the same conditions.
[0017] 2. The preparation process of the present invention is simple, does not require complicated tooling equipment, and is easy to promote and implement. By reasonably proportioning the components in the coating, the content of the cerium-zirconium solid solution is increased, and the redox activity and oxygen storage capacity of the cerium-zirconium solid solution itself are fully utilized, thereby improving the catalytic performance.
[0018] 3. The present invention optimizes the material composition of the cerium-zirconium solid solution and reduces the attenuation of pore volume by increasing the zirconium content, thereby enhancing material stability, reducing the degradation coefficient, ensuring that it has a larger pore volume and specific surface area, and significantly enhancing the anti-aging performance of the catalyst. After aging, it can still retain good catalytic activity, thereby extending the service life and improving the catalytic utilization rate, and having a better ability to purify carbon monoxide and nitrogen oxides; by precisely controlling the pH value and particle size of the slurry, the coating in the inactive alumina state will not reduce its firmness compared to the coating with active alumina under the same conditions. DETAILED DESCRIPTION
[0019] Now the present invention will be further described: Example 1
[0020] This embodiment discloses a catalyst without active alumina, comprising a catalyst carrier and a coating coated on the surface of the catalyst carrier. The coating comprises the following components based on the total weight of the oxide: cerium-zirconium solid solution Ce 0.3 Zr 0.6 La 0.04 Y 0.02 Nd 0.04 O288%, barium acetate oxide 6%, neodymium nitrate oxide 1.05%, binder aluminum oxide 3.6%, precious metal Pt oxide 0.36%, Rh oxide 0.072%. The degradation coefficient of the cerium-zirconium solid solution is defined as the ratio of the difference between its fresh specific surface area and the specific surface area after the 1000°C, 4-hour calcination aging test to the fresh specific surface area. The cerium-zirconium solid solution Ce selected in this embodiment is 0.3 Zr 0.6 La 0.04 Y 0.02 Nd 0.04 O2 fresh specific surface area is 60m 2 / g, the specific surface area after aging test is 52m 2 / g, and the deterioration coefficient is 13.33%. Barium acetate and neodymium nitrate as additives have the advantages of being easily soluble and being able to adjust pH and viscosity.
[0021] This embodiment also discloses a method for preparing the above catalyst, which includes the following steps.
[0022] (1) Selecting cerium-zirconium solid solution: Select the above cerium-zirconium solid solution Ce according to the degradation coefficient of the cerium-zirconium solid solution. 0.3 Zr 0.6La 0.04 Y 0.02 Nd 0.04 O2, wherein the pore size of the cerium-zirconium solid solution is ≥7nm and the D50 particle size is ≥20μm.
[0023] (2) Weighing raw materials: Calculate and weigh the cerium-zirconium solid solution Ce according to the content of each component of the catalyst coating above. 0.3 Zr 0.6 La 0.04 Y 0.02 Nd 0.04 O2, barium acetate, neodymium nitrate, aluminum gel, precious metal Pt salt solution and precious metal Ph salt solution.
[0024] (3) Step-by-step mixing: add barium acetate and pure water in a ratio of 1:10 into a ball mill and stir with a stirrer to dissolve; add cerium zirconium solid solution Ce 0.3 Zr 0.6 La 0.04 Y 0.02 Nd 0.04 O2, stir for 5 minutes and then let it stand for 0.5 hours; then add the corresponding precious metal salt solutions in the order of Pt first and then Rh, stir for 5 minutes after each addition and then let it stand, and there is a 0.5 hour interval between the two precious metal salt solutions; finally, add neodymium nitrate and binder, stir for 5 minutes and then let it stand for 0.5 hours, and control the solid content to 38-42% by diluting with pure water.
[0025] (4) Adjusting the pH value and particle size: Measure the pH value and particle size, and use a stepwise dripping method to add nitric acid or tetraethylammonium hydroxide to adjust the pH value to 3-5, wherein the pH value is measured after each dripping, and the operation is repeated until the pH reaches 3-5. The dripping amount each time is 0.5-1% of the total mass of the coating; add zirconium oxide ball milling beads with a diameter of 2-3 mm for ball milling, and the addition amount is 10-20% of the total mass of the coating. The ball milling time is 3-5 minutes, and the particle size is adjusted to 15-60 μm; filter out the ball milling beads to obtain a coating slurry; During the above steps (1) to (4), the temperature is controlled at 20-30°C throughout the process to ensure the stable reaction of each material.
[0026] (5) Preparation of catalyst: The coating slurry was evenly coated on a 0.127 L 300 mesh catalyst carrier with a coating amount of 80 g / L. The catalyst was formed after drying and calcining at 550 degrees Celsius for 3 hours.
[0027] Example 2 The catalyst without activated alumina disclosed in this embodiment is different from that in embodiment 1 in that the cerium-zirconium solid solution in the coating is Ce 0.4 Zr 0.5 La 0.04 Y 0.02 Nd0.04 O2, its fresh specific surface area is 65m 2 / g, the specific surface area after aging test is 54m 2 / g, the degradation coefficient is 16.92%.
[0028] The preparation method of the catalyst is basically the same as that of Example 1, except that: according to the composition of the above coating, the cerium-zirconium solid solution material selected and weighed is Ce 0.4 Zr 0.5 La 0.04 Y 0.02 Nd 0.04 O2.
[0029] Example 3 The catalyst without activated alumina disclosed in this embodiment is different from that in embodiment 1 in that the cerium-zirconium solid solution in the coating is Ce 0.4 Zr 0.5 La 0.05 Y 0.05 O2, fresh specific surface area is 64m 2 / g, the specific surface area after aging test is 53m 2 / g, the degradation coefficient is 17.19%.
[0030] The preparation method of the catalyst is basically the same as that of Example 1, except that: according to the composition of the above coating, the cerium-zirconium solid solution material selected and weighed is Ce 0.4 Zr 0.5 La 0.05 Y 0.05 O2.
[0031] Example 4 The catalyst disclosed in this embodiment without activated alumina is basically the same as that in Example 1, except that the types and contents of the precious metal oxides in the components contained in the coating are different, including 0.196% of the precious metal Pd oxide, 0.196% of the Pt oxide, and 0.039% of the Rh oxide. The cerium-zirconium solid solution is the same as that in Example 1. 0.3 Zr 0.6 La 0.04 Y 0.02 Nd 0.04 O 2 。
[0032] The catalyst preparation method is basically the same as that in Example 1, except that: in step (2), according to the content of each component in the above-mentioned catalyst coating, the corresponding three precious metal salt solutions, including precious metal Pd, Pt, and Rh salt solutions, are calculated and weighed; in step (3), the precious metal salt solutions are added in the order of precious metals Pd, Pt, and Rh, and after each addition, they are stirred for 5 minutes and then allowed to stand, and the interval between different precious metal salt solutions is 0.5 hours.
[0033] Comparative Example 1 The catalyst proposed in Comparative Example 1 is different from that in Example 1 in that the catalyst coating has a fresh specific surface area of 150 m 2 / g, aging specific surface area is 100m 2 / g of active alumina replaces half of the cerium-zirconium solid solution, that is, Ce 0.3 Zr 0.6 La 0.04 Y 0.02 Nd 0.04 O2 content is 44%, the activated alumina content is 44%.
[0034] The preparation method of the catalyst is basically the same as that of Example 1, except that: according to the component content in the coating, the activated alumina is weighed to replace half of the cerium-zirconium solid solution Ce. 0.3 Zr 0.6 La 0.04 Y 0.02 Nd 0.04 O2, in step (3), the weighed cerium-zirconium solid solution and activated alumina are added into the ball mill at the same time and stirred.
[0035] Comparative Example 2 Comparative Example 2 is basically the same as Example 4, except that: the catalyst coating component uses a fresh specific surface area of 150m 2 / g, aging specific surface area is 100m 2 / g of activated alumina replaces half of the cerium-zirconium solid solution, Ce 0.3 Zr 0.6 La 0.04 Y 0.02 Nd 0.04 O2 content is The content of activated alumina is 44%. In the catalyst preparation method, activated alumina is weighed to replace half of the cerium-zirconium solid solution, and the two are added into a ball mill at the same time and stirred.
[0036] The catalysts prepared in Examples 1-4 and Comparative Examples 1-2 were subjected to performance tests, including coating shedding tests and catalytic effect tests. The coating shedding test conditions were to place the prepared catalysts in ultrasonic waves of the same power for 30 minutes. The test results are shown in Table 1.
[0037] Example Coating weight before ultrasonic Coating weight after ultrasonic Dropout rate Example 1 10.22 9.98 2.35% Example 2 10.57 10.28 2.74% Example 3 10.35 10.07 2.71% Example 4 10.51 10.17 3.24% Comparative Example 1 10.25 9.95 2.93% Comparative Example 2 10.37 9.93 4.24% The catalytic effect test is to first weld the prepared fresh catalyst and place it on the same vehicle for testing, and record the pollutant emission data in the fresh state; then the catalyst is subjected to high temperature aging treatment at 950℃ for 5 hours, and after aging, it is welded and placed on the same vehicle for testing, and the pollutant emission data in the aging state is recorded. The test data refer to Table 2 and Table 3.
[0038] Example CO (mg) NO (mg) Example 1 554.25 29.21 Example 2 451.65 35.69 Example 3 402.51 39.59 Example 4 505.19 31.57 Comparative Example 1 558.32 37.56 Comparative Example 2 652.19 32.69 Example CO (mg) NO (mg) Example 1 710.32 36.94 Example 2 650.21 39.61 Example 3 622.73 43.51 Example 4 695.51 38.51 Comparative Example 1 973.75 73.95 Comparative Example 2 1015.35 75.15 The data in Table 1 show that the coating firmness of the catalyst coating of single cerium-zirconium solid solution and no activated alumina meets the requirements, and the coating shedding rate is lower than that of the catalyst coating containing activated alumina under the same conditions. The data in Tables 2 and 3 show that in the fresh state, the catalytic effects of the catalyst coating containing activated alumina and the catalyst coating containing no activated alumina on CO and NO are not much different. In the aged state, the catalyst coating containing no activated alumina has a better catalytic effect on CO and NO. The cerium-zirconium solid solution makes the precious metals platinum, palladium and rhodium better maintain their activity, are not easy to deactivate, and have a higher coating utilization rate.
[0039] The specific embodiments described herein are merely illustrative of the principles and effects of the present invention and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical ideas disclosed by the present invention are still covered by the claims of the present invention.
Claims
1. A catalyst without activated alumina, comprising a catalyst carrier and a coating applied on the surface of the catalyst carrier, characterized in that: The coating comprises the following components according to the total weight of oxides: 80-90% cerium-zirconium solid solution, 5.5-15% oxide of auxiliary agent, 3-5% oxide of binder, and 0-3% oxide of precious metal; the cerium-zirconium solid solution is Ce x Zr y M z O2, wherein 0.05≤x≤0.5, 0.5≤y≤0.8, 0≤z≤0.2, x+y+z=1, and M is at least one of the rare elements La, Y, Nd, and Pr; the degradation coefficient of the cerium-zirconium solid solution is defined as the ratio of the difference between its fresh specific surface area and the specific surface area after the aging test to the fresh specific surface area, and the degradation coefficient of the cerium-zirconium solid solution is ≤40%; the additives include at least barium acetate and neodymium nitrate; the precious metals include at least one of Pd and Pt and Rh.
2. The catalyst without activated alumina according to claim 1, characterized in that: The mass ratio of the sum of the oxides of the noble metals Pd and Pt to the oxide of Rh is 1:1-20:
1.
3. The catalyst without activated alumina according to claim 1, characterized in that: The degradation coefficient is ≤20%.
4. The catalyst without activated alumina according to claim 1, characterized in that: The auxiliary agent also includes at least one of cerium acetate and lanthanum acetate.
5. The catalyst without activated alumina according to claim 1, characterized in that: The oxide content of the barium acetate is 5-10%, and the oxide content of the neodymium nitrate is 0.5-5%.
6. The catalyst containing no activated alumina according to claim 1, characterized in that: The adhesive is aluminum glue, silica gel or zirconium glue.
7. A method for preparing a catalyst without activated alumina as claimed in any one of claims 1 to 6, characterized in that: The steps include: (1) Selecting cerium-zirconium solid solution: Selecting a suitable cerium-zirconium solid solution according to the degradation coefficient of the cerium-zirconium solid solution, wherein the pore size of the cerium-zirconium solid solution is ≥7 nm and the D50 particle size is ≥20 μm; (2) Weighing raw materials: Calculate and weigh the cerium-zirconium solid solution, additive, binder, and noble metal salt solution according to the content of each component of the catalyst coating; (3) Step-by-step mixing: Add additives other than neodymium nitrate and pure water in a ratio of 1:5-1:10 into a ball mill and stir with a stirrer to dissolve; add cerium-zirconium solid solution, stir for 5-10 minutes and let stand for 0.5-1 hour; then add precious metal salt solutions in the order of precious metals Pd, Pt, and Rh, stir for 5-10 minutes after each addition and then let stand, with an interval of at least 0.5 hour between different precious metal salt solutions; finally, add neodymium nitrate and binder, stir for 5-10 minutes and let stand for 0.5-1 hour; control the solid content to be 38-42%; (4) Adjusting pH value and particle size: Measure pH value and particle size, add nitric acid or tetraethylammonium hydroxide to adjust pH value to 3-5; add ball milling beads for ball milling to adjust particle size to 15-60 μm; filter out ball milling beads to obtain coating slurry; (5) Preparation of catalyst: The coating slurry is evenly coated on the catalyst carrier at a coating amount of 80-100 g / L, and then dried and calcined to form a catalyst.
8. The method for preparing a catalyst without activated alumina according to claim 7, characterized in that: In the step (4), nitric acid or tetraethylammonium hydroxide is added gradually by dripping, and the pH value is measured after each dripping. The operation is repeated until the pH reaches 3-5. The amount of each dripping is 0.5-1% of the total mass of the coating.
9. The method for preparing a catalyst without activated alumina according to claim 7, characterized in that: The ball milling fine beads are zirconium oxide with a diameter of 2-3 mm, and the addition amount thereof is 10-20% of the total mass of the coating, and the ball milling time is 3-5 minutes.
Citation Information
Patent Citations
Preparation method of cerium-zirconium based solid solution
CN104492414A
Method of producing oxide compositions of cerium-zirconium and rare-earth elements
RU2766540C1
Palladium-Supported Catalyst Composites
US20100212293A1
Automotive Catalysts With Palladium Supported In An Alumina-Free Layer
US20180071679A1
Exhaust gas purification catalyst
US20190093531A1