ZnCo2O4 / Co0. 2Cd0. 8S-Vs composite catalyst rich in sulfur vacancies and application thereof

Co0.2Cd0.8S-Vs and ZnCo2O4 were synthesized by hydrothermal method to form ZnCo2O4/Co0.2Cd0.8S-Vs composite catalyst, which solved the photocorrosion problem of photocatalysts, achieved efficient catalytic hydrogen production and high stability, and catalytic performance Significantly improved.

CN118925751AActive Publication Date: 2024-11-12CHANGZHOU UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410997517.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

Existing photocatalysts such as CdS are prone to photocorrosion after light irradiation, resulting in reduced catalytic activity and low hydrogen production efficiency. The preparation method is cumbersome, and the catalyst stability and hydrogen production rate are insufficient.

Method used

Co0.2Cd0.8S-Vs were synthesized by hydrothermal method and compounded with ZnCo2O4 to form ZnCo2O4/Co0.2Cd0.8S-Vs composite catalyst, and efficient catalytic production of H2 or H2O2 was achieved under the co-action of ultrasound and light.

Benefits of technology

The composite catalyst has high catalytic activity and stability, and has the best hydrogen production performance under piezoelectric photocatalytic conditions. The catalytic performance exceeds Co0.2Cd0.8S and CdS. The preparation method is simple, energy-saving and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925751A_ABST
    Figure CN118925751A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of piezoelectric electro-catalysts, and particularly relates to a ZnCo2O4 / Co0. 2Cd0. 8S-Vs composite catalyst rich in sulfur vacancies and application thereof. The preparation method comprises the following steps: preparing Co0. 2Cd0. 8S through a hydrothermal synthesis method, preparing Co0. 2Cd0. 8S-Vs with sulfur vacancies through NaOH etching, preparing a ZnCo2O4 / Co0. 2Cd0. 8S-Vs composite catalyst rich in sulfur vacancies through a simple impregnation method by taking cobalt zinc oxide as a cocatalyst, and carrying out piezoelectric photocatalytic production of H2 or pressure point photocatalytic production of H2O2 under the synergistic effect of sunlight irradiation and ultrasonic vibration. The synthesis method is simple, green, pollution-free and simple and convenient to operate. The prepared catalyst has the characteristics of rich active sites, excellent stability, no secondary pollution and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of piezoelectric photocatalysts, and specifically relates to a ZnCo2O4 rich in sulfur vacancies.

[0002] / Co 0.2 Cd 0.8 S-Vs composite catalyst and its application. Background Art

[0003] Hydrogen energy is a green energy with zero pollution and high calorific value. The concept of using solar energy to decompose water to produce hydrogen is considered by many researchers to be the ultimate solution to the future energy crisis of mankind. Semiconductor catalysts are an important part of the photocatalytic water decomposition process. To date, many photocatalytic materials, such as CdS, have been intensively studied as potential catalysts for H2 evolution.

[0004] For example, patent CN109876827A discloses a double Z-type single heterojunction CuO / WO3 / CdS photocatalyst and its preparation method and application. The prepared catalyst can inhibit the recombination of electrons and holes, and efficiently utilize sunlight to improve the catalytic activity of the photocatalyst. Patent CN117205945A discloses an α-NiS / CdS photocatalyst and its preparation method and application. It uses NiS to replace traditional precious metal catalysts, reduces production costs, and has higher catalytic activity and stability. However, the preparation methods of the above catalysts are relatively cumbersome, and the final hydrogen production efficiency of the obtained samples is not high. In addition, the photocorrosion of CdS is mainly due to the fact that after visible light irradiation, the lattice sparseness of the CdS surface is rapidly oxidized through the light-producing holes, resulting in serious damage to the CdS surface, thereby seriously reducing the activity of the CdS catalyst and the hydrogen production rate. Summary of the invention

[0005] The present invention aims to provide a ZnCo2O4 / Co 0.2 Cd 0.8 The S-Vs composite catalyst is applied to piezoelectric photocatalytic H2 production and photocatalytic H2O2 production, and has high catalytic activity and good stability.

[0006] The sulfur vacancy-rich ZnCo2O4 / Co 0.2 Cd 0.8 The S-Vs composite catalyst, the preparation method thereof comprises the following steps:

[0007] (1)Co 0.2 Cd 0.8 Preparation of S-Vs:

[0008] CoCl2·6H2O and Cd(CH3COO)2·2H2O were mixed in a molar ratio of 1:4 to 1:9, and C2H5NS was added and dissolved in distilled water, stirred for 1 hour, and then ethylenediamine was added and stirred for 1 hour to make it evenly mixed. Then the mixed solution was transferred to a reactor with a polytetrafluoroethylene liner and placed in an oven at 180°C for 12 hours. After the reaction was completed, it was cooled to room temperature, and the solid in the reactor was washed three times with deionized water and anhydrous ethanol, and dried at 60°C overnight to obtain yellow-green Co without vacancies. 0.2 Cd 0.8 S.

[0009] Then Co 0.2 Cd 0.8 S and NaOH are dispersed in aqueous solution and ultrasonicated to obtain enough bubbles to obtain Co 0.2 Cd 0.8 S-Vs provides conditions (ultrasonic time is preferably 20 min), after the reaction is completed, the solid is separated, washed and dried at room temperature to obtain Co 0.2 Cd 0.8 S-Vs.

[0010] Furthermore, the mass ratio of C2H5NS to CoCl2·6H2O is 0.119:0.381.

[0011] (2) Preparation of ZnCo2O4:

[0012] Disperse Co(CH3COO)2·4H2O and Zn(CH3COO)2·2H2O in distilled water and stir to mix, then add CH4N2O and NH4F and stir to mix thoroughly, then transfer the mixture to a reactor lined with polytetrafluoroethylene, place the reactor in an oven at 120°C for 6 hours, cool to room temperature after the reaction, wash the solid in the reactor with deionized water and anhydrous ethanol three times each, dry at 60°C overnight, and obtain a pink-purple ZnCo2O4 precursor. Finally, place the precursor in a tubular furnace, heat to 400°C at a rate of 5°C / min, and calcine for 2 hours to obtain black ZnCo2O4.

[0013] Furthermore, the mass ratio of Co(CH3COO)2·4H2O and Zn(CH3COO)2·2H2O is 0.22:0.498.

[0014] (3) ZnCo2O4 / Co 0.2 Cd 0.8 Preparation of S-Vs composite catalyst:

[0015] Co 0.2 Cd 0.8The S-Vs catalyst and ZnCo2O4 catalyst were dissolved in a solvent and stirred. Filtered, washed and dried at room temperature to obtain a yellow-green powder, namely ZnCo2O4 / Co 0.2 Cd 0.8 S-Vs composite catalyst.

[0016] Among them, the added mass of ZnCo2O4 is Co 0.2 Cd 0.8 The content of S-Vs is 1 to 7% by mass, preferably 3 to 5% by mass.

[0017] Solvents include deionized water and anhydrous ethanol.

[0018] The stirring speed is 400r / min and the time is 20h.

[0019] The composite catalyst prepared by the above method is used for piezoelectric photocatalytic hydrogen production or for photocatalytic H2O2 production.

[0020] The specific method of using the catalyst for piezoelectric photocatalytic hydrogen production is: ZnCo2O4 / Co 0.2 Cd 0.8 The S-Vs composite catalyst is uniformly dispersed in water, and then a sacrificial agent is added, N2 is passed, and H2 is produced in a sealed manner under the combined conditions of ultrasound and light.

[0021] Among them, the sacrificial agent is lactic acid, the ultrasonic power is 240W, and the light power is 55W.

[0022] ZnCo2O4 / Co 0.2 Cd 0.8 The dosage of S-Vs composite catalyst in water is 2 mg / 18 mL.

[0023] The specific method of using the catalyst for piezoelectric photocatalytic H2O2 production is as follows: ZnCo2O4 / Co 0.2 Cd 0.8 The S-Vs composite catalyst is added into distilled water, fully dispersed and then reacted under ultrasound and sunlight irradiation.

[0024] Among them, the ultrasonic power is 240W; the light power is 55W.

[0025] ZnCo2O4 / Co 0.2 Cd 0.8 The dosage of S-Vs composite catalyst in water is 5 mg / 10 mL.

[0026] The beneficial effects of the present invention are:

[0027] (1) The present invention synthesizes Co with appropriate Co doping amount and containing sulfur vacancies by hydrothermal method 0.2 Cd 0.8S-Vs was composited with ZnCo2O4 to form a heterojunction by impregnation to prepare ZnCo2O4 / Co 0.2 Cd 0.8 The S-Vs composite catalyst has simple synthesis conditions, is easy to operate, and has the characteristics of rapidity, high efficiency, energy saving and environmental protection.

[0028] (2) The introduction of the co-catalyst ZnCo2O4 did not change the 0.2 Cd 0.8 Crystal structure of S-Vs, ZnCo2O4 / Co 0.2 Cd 0.8 The S-Vs composite catalyst has high crystallinity and purity.

[0029] (3) ZnCo2O4 / Co 0.2 Cd 0.8 The S-Vs composite catalyst produces H2 or H2O2 under the synergistic effects of photocatalysis, piezocatalysis and piezoelectric light, among which the catalytic performance under the common conditions of piezoelectric light is the best, which is Co 0.2 Cd 0.8 It is 3.35 times that of S and 11.51 times that of CdS. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 The ZnCo2O4 / Co synthesized in Example 1 0.2 Cd 0.8 Scanning electron microscopy image of the S-Vs composite catalyst;

[0031] Figure 2 YesCo 0.2 Cd 0.8 S.Co 0.2 Cd 0.8 XRD patterns of S-Vs, ZnCo2O4 and CdS catalysts;

[0032] Figure 3 The ZnCo2O4 / Co synthesized in Example 1-4 0.2 Cd 0.8 XRD pattern of S-Vs composite catalyst;

[0033] Figure 4 It is the performance diagram of H2 production of different catalysts under piezoelectric illumination conditions;

[0034] Figure 5 It is the performance diagram of H2 production of different catalysts under piezoelectric action only;

[0035] Figure 6 This is a performance graph of different catalysts producing H2 under light alone.

[0036] Figure 7This is a performance diagram of the catalyst synthesized in Example 1-4 for producing H2O2 under piezoelectric illumination conditions;

[0037] Figure 8 This is the color change of the solution after CdS was exposed to light for two hours. It can be seen that it clearly changed from orange-red to yellow-green.

[0038] Fig. 9 For Co 0.2 Cd 0.8 The color of the solution after two hours of illumination showed almost no change.

[0039] Fig.10 3% ZnCo2O4 / Co 0.2 Cd 0.8 The color change of the solution after S-Vs illumination for two hours showed almost no change. DETAILED DESCRIPTION

[0040] The present invention is not limited to the following specific embodiments. A person skilled in the art can implement the present invention in various other specific embodiments according to the contents disclosed in the present invention, or any simple changes or modifications made to the design structure and ideas of the present invention fall within the protection scope of the present invention. It should be noted that the embodiments and features in the embodiments of the present invention can be combined with each other without conflict. The H2 production efficiency is calculated according to the following formula:

[0041]

[0042] R: H2 production rate, unit: μmol / (g·h), V: hydrogen volume, unit: μL, m: catalyst mass, unit: g, t: reaction time, unit: h.

[0043] The formula for calculating the H2O2 production rate is:

[0044] Y=0.004X+0.0041

[0045]

[0046] Y: measured absorbance value, R: H2O2 production rate, unit: μmol / (g·h), V: solvent volume, unit: L, m: catalyst mass, unit: g, t: reaction time, unit: h.

[0047] Example 1

[0048] (1) 0.119 g of CoCl2·6H2O and 0.533 g of Cd(CH3COO)2·2H2O were mixed, and 0.381 g of C2H5NS was added and dissolved in distilled water. The mixture was stirred for 1 h, and then 25 ml of ethylenediamine was added and stirred for 1 h to make it uniformly mixed. The mixture was then transferred to a reactor lined with polytetrafluoroethylene and placed in an oven at 180°C for 12 h. After the reaction was completed, the mixture was cooled to room temperature. The solid in the reactor was washed three times with deionized water and anhydrous ethanol, respectively, and dried at 60°C overnight to obtain a yellow-green Co 0.2 Cd 0.8 S.

[0049] The yellow-green Co 0.2 Cd 0.8 S catalyst for piezoelectric photocatalytic H2 production:

[0050] Weigh 2 mg Co 0.2 Cd 0.8 S catalyst and 18 mL of water were mixed and ultrasonically dispersed for 0.5 h, then 2 mL of sacrificial agent solution lactic acid was added, followed by 30 min of N2, and finally sealed for 2 h under ultrasound (240 W) and light (55 W xenon lamp simulated sunlight). After the experiment, 0.5 mL of gas in the tube was extracted, the peak area was detected by gas chromatograph, and the H2 production rate was calculated. The H2 production rate was 3.82 mmol / (g·h) after analysis and calculation.

[0051] The yellow-green Co 0.2 Cd 0.8 S catalyst for piezoelectric photocatalytic production of H2O2

[0052] 5 mg Co 0.2 Cd 0.8 S was mixed with 10 mL of distilled water and dispersed for 0.5 h under ultrasonic (240 W) and light (55 W xenon lamp simulated sunlight) conditions to make the catalyst evenly dispersed in the water. Then 500 μL of the upper clear liquid was taken and 2 mL of 0.1 mol / L potassium iodide solution and 50 μL of 0.01 mol / L ammonium molybdate solution were added thereto. After oscillation for 10 min, the absorbance was measured at 352 nm by an ultraviolet spectrophotometer to calculate the H2O2 production rate. The H2O2 production rate was calculated and analyzed to be 86.8 μmol / (g·h).

[0053] Then 0.2 g Co 0.2 Cd 0.8 S and 0.8 g NaOH were dispersed in aqueous solution and ultrasonicated for 20 min to obtain enough bubbles to obtain Co 0.2 Cd 0.8S-Vs provides the conditions, and after the reaction is completed, the solid is separated, washed and dried at room temperature to obtain Co 0.2 Cd 0.8 S-Vs.

[0054] The obtained Co 0.2 Cd 0.8 S-Vs catalysts are used in piezoelectric photocatalytic H2 production:

[0055] Weigh 2 mg Co 0.2 Cd 0.8 S-Vs catalyst and 18 mL of water were mixed and ultrasonically dispersed for 0.5 h, then 2 mL of sacrificial agent solution lactic acid was added, followed by 30 min of N2, and finally sealed for 2 h under ultrasound (240 W) and light (55 W xenon lamp simulated sunlight). After the experiment, 0.5 mL of gas in the tube was extracted, the peak area was detected by gas chromatograph, and the H2 production rate was calculated. The H2 production rate was 5.13 mmol / (g·h) after analysis and calculation.

[0056] (2) Disperse 0.498g Co(CH3COO)2·4H2O and 0.22g Zn(CH3COO)2·2H2O in 40ml distilled water and stir to mix, then add 0.36g CH4N2O and 0.074g NH4F and stir to mix thoroughly, then transfer the mixture to a reactor lined with polytetrafluoroethylene, place the reactor in an oven at 120℃ for 6h, cool to room temperature after the reaction, wash the solid in the reactor with deionized water and anhydrous ethanol three times each, dry at 60℃ overnight, and obtain a pink-purple ZnCo2O4 precursor. Finally, place the precursor in a tubular furnace, heat to 400℃ at a rate of 5℃ / min, and calcine for 2h to obtain black ZnCo2O4.

[0057] The prepared ZnCo2O4 catalyst was applied to piezoelectric photocatalytic H2 production:

[0058] 2mg ZnCo2O4 catalyst and 18mL water were mixed and ultrasonically dispersed for 0.5h. Then 2mL sacrificial agent was added, and the sacrificial agent solution was lactic acid. Then N2 was passed for 30min, and finally sealed for 2h under ultrasound (240W) and light (55W xenon lamp simulated sunlight). After the experiment was completed, 0.5mL of gas in the tube was extracted, and the peak area was detected by gas chromatograph to calculate the H2 production rate. The H2 production rate was calculated and analyzed to be 6.9μmol / (g·h).

[0059] (3) Co 0.2 Cd 0.8 S-Vs and ZnCo2O4 were dissolved in deionized water and stirred at a stirring speed of 400 r / min for 20 h; filtered, washed and dried at room temperature to finally obtain an orange powder, namely ZnCo2O4 / Co0.2 Cd 0.8 S-Vs composite catalyst, denoted as 3% ZnCo2O4 / Co 0.2 Cd 0.8 S-Vs. Among them, the mass of ZnCo2O4 is Co 0.2 Cd 0.8 3% of S-Vs mass.

[0060] The 3% ZnCo2O4 / Co prepared in Example 1 0.2 Cd 0.8 S-Vs for piezoelectric photocatalytic H2 production:

[0061] 2mg 3% ZnCo2O4 / Co 0.2 Cd 0.8 S-Vs was mixed with 18 mL of distilled water and ultrasonically dispersed for 0.5 h to make the catalyst evenly dispersed in the water. Then 2 mL of sacrificial agent was added, and the sacrificial agent solution was lactic acid. Then N2 was passed for 30 min, and finally sealed for 2 h under ultrasound (240 W) and light (55 W xenon lamp simulated sunlight). After the experiment was completed, 0.5 mL of gas in the tube was extracted, and the peak area was detected by gas chromatograph to calculate the H2 production rate. The H2 production rate was calculated to be 12.78 mmol / (g·h).

[0062] The 3% ZnCo2O4 / Co prepared in Example 1 0.2 Cd 0.8 S-Vs for piezoelectric photocatalytic H2O2 production:

[0063] 5mg 3% ZnCo2O4 / Co 0.2 Cd 0.8 S-Vs was mixed with 10 mL of distilled water and dispersed for 0.5 h under ultrasound (240 W) and light (55 W xenon lamp simulated sunlight) conditions to make the catalyst evenly dispersed in the water. Then 500 μL of the upper clear liquid was taken and 2 mL of 0.1 mol / L potassium iodide solution and 50 μL of 0.01 mol / L ammonium molybdate solution were added thereto. After oscillation for 10 min, the absorbance was measured at 352 nm by an ultraviolet spectrophotometer, and the H2O2 production rate was calculated. The H2O2 production rate was calculated and analyzed to be 542.92 μmol / (g·h).

[0064] Example 2

[0065] Compared with Example 1, the difference is that in step (3), the mass of ZnCo2O4 added is Co 0.2 Cd 0.8 The weight of S-Vs was 1%, and the others were the same as in Example 1. The composite catalyst prepared was recorded as 1% ZnCo2O4 / Co 0.2 Cd 0.8S-Vs.

[0066] The 1% ZnCo2O4 / Co prepared in Example 2 0.2 Cd 0.8 S-Vs was applied to piezoelectric photocatalytic H2 production in the same manner as in Example 1, and its H2 production rate was 5.78 mmol / (g·h).

[0067] The 1% ZnCo2O4 / Co prepared in Example 2 0.2 Cd 0.8 S-Vs was applied to piezoelectric photocatalysis to produce H2O2, and the application method was the same as in Example 1. The H2O2 production rate was 103.8 μmol / (g·h).

[0068] Example 3

[0069] Compared with Example 1, the difference is that in step (3), the mass of ZnCo2O4 added is Co 0.2 Cd 0.8 The weight of S-Vs was 5%, and the others were the same as in Example 1. The composite catalyst prepared was recorded as 5% ZnCo2O4 / Co 0.2 Cd 0.8 S-Vs.

[0070] The 5% ZnCo2O4 / Co prepared in Example 3 0.2 Cd 0.8 S-Vs was applied to piezoelectric photocatalytic H2 production in the same manner as in Example 1, and the H2 production rate was 10.42 mmol / (g·h).

[0071] The 5% ZnCo2O4 / Co prepared in Example 3 0.2 Cd 0.8 S-Vs was applied to piezoelectric photocatalysis to produce H2O2. The application method was the same as in Example 1. The H2O2 production rate was 337.57 μmol / (g·h).

[0072] Example 4

[0073] Compared with Example 1, the difference is that in step (3), the mass of ZnCo2O4 added is Co 0.2 Cd 0.8 The weight of S-Vs was 7%, and the others were the same as in Example 1. The composite catalyst obtained was recorded as 7% ZnCo2O4 / Co 0.2 Cd 0.8 S-Vs.

[0074] The 7% ZnCo2O4 / Co prepared in Example 4 0.2 Cd 0.8S-Vs was applied to piezoelectric photocatalytic H2 production in the same manner as in Example 1, and the H2 production rate was 8.39 mmol / (g·h).

[0075] The 7% ZnCo2O4 / Co prepared in Example 4 0.2 Cd 0.8 S-Vs was applied to piezoelectric photocatalysis to produce H2O2. The application method was the same as in Example 1. The H2O2 production rate was 309.2 μmol / (g·h).

[0076] Example 5

[0077] Compared with Example 1, the difference is that in step (3), Co 0.2 Cd 0.8 S-Vs and ZnCo2O4 were dissolved in anhydrous ethanol, and the rest was the same as in Example 1.

[0078] The 3% ZnCo2O4 / Co prepared in Example 5 0.2 Cd 0.8 S-Vs was applied to piezoelectric photocatalytic H2 production in the same manner as in Example 1, and the H2 production rate was 6.19 mmol( / g·h).

[0079] Example 6

[0080] Compared with Example 1, the difference is that in step (1), the added amounts of CoCl2·6H2O and Cd(CH3COO)2·2H2O are 0.0595 g and 0.5996 g, respectively, and the rest are the same as Example 1.

[0081] The 3% ZnCo2O4 / Co prepared in Example 6 0.1 Cd 0.9 S-Vs was applied to piezoelectric photocatalytic H2 production in the same manner as in Example 1, with a H2 production rate of 1.45 mmol ( / g·h).

[0082] Example 7

[0083] Compared with Example 1, the difference is that in step (1), the added amounts of CoCl2·6H2O and Cd(CH3COO)2·2H2O are 0.1785 g and 0.4664 g, respectively, and the rest are the same as Example 1.

[0084] The 3% ZnCo2O4 / Co prepared in Example 6 0.3 Cd 0.7 S-Vs was applied to piezoelectric photocatalytic H2 production in the same manner as in Example 1, and the H2 production rate was 7.81 mmol ( / g·h).

[0085] Example 8

[0086] Compared with Example 1, the difference is that in step (1), the added amounts of CoCl2·6H2O and Cd(CH3COO)2·2H2O are 0.238 g and 0.402 g, respectively, and the rest are the same as Example 1.

[0087] The 3% ZnCo2O4 / Co prepared in Example 6 0.4 Cd 0.6 S-Vs was applied to piezoelectric photocatalytic H2 production in the same manner as in Example 1, and the H2 production rate was 3.4 mmol / (g·h).

[0088] Comparative Example 1

[0089] Compared with Example 1, the difference is that the application method is changed from ultrasound (240W) and light (55W xenon lamp simulated sunlight) to ultrasound (240W), and the rest is the same as Example 1. 3% ZnCo2O4

[0090] / Co 0.2 Cd 0.8 The H2 production rate of S-Vs catalyst is 408.48 μmol / (g·h).

[0091] Compared with Example 1, the difference is that the application method is changed from ultrasound (240W) and light (55W xenon lamp simulated sunlight) to light only (55W xenon lamp simulated sunlight), and the rest is the same as Example 1. 3% ZnCo2O4 / Co 0.2 Cd 0.8 The H2 production rate of S-Vs catalyst is 1.79mmol / (g·h).

[0092] Comparative Example 2

[0093] After 0.119g CoCl2·6H2O and 0.533g Cd(CH3COO)2·2H2O were mixed, 0.381g C2H5NS was added and dissolved in distilled water, stirred for 1h, and then 25ml ethylenediamine was added and stirred for 1h to make it evenly mixed. Then the mixture was transferred to a reactor with a polytetrafluoroethylene liner and placed in an oven at 180°C for 12h. After the reaction was completed, it was cooled to room temperature, and the solid in the reactor was washed three times with deionized water and anhydrous ethanol respectively, and dried at 60°C overnight to obtain yellow-green Co without vacancies. 0.2 Cd 0.8 S.

[0094] Disperse 0.498g Co(CH3COO)2·4H2O and 0.22g Zn(CH3COO)2·2H2O in 40ml distilled water and stir to mix, then add 0.36g CH4N2O and 0.074g NH4F and stir to mix thoroughly, then transfer the mixture to a reactor lined with polytetrafluoroethylene, place the reactor in an oven at 120°C for 6h, cool to room temperature after the reaction, wash the solid in the reactor with deionized water and anhydrous ethanol three times each, dry at 60°C overnight, and obtain a pink-purple ZnCo2O4 precursor. Finally, place the precursor in a tubular furnace, heat to 400°C at a rate of 5°C / min, and calcine for 2h to obtain black ZnCo2O4.

[0095] Co 0.2 Cd 0.8 S and ZnCo2O4 were dissolved in deionized water and stirred at a stirring speed of 400 r / min for 20 h; filtered, washed and dried at room temperature to finally obtain an orange powder, namely ZnCo2O4 / Co 0.2 Cd 0.8 S-Vs composite catalyst, denoted as 3% ZnCo2O4 / Co 0.2 Cd 0.8 S. Among them, the mass of ZnCo2O4 is Co 0.2 Cd 0.8 3% of S mass.

[0096] The 3% ZnCo2O4 / Co prepared in Comparative Example 2 0.2 Cd 0.8 S catalyst is used in piezoelectric photocatalytic H2 production:

[0097] 2mg 3% ZnCo2O4 / Co 0.2 Cd 0.8 S was mixed with 18 mL of distilled water and ultrasonically dispersed for 0.5 h to make the catalyst evenly dispersed in the water, and then 2 mL of sacrificial agent was added. The sacrificial agent solution was lactic acid, and then N2 was passed for 30 min. Finally, it was sealed for 2 h under ultrasonic (240 W) and light (55 W xenon lamp simulated sunlight). After the experiment was completed, 0.5 mL of gas in the tube was extracted, and the peak area was detected by gas chromatograph to calculate the H2 production rate. The H2 production rate was calculated to be 6.59 mmol / (g·h).

[0098] Comparative Example 3

[0099] After mixing 0.119g CoCl2·6H2O and 0.533g Cd(CH3COO)2·2H2O, 0.381g C2H5NS was added and dissolved in distilled water, stirred for 1h, and then 25ml ethylenediamine was added and stirred for 1h to make it evenly mixed. Then the mixture was transferred to a reactor with a polytetrafluoroethylene liner and placed in an oven at 180°C for 12h. After the reaction was completed, it was cooled to room temperature, and the solid in the reactor was washed three times with deionized water and anhydrous ethanol respectively, and kept at 60°C overnight to obtain a yellow-green Co without vacancies. 0.2 Cd 0.8 S. Then 0.2g Co 0.2 Cd 0.8 S and 0.8 g NaOH were dispersed in aqueous solution and ultrasonicated for 20 min to obtain enough bubbles to obtain Co 0.2 Cd 0.8 S-Vs provides the conditions, and after the reaction is completed, the solid is separated, washed and dried at room temperature to obtain Co 0.2 Cd 0.8 S-Vs.

[0100] 0.631 g Bi(NO3)3·5H2O and 0.157 g Na2MoO4 were dispersed in 60 ml distilled water and stirred thoroughly. The mixture was then transferred to a polytetrafluoroethylene-lined reactor. The reactor was placed in an oven at 160°C for 14 h. After the reaction was completed, it was cooled to room temperature. The solid in the reactor was washed three times with deionized water and anhydrous ethanol respectively, and dried at 60°C overnight to obtain yellow Bi2MoO6.

[0101] Co 0.2 Cd 0.8 S-Vs and Bi2MoO6 were dissolved in deionized water and stirred at a stirring speed of 400 r / min for 20 h; filtered, washed and dried at room temperature to finally obtain an orange powder, namely Bi2MoO6 / Co 0.2 Cd 0.8 S-Vs composite catalyst, denoted as 3% Bi2MoO6 / Co 0.2 Cd 0.8 S-Vs. Among them, the mass of Bi2MoO6 is Co 0.2 Cd 0.8 3% of S-Vs mass.

[0102] The 3% Bi2MoO6 / Co 0.2 Cd 0.8 -Vs catalysts for piezoelectric photocatalytic H2 production:

[0103] 2mg 3% Bi2MoO6 / Co 0.2 Cd 0.8-Vs was mixed with 18mL of distilled water and ultrasonically dispersed for 0.5h to make the catalyst evenly dispersed in the water, and then 2mL of sacrificial agent was added. The sacrificial agent solution was lactic acid, and then N2 was passed for 30min. Finally, it was sealed for 2h under ultrasonic (240W) and light (55W xenon lamp simulated sunlight). After the experiment was completed, 0.5mL of gas in the tube was extracted, and the peak area was detected by gas chromatograph to calculate the H2 production rate. The H2 production rate was calculated to be 5.18mmol / (g·h).

[0104] The 3% Bi2MoO6 / Co 0.2 Cd 0.8 -Vs catalyst for piezoelectric photocatalytic H2O2 production:

[0105] 5mg 3% Bi2MoO6 / Co 0.2 Cd 0.8 -Vs was mixed with 10 mL of distilled water and dispersed for 0.5 h under ultrasound (240 W) and light (55 W xenon lamp simulated sunlight) conditions to make the catalyst evenly dispersed in the water. Then 500 μL of the upper clear liquid was taken and 2 mL of 0.1 mol / L potassium iodide solution and 50 μL of 0.01 mol / L ammonium molybdate solution were added thereto. After oscillation for 10 min, the absorbance was measured at 352 nm by an ultraviolet spectrophotometer to calculate the H2O2 production rate. The H2O2 production rate was calculated and analyzed to be 97.08 μmol / (g·h).

[0106] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A sulfur-vacancy-rich ZnCo2O4 / Co 0.2 Cd 0.8 The S-Vs composite catalyst is characterized by: The catalyst is composed of Co 0.2 Cd 0.8 S-Vs and ZnCo2O4 form a heterojunction structure, in which ZnCo2O4 is Co 0.2 Cd 0.8 S-Vs 1-7% of mass.

2. The sulfur vacancy-rich ZnCo2O4 / Co according to claim 1 0.2 Cd 0.8 The S-Vs composite catalyst is characterized by: The preparation method of ZnCo2O4 is as follows: Co(CH3COO)2·4H2O and Zn(CH3COO)2·2H2O are stirred and mixed in distilled water, CH4N2O and NH4F are added and stirred and mixed thoroughly, and then the mixed solution is transferred to a reactor, placed in an oven at 120°C for 6 hours, cooled to room temperature after the reaction is completed, and the solid in the reactor is washed three times with deionized water and anhydrous ethanol respectively, and dried at 60°C overnight to obtain a pink-purple ZnCo2O4 precursor; finally, the precursor is placed in a tubular furnace for calcination to obtain black ZnCo2O4.

3. The sulfur vacancy-rich ZnCo2O4 / Co according to claim 2 0.2 Cd 0.8 The S-Vs composite catalyst is characterized by: The mass ratio of Co(CH3COO)2·4H2O to Zn(CH3COO)2·2H2O is 0.22:0.

498. In a tube furnace, the precursor is heated to 400°C at a rate of 5°C / min and calcined for 2h.

4. The sulfur vacancy-rich ZnCo2O4 / Co according to claim 1 0.2 Cd 0.8 The S-Vs composite catalyst is characterized by: The Co 0.2 Cd 0.8 The preparation method of S-Vs is as follows: after mixing CoCl2·6H2O and Cd(CH3COO)2·2H2O, C2H5NS is added and dissolved in distilled water, stirred for 1 hour, and then ethylenediamine is added and stirred for 1 hour to make it evenly mixed, and then the mixed solution is transferred to a reactor and placed in an oven at 180°C for 12 hours. After the reaction is completed, it is cooled to room temperature, and the solid in the reactor is washed three times with deionized water and anhydrous ethanol respectively, and dried at 60°C overnight to obtain yellow-green Co without vacancies. 0.2 Cd 0.8 S; then Co 0.2 Cd 0.8 S and NaOH were dispersed in aqueous solution, and sufficient bubbles were obtained by ultrasound. After the reaction was completed, the solid was separated, washed and dried at room temperature to obtain Co 0.2 Cd 0.8 S~Vs.

5. The sulfur vacancy-rich ZnCo2O4 / Co according to claim 4 0.2 Cd 0.8 The S-Vs composite catalyst is characterized by: The mass ratio of C2H5NS to CoCl2·6H2O is 0.119:0.381; the molar ratio of CoCl2·6H2O to Cd(CH3COO)2·2H2O is 1:4-1:

9.

6. A ZnCo2O4 / Co rich in sulfur vacancies according to claim 1 0.2 Cd 0.8 The preparation method of the S-Vs composite catalyst is characterized in that: The preparation method of the composite catalyst is: 0.2 Cd 0.8 S-Vs and ZnCo2O4 are dissolved in a solvent in proportion, stirred for 20 to 24 hours, filtered, washed and dried to obtain ZnCo2O4 / Co 0.2 Cd 0.8 S-Vs composite catalyst.

7. A sulfur vacancy-rich ZnCo2O4 / Co according to claim 1 0.2 Cd 0.8 The application of S-Vs composite catalyst is characterized by: The sulfur vacancy-rich ZnCo2O4 / Co 0.2 Cd 0.8 The S-Vs composite catalyst is used for photocatalytic hydrogen production or photocatalytic H2O2 production.

8. The sulfur vacancy-rich ZnCo2O4 / Co according to claim 7 0.2 Cd 0.8 The application of S-Vs composite catalyst is characterized by: The method for using the catalyst for photocatalytic hydrogen production is: ZnCo2O4 / Co 0.2 Cd 0.8 The S-Vs composite catalyst was added into distilled water, and then lactic acid was added after being fully dispersed, and then N2 was passed through, and finally a closed reaction was carried out under ultrasound and sunlight irradiation.

9. The sulfur vacancy-rich ZnCo2O4 / Co according to claim 7 0.2 Cd 0.8 The application of S-Vs composite catalyst is characterized by: The method for using the catalyst to produce H2O2 by photocatalysis is as follows: ZnCo2O4 / Co 0.2 Cd 0.8 The S-Vs composite catalyst is added into distilled water, fully dispersed and then reacted under ultrasound and sunlight irradiation.

Citation Information

Patent Citations

  • MCS / ZCO composite photocatalyst for photocatalytic hydrogen production and preparation method of MCS / ZCO composite photocatalyst

    CN114749189A

  • Preparation and application of CdS-Vs / Co2RuS6 composite catalyst rich in sulfur vacancy

    CN116371425A

  • Preparation method of Co0. 2Cd0. 8S / CaTiO3 / NiSx material and application thereof in photocatalytic nitrogen fixation