Composite material for improving mechanical properties of hexagonal system MnNiGe and MnCoGe-based alloy, and preparation method and application thereof
The MnNiGe and MnCoGe-based alloys are bonded to low-melting metals by hot pressing or discharge plasma sintering, solving the problems of alloy fragility and reduced thermal conductivity, and achieving high mechanical properties and multifunctional properties of Mn(Ni,Co) Ge alloy composite materials are suitable for magnetostrictive and other fields, and are inexpensive.
Patent Information
- Application Number
- CN202410990967.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
Mn(Ni,Co)Ge alloys are brittle due to huge negative expansion and stress during structural phase transition, which limits the acquisition of large samples and further research and application of their physical effects. The existing enhancement methods reduce thermal conductivity and electrical conductivity. Rate and costly.
The MnNiGe and MnCoGe-based alloy powder are bonded to the low-melting metal by hot pressing or discharge plasma sintering method. The mass ratio is (1-4): 1, the temperature is 80-400℃, the pressure is stronger than 50MPa, and the hot pressing time is 3-30 Minutes, maintain the phase change and physical effects of the alloy while improving the mechanical properties.
Mn(Ni,Co)Ge alloy composite material with smooth and dense surface, high cycle stability and multifunctional properties is obtained. It is used in magnetostrictive, magnetic drive, solid state refrigeration and other fields, overcomes the fragility of alloys and maintains high thermal conductivity. and conductivity, and low production cost.
Smart Images

Figure CN118926529A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of composite materials for greatly improving the mechanical properties of hexagonal MnNiGe and MnCoGe based alloys, and more specifically to a composite material for improving the mechanical properties of hexagonal MnNiGe and MnCoGe based alloys, a preparation method and an application thereof. Background Art
[0002] Mn(Ni,Co)Ge alloy undergoes structural transformation from high-temperature austenite to low-temperature martensite, and the magnetic states of the austenite phase and martensite phase are different before and after the phase transformation. The magnetic properties and structures of the two phases of the primary magnetic phase change alloy are quite different before and after the phase transformation, which is often accompanied by physical effects such as magnetocaloric effect, magneto-induced strain, negative thermal expansion, and shape memory. Therefore, Mn(Ni,Co)Ge alloy has broad application prospects in the fields of magnetic refrigeration, sensors, precision control, etc.
[0003] However, during the structural phase transition process, the volume of the Mn(Ni,Co)Ge alloy has huge negative expansion and huge stress, which makes the prepared samples fragile and it is impossible to obtain large samples for testing, thus limiting the further research and application of the rich physical effects of the alloy.
[0004] In order to reduce the probability of breakage of samples made from Mn(Ni,Co)Ge alloy, it is necessary to improve the mechanical strength of the samples made from Mn(Ni,Co)Ge alloy. There are many ways to improve the mechanical properties, such as strong magnetic field solidification, epoxy resin bonding, strong plastic and ductile metal bonding, etc. However, strong magnetic field solidification, epoxy resin bonding, and strong plastic and ductile metal bonding all have their own defects, which will not only reduce the thermal conductivity and electrical conductivity of Mn(Ni,Co)Ge brittle alloy, but also increase the preparation cost. Therefore, in order to promote further research and application of Mn(Ni,Co)Ge brittle alloy, it is urgently necessary to study a preparation method that maintains high thermal conductivity and electrical conductivity of the alloy, improves mechanical strength and reduces cost. Summary of the invention
[0005] In view of the deficiencies of the above-mentioned prior art, the purpose of the present invention is to provide a composite material, preparation method and application for improving the mechanical properties of hexagonal MnNiGe and MnCoGe based alloys. The composite material is prepared by hot pressing of a low melting point metal / alloy bonded by hot pressing or discharge plasma sintering, which solves the problem that the Mn(Ni,Co)Ge alloy is fragile and difficult to obtain a bulk sample. The composite material still maintains phase change, retains a rich physical effect, and greatly improves the mechanical properties, and is used in the fields of magnetostriction, magnetic drive, solid-state refrigeration devices, etc. In addition, the preparation method also has the characteristics of low preparation cost and simple preparation.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0007] The first object of the present invention is to provide a preparation method for improving the mechanical properties of hexagonal MnNiGe and MnCoGe based alloys, which comprises hot pressing MnNiGe and MnCoGe based alloy powders with low melting point metals or performing spark plasma sintering on MnNiGe and MnCoGe based alloy powders with low melting point metals, wherein the mass ratio of MnNiGe and MnCoGe based alloy powders to low melting point metals is (1 to 4):1.
[0008] Preferably, the low melting point metal is any one of pure metals Ga, In, Sn, or alloys containing Ga, In, Sn.
[0009] Preferably, in the hot pressing or spark plasma sintering preparation process, the temperature is 80-400° C., the pressure is greater than 50 MPa, and the hot pressing or sintering time is 3-30 minutes.
[0010] Preferably, the chemical formula of the MnNiGe and MnCoGe based alloys is: 1-x Fe x NiGe and Mn 1-y Co 1+y Ge; wherein, 0≤x≤0.24, 0≤y≤0.09, and x and y represent the atomic ratio content.
[0011] Preferably, the preparation method of the hexagonal MnNiGe and MnCoGe based alloys comprises the following steps:
[0012] Step 1: Calculate the required mass of Mn, Ni, Co, Fe and Ge elements according to the stoichiometric ratio and prepare the ingredients;
[0013] The raw materials prepared above were placed in a water-cooled copper crucible arc furnace, and the vacuum degree in the furnace was drawn to 5×10 -3 Pa, and then the vacuum degree was reduced to 5×10 -3 Pa, fill with argon gas with a purity of 99.999% at 0.8 atmospheres, and perform arc melting for 4 to 5 times at a current of 40A to obtain a bulk ingot, or further take part of the ingot and prepare it by melt rapid quenching method;
[0014] The block ingot or alloy strip prepared as described above is sealed in a vacuum quartz tube, heat treated in a high temperature furnace to obtain an alloy block or strip, and the block or alloy strip is ground into powder using an agate mortar.
[0015] Preferably, the mass of the prepared Mn, Ni, Co, Fe, Ge elemental single substances in step 1 needs to be accurate to two decimal places in milligrams, and the purity of the single substances needs to be controlled to be above 99.99%.
[0016] Preferably, when the bulk ingot or alloy strip in step 3 is Mn 1-y Co 1+y When Ge alloy is used, Mn 1-y Co 1+y The heat treatment process of Ge alloy is: annealing temperature 500℃~900℃, treatment time 96~168h, and rapid cooling in water after treatment.
[0017] Preferably, when the bulk ingot or alloy strip in step 3 is Mn 1-x Fe x In NiGe alloy, Mn 1-x Fe x The heat treatment process of NiGe alloy is as follows: the primary annealing temperature is 600-850°C and the treatment time is 96-168h; then it is taken out and quickly put into cold water for quenching, and after quenching, it is sent to the same high-temperature furnace for secondary annealing again. The secondary annealing temperature is 300-1200°C, the treatment time is 0-120h, and it is cooled with the furnace.
[0018] The second object of the present invention is to provide a MnNiGe and MnCoGe based alloy composite material obtained by a preparation method for improving the mechanical properties of hexagonal MnNiGe and MnCoGe based alloys.
[0019] The third object of the present invention is to provide a MnNiGe and MnCoGe based alloy composite material for use in magnetostriction, magnetic drive and solid-state refrigeration devices.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] 1. The Mn(Ni, Co)Ge alloy composite material provided by the present invention has a smooth and dense surface, high cycle stability, high corrosion resistance, and still retains the phase change of the Mn(Ni, Co)Ge alloy.
[0022] 2. The method for improving the mechanical properties of hexagonal MnNiGe and MnCoGe based alloys provided by the present invention has the characteristics of low cost and simple preparation.
[0023] 3. The Mn(Ni,Co)Ge alloy composite material provided by the present invention has multifunctional properties near the phase transition, including giant magnetocaloric effect, negative thermal expansion, magneto-induced strain, etc., and can be widely used in solid-state refrigeration devices, magnetic drives, magnetic / thermal sensitive elements, thermomagnetic-electric conversion and other fields.
[0024] 4. The Mn(Ni,Co)Ge alloy composite material provided by the present invention is a MnNiGe and MnCoGe based alloy composite material prepared by hot pressing or spark plasma sintering of MnNiGe and MnCoGe based alloy powders with low melting point metals, which overcomes the problems that the volume of MnNiGe and MnCoGe based alloys changes greatly before and after the martensitic phase transformation, resulting in large internal stress, the prepared alloy samples are fragile, and the thermal conductivity, electrical conductivity and mechanical strength of the broken alloy particles are not high. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The composite material Mn provided in Example 1 of the present invention 0.84 Fe 0.16 Morphology of NiGe / Sn and precursor alloys;
[0026] Figure 2 The composite material Mn of the alloy provided in Example 1 of the present invention 0.84 F e0.16 XRD patterns of NiGe / Sn and precursor alloys;
[0027] Figure 3 The composite material sample Mn provided in Example 2 of the present invention 0.975 Co 1.035 Elemental mapping of Ge / Sn;
[0028] Figure 4 The composite material sample Mn provided in Example 2 of the present invention 0.975 Co 1.035 Ge / Sn and Precursor Mn 0.975 Co 1.035 Thermomagnetic curve of Ge;
[0029] Figure 5 The composite material Mn provided in Example 4 of the present invention 0.84 Fe 0.16 Isothermal magnetization curves of NiGe / Sn and precursor alloys;
[0030] Figure 6 The composite material Mn provided in Example 4 of the present invention 0.84 Fe 0.16 Negative thermal expansion curves of NiGe / Sn and precursor alloys. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention is described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] It should be noted that when the present invention involves a numerical range, it should be understood that the two endpoints of each numerical range and any value between the two endpoints can be selected. Since the steps and methods used are the same as those in Examples 1-5, in order to avoid redundancy, the present invention describes a preferred embodiment, but the present invention is not limited thereto, but can also be specifically implemented in other ways within the scope of the technical solution defined in the attached claims. According to the composition Mn 1-x Fe x NiGe and Mn 1-y Co 1+ y Ge can be used to make corresponding composite materials to improve the mechanical properties of hexagonal MnNiGe and MnCoGe based alloys.
[0033] The invention discloses a preparation method for improving the mechanical properties of hexagonal MnNiGe and MnCoGe based alloys, which comprises hot pressing MnNiGe and MnCoGe based alloy powders with low melting point metals or spark plasma sintering MnNiGe and MnCoGe based alloy powders with low melting point metals, wherein the mass ratio of MnNiGe and MnCoGe based alloy powders to low melting point metals is (1 to 4):1. 1-x Fe x NiGe and Mn 1-y Co 1+y In Ge alloys, the mechanical properties of the alloy are improved by bonding with low-melting-point metals / alloys through hot pressing or spark plasma sintering to obtain a composite material with excellent comprehensive properties.
[0034] Among them, the chemical formula of MnNiGe and MnCoGe based alloys is: Mn 1-x Fe x NiGe and Mn 1-y Co 1+y Ge, Mn 1-x Fe x NiGe with low melting point metals and Mn 1-y Co 1+y Ge is combined with low melting point metals to make corresponding composite materials to improve the mechanical properties of hexagonal MnNiGe and MnCoGe based alloys.
[0035] Based on the above principle, the actual alloy chemical formula is Mn 1-x Fe x NiGe and Mn 1-y Co 1+y Ge; wherein 0≤x≤0.24, 0≤y≤0.09, and x / y represents the atomic percentage content. The process for preparing the composite material is hot pressing or spark plasma sintering with a low melting point metal / alloy. In the hot pressing or spark plasma sintering preparation process: the hot pressing or spark plasma sintering temperature is 80-400°C, the pressure is greater than 50MPa, and the hot pressing or sintering time is 3-30 minutes.
[0036] The technical solution of the present invention is further illustrated below in the form of specific examples.
[0037] Example 1
[0038] To satisfy the alloy's chemical formula Mn 1-x Fe x NiGe, x is 0.16.
[0039] This embodiment is a Mn(Ni,Co)Ge composite material with good mechanical properties. The required mass of Mn, Fe, Ni, Co, and Ge elements is calculated according to the stoichiometric ratio and the purity of the metal elements is above 99.95%. The prepared raw materials are placed in a water-cooled copper crucible arc melting furnace and the vacuum is drawn to 5×10 -3 Pa, fill with 0.8 atmospheres of argon gas with a purity of 99.999%, and perform arc melting. Use a small current to melt the element into a uniform ingot.
[0040] The ingot is sealed in a vacuum quartz tube, and then the sealed sample is placed in a high-temperature furnace for annealing heat treatment at 850°C for 120 hours. The sample is then taken out and quickly quenched in cold water. The quenched sample is placed in the same high-temperature furnace and annealed for the second time at 500°C for 10 hours. After cooling in the furnace, a bulk sample with good imaging and uniformity is obtained, which is the precursor alloy.
[0041] The bulk sample was ground into fine particles using an agate mortar under vacuum, and alloy particles with a particle size of less than 30 μm were sieved out using a sieve. Commercial Sn powder and alloy powder particles were mixed evenly in a mass ratio of 1:1 and then loaded into a hot-pressed cemented carbide mold. During hot-pressing sintering, the vacuum degree should be drawn to 7×10 -3 Pa, the heating rate is 25℃ / min, the hot pressing temperature is 280℃, the pressure is set to 100MPa, the hot pressing is 5min, and the pressure is maintained until the sample is cooled to room temperature to obtain a composite material.
[0042] Composite Material Mn0.84 Fe 0.16 The morphology of NiGe / Sn and precursor alloys is shown in the attached figure. Figure 1 The XRD patterns of the composite material and the precursor alloy are shown in the attached Figure 2 As shown. Figure 1 It can be seen that Mn 0.84 Fe 0.16 The mechanical properties of NiGe / Sn composite materials are greatly improved compared to the precursor alloy samples. This is because the low melting point metal Sn plays a good bonding role, allowing the sample to maintain a good bulk shape. Figure 2 In addition to being able to observe Mn 0.84 Fe 0.16 NiGe alloys, Sn were also observed.
[0043] Example 2
[0044] The chemical formula of the alloy is Mn 1-y Co 1+y Ge, y is 0.035.
[0045] This embodiment is a Mn(Ni,Co)Ge composite material with good mechanical properties. The specific preparation method of the bulk alloy is almost the same as the preparation process of Example 1, except that after the sample is smelted, it is annealed at 850°C in the same high-temperature furnace for 120 hours and quenched in water. A bulk sample with good phase formation and uniformity is obtained, and a temperature-induced magnetic-structural coupling phase transition and a magnetic field-induced variable magnetic martensitic phase transition are obtained.
[0046] The bulk sample was ground into fine particles using an agate mortar under vacuum, and alloy particles with a particle size of less than 30 μm were sieved out using a sieve. Commercial Sn powder and alloy powder particles were mixed evenly in a mass ratio of 1:1 and then loaded into a hot pressing cemented carbide mold. The hot pressing sintering conditions were a hot pressing temperature of 280°C, a pressure set to 100 MPa, hot pressing for 5 minutes, and the pressure was maintained until the sample cooled to room temperature, thus obtaining a composite material.
[0047] Example 2 The composite material sample Mn prepared 0.975 Co 1.035 The element mapping diagram of Ge / Sn is shown in the attached figure. Figure 3 As shown. Composite material sample Mn 0.975 Co 1.035 Ge / Sn and Precursor Mn 0.975 Co 1.035 The thermomagnetic curve of Ge is shown in the attached figure. Figure 4 As shown, it was found that the composite material still maintained the first-order martensitic phase transformation.
[0048] Example 3
[0049] The chemical formula of the alloy is Mn 1-y Co 1+y Ge, y is 0.02.
[0050] This embodiment is a Mn(Ni,Co)Ge composite material with good mechanical properties. The specific preparation method of the bulk alloy is almost the same as the preparation process of Example 2, except that the composition of the precursor is Mn 0.98 Co 0.02 Ge was hot-pressed with low-melting-point metal Sn to prepare a composite material, which also achieved good results. The microstructure was uniform, the mechanical properties of the alloy were improved, and a first-order martensitic phase transformation was obtained.
[0051] Example 4
[0052] The chemical formula of the alloy is Mn 1-x Fe x NiGe, x is 0.16.
[0053] This embodiment is a Mn(Ni,Co)Ge composite material with good mechanical properties. The specific preparation method of the bulk alloy is almost the same as the preparation process of Example 1, except that the precursor alloy is ground with an agate mortar and then mixed with commercial Sn powder at a mass ratio of 2:1. The hot pressing sintering conditions are a hot pressing temperature of 280°C, a pressure set to 100MPa, hot pressing for 5min, and the pressure is maintained until the sample cools to room temperature, thereby obtaining a composite material.
[0054] Composite Material Mn 0.84 Fe 0.16 The isothermal magnetization curves of NiGe / Sn and precursor alloys are shown in the attached figure. Figure 5 As shown in FIG. 1 , it can be seen that after the material prepared in Example 4 is compounded, the alloy still maintains the first-order phase transition property, but the magnetic hysteresis is greatly reduced, which is more conducive to practical application. The negative thermal expansion curves of the composite material and the precursor alloy are shown in FIG. Figure 6 As shown, an excellent negative thermal expansion performance with a large expansion coefficient and a wide temperature range is obtained.
[0055] Example 5 The general chemical formula of the alloy is Mn 1-x Fe x NiGe, x is 0.16.
[0056] This embodiment is a Mn(Ni,Co)Ge composite material with good mechanical properties. The specific preparation method of the bulk alloy is almost the same as the preparation process of Example 1, except that the precursor alloy is ground with an agate mortar and then mixed with commercial In powder at a mass ratio of 2:1. The conditions of spark plasma sintering are sintering temperature of 200°C, pressure set to 50MPa, hot pressing for 5min, and the pressure is maintained until the sample cools to room temperature, thereby obtaining a composite material.
[0057] The composite material still maintains the primary martensitic phase transformation properties and obtains excellent mechanical properties and magnetic properties.
[0058] Any of the methods for significantly improving the mechanical properties of hexagonal MnNiGe and MnCoGe based alloys in Examples 1 to 5 has the above-mentioned characteristics of improving mechanical properties. It can be inferred that the above-mentioned method for preparing Mn(Ni,Co)Ge composite materials can obtain relatively large negative thermal expansion and magneto-strain effects while ensuring the improvement of mechanical properties when the values are taken as the two endpoints of the numerical range and any value between the two endpoints.
[0059] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for improving the mechanical properties of hexagonal MnNiGe and MnCoGe based alloys, characterized in that: The method comprises hot pressing MnNiGe and MnCoGe based alloy powders with low melting point metal or performing spark plasma sintering on MnNiGe and MnCoGe based alloy powders with low melting point metal, wherein the mass ratio of MnNiGe and MnCoGe based alloy powders to low melting point metal is (1-4):
1.
2. A method for preparing hexagonal MnNiGe and MnCoGe based alloys for improving mechanical properties according to claim 1, characterized in that: The low melting point metal is any one of pure metals of Ga, In, and Sn, or alloys containing Ga, In, and Sn.
3. A method for preparing hexagonal MnNiGe and MnCoGe based alloys for improving mechanical properties according to claim 1, characterized in that: In the hot pressing or spark plasma sintering preparation process, the temperature is 80 to 400° C., the pressure is greater than 50 MPa, and the hot pressing or sintering time is 3 to 30 minutes.
4. A method for preparing hexagonal MnNiGe and MnCoGe based alloys for improving mechanical properties according to claim 1, characterized in that: The chemical formula of the MnNiGe and MnCoGe based alloys is: 1-x Fe x NiGe and Mn 1-y Co 1+y Ge; wherein, 0≤x≤0.24, 0≤y≤0.09, and x and y represent the atomic ratio content.
5. A method for preparing hexagonal MnNiGe and MnCoGe based alloys for improving mechanical properties according to claim 1, characterized in that: The preparation method of the hexagonal MnNiGe and MnCoGe based alloys comprises the following steps: Calculate the required mass of Mn, Ni, Co, Fe, and Ge elements according to the stoichiometric ratio and prepare the ingredients; The raw materials prepared above were placed in a water-cooled copper crucible electric arc furnace, and the vacuum degree in the furnace was drawn to 5×10 -3 Pa, and then the vacuum degree was reduced to 5×10 -3 Pa, fill with 99.999% pure argon gas at 0.8 atmospheres, and perform arc melting 4 to 5 times at a current of 40A to obtain a bulk ingot, or further take part of the ingot to prepare alloy strips by melt rapid quenching method; The block ingot or alloy strip prepared above is sealed in a vacuum quartz tube, heat-treated in a high-temperature furnace to obtain an alloy block or strip, and the block or alloy strip is ground into powder using an agate mortar.
6. A method for improving the mechanical properties of hexagonal MnNiGe and MnCoGe based alloys according to claim 5, characterized in that: The mass of the prepared Mn, Ni, Co, Fe, and Ge elements in step 1 must be accurate to two decimal places in milligrams, and the purity of the elements must be controlled to be above 99.99%.
7. A method for improving the mechanical properties of hexagonal MnNiGe and MnCoGe based alloys according to claim 5, characterized in that: When the bulk ingot or alloy strip in step 3 is Mn 1-y Co 1+y When Ge alloy is used, Mn 1-y Co 1+y The heat treatment process of the Ge alloy is as follows: annealing temperature of 500° C. to 900° C., treatment time of 96 to 168 hours, and rapid cooling in water after treatment.
8. A method for improving the mechanical properties of hexagonal MnNiGe and MnCoGe based alloys according to claim 5, characterized in that: When the bulk ingot or alloy strip in step 3 is Mn 1-x Fe x NiGe alloy, Mn 1-x Fe x The heat treatment process of NiGe alloy is as follows: primary annealing temperature is 600-850°C, and treatment time is 96-168h; then it is taken out and quickly placed in cold water for quenching. After quenching, it is sent back to the same high-temperature furnace for secondary annealing. The secondary annealing temperature is 300-1200°C, and the treatment time is 0-120h, and it is cooled with the furnace.
9. A MnNiGe and MnCoGe based alloy composite material obtained by the preparation method for improving the mechanical properties of hexagonal MnNiGe and MnCoGe based alloys according to any one of claims 1 to 8.
10. Use of the MnNiGe and MnCoGe based alloy composite material according to claim 9 in magnetostriction, magnetic drive and solid-state refrigeration devices.
Citation Information
Patent Citations
Magnetic material for magnetic refrigeration
CN101064204A
Preparation method of bonding martensitic phase change material
CN105448443A
Negative expansion material, and preparation method and application thereof
CN105624514A
LaFeSi based magnetic refrigeration composite material and preparation method and application thereof
CN106906408A
Preparation method of magneto-thermal composite material bonded by low-melting-point alloy
CN107855518A