Method for manufacturing metal hollow frame through 3D printing and metal hollow frame
By using layer-by-layer printing technology and transition layer model in 3D printing, laser parameters and scanning paths are adjusted, the thermal stress problem caused by ultra-fast solidification of lasers is solved, unsupported metal hollow frame printing is achieved, and the molding quality is improved and Material utilization.
Patent Information
- Application Number
- CN202410913632.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The contraction stress and thermal stress formed during ultra-fast solidification of lasers cause the metal hollow frame to easily warp or break when printing in large suspended cross-sections, making it impossible to complete the printing of parts, and a large number of auxiliary support structures are required, resulting in material utilization and printing efficiency. Low.
By establishing a transition layer model in 3D printing and splitting it into multi-layer slice layer and body slice layer, layer-by-layer printing technology is used to adjust laser parameters and scanning paths, reduce heat input and stress, and achieve unsupported hollow frames body printing.
It improves the forming quality of the hollow frame, reduces the risk of warping and fracture, improves material utilization and printing efficiency, simplifies the process flow, and reduces the generation of metal waste.
Smart Images

Figure CN118926543A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of additive manufacturing, and in particular, to a method for manufacturing a metal hollow frame by 3D printing and the metal hollow frame. Background Art
[0002] As an important branch of 3D printing technology, laser selective melting is a rapid prototyping technology that can directly form high-density and high-precision metal parts of metal hollow frames (such as mobile phone hollow frames). It is particularly suitable for the manufacturing process of complex hollow frame structure parts. Compared with traditional forging and precision casting processes, it can save a lot of raw materials and shorten the processing cycle.
[0003] However, due to the shrinkage stress and accumulated thermal stress formed during the ultra-fast laser solidification process, the protruding cross-section that can usually be formed is generally within 0 to 2 mm. If it is larger, it will warp or even break, and the part cannot be printed. It is often necessary to add a large amount of auxiliary support to complete the printing of large suspended cross-sections. The weight of the support structure is usually 30 to 150% of the weight of the part, resulting in a significant reduction in material utilization and printing efficiency, increasing the cost of part manufacturing, and reducing the mass production of parts. Therefore, it is urgent to adopt a new process solution to solve the problem.
[0004] The contents of the background technology section are merely the technologies known to the inventors and do not necessarily represent the prior art in the field. Summary of the invention
[0005] In order to solve the above-mentioned existing technical problems, the first aspect of the present application provides a method for manufacturing a metal hollow frame by 3D printing. The metal hollow frame to be manufactured includes at least three frames and a connecting portion located between adjacent frames of the at least three frames. The method includes:
[0006] Modeling, including:
[0007] A main body printing model is established according to the structure of the metal hollow frame; along the printing direction of the 3D printing, the main body printing model includes a suspended part, and the suspended part corresponds to a frame of the metal hollow frame and two connecting parts located on both sides of the frame;
[0008] Establishing a transition layer model on the surface of the suspended portion, wherein the transition layer model extends in a direction opposite to the printing direction; and
[0009] The transition layer model is split into a first printing model and a second printing model, wherein the first printing model corresponds to the connecting portion and the second printing model corresponds to the frame.
[0010] The second printing model includes at least three sub-printing models;
[0011] Perform slicing and path planning processing, including:
[0012] The main body printing model, the first printing model and the second printing model are sliced respectively to obtain a multi-layer main body slice layer and at least seven transition layer slice layers, wherein each transition layer slice layer includes a first slice region corresponding to the first printing model and a second slice region corresponding to the second printing model, and each second slice region includes at least three border slice sub-regions corresponding to the at least three sub-printing models; wherein the thickness of the second slice region in the at least seven transition layer slice layers increases first and then decreases as the number of layers increases, until it becomes equal to the thickness of one main body slice layer in the multi-layer main body slice layer; and
[0013] Performing line scanning on the multi-layer body slice layer and the at least seven layers of transition layer slice layers, thereby completing path planning processing;
[0014] Feeding metal powder into a 3D printing device, printing in the printing direction based on the planned path, and obtaining a printed part on a substrate, wherein the printed part includes a frame and a transition layer connected to the frame; and
[0015] The substrate and the transition layer are removed to obtain the metal hollow frame.
[0016] In some embodiments of the present application, the thickness of the second slicing region in the second layer of the at least seven transition layer slicing layers is 1 to 3 times the thickness of a main body slicing layer in the multi-layer main body slicing layers, the thickness of the second slicing region in each of the third to sixth layers of the at least seven transition layer slicing layers is 1 to 2 times the thickness of a main body slicing layer in the multi-layer main body slicing layers, and the thickness of the second slicing region in the seventh layer of the at least seven transition layer slicing layers is equal to the thickness of a main body slicing layer in the multi-layer main body slicing layers.
[0017] In some embodiments of the present application, the thickness of the transition layer model is 0.3-3.5 mm, the length of the transition layer model extending in the direction opposite to the printing direction is 0.5-5.5 mm, the connecting portion includes an R angle and / or a C angle, the radius of the R angle is 0.5-6.5 mm, and the angle of the C angle is 45°-75°;
[0018] The number of the sub-printing models is 3 to 7, and the length of each sub-printing model is ≤65 mm.
[0019] In some embodiments of the present application, the thickness of one body slicing layer in the multi-layer body slicing layer is 20-100 μm, the overlapping width of the first slicing region and the second slicing region in each transition layer slicing layer is 0.05-0.15 mm, and the overlapping width of adjacent slicing sub-regions is 0.05-0.15 mm;
[0020] The at least three border slice sub-regions include a first border slice sub-region, a second border slice sub-region, and a third border slice sub-region located between the first border slice sub-region and the second border slice sub-region, the first border slice sub-region and the second border slice sub-region being adjacent to the first slice region respectively;
[0021] Each body slice layer includes a first solid portion and a first contour portion, each first slice region includes a second solid portion and a second contour portion, and each border slice sub-region includes a third solid portion and a third contour portion;
[0022] When line scanning is performed on the multi-layer body slice layer and the at least seven transition layer slice layers, the first contour portion and the first entity portion have a spot compensation of 0.06 to 0.15 mm, the second contour portion and the second entity portion have a spot compensation of 0.06 to 0.15 mm, and the third contour portion and the third entity portion have a spot compensation of 0.1 to 0.15 mm.
[0023] In some embodiments of the present application, when line scanning is performed on the multi-layer body slice layer, the scanning angle of the first layer of the multi-layer body slice layer is 30° to 70°, and the scanning angles of other layers of the multi-layer body slice layer are increased by 50° to 90° on the scanning angle of the previous layer;
[0024] When line scanning is performed on the at least seven transition layer slice layers, the scanning angle of the first layer of the at least seven transition layer slice layers is 30° to 70°, and the scanning angles of the other layers of the at least seven transition layer slice layers are increased by 50° to 90° on the scanning angle of the previous layer.
[0025] In some embodiments of the present application, feeding metal powder into a 3D printing device, printing in the printing direction based on a planned path, and obtaining a print on a substrate includes:
[0026] Setting laser parameters of the 3D printing device; and
[0027] The metal powder is fed into the 3D printer, and under an inert gas atmosphere, in accordance with the printing direction, the portion of the frame that is not connected to the transition layer is first printed on the substrate based on the planned path of the multi-layer body slicing layer, and then the transition layer is printed based on the planned path of the at least seven transition layer slicing layers, and then the remaining portion of the frame is printed on the transition layer based on the planned path of the multi-layer body slicing layer, to obtain the printed part located on the substrate.
[0028] In some embodiments of the present application, setting the laser parameters of the 3D printing device includes:
[0029] Respectively set laser parameters corresponding to the first entity portion, the first contour portion, the second entity portion, the second contour portion, the third entity portion of the first to sixth layers of the at least seven transition layer slice layers, and the third contour portion of the first to sixth layers of the at least seven transition layer slice layers; and
[0030] The laser parameters of the other layers of the at least seven transition layer slicing layers are set so that the laser parameters of the other layers of the at least seven transition layer slicing layers change by no more than 20% based on the previous layer until they are the same as the laser parameters of the first solid part and the first contour part.
[0031] In some embodiments of the present application, the laser parameters set for the first entity portion include laser power: 150-320W, laser scanning speed: 800-1500mm / s, laser scanning spacing: 0.05-0.15mm; the laser parameters set for the first contour portion include laser power: 150-280W, laser scanning speed: 400-1200mm / s;
[0032] The laser parameters set for the second entity part include laser power: 150-320W, laser scanning speed: 800-1500mm / s, laser scanning spacing: 0.05-0.15mm; the laser parameters set for the second contour part include laser power: 150-280W, laser scanning speed: 400-1200mm / s;
[0033] The laser parameters set for the third entity part of the first border slicing sub-region and the second border slicing sub-region of the first to sixth layers of the at least seven transition layer slicing layers include laser power: 40-130W, laser scanning speed: 400-2500mm / s, laser scanning spacing: 0.03-0.08mm; the laser parameters set for the third contour part of the first border slicing sub-region and the second border slicing sub-region of the first to sixth layers of the at least seven transition layer slicing layers include laser power: 40-100W; laser scanning speed: 500-1800mm / s;
[0034] The laser parameters set for the third entity part of the third border slicing sub-area of the first to sixth layers of the at least seven transition layer slicing layers include laser power: 20~110W, laser scanning speed: 600~2500mm / s, laser scanning spacing: 0.03~0.07mm; the laser parameters set for the third contour part of the third border slicing sub-area of the first to sixth layers of the at least seven transition layer slicing layers include laser power: 40~100W; laser scanning speed: 500~1800mm / s.
[0035] In some embodiments of the present application, setting the laser parameters of the 3D printing device further includes:
[0036] Setting the spot diameter range and substrate temperature of the 3D printer;
[0037] The diameter of the light spot is in the range of 50 to 90 μm, and the temperature of the substrate is in the range of 25 to 200° C.
[0038] In some embodiments of the present application, the metal hollow frame includes four frames and four connecting parts, the metal powder is titanium alloy powder, the particle size range of the titanium alloy powder is: 15 to 85 μm, the powder oxygen content is ≤1300 ppm, and the powder fluidity is ≤35s / 50g.
[0039] In some embodiments of the present application, the method further includes:
[0040] The substrate and the printed part are subjected to vacuum annealing, comprising:
[0041] At vacuum degree <10 -3 Pa, firstly heat the substrate and the printed part to 300-500°C at a first heating rate of <5°C / min, and keep them warm for 1-2h; then heat them to 550-850°C at a second heating rate of <3°C / min, and keep them warm for 4-15h; after the insulation is completed, slowly cool them to room temperature with the furnace.
[0042] The second aspect of the present application provides a metal hollow frame made by the above method.
[0043] The present application sets the thickness of the second to seventh layers of the transition layer slicing layer to first increase and then decrease to be equal to the thickness of a main body slicing layer, thereby reducing the heat input of the current printing layer, while reducing the thermal stress input to the formed layer, reducing the risk of warping and cracking, and providing a stable thermal conductive layer and stress dispersion space for subsequent conventional energy input printing of the main body, thereby improving the molding quality of the printed part, and ultimately realizing the support-free 3D printing of the hollow frame.
[0044] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] The following is a detailed description of the implementation methods of the present application in conjunction with the accompanying drawings. Here, the accompanying drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application.
[0046] Figure 1 This is a process flow chart for manufacturing a metal hollow frame by 3D printing provided in one embodiment of the present application. DETAILED DESCRIPTION
[0047] In the following, only some exemplary embodiments are briefly described. As those skilled in the art will appreciate, the described embodiments may be modified in various ways without departing from the spirit or scope of the present application. Therefore, the drawings and descriptions are considered to be exemplary and non-restrictive in nature.
[0048] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, which are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application. In addition, the terms "first" and "second" are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present application, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined.
[0049] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection, an electrical connection, or mutual communication; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0050] In the present application, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may include that the first and second features are in direct contact, or may include that the first and second features are not in direct contact but are in contact through another feature between them. Moreover, a first feature being "above", "above" and "above" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" and "below" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply means that the first feature is lower in level than the second feature.
[0051] The disclosure below provides many different embodiments or examples to realize the different structures of the present application. In order to simplify the disclosure of the present application, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present application. In addition, the present application can repeat reference numbers and / or reference letters in different examples, and this repetition is for the purpose of simplification and clarity, which itself does not indicate the relationship between the various embodiments and / or settings discussed.
[0052] The preferred embodiments of the present application are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present application and are not used to limit the present application.
[0053] Figure 1 A method for manufacturing a metal hollow frame by 3D printing provided in an embodiment of the present application is shown, comprising the following steps S1 to S4.
[0054] S1: Modeling.
[0055] This step includes:
[0056] A main body printing model is established according to the structure of the metal hollow frame; along the printing direction of 3D printing, the main body printing model includes a suspended part, and the suspended part corresponds to a frame of the metal hollow frame and two connecting parts located on both sides of the frame;
[0057] Establishing a transition layer model on the surface of the suspended portion, wherein the transition layer model extends in a direction opposite to the printing direction; and
[0058] The transition layer model is split into a first printing model and a second printing model, the first printing model corresponds to the connection part, the second printing model corresponds to the frame, and the second printing model includes at least three sub-printing models.
[0059] The metal hollow frame to be printed in this application includes at least three frames and connecting parts between adjacent frames. It can be, for example, a metal mobile phone hollow frame, or a computer screen frame, etc., without any limitation. Generally, the metal hollow frame includes four frames and four connecting parts, and is, for example, a rectangular or square structure. Of course, it can also include three or more frames, without any limitation.
[0060] The suspended part described in this application refers to the part without support. For example, for a triangular metal hollow frame, if the printing direction of 3D printing is from one side of the triangle toward the vertex corresponding to the side, then the other two sides of the triangular metal hollow frame belong to the suspended part. For another example, for a rectangular metal frame, if the printing direction of 3D printing is from one side toward another side, then the other side of the quadrilateral metal hollow frame is the suspended part. That is, the suspended part in this application is one or more, depending on the printing direction and the shape of the metal hollow frame to be manufactured.
[0061] Optionally, the metal hollow frame is a titanium alloy hollow frame. In particular, TC4 titanium alloy has a series of excellent properties such as light weight, high strength, corrosion resistance, heat resistance, non-magnetic, good biocompatibility, etc. The titanium alloy mobile phone hollow frame structure leads the trend of the current consumer electronics market and has a wide range of applications in mobile phones.
[0062] Optionally, the connection portion includes an R angle and / or a C angle. The radius of the R angle may be 0.5 to 6.5 mm. The angle of the C angle may be 45° to 75°. The force distribution of the connection portion obtained within this range is good, which can improve the quality of the obtained print.
[0063] Optionally, the thickness of the transition layer model is 0.3 to 3.5 mm. Optionally, the length (i.e., width) of the transition layer model extending in the direction opposite to the printing direction is 0.5 to 5.5 mm. Within this range, the transition layer model can reduce the thermal stress input to the formed layer during the subsequent printing process, thereby reducing the risk of warping and cracking.
[0064] In the present application, the first printing model corresponds to the connecting part, and the second printing model corresponds to the frame. That is, for a hollow frame of a titanium alloy mobile phone, the printing model includes a main body printing model, two first printing models and a second printing model, wherein the second printing model includes at least three sub-printing models. Optionally, the number of sub-printing models is 3 to 7, which makes it easy to give energy to each model separately, thereby reducing the risk of warping and cracking. Optionally, the main body printing model and each first printing model can also be split into multiple sub-models, which can be set as needed without restriction.
[0065] S2: Perform slicing and path planning processing.
[0066] This step includes:
[0067] Slicing the main body printing model, the first printing model and the second printing model respectively to obtain a multi-layer main body slice layer and at least seven transition layer slice layers; and
[0068] Line scanning is performed on the multiple body slice layers and the at least seven transition layer slice layers, thereby completing the path planning process.
[0069] Among them, each transition layer slicing layer includes a first slicing area corresponding to the first printing model and a second slicing area corresponding to the second printing model, and each second slicing area includes at least three border slicing sub-areas. That is, for a titanium alloy mobile phone hollow frame, each slicing layer and each transition layer slicing layer include two first slicing areas and one second slicing area, and each second slicing area includes at least three border slicing sub-areas. At least three border slicing sub-areas include a first border slicing sub-area, a second border slicing sub-area, and a third border slicing sub-area located between the first border slicing sub-area and the second border slicing sub-area, and the first border slicing sub-area and the second border slicing sub-area are adjacent to the first slicing area respectively. The number of the first border slicing sub-area and the second border slicing sub-area are 1 respectively, and the number of the third border slicing sub-area is 1 or more. Optionally, the total number of slicing sub-areas is 3 to 7, that is, the number of the third border slicing sub-area is 1 to 5.
[0070] When the main body printing model and each first printing model are also split into multiple sub-models, each main body slice layer and each first slice area also include multiple sub-areas. Optionally, the length of each border slice sub-area is ≤65mm. When each main body slice layer and each first slice area also include multiple sub-areas, the length of each sub-area is also preferably ≤65mm. This makes it convenient to empower each area, which is conducive to printing a better quality print.
[0071] The thickness of the second slicing region in at least seven transitional slicing layers first increases from the second layer and then decreases as the number of layers increases until it becomes equal to the thickness of one main slicing layer in the multi-layer main slicing layer.
[0072] Optionally, the thickness of one body slice layer in the multi-layer body slice layer is defined as WW, the thickness of the second slice region in the second layer of at least seven transition layer slice layers is equal to 1 to 3 times W, the thickness of the second slice region in each of the third to sixth layers of at least seven transition layer slice layers is 1 to 2 times W, and the thickness of the second slice region in the seventh layer of at least seven transition layer slice layers may be equal to W. When the number of transition layer slice layers exceeds seven, the thickness of the latter may be equal to the thickness of the seventh layer until the entire transition layer slice is completed.
[0073] By setting the thickness of the second to seventh layers of the transition layer slice layer to first increase and then decrease to be equal to the thickness of a main body slice layer, the heat input of the current printing layer can be reduced, and the thermal stress input to the formed layer can be reduced, thereby finely controlling the laser energy input density of different layers. Low energy input is used in areas farther from the frame to reduce the overheating of the printed material in the area, forming a solid powder bonding layer, and relying on the gradual change of subsequent layer thickness, reducing the stress change caused by the cumulative effect of thermal stress of the solidified layer caused by heat penetration, thereby reducing the warping of the transition layer, providing a stable thermal conductive layer and stress dispersion space for subsequent conventional energy input printing of the main body, improving the molding quality of the printed part, and ultimately realizing the support-free 3D printing of the hollow frame.
[0074] Optionally, the thickness of one body slice layer in the multi-layer body slice layer is 20-100 μm (i.e., W can be 20-100 μm). At this time, the thickness of the second layer of at least seven transition layer slice layers can be 20-300 μm, and further optionally 60-120 μm; the thickness of the third to sixth layers can be 20-200 μm, and further optionally 40-100 μm.
[0075] Optionally, the overlap width of the first slicing area and the second slicing area in each transition layer slicing layer is 0.05-0.15 mm, and the overlap width of adjacent slicing sub-areas is 0.05-0.15 mm. That is, the overlap width of adjacent slicing areas is 0.05-0.15 mm. The overlap between areas can ensure the continuity of printing.
[0076] Optionally, each body slice layer includes a first entity part and a first contour part, each first slice area includes a second entity part and a second contour part, and each border slice sub-area includes a third entity part and a third contour part. Optionally, when line scanning is performed on multiple body slice layers and at least seven transition layer slice layers, the first contour part and the first entity part have a spot compensation of 0.06 to 0.15 mm, the second contour part and the second entity part have a spot compensation of 0.06 to 0.15 mm, and the third contour part and the third entity part have a spot compensation of 0.1 to 0.15 mm.
[0077] Optionally, when line scanning is performed on a multi-layer body slice layer, the scanning angle of the first layer of the multi-layer body slice layer is 30° to 70°, and the scanning angles of other layers of the multi-layer body slice layer are increased by 50° to 90° on the scanning angle of the previous layer. When line scanning is performed on at least seven transition layer slice layers, the scanning angle of the first layer of the at least seven transition layer slice layers is 30° to 70°, and the scanning angles of other layers of the at least seven transition layer slice layers are increased by 50° to 90° on the scanning angle of the previous layer.
[0078] S3: feeding metal powder into a 3D printing device, printing is performed in a printing direction based on a planned path, and a printed part is obtained on a substrate, wherein the printed part includes a frame and a transition layer connected to the frame.
[0079] Optionally, when preparing a titanium alloy hollow frame, the titanium alloy powder used has a particle size range of 15 to 85 μm, a powder oxygen content of ≤1300 ppm, and a powder fluidity of ≤35 s / 50 g.
[0080] Optionally, this step includes:
[0081] Setting laser parameters for 3D printing equipment; and
[0082] The metal powder is fed into a 3D printer. In an inert gas atmosphere, the portion of the frame that is not connected to the transition layer is first printed on the substrate based on the planned path of the multi-layer body slicing layer according to the printing direction. Then, the transition layer is printed based on the planned path of at least seven layers of transition layer slicing layers. Then, the remaining portion of the frame is printed on the transition layer based on the planned path of the multi-layer body slicing layer to obtain a printout on the substrate.
[0083] Optionally, setting laser parameters of the 3D printing device includes:
[0084] respectively setting laser parameters corresponding to the first entity portion, the first contour portion, the second entity portion, the second contour portion, the third entity portion of the first to sixth layers of the at least seven transition layer slice layers, and the third contour portion of the first to sixth layers of the at least seven transition layer slice layers; and
[0085] The laser parameters of the other layers of the at least seven transition layer slice layers are set so that the laser parameters of the other layers of the at least seven transition layer slice layers change by no more than 20% based on the previous layer until they are the same as the laser parameters of the first solid part and the first contour part.
[0086] By individually energizing different slice layers and different areas, the risk of warping can be reduced by reducing thermal stress input.
[0087] Optionally, the laser parameters set for the first entity portion include laser power: 150-320W, laser scanning speed: 800-1500mm / s, laser scanning spacing: 0.05-0.15mm. Optionally, the laser parameters set for the first contour portion include laser power: 150-280W, laser scanning speed: 400-1200mm / s. That is, the frame is printed using the above laser parameters.
[0088] Optionally, the laser parameters set for the second entity portion include laser power: 150-320W, laser scanning speed: 800-1500mm / s, laser scanning spacing: 0.05-0.15mm; the laser parameters set for the second contour portion include laser power: 150-280W, laser scanning speed: 400-1200mm / s. That is, the portion of the transition layer corresponding to the connection portion of the metal hollow frame is printed using the above laser parameters.
[0089] Optionally, the laser parameters set for the third solid part of the first border slicing sub-area and the second border slicing sub-area of the first to sixth layers of at least seven transition layer slicing layers include laser power: 40~130W, laser scanning speed: 400~2500mm / s, laser scanning spacing: 0.03~0.08mm; the laser parameters set for the third contour part of the first border slicing sub-area and the second border slicing sub-area of the first to sixth layers of at least seven transition layer slicing layers include laser power: 40~100W; laser scanning speed: 500~1800mm / s.
[0090] Optionally, the laser parameters set for the third solid part of the third border slicing sub-area of the first to sixth layers of at least seven transition layer slicing layers include laser power: 20~110W, laser scanning speed: 600~2500mm / s, laser scanning spacing: 0.03~0.07mm; the laser parameters set for the third contour part of the third border slicing sub-area of the first to sixth layers of at least seven transition layer slicing layers include laser power: 40~100W; laser scanning speed: 500~1800mm / s.
[0091] That is, the portion of the transition layer corresponding to the frame of the metal hollow frame is printed using the above laser parameters.
[0092] In some specific embodiments, the scanning angle of the first layer of the transition layer slicing layer is 30°~70°, the laser power of the third entity part of the first border slicing sub-region and the second border slicing sub-region of the first layer is: 40~130W, laser scanning speed: 400~2500mm / s, laser scanning spacing: 0.03~0.08mm, the laser power of the third contour part of the first border slicing sub-region and the second border slicing sub-region of the first layer is: 40~100W, laser scanning speed: 500~1800mm / s, the laser power of the third entity part of the third border slicing sub-region of the first layer is: 20~110W, laser scanning speed: 600~2500mm / s, laser scanning spacing: 0.03~0.07mm, and the laser parameters set for the third contour part of the third border slicing sub-region of the first layer include laser power: 40~100W, laser scanning speed: 500~1800mm / s.
[0093] In some specific embodiments, the scanning angle of the second layer of the transition layer slicing layer is increased by 50° to 90° on the scanning angle of the first layer, the laser power of the first border slicing sub-region and the third entity part of the second border slicing sub-region of the second layer is: 40 to 120 W, laser scanning speed: 400 to 2500 mm / s, laser scanning spacing: 0.03 to 0.08 mm, the laser power of the third contour part of the first border slicing sub-region and the second border slicing sub-region of the second layer is: 40 to 100 W, laser scanning speed: 500 to 1800 mm / s, the laser power of the third entity part of the third border slicing sub-region of the second layer is: 20 to 110 W, laser scanning speed: 600 to 2500 mm / s, laser scanning spacing: 0.03 to 0.07 mm, and the laser parameters set for the third contour part of the third border slicing sub-region of the second layer include laser power: 40 to 100 W, laser scanning speed: 500 to 1800 mm / s.
[0094] In some specific embodiments, the scanning angle of the third layer of the transition layer slicing layer is increased by 50° to 90° on the scanning angle of the second layer; the laser power of the third entity part of the first border slicing sub-region and the second border slicing sub-region of the third layer is: 60 to 120 W, laser scanning speed: 400 to 1500 mm / s, laser scanning spacing: 0.03 to 0.08 mm; the laser power of the third contour part of the first border slicing sub-region and the second border slicing sub-region of the third layer is: 40 to 100 W, laser scanning speed: 500 to 1800 mm / s; the laser power of the third entity part of the third border slicing sub-region of the third layer is: 40 to 110 W, laser scanning speed: 600 to 2500 mm / s, laser scanning spacing: 0.03 to 0.07 mm; the laser parameters set for the third contour part of the third border slicing sub-region of the second layer include laser power: 40 to 100 W, laser scanning speed: 500 to 1800 mm / s.
[0095] In some specific embodiments, the scanning angles of the fourth to sixth layers of the transition layer slice layer are increased by 50° to 90° on the scanning angle of the previous layer, and the other parameters remain unchanged. That is, except for the scanning angle, the laser parameters of the fourth to sixth layers of the transition layer slice layer are the same as those of the third layer.
[0096] In some specific embodiments, the scanning angle of the seventh and subsequent transitional slice layers is increased by 50° to 90° on the scanning angle of the previous layer, and the laser parameters are changed by no more than 20% on the basis of the previous layer until they are the same as the laser parameters of the first entity part and the first contour part (i.e., the laser parameters of the printing frame). In some specific embodiments, the laser power in the laser parameters is changed by no more than 20% on the basis of the previous layer, and the remaining parameters can be gradually changed until they are the same as the laser parameters of the first entity part and the first contour part (i.e., the laser parameters of the printing frame).
[0097] This setting gradually reduces the energy input from the edge area to the middle area, which can avoid the risk of warping and cracking of the current layer. By carefully controlling the laser energy input density at different positions in the same layer and different positions in different layers, low energy input is used in areas farther from the edge to reduce the overheating of the printed material in this area, forming a solid powder bonding layer, and relying on the gradual increase of subsequent layer thickness, reducing the cumulative effect of thermal stress in the solidified layer caused by heat penetration, resulting in stress changes, thereby reducing the warping of the transition layer, providing a stable thermal conductive layer and stress dispersion space for subsequent conventional energy input printing of the part body, and improving the part molding quality.
[0098] Optionally, setting the laser parameters of the 3D printing device also includes: setting the spot diameter range and substrate temperature of the 3D printer. Optionally, the spot diameter range is 50 to 90 μm, and the substrate temperature is 25 to 200° C. Optionally, the inert gas is argon or the like.
[0099] After printing is completed, cool the substrate temperature to below 70°C, remove the substrate and printed parts, and clean the residual powder on the surface of the printed parts.
[0100] S4: removing the substrate and the transition layer to obtain a metal hollow frame.
[0101] Optionally, the substrate and the transition layer are removed by wire cutting, and the wire cutting wire feeding direction may be perpendicular to the width direction of the hollow frame.
[0102] Optionally, after cutting, the printed part is sandblasted, with a sand material diameter of 150-300 mesh and a sandblasting pressure of 0.2-0.6 MPa, until the surface color of the part is uniform. Sandblasting can make the texture of the metal hollow frame better.
[0103] Optionally, the method further comprises, before step S4, vacuum annealing the substrate and the printed part. Further, optionally, placing the printed part and the substrate together in a high vacuum furnace for vacuum annealing, and performing vacuum annealing at a vacuum degree of less than 10 -3 Pa, first heat the substrate and the printed part to 300-500°C at a first heating rate of <5°C / min, and keep them warm for 1-2h; then heat them to 550-850°C at a second heating rate of <3°C / min, and keep them warm for 4-15h; after the insulation is completed, slowly cool them to room temperature with the furnace.
[0104] The present application further provides a metal hollow frame made by the above method. The metal hollow frame made by the present application has very good molding accuracy.
[0105] The present invention is described below with reference to specific embodiments. The process condition values taken in the following embodiments and comparative examples are exemplary, and their possible numerical ranges are as shown in the above-mentioned invention summary. For process parameters not particularly noted, conventional techniques can be used. It should be noted that, in the absence of conflict, the embodiments in this application and the features in the embodiments can be combined with each other.
[0106] Example 1
[0107] This embodiment adopts Figure 1 The method shown is to manufacture a hollow titanium alloy mobile phone frame, which is a rectangular structure, including four frames (two long sides and two short sides) and connecting parts between the connected frames (four in total), and the printing direction is from one short side (hereinafter referred to as the first short side) to the other short side (hereinafter referred to as the second short side). The specific steps are as follows:
[0108] 1. Modeling:
[0109] The main body printing model is established according to the structure of the metal hollow frame. The suspended part of the main body printing model corresponds to the second short side of the hollow frame of the titanium alloy mobile phone and two R corners on both sides of the second short side.
[0110] A transition layer model is established on the surface of the suspended part, wherein the transition layer model extends in the direction opposite to the printing direction. The thickness of the transition layer model is designed to be 0.4 mm, the width (length extending to the first short side) is 4 mm, and the two ends are R angles with a radius of 3 mm.
[0111] The transition layer model is split into two first printing models and one second printing model. The first printing model corresponds to the connection part, the second printing model corresponds to the frame, and the second printing model includes five sub-printing models. The lengths of the five sub-printing models are 25mm, 20mm, 30mm, 20mm and 25mm respectively. The main body printing model and each first printing model are split into three sub-models respectively.
[0112] 2. Perform slicing and path planning:
[0113] The main body printing model, the first printing model and the second printing model are sliced to obtain the main body slice layer and the transition layer slice layer, wherein each transition layer slice layer includes a first slice area corresponding to the first printing model and a second slice area corresponding to the second printing model. The main body slice layer has 3152 layers, and each main body slice layer includes 3 main body slice sub-areas; the transition layer slice layer has 7 layers, and each transition layer slice layer includes 2 first slice areas and 1 second slice area, each first slice area includes 3 connection portion slice sub-areas, and each second slice area includes 5 border slice sub-areas. The 5 border slice sub-areas include 1 first border slice sub-area, 1 second border slice sub-area and 3 third border slice sub-areas, wherein the first border slice sub-area and the second border slice sub-area are adjacent to the first slice area, and the 3 third border slice sub-areas are located between the 1 first border slice sub-area and the 1 second border slice sub-area. The sizes of the 3 main body slice sub-areas are the same, the sizes of the 3 connection portion slice sub-areas are also the same, and the sizes of the 5 border slice sub-areas are the same as the 5 sub-printing models. The thickness of each layer in the main slice layer is 40μm. The thickness of the first layer of the transition layer slice layer is 40μm, the thickness of the second layer is 120μm, the thickness of the third layer is 80μm, the thickness of the fourth layer is 80μm, and the thickness of each layer after the fifth layer is 40μm. The overlapping width of two adjacent slice sub-areas is 0.07mm.
[0114] Each body slice sub-region includes a first solid portion and a first contour portion, each connection portion slice sub-region includes a second solid portion and a second contour portion, and each border slice sub-region includes a third solid portion and a third contour portion.
[0115] Line scanning is performed on the main body slice layer and the transition layer slice layer to complete the path planning process. Among them, the first contour part and the first entity part have a spot compensation of 0.14mm, the second contour part and the second entity part have a spot compensation of 0.14mm, and the third contour part and the third entity part have a spot compensation of 0.1mm.
[0116] The scanning angle of the first layer of the main slicing layer is 40°, the scanning angle of the second layer is 130°, and the scanning angle of the third layer and thereafter is 90° more than the scanning angle of the previous layer. The scanning angle of the first layer of the first slicing area of the transition layer slicing layer is 40°, the scanning angle of the second layer is 130°, and the scanning angle of the third layer and thereafter is 90° more than the scanning angle of the previous layer. The scanning angle of the first layer of the second slicing area of the transition layer slicing layer is 50°, the scanning angle of the second layer is 140°, and the scanning angle of the third layer and thereafter is 90° more than the scanning angle of the previous layer.
[0117] 3. Laser 3D printing:
[0118] 3.1 Set the laser parameters of the 3D printing equipment.
[0119] Among them, the laser parameters set for the first entity part of the three body slice sub-areas in each layer of the body slice layer include laser power: 260W, laser scanning speed: 1200mm / s, laser scanning spacing: 0.14mm; the laser parameters set for the first contour part of the three body slice sub-areas of the body slice layer include laser power: 190W, laser scanning speed: 1100mm / s.
[0120] The laser parameters set for the second entity part of the 6 connecting part slicing sub-areas of the 2 first slicing areas in each layer of the transition layer slicing layer include laser power: 260W, laser scanning speed: 1200mm / s, laser scanning spacing: 0.14mm; the laser parameters set for the second contour part of the 6 second sub-slicing areas of the 2 first slicing areas in each layer of the transition layer slicing layer include laser power: 190W, laser scanning speed: 1100mm / s.
[0121] The laser parameters set for the third solid part of the first border slicing sub-region and the second border slicing sub-region in the second slicing area in the first layer of the transition layer slicing layer include laser power: 90W, laser scanning speed: 1000mm / s, laser scanning spacing: 0.06mm; the laser parameters set for the third contour part of the first border slicing sub-region and the second border slicing sub-region include laser power: 50W, laser scanning speed: 1200mm / s.
[0122] The laser parameters set for the third entity part of the first of the three third border slicing sub-areas in the second slicing area in the first layer of the transition layer slicing layer include laser power: 80W, laser scanning speed: 1500mm / s, laser scanning spacing: 0.06mm; the laser parameters set for the third entity parts of the second and third of the three third border slicing sub-areas include laser power: 45W, laser scanning speed: 1800mm / s, laser scanning spacing: 0.04mm; the laser parameters set for the third contour parts of the three third border slicing sub-areas include laser power: 50W, laser scanning speed: 1200mm / s.
[0123] The laser parameters set for the third solid part of the first border slicing sub-region and the second border slicing sub-region in the second slicing area in the second layer of the transition layer slicing layer include laser power: 110W, laser scanning speed: 800mm / s, laser scanning spacing: 0.08mm; the laser parameters set for the third contour part of the first border slicing sub-region and the second border slicing sub-region include laser power: 50W, laser scanning speed: 1200mm / s.
[0124] The laser parameters set for the third physical parts of the first and third of the three third border slice sub-areas in the second slice area in the second layer of the transition layer slicing layer include laser power: 90W, laser scanning speed: 1200mm / s, laser scanning spacing: 0.06mm; the laser parameters set for the third physical part of the second of the three third border slice sub-areas include laser power: 55W, laser scanning speed: 1800mm / s, laser scanning spacing: 0.04mm; the laser parameters set for the third contour parts of the three third border slice sub-areas include laser power: 50W, laser scanning speed: 1200mm / s.
[0125] The laser parameters set for the third solid part of the first border slicing sub-region and the second border slicing sub-region in the second slicing area in the third layer of the transition layer slicing layer include laser power: 120W, laser scanning speed: 900mm / s, laser scanning spacing: 0.07mm; the laser parameters set for the third contour part of the first border slicing sub-region and the second border slicing sub-region include laser power: 50W, laser scanning speed: 1200mm / s.
[0126] The laser parameters set for the third physical parts of the first and third of the three third border slice sub-areas in the second slice area in the third layer of the transition layer slicing layer include laser power: 100W, laser scanning speed: 1100mm / s, laser scanning spacing: 0.06mm; the laser parameters set for the third physical part of the second of the three third border slice sub-areas include laser power: 80W, laser scanning speed: 1000mm / s, laser scanning spacing: 0.05mm; the laser parameters set for the third contour parts of the three third border slice sub-areas include laser power: 50W, laser scanning speed: 1200mm / s.
[0127] For the third solid part of the first border slicing sub-region and the second border slicing sub-region in the second slicing area of each layer from the fourth to the sixth layer of the transition layer slicing layer, the laser parameters set include laser power: 110W, laser scanning speed: 1200mm / s, laser scanning spacing: 0.08mm; the laser parameters set in the third contour part of the first border slicing sub-region and the second border slicing sub-region include laser power: 50W, laser scanning speed: 1200mm / s.
[0128] For the third entity parts of the first and third of the three third border slice sub-areas in the second slice area of each layer from the fourth to the sixth layer of the transition layer slicing layer, the laser parameters set include laser power: 110W, laser scanning speed: 1100mm / s, laser scanning spacing: 0.06mm; the laser parameters set for the third entity part of the second of the three third border slice sub-areas include laser power: 100W, laser scanning speed: 1200mm / s, laser scanning spacing: 0.05mm; the laser parameters set for the third contour parts of the three third border slice sub-areas include laser power: 50W, laser scanning speed: 1200mm / s.
[0129] The laser power of the second slicing region of each layer above the sixth layer of the transition layer slicing layer is increased by 10% based on the previous layer until it is the same as the laser power of the three body slicing sub-regions in each layer of the body slicing layer.
[0130] 3.2 Printing
[0131] The metal powder is fed into the 3D printer, and under an argon atmosphere, the oxygen content in the 3D printer is reduced to 300ppm. According to the printing direction, the part of the frame that is not connected to the transition layer (i.e., the first short side, two R corners on both sides of the first short side, and two long sides of the hollow frame of the titanium alloy mobile phone) is first printed on the substrate based on the planned path of the multi-layer body slicing layer, and then the transition layer is printed on the substrate based on the planned path of the transition layer slicing layer, and then the remaining part of the frame (i.e., the second short side and the R corners on both sides of the second short side) is printed on the transition layer based on the planned path of the body slicing layer to obtain a print on the substrate.
[0132] Titanium alloy powder particle size range: 15-53μm, powder oxygen content 1150ppm, powder fluidity 28.3s / 50g. 3D printer spot diameter setting: 80μm, substrate temperature: 100℃;
[0133] 3.3 Cleaning
[0134] After the printing process is completed, the substrate temperature is cooled to below 70°C, taken out, and the residual powder on the surface is cleaned.
[0135] 4. Stress relief treatment:
[0136] Put the printed part and the substrate into a high vacuum furnace for vacuum annealing. -3 Under the condition of Pa, the substrate and the printed part are first heated to 500°C at a first heating rate of 2°C / min and kept at this temperature for 1.5h; then heated to 800°C at a second heating rate of 1°C / min and kept at this temperature for 10h; after the insulation, they are slowly cooled to room temperature with the furnace.
[0137] 5. Post-processing
[0138] The substrate and transition layer are removed by wire cutting, and the wire cutting direction is perpendicular to the width direction of the hollow frame. Then the metal hollow frame separated by wire cutting is sandblasted, with a sand material diameter of 230 mesh and a sandblasting pressure of 0.3MPa, until the surface color of the part is uniform.
[0139] Example 2
[0140] This embodiment adopts Figure 1 The method shown is to manufacture a hollow titanium alloy mobile phone frame, which is a rectangular structure, including four frames (two long sides and two short sides) and connecting parts between the connected frames (four in total), and the printing direction is from one short side (hereinafter referred to as the first short side) to the other short side (hereinafter referred to as the second short side). The specific steps are as follows:
[0141] 1. Modeling:
[0142] The main body printing model is established according to the structure of the metal hollow frame. The suspended part of the main body printing model corresponds to the second short side of the hollow frame of the titanium alloy mobile phone and two C corners on both sides of the second short side.
[0143] A transition layer model is established on the surface of the suspended part, wherein the transition layer model extends in the direction opposite to the printing direction. The thickness of the transition layer model is designed to be 0.68 mm, the width (length extending to the first short side) is 3 mm, the two ends are C-angle structures, the angle of the C-angle is 60°, and the plane length on the C-angle is 4 mm.
[0144] The transition layer model is split into two first printing models and one second printing model. The first printing model corresponds to the connection part, and the second printing model corresponds to the frame. Each second printing model includes three sub-printing models. The lengths of the three sub-printing models are 45mm, 60mm, and 45mm respectively. The main body printing model and each first printing model are split into two sub-models respectively.
[0145] 2. Perform slicing and path planning:
[0146] The main body printing model, the first printing model and the second printing model are sliced to obtain the main body slice layer and the transition layer slice layer, wherein each transition layer slice layer includes a first slice area corresponding to the first printing model and a second slice area corresponding to the second printing model. The main body slice layer has 3410 layers, and each main body slice layer includes 2 main body slice sub-areas; the transition layer slice layer has 10 layers, and each transition layer slice layer includes 2 first slice areas and 1 second slice area, each first slice area includes 2 connection portion slice sub-areas, and each second slice area includes 3 border slice sub-areas. The 3 border slice sub-areas include 1 first border slice sub-area, 1 second border slice sub-area and 1 third border slice sub-area, wherein the first border slice sub-area and the second border slice sub-area are adjacent to the first slice area, and the third border slice sub-area is located between the first border slice sub-area and the second border slice sub-area. The sizes of the 2 main body slice sub-areas are the same, the sizes of the 2 connection portion slice sub-areas are also the same, and the sizes of the 3 border slice sub-areas are the same as the 3 sub-printing models. The thickness of each layer in the main slice layer is 60μm. The thickness of the first layer of the transition layer slice layer is 60μm, the thickness of the second layer is 100μm, the thickness of the third layer is 80μm, the thickness of the fourth layer is 80μm, and the thickness of each layer after the fifth layer is 60μm. The overlapping width of two adjacent slice sub-areas is 0.1mm.
[0147] Each body slice sub-region includes a first solid portion and a first contour portion, each connection portion slice sub-region includes a second solid portion and a second contour portion, and each border slice sub-region includes a third solid portion and a third contour portion.
[0148] Line scanning is performed on the main body slice layer and the transition layer slice layer to complete the path planning process. Among them, the first contour part and the first entity part have a spot compensation of 0.12mm, the second contour part and the second entity part have a spot compensation of 0.12mm, and the third contour part and the third entity part have a spot compensation of 0.11mm.
[0149] The scanning angle of the first layer of the main slicing layer is 55°, the scanning angle of the second layer is 145°, and the scanning angle of the third layer and thereafter is 90° more than the scanning angle of the previous layer. The scanning angle of the first layer of the first slicing area of the transition layer slicing layer is 55°, the scanning angle of the second layer is 145°, and the scanning angle of the third layer and thereafter is 90° more than the scanning angle of the previous layer. The scanning angle of the first layer of the second slicing area of the transition layer slicing layer is 45°, the scanning angle of the second layer is 115°, and the scanning angle of the third layer and thereafter is 70° more than the scanning angle of the previous layer.
[0150] 3. Laser 3D printing:
[0151] 3.1 Set the laser parameters of the 3D printing equipment.
[0152] Among them, the laser parameters set for the first entity part of the two body slice sub-areas in each layer of the body slice layer include laser power: 285W, laser scanning speed: 1100mm / s, laser scanning spacing: 0.13mm; the laser parameters set for the first contour part of the two body slice sub-areas of the body slice layer include laser power: 200W, laser scanning speed: 900mm / s.
[0153] The laser parameters set for the second entity part of the 4 connecting slicing sub-areas of the 2 first slicing areas in each layer of the transition layer slicing layer include laser power: 285W, laser scanning speed: 1100mm / s, laser scanning spacing: 0.13mm; the laser parameters set for the second contour part of the 4 second sub-slicing areas of the 2 first slicing areas in each layer of the transition layer slicing layer include laser power: 200W, laser scanning speed: 900mm / s.
[0154] The laser parameters set for the third entity part of the first border slice sub-area in the second slice area in the first layer of the transition layer slice layer include laser power: 75W, laser scanning speed: 1300mm / s, laser scanning spacing: 0.06mm; the laser parameters set for the third entity part of the second border slice sub-area include laser power: 75W, laser scanning speed: 1200mm / s, laser scanning spacing: 0.06mm; the laser parameters set for the third entity part of the third border slice sub-area include laser power: 60W, laser scanning speed: 1700mm / s, laser scanning spacing: 0.03mm. The laser parameters set for the third contour part of the first border slice sub-area, the second border slice sub-area and the third border slice sub-area in the second slice area in the first layer of the transition layer slice layer include laser power: 40W, laser scanning speed: 1300mm / s.
[0155] The laser parameters set for the third entity part of the first border slice sub-area and the second border slice sub-area in the second slice area in each layer of the second layer and the third layer of the transition layer slice layer include laser power: 90W, laser scanning speed: 1250mm / s, laser scanning spacing: 0.06mm; the laser parameters set for the third entity part of the second border slice sub-area include laser power: 70W, laser scanning speed: 1200mm / s, laser scanning spacing: 0.05mm. The laser parameters set for the third contour part of the first border slice sub-area, the second border slice sub-area and the third border slice sub-area in the second slice area in each layer of the second layer and the third layer of the transition layer slice layer include laser power: 40W, laser scanning speed: 1300mm / s.
[0156] The laser parameters set for the third entity part of the first border slice sub-area and the second border slice sub-area in the second slice area in each of the fourth to sixth layers of the transition layer slice layer include laser power: 100W, laser scanning speed: 1100mm / s, laser scanning spacing: 0.06mm; the laser parameters set for the third entity part of the second border slice sub-area include laser power: 90W, laser scanning speed: 1500mm / s, laser scanning spacing: 0.05mm. The laser parameters set for the third contour part of the first border slice sub-area, the second border slice sub-area and the third border slice sub-area in the second slice area in each of the fourth to sixth layers of the transition layer slice layer include laser power: 40W, laser scanning speed: 1300mm / s.
[0157] The laser power of the second slice region of the seventh and subsequent layers of the transition layer slice layer is increased by 15% based on the previous layer, until it is the same as the laser power of the two body slice sub-regions in each layer of the body slice layer.
[0158] 3.2 Printing
[0159] The metal powder is fed into the 3D printer, and under an argon atmosphere, the oxygen content in the 3D printer is reduced to 200ppm. According to the printing direction, the part of the frame not connected to the transition layer (i.e., the first short side, two C corners on both sides of the first short side, and two long sides of the hollow frame of the titanium alloy mobile phone) is first printed on the substrate based on the planned path of the multi-layer body slicing layer, and then the transition layer is printed on the substrate based on the planned path of the transition layer slicing layer, and then the remaining part of the frame (i.e., the second short side and the C corners on both sides of the second short side) is printed on the transition layer based on the planned path of the body slicing layer to obtain a print on the substrate.
[0160] Titanium alloy powder particle size range: 15-53μm, powder oxygen content 950ppm, powder fluidity 32.5s / 50g. 3D printer spot diameter setting: 75μm, substrate temperature: 150℃;
[0161] 3.3 Cleaning
[0162] After the printing process is completed, the substrate temperature is cooled to below 70°C, taken out, and the residual powder on the surface is cleaned.
[0163] 4. Stress relief treatment:
[0164] Put the printed part and the substrate into a high vacuum furnace for vacuum annealing. -3 Under the condition of Pa, the substrate and the printed part are first heated to 400°C at a first heating rate of 3°C / min and kept at this temperature for 1h; then heated to 750°C at a second heating rate of 2°C / min and kept at this temperature for 6h; after the insulation, they are slowly cooled to room temperature with the furnace.
[0165] 5. Post-processing
[0166] The substrate and transition layer are removed by wire cutting, and the wire cutting direction is perpendicular to the width direction of the hollow frame. Then the metal hollow frame separated by wire cutting is sandblasted, with a sand material diameter of 230 mesh and a sandblasting pressure of 0.3MPa, until the surface color of the part is uniform.
[0167] Example 3
[0168] This embodiment adopts Figure 1 The method shown is to manufacture a hollow titanium alloy mobile phone frame, which is a rectangular structure, including four frames (two long sides and two short sides) and connecting parts between the connected frames (four in total), and the printing direction is from one short side (hereinafter referred to as the first short side) to the other short side (hereinafter referred to as the second short side). The specific steps are as follows:
[0169] 1. Modeling:
[0170] The main body printing model is established according to the structure of the metal hollow frame. The suspended part of the main body printing model corresponds to the second short side of the hollow frame of the titanium alloy mobile phone and two C corners on both sides of the second short side.
[0171] A transition layer model is established on the surface of the suspended part, wherein the transition layer model extends in the direction opposite to the printing direction. The thickness of the transition layer model is designed to be 1.08 mm, the width is 5 mm, the two ends are C-angle structures, the angle of the C-angle is 45°, and the length of the plane on the C-angle is 5 mm.
[0172] The transition layer model is split into two first printing models and one second printing model. The first printing model corresponds to the connection part, the second printing model corresponds to the frame, and the second printing model includes 7 sub-printing models. The lengths of the 7 sub-printing models are 30mm, 25mm, 25mm, 20mm, 25mm, 25mm and 30mm respectively. The main body printing model and each first printing model are split into 3 sub-models respectively.
[0173] 2. Perform slicing and path planning:
[0174] The main body printing model, the first printing model and the second printing model are sliced to obtain the main body slice layer and the transition layer slice layer, wherein each transition layer slice layer includes a first slice area corresponding to the first printing model and a second slice area corresponding to the second printing model. The main body slice layer has 2654 layers, and each main body slice layer includes 3 main body slice sub-areas; the transition layer slice layer has 12 layers, and each transition layer slice layer includes 2 first slice areas and 1 second slice area, each first slice area includes 3 connection portion slice sub-areas, and each second slice area includes 7 border slice sub-areas. The 7 border slice sub-areas include 1 first border slice sub-area, 1 second border slice sub-area and 5 third border slice sub-areas, wherein the first border slice sub-area and the second border slice sub-area are adjacent to the first slice area, and the 5 third border slice sub-areas are located between the 1 first border slice sub-area and the 1 second border slice sub-area. The sizes of the 3 main body slice sub-areas are the same, the sizes of the 3 connection portion slice sub-areas are also the same, and the sizes of the 7 border slice sub-areas are the same as the 7 sub-printing models. The thickness of each layer in the main slice layer is 80μm. The thickness of the first layer of the transition layer slice layer is 80μm, the thickness of the second layer is 120μm, the thickness of the third layer is 120μm, the thickness of the fourth layer is 100μm, the thickness of the fifth layer is 100μm, and the thickness of the sixth layer and subsequent layers is 80μm. The overlapping width of two adjacent slice sub-areas is 0.11mm.
[0175] Each body slice sub-region includes a first solid portion and a first contour portion, each connection portion slice sub-region includes a second solid portion and a second contour portion, and each border slice sub-region includes a third solid portion and a third contour portion.
[0176] Line scanning is performed on the main body slice layer and the transition layer slice layer to complete the path planning process. Among them, the first contour part and the first entity part have a spot compensation of 0.1mm, the second contour part and the second entity part have a spot compensation of 0.1mm, and the third contour part and the third entity part have a spot compensation of 0.11mm.
[0177] The scanning angle of the first layer of the main slicing layer is 40°, the scanning angle of the second layer is 100°, and the scanning angle of the third layer and thereafter is 60° more than the scanning angle of the previous layer. The scanning angle of the first layer of the first slicing area of the transition layer slicing layer is 40°, the scanning angle of the second layer is 100°, and the scanning angle of the third layer and thereafter is 60° more than the scanning angle of the previous layer. The scanning angle of the first layer of the second slicing area of the transition layer slicing layer is 40°, the scanning angle of the second layer is 100°, and the scanning angle of the third layer and thereafter is 60° more than the scanning angle of the previous layer.
[0178] 3. Laser 3D printing:
[0179] 3.1 Set the laser parameters of the 3D printing equipment.
[0180] Among them, the laser parameters set for the first entity part of the three body slice sub-areas in each layer of the body slice layer include laser power: 310W, laser scanning speed: 950mm / s, laser scanning spacing: 0.11mm; the laser parameters set for the first contour part of the three body slice sub-areas of the body slice layer include laser power: 210W, laser scanning speed: 800mm / s.
[0181] The laser parameters set for the second entity part of the 6 connecting part slicing sub-areas of the 2 first slicing areas in each layer of the transition layer slicing layer include laser power: 310W, laser scanning speed: 950mm / s, laser scanning spacing: 0.11mm; the laser parameters set for the second contour part of the 6 second sub-slicing areas of the 2 first slicing areas in each layer of the transition layer slicing layer include laser power: 210W, laser scanning speed: 800mm / s.
[0182] The laser parameters set for the third solid part of the first border slicing sub-region and the second border slicing sub-region in the second slicing area in the first layer of the transition layer slicing layer include laser power: 78W, laser scanning speed: 2000mm / s, laser scanning spacing: 0.04mm; the laser parameters set for the third contour part of the first border slicing sub-region and the second border slicing sub-region include laser power: 40W, laser scanning speed: 1300mm / s.
[0183] The laser parameters set for the third physical parts of the first and fifth of the five third border slice sub-areas in the second slice area in the first layer of the transition layer slicing layer include laser power: 78W, laser scanning speed: 2000mm / s, laser scanning spacing: 0.04mm; the laser parameters set for the third physical parts of the second to fourth of the five third border slice sub-areas include laser power: 45W, laser scanning speed: 1700mm / s, laser scanning spacing: 0.03mm; the laser parameters set for the third contour parts of the five third border slice sub-areas include laser power: 40W, laser scanning speed: 1300mm / s.
[0184] For the third solid part of the first border slicing sub-region and the second border slicing sub-region in the second slicing area in each layer of the second layer and the third layer of the transition layer slicing layer, the laser parameters set include laser power: 90W, laser scanning speed: 1600mm / s, laser scanning spacing: 0.04mm; the laser parameters set for the third contour part of the first border slicing sub-region and the second border slicing sub-region include laser power: 40W, laser scanning speed: 1300mm / s.
[0185] For the third entity parts of the first and fifth of the five third border slice sub-areas in the second slice area in each layer of the second layer and the third layer of the transition layer slicing layer, the laser parameters set include laser power: 90W, laser scanning speed: 1600mm / s, laser scanning spacing: 0.04mm; the laser parameters set for the third entity parts of the second to fourth of the five third border slice sub-areas include laser power: 55W, laser scanning speed: 1500mm / s, laser scanning spacing: 0.03mm; the laser parameters set for the third contour parts of the five third border slice sub-areas include laser power: 40W, laser scanning speed: 1300mm / s.
[0186] For the third solid part of the first border slicing sub-region and the second border slicing sub-region in the second slicing area in each layer from the fourth to the sixth layer of the transition layer slicing layer, the laser parameters set include laser power: 105W, laser scanning speed: 1350mm / s, laser scanning spacing: 0.05mm; the laser parameters set for the third contour part of the first border slicing sub-region and the second border slicing sub-region include laser power: 40W, laser scanning speed: 1300mm / s.
[0187] For the third entity parts of the first and fifth of the five third border slice sub-areas in the second slice area in each layer from the fourth to the sixth layer of the transition layer slicing layer, the laser parameters set include laser power: 105W, laser scanning speed: 1350mm / s, laser scanning spacing: 0.05mm; the laser parameters set for the third entity parts of the second to the fourth of the five third border slice sub-areas include laser power: 70W, laser scanning speed: 1450mm / s, laser scanning spacing: 0.05mm; the laser parameters set for the third contour parts of the five third border slice sub-areas include laser power: 40W, laser scanning speed: 1300mm / s.
[0188] The laser power of the second slicing region of each layer above the sixth layer of the transition layer slicing layer is increased by 18% based on the previous layer until it is the same as the laser power of the three body slicing sub-regions in each layer of the body slicing layer.
[0189] 3.2 Printing
[0190] The metal powder is fed into the 3D printer, and under an argon atmosphere, the oxygen content in the 3D printer is reduced to 300ppm. According to the printing direction, the part of the frame not connected to the transition layer (i.e., the first short side, two C corners on both sides of the first short side, and two long sides of the hollow frame of the titanium alloy mobile phone) is first printed on the substrate based on the planned path of the multi-layer body slicing layer, and then the transition layer is printed on the substrate based on the planned path of the transition layer slicing layer, and then the remaining part of the frame (i.e., the second short side and the C corners on both sides of the second short side) is printed on the transition layer based on the planned path of the body slicing layer to obtain a print on the substrate.
[0191] Titanium alloy powder particle size range: 15-53μm, powder oxygen content 1000ppm, powder fluidity 30.5s / 50g. 3D printer spot diameter setting: 70μm, substrate temperature: 120℃;
[0192] 3.3 Cleaning
[0193] After the printing process is completed, the substrate temperature is cooled to below 70°C, taken out, and the residual powder on the surface is cleaned.
[0194] 4. Stress relief treatment:
[0195] Put the printed part and the substrate into a high vacuum furnace for vacuum annealing. -3 Under the condition of Pa, the substrate and the printed part are first heated to 450°C at a first heating rate of 4°C / min and kept at this temperature for 2h; then heated to 600°C at a second heating rate of 1.5°C / min and kept at this temperature for 12h; after the insulation, they are slowly cooled to room temperature with the furnace.
[0196] 5. Post-processing
[0197] The substrate and transition layer are removed by wire cutting, and the wire cutting direction is perpendicular to the width direction of the hollow frame. Then the metal hollow frame separated by wire cutting is sandblasted, with a sand material diameter of 230 mesh and a sandblasting pressure of 0.3MPa, until the surface color of the part is uniform.
[0198] The method provided in the present application has made fine adjustments to the model design, scanning path and laser process parameters, reduced the heat input in the hollow part, and realized the support-free printing of the vertical metal hollow frame. The material utilization rate is high and the structural strength is high. Traditional CNC or manual removal of support structures is no longer required. The process is simple, the forming accuracy is good, the efficiency is high, no excess metal waste is generated, and the material utilization rate is high.
[0199] The above is only an example embodiment of the present application and is not intended to limit the present application. Although the present application is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principles of the present application shall be included in the protection scope of the present application.
Claims
1. A method for manufacturing a metal hollow frame by 3D printing, characterized in that: The metal hollow frame to be manufactured includes at least three frames and a connecting portion between adjacent frames among the at least three frames, and the method includes: Modeling, including: A main body printing model is established according to the structure of the metal hollow frame; along the printing direction of the 3D printing, the main body printing model includes a suspended part, and the suspended part corresponds to a frame of the metal hollow frame and two connecting parts located on both sides of the frame; Establishing a transition layer model on the surface of the suspended portion, wherein the transition layer model extends in a direction opposite to the printing direction; and Splitting the transition layer model into a first printing model and a second printing model, wherein the first printing model corresponds to the connecting portion, the second printing model corresponds to the frame, and the second printing model includes at least three sub-printing models; Perform slicing and path planning processing, including: The main body printing model, the first printing model and the second printing model are sliced respectively to obtain a multi-layer main body slice layer and at least seven transition layer slice layers, wherein each transition layer slice layer includes a first slice region corresponding to the first printing model and a second slice region corresponding to the second printing model, and each second slice region includes at least three border slice sub-regions corresponding to the at least three sub-printing models; wherein the thickness of the second slice region in the at least seven transition layer slice layers increases first and then decreases as the number of layers increases, until it becomes equal to the thickness of one main body slice layer in the multi-layer main body slice layer; and Performing line scanning on the multi-layer body slice layer and the at least seven layers of transition layer slice layers, thereby completing path planning processing; Feeding metal powder into a 3D printing device, printing in the printing direction based on the planned path, and obtaining a printed part on a substrate, wherein the printed part includes a frame and a transition layer connected to the frame; and The substrate and the transition layer are removed to obtain the metal hollow frame.
2. The method according to claim 1, characterized in that The thickness of the second slicing region in the second layer of the at least seven transition layer slicing layers is 1 to 3 times the thickness of a main body slicing layer in the multi-layer main body slicing layers, the thickness of the second slicing region in each of the third to sixth layers of the at least seven transition layer slicing layers is 1 to 2 times the thickness of a main body slicing layer in the multi-layer main body slicing layers, and the thickness of the second slicing region in the seventh layer of the at least seven transition layer slicing layers is equal to the thickness of a main body slicing layer in the multi-layer main body slicing layers.
3. The method according to claim 1, characterized in that The thickness of the transition layer model is 0.3-3.5 mm, the length of the transition layer model extending in the direction opposite to the printing direction is 0.5-5.5 mm, the connecting portion includes an R angle and / or a C angle, the radius of the R angle is 0.5-6.5 mm, and the angle of the C angle is 45°-75°; The number of the sub-printing models is 3 to 7, and the length of each sub-printing model is ≤65 mm.
4. The method according to claim 1, characterized in that: The thickness of one body slicing layer in the multi-layer body slicing layer is 20-100 μm, the overlapping width of the first slicing area and the second slicing area in each transition layer slicing layer is 0.05-0.15 mm, and the overlapping width of adjacent slicing sub-areas is 0.05-0.15 mm; The at least three border slice sub-regions include a first border slice sub-region, a second border slice sub-region, and a third border slice sub-region located between the first border slice sub-region and the second border slice sub-region, the first border slice sub-region and the second border slice sub-region being adjacent to the first slice region respectively; Each body slice layer includes a first solid portion and a first contour portion, each first slice region includes a second solid portion and a second contour portion, and each border slice sub-region includes a third solid portion and a third contour portion; When line scanning is performed on the multi-layer body slice layer and the at least seven transition layer slice layers, the first contour portion and the first entity portion have a spot compensation of 0.06 to 0.15 mm, the second contour portion and the second entity portion have a spot compensation of 0.06 to 0.15 mm, and the third contour portion and the third entity portion have a spot compensation of 0.1 to 0.15 mm.
5. The method according to claim 4, characterized in that When line scanning is performed on the multi-layer body slice layer, the scanning angle of the first layer of the multi-layer body slice layer is 30° to 70°, and the scanning angles of other layers of the multi-layer body slice layer are increased by 50° to 90° on the scanning angle of the previous layer; When line scanning is performed on the at least seven transition layer slice layers, the scanning angle of the first layer of the at least seven transition layer slice layers is 30° to 70°, and the scanning angles of the other layers of the at least seven transition layer slice layers are increased by 50° to 90° on the scanning angle of the previous layer.
6. The method according to claim 4, characterized in that The metal powder is fed into the 3D printing device, and printing is performed in the printing direction based on the planned path to obtain a printed part on the substrate, including: Setting laser parameters of the 3D printing device; and The metal powder is fed into the 3D printer, and under an inert gas atmosphere, in accordance with the printing direction, the portion of the frame that is not connected to the transition layer is first printed on the substrate based on the planned path of the multi-layer body slicing layer, and then the transition layer is printed based on the planned path of the at least seven transition layer slicing layers, and then the remaining portion of the frame is printed on the transition layer based on the planned path of the multi-layer body slicing layer, to obtain the printed part located on the substrate.
7. The method according to claim 6, characterized in that Setting the laser parameters of the 3D printing device includes: Respectively set laser parameters corresponding to the first entity portion, the first contour portion, the second entity portion, the second contour portion, the third entity portion of the first to sixth layers of the at least seven transition layer slice layers, and the third contour portion of the first to sixth layers of the at least seven transition layer slice layers; and The laser parameters of the other layers of the at least seven transition layer slicing layers are set so that the laser parameters of the other layers of the at least seven transition layer slicing layers change by no more than 20% based on the previous layer until they are the same as the laser parameters of the first solid part and the first contour part.
8. The method according to claim 7, characterized in that The laser parameters set for the first entity part include laser power: 150-320W, laser scanning speed: 800-1500mm / s, laser scanning spacing: 0.05-0.15mm; the laser parameters set for the first contour part include laser power: 150-280W, laser scanning speed: 400-1200mm / s; The laser parameters set for the second entity part include laser power: 150-320W, laser scanning speed: 800-1500mm / s, laser scanning spacing: 0.05-0.15mm; the laser parameters set for the second contour part include laser power: 150-280W, laser scanning speed: 400-1200mm / s; The laser parameters set for the third entity part of the first border slicing sub-region and the second border slicing sub-region of the first to sixth layers of the at least seven transition layer slicing layers include laser power: 40-130W, laser scanning speed: 400-2500mm / s, laser scanning spacing: 0.03-0.08mm; the laser parameters set for the third contour part of the first border slicing sub-region and the second border slicing sub-region of the first to sixth layers of the at least seven transition layer slicing layers include laser power: 40-100W; laser scanning speed: 500-1800mm / s; The laser parameters set for the third entity part of the third border slicing sub-area of the first to sixth layers of the at least seven transition layer slicing layers include laser power: 20~110W, laser scanning speed: 600~2500mm / s, laser scanning spacing: 0.03~0.07mm; the laser parameters set for the third contour part of the third border slicing sub-area of the first to sixth layers of the at least seven transition layer slicing layers include laser power: 40~100W; laser scanning speed: 500~1800mm / s.
9. The method according to claim 7, characterized in that: Setting the laser parameters of the 3D printing device also includes: Setting the spot diameter range and substrate temperature of the 3D printer; The diameter of the light spot is in the range of 50 to 90 μm, and the temperature of the substrate is in the range of 25 to 200° C.
10. The method according to claim 1, characterized in that The metal hollow frame includes four frames and four connecting parts. The metal powder is titanium alloy powder. The particle size range of the titanium alloy powder is 15 to 85 μm, the powder oxygen content is ≤1300 ppm, and the powder fluidity is ≤35 s / 50 g.
11. The method according to claim 1, characterized in that: Also includes: The substrate and the printed part are subjected to vacuum annealing, comprising: At vacuum degree <10 -3 Pa, firstly heat the substrate and the printed part to 300-500°C at a first heating rate of <5°C / min, and keep them warm for 1-2h; then heat them to 550-850°C at a second heating rate of <3°C / min, and keep them warm for 4-15h; after the insulation is completed, slowly cool them to room temperature with the furnace.
12. A metal hollow frame made by the method according to any one of claims 1 to 11.
Citation Information
Cited By
Method and system for constructing 3D printing model of titanium alloy stent
CN120163022A
High-precision high-pressure-resistant square box body assembly and 3D printing method thereof
CN120790963A
High-precision high-pressure-resistant square box body assembly and 3D printing method thereof
CN120790963B