Lithium-rich manganese-based positive electrode precursor material as well as preparation method and application thereof
By setting a gradient distribution of manganese and a porous aluminum hydroxide coating layer in the lithium-rich manganese-based cathode precursor material, the rate performance and cycle performance of the material were solved, and the high discharge capacity and structural stability were improved.
Patent Information
- Application Number
- CN202410956097.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-12
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium-ion batteries and relates to a lithium-rich manganese-based positive electrode precursor material and a preparation method and application thereof. Background Art
[0002] Lithium-rich manganese-based materials have been widely studied and paid attention to due to their high specific capacity (more than 250mAh / g) and high manganese content. They provide high discharge capacity while ensuring its safety and low cost. They are also identified as one of the candidates for the next generation of lithium-ion battery positive electrode materials. Since JR Dahn et al. discovered in 2001 that lithium-rich manganese-based positive electrode materials have ultra-high specific capacity at a charging voltage above 4.5V, lithium-rich manganese-based materials have attracted more and more attention from the scientific research and industry. After modification, the specific capacity of lithium-rich manganese-based materials can reach more than 300mAh / g. The team led by Xia Dingguo of Peking University synthesized lithium-rich manganese-based materials with an O2 structure, with a specific capacity of up to 400mAh / g. In terms of cost, the cobalt and nickel content of lithium-rich manganese-based materials is only about 1 / 3 of that of ternary materials, and can even be cobalt-free, which can reduce the cost of positive electrode materials by 20-40%. Moreover, as the synthesis and modification technologies become more mature, the cost of lithium-rich manganese-based materials will be further reduced. In addition, a higher Mn content also improves the thermal stability of the material and battery safety. Unfortunately, poor rate capability and cycle performance seriously hinder the further application of lithium-rich manganese-based materials and are the main factors limiting their commercialization.
[0003] During the first charging process of lithium-rich manganese-based cathode materials, part of the Li + It is released in the form of Li2O, but cannot be re-embedded during the discharge process, resulting in a low initial charge and discharge efficiency of the material. At the same time, the release of Li2O will cause part of the lattice oxygen to be released to generate oxygen. The generation of oxygen will damage the surface of the electrode, causing the inside of the electrode to be corroded by the electrolyte, resulting in poor stability, causing changes in the surface composition and structure of the material and gradually spreading to the inside. The impedance of the battery increases, resulting in poor cyclability of the material, which seriously affects the life of the battery.
[0004] CN113788500A discloses a surface modification method of a lithium-rich manganese-based positive electrode material and a lithium-rich manganese-based positive electrode material. By mixing the lithium-rich manganese-based material with a stannous salt solution, a tin-surface-modified positive electrode material is obtained, and a higher discharge capacity and cycle performance are obtained. However, the tin salt solution has certain dangers and will cause certain harm to operators during production. CN110890541A discloses a preparation method of a surface-modified lithium-rich manganese-based positive electrode material and a lithium-ion battery. The surface of the lithium-rich manganese-based material is modified by adding a fast ion conductor coating liquid such as a phosphate solution, so that the total alkali content on the surface of the material is significantly reduced, and the first coulomb efficiency and rate are improved. However, the surface modification of the fast ion conductor coating liquid is affected by the liquid concentration and the uniformity of ion dispersion, and the modification process is not easy to control.
[0005] Therefore, how to improve the rate performance and cycle performance of lithium-rich manganese-based positive electrode materials is currently in urgent need of research. Summary of the invention
[0006] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a lithium-rich manganese-based positive electrode precursor material and its preparation method and application. The lithium-rich manganese-based positive electrode precursor material provided by the present invention has a gradient setting of manganese in the core and the transition layer, and the core and the transition layer are naturally connected, and the porous lithium hydroxide coating layer is synergistically coated, so that the lithium-rich manganese positive electrode material prepared from the lithium-rich manganese-based positive electrode precursor has good rate performance and cycle stability.
[0007] To achieve this object, the present invention adopts the following technical solutions:
[0008] In the first aspect, the present invention provides a lithium-rich manganese-based positive electrode precursor material, which includes a manganese-based precursor material core, a manganese-based precursor material transition layer and a porous aluminum hydroxide coating layer from the inside to the outside; the molar ratio of manganese in the manganese-based precursor material transition layer gradually decreases from the surface of the core to the outside.
[0009] The lithium-rich manganese-based positive electrode precursor material provided by the present invention has a gradient setting of manganese in the precursor material in the core and the precursor material in the transition layer, and the manganese content decreases from the inside to the outside (the manganese content in the core gradually decreases, that is, the manganese content in the transition layer decreases gradually), and the core and the transition layer grow closely and are naturally connected, so that a natural gradual transition of the manganese content is achieved, which can effectively alleviate the stress changes and side reactions inside the material during the charge and discharge process. The high manganese content inside ensures the high discharge capacity of the lithium-rich manganese material, and the low manganese content in the middle layer provides the material with a high operating voltage and The structural stability improves the cycle stability of the lithium-rich manganese-based positive electrode material; at the same time, a porous aluminum hydroxide coating layer is formed on the surface of the transition layer, and the thickness is uniform and controllable. On the one hand, it reduces the direct contact between the transition metal and the electrolyte, which plays a role in reducing surface side reactions and stabilizing the structure; on the other hand, the aluminum coating forms a large number of porous structures on the surface, which not only increases the specific surface area of the precursor, but also facilitates the subsequent mixed lithium sintering. At the same time, the positive electrode material inherits the porous structure of the precursor surface, which accelerates the deintercalation of lithium ions during the charge and discharge process and improves the rate performance of the lithium-rich manganese-based positive electrode material. The gradient setting of manganese in the core and transition layer of the precursor material and the aluminum hydroxide surface coating work together to make the lithium-rich manganese-based positive electrode material prepared from the lithium-rich manganese-based positive electrode precursor have good rate performance and cycle stability.
[0010] In the present invention, the manganese concentration gradient distribution and the surface coating of porous aluminum hydroxide must cooperate with each other to achieve the simultaneous improvement of the rate performance and cycle performance of the lithium-rich manganese-based positive electrode material; and in the present invention, if a non-aluminum hydroxide coating layer is selected, such as zirconium hydroxide, the rate performance cannot be improved. Although zirconium hydroxide can also reduce the direct contact between the transition metal and the electrolyte and play a role in stabilizing the structure of the positive electrode material, zirconium hydroxide cannot provide a porous structure on the surface and increase the specific surface area of the precursor, and cannot effectively improve the deintercalation ability of lithium ions during the charge and discharge process, resulting in the inability to improve the rate performance.
[0011] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.
[0012] Preferably, the core of the manganese-based precursor material includes a first manganese-based hydroxide, and the transition layer of the manganese-based precursor material includes a second manganese-based hydroxide.
[0013] Preferably, the first manganese-based hydroxide and the second manganese-based hydroxide each independently further include a transition metal element in addition to the manganese element.
[0014] Preferably, the transition metal element includes nickel and / or cobalt.
[0015] In the present invention, the first manganese-based hydroxide and the second manganese-based hydroxide may include other transition metal elements in addition to manganese, and those skilled in the art may make adaptive selections and adjustments according to actual needs.
[0016] In a second aspect, the present invention provides a method for preparing the lithium-rich manganese-based positive electrode precursor material as described in the first aspect, the preparation method comprising the following steps:
[0017] Adding a first manganese-based mixed salt solution, a precipitant solution and a complexing agent solution in parallel to perform a first coprecipitation reaction to obtain a manganese-based precursor material core;
[0018] After obtaining the core of the manganese-based precursor material, a second manganese-based mixed salt solution is additionally added to the raw material added in parallel, and a second coprecipitation reaction is performed to obtain intermediate particles;
[0019] After obtaining the intermediate particles, stop adding the first manganese-based mixed salt solution and the second manganese-based mixed salt solution, and replace them with adding aluminum salt solution to perform a third coprecipitation reaction to obtain the lithium-rich manganese-based positive electrode precursor material.
[0020] It can be understood that during the reaction processes of the first coprecipitation reaction, the second coprecipitation reaction and the third coprecipitation reaction in the present invention, the precipitant solution and the complexing agent solution are always present, and during the preparation process, the feed flow rate can be adaptively adjusted according to actual needs at different stages.
[0021] The preparation method provided by the present invention realizes the gradient decreasing distribution of manganese from the inside to the outside through a step-by-step co-precipitation reaction, and in the second co-precipitation reaction process, the first manganese-based mixed salt solution and the second mixed salt solution are simultaneously mixed, so that the gradient transition of manganese concentration in the inner core and the transition layer can be realized, and there is no obvious interface distribution between the inner core and the transition layer, and they are naturally connected; at the same time, through the third co-precipitation reaction, a porous aluminum hydroxide coating layer with uniform and controllable thickness is directly obtained, so that the lithium-rich manganese-based positive electrode material prepared from the lithium-rich manganese-based positive electrode precursor has good rate performance and cycle stability at the same time; and the preparation method is simple and easy to control, does not need to add a complicated preparation process, and is suitable for large-scale production.
[0022] In the present invention, during the second coprecipitation reaction, if the addition of the first manganese-based mixed salt solution is stopped and directly replaced with the second manganese-based mixed salt solution, the natural connection between the inner core and the transition layer cannot be maintained, and the manganese content cannot be naturally transitioned, resulting in a large difference in the content of transition metal elements between the inner core and the transition layer, obvious interface stratification, increased phase boundary resistance between the materials, and poor electrochemical performance of the positive electrode material.
[0023] Preferably, the concentrations of the first manganese-based mixed salt solution and the second manganese-based mixed salt solution are independently 85 to 115 g / L, for example, 85 g / L, 90 g / L, 95 g / L, 100 g / L, 105 g / L, 110 g / L or 115 g / L, etc., but are not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0024] Preferably, in the first manganese-based mixed salt solution, the molar amount of manganese accounts for ≥60%, for example, 60%, 63%, 65%, 68%, 70%, 73%, 75%, 78%, 80%, 83%, 85%, 88%, 90%, 93%, 95% or 98%, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0025] Preferably, in the second manganese-based mixed salt solution, the molar amount of manganese accounts for 25% to 55%, for example, 25%, 28%, 30%, 33%, 35%, 38%, 40%, 43%, 45%, 48%, 50%, 53% or 55%, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0026] It should be noted that the molar ratio of manganese in the present invention is the ratio of manganese to the total molar ratio of all metal elements in the mixed salt solution.
[0027] Preferably, the mass fraction of the precipitant solution is 30-35%, for example 30%, 31%, 32%, 33%, 34% or 35%, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0028] Preferably, the concentration of the complexing agent solution is 5-40 g / L, for example 5 g / L, 10 g / L, 15 g / L, 20 g / L, 25 g / L, 30 g / L, 35 g / L or 40 g / L, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0029] Preferably, during the second co-precipitation reaction, the feed rate of the first nickel-cobalt-manganese mixed salt solution V1=VV*t / T, V is the feed rate of the first nickel-cobalt-manganese mixed salt solution during the first co-precipitation reaction, t is the actual reaction time of the second co-precipitation reaction, and T is the theoretical reaction time of the second co-precipitation reaction.
[0030] Preferably, during the second co-precipitation reaction, the feed rate of the second nickel-cobalt-manganese mixed salt solution V2=V*t / T, V is the feed rate of the first nickel-cobalt-manganese mixed salt solution during the first co-precipitation reaction, t is the actual reaction time of the second co-precipitation reaction, and T is the theoretical reaction time of the second co-precipitation reaction (i.e., the total time of the second co-precipitation reaction).
[0031] It should be noted that t is a continuously changing value (e.g., during the reaction, t ranges from 0 to T), and the feed rate changes at any time as t changes.
[0032] In the present invention, during the second coprecipitation reaction, by regulating the feed rate V1=VV*t / T of the first nickel-cobalt-manganese mixed salt solution and the feed rate V2=V*t / T of the second nickel-cobalt-manganese mixed salt solution, the continuous decrease and natural transition of manganese concentration can be better achieved, thereby avoiding structural mutations caused by excessive element differences and affecting the electrochemical properties and structural stability of the positive electrode material.
[0033] Preferably, the reaction temperatures of the first coprecipitation reaction and the second coprecipitation reaction are each independently 50-60°C, for example, 50°C, 51°C, 52°C, 53°C, 54°C, 55°C, 56°C, 57°C, 58°C, 59°C or 60°C, etc., but are not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0034] Preferably, the pH values of the first coprecipitation reaction and the second coprecipitation reaction are each independently 9 to 12, for example 9, 9.3, 9.5, 9.8, 10, 10.3, 10.5, 10.8, 11, 11.3, 11.5, 11.8 or 12, etc., but are not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0035] Preferably, the theoretical reaction time of the second coprecipitation reaction is 10 to 40 h, for example 10 h, 15 h, 20 h, 25 h, 30 h, 35 h or 40 h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0036] Preferably, D501 of the core of the manganese-based precursor material is 5 to 12 μm, for example, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm or 12 μm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0037] Preferably, D502 of the intermediate particles and D501 of the manganese-based precursor material core satisfy: D502-D501=1~5μm, for example 1μm, 2μm, 3μm, 4μm or 5μm, etc., but are not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0038] In the present invention, by further limiting the D501 of the core of the manganese-based precursor material to 5 to 12 μm, and the D502 of the intermediate particles and the D501 of the core of the manganese-based precursor material satisfying the condition of D502-D501=1 to 5 μm, the coordination of high manganese and low manganese precursor materials can be better achieved, and more beneficial performance can be exerted. At the same time, the stress changes and side reactions inside the material during the charge and discharge process are alleviated, and the cycle stability is improved.
[0039] Preferably, the concentration of the aluminum salt solution is 20-50 g / L, for example 20 g / L, 30 g / L, 40 g / L or 50 g / L, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0040] Preferably, the pH value of the third coprecipitation reaction is 8-10, for example 8, 8.3, 8.5, 8.8, 9, 9.3, 9.5, 9.8 or 10, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0041] Preferably, D503 of the manganese-based precursor material and D502 of the intermediate particles satisfy: D503-D502=0.1~2μm, for example 0.1μm, 0.3μm, 0.5μm, 0.8μm, 1μm, 1.3μm, 1.5μm, 1.8μm or 2μm, etc., but are not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0042] In the present invention, by adjusting D503-D502=0.1-2 μm, the thickness of the coating layer of the porous aluminum hydroxide is adjusted, which is more conducive to increasing the deintercalation rate of lithium ions during the charge and discharge process and improving the rate performance.
[0043] Preferably, after the third coprecipitation reaction is completed, solid-liquid separation, washing and drying are performed.
[0044] As a preferred technical solution, the preparation method comprises the following steps:
[0045] Adding a first manganese-based mixed salt solution, a precipitant solution and a complexing agent solution in parallel, wherein the molar amount of manganese accounts for ≥60%, to perform a first coprecipitation reaction, and obtain a manganese-based precursor material core having a D501 of 5 to 12 μm;
[0046] After obtaining the manganese-based precursor material core, a second manganese-based mixed salt solution having a molar amount of manganese of 25% to 55% is additionally added to the raw material added in parallel, and a second coprecipitation reaction is performed to obtain intermediate particles, wherein D502 of the intermediate particles and D501 of the manganese-based precursor material core satisfy: D502-D501=1 to 5 μm;
[0047] After obtaining the intermediate particles, stop adding the first manganese-based mixed salt solution and the second manganese-based mixed salt solution, replace with adding the aluminum salt solution, and perform a third coprecipitation reaction to obtain the manganese-based positive electrode precursor material, wherein the D503 of the manganese-based precursor material and the D502 of the intermediate particles satisfy: D503-D502=0.1-2 μm;
[0048] Among them, during the second co-precipitation reaction process, the feeding rate of the first nickel-cobalt-manganese mixed salt solution V1 = V-Vt / T, and the feeding rate of the second nickel-cobalt-manganese mixed salt solution V2 = Vt / T, V is the feeding rate of the first nickel-cobalt-manganese mixed salt solution during the first co-precipitation reaction, t is the actual reaction time of the second co-precipitation reaction, and T is the theoretical reaction time of the second co-precipitation reaction.
[0049] In addition to the special limitations of the above products and preparation methods, it should be noted that the types of raw materials and preparation parameters (such as the feed flow rate of each substance) in the coprecipitation process provided by the present invention are all conventional technical means, and those skilled in the art can make adaptive selections and adjustments according to actual needs:
[0050] Optionally, the first coprecipitation reaction, the second coprecipitation reaction and the third coprecipitation reaction can be carried out in a reaction kettle having a bottom liquid, that is, before the raw materials for preparing the first coprecipitation reaction are added in parallel, the reaction kettle contains a bottom liquid, the bottom liquid includes water and alkali solution, and the pH value of the bottom liquid is 11 to 13;
[0051] Optionally, the salt in the first nickel-cobalt-manganese mixed salt solution and the second nickel-cobalt-manganese mixed salt solution includes but is not limited to at least one of chloride, sulfate, acetate or nitrate;
[0052] Optionally, the precipitant solution includes an alkali solution, such as a sodium hydroxide solution and / or a potassium hydroxide solution;
[0053] Optionally, the complexing agent solution includes but is not limited to at least one of an aqueous ammonia solution, a sodium acetate solution, a sodium oxalate solution or ethylenediaminetetraacetic acid (EDTA);
[0054] Optionally, the stirring speeds of the first coprecipitation reaction, the second coprecipitation reaction and the third coprecipitation reaction are each independently 400 to 800 rpm;
[0055] Optionally, the washing process includes washing with alkali solution and pure water 3 to 5 times in sequence;
[0056] Optionally, the drying temperature may be 80-130°C.
[0057] In a third aspect, the present invention provides a lithium-rich manganese-based positive electrode material, which is obtained by mixing and sintering the lithium-rich manganese-based positive electrode precursor material as described in the first aspect or the lithium-rich manganese-based positive electrode precursor material prepared by the preparation method as described in the second aspect with a lithium source.
[0058] The lithium-rich manganese-based positive electrode material provided by the present invention has a core and a transition layer that realize a manganese gradient design (the core has a higher manganese content, and the transition layer has a lower manganese content). At the same time, after sintering, the aluminum hydroxide coating layer forms an aluminum oxide coating with a dense structure and a uniform and controllable thickness, thereby ensuring that the rate performance and cycle performance of the lithium-rich manganese-based positive electrode material are effectively improved.
[0059] It should be noted that the preparation process of the lithium-rich manganese-based positive electrode material in the present invention is a conventional technical solution, and those skilled in the art can adaptably select it based on existing conventional technologies.
[0060] Exemplarily, the present invention provides a method for preparing a lithium-rich manganese-based positive electrode material:
[0061] The lithium source and the lithium-rich manganese-based positive electrode precursor material are mixed at a total molar ratio of the lithium element in the lithium source to all metal elements in the lithium-rich manganese-based positive electrode precursor material of (1.2-1.6):1, and after mixing, they are sintered in an oxygen-containing atmosphere (such as an air atmosphere or an oxygen atmosphere) at a sintering temperature of 800-1200° C. and a sintering time of 8-20 hours to obtain the lithium-rich manganese-based positive electrode material;
[0062] Furthermore, the lithium source includes at least one of LiOH, CH3COOLi or Li2CO3.
[0063] Due to space limitations and to avoid redundancy, the present invention does not list all point values within the above numerical range one by one, but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0064] In a fourth aspect, the present application also provides a positive electrode material, which is obtained by the above-mentioned method for preparing the positive electrode material.
[0065] In a fifth aspect, the present invention further provides a lithium-ion battery, wherein the lithium-ion battery comprises the lithium-rich manganese-based positive electrode material as described in the third aspect.
[0066] Compared with the prior art, the present invention has the following beneficial effects:
[0067] (1) The lithium-rich manganese-based positive electrode precursor material provided by the present invention has a manganese gradient setting in the precursor material in the core and the precursor material in the transition layer, and the manganese content decreases from the inside to the outside (the manganese content in the core gradually decreases, that is, the manganese content in the transition layer decreases gradually), and the core and the transition layer grow closely and are naturally connected, realizing a natural gradual transition of the manganese content, which can effectively alleviate the stress changes and side reactions inside the material during the charge and discharge process. The high manganese content inside ensures the high discharge capacity of the lithium-rich manganese material, and the low manganese content in the middle layer provides the material with a high working voltage. The pressure and structural stability of the lithium-rich manganese-based positive electrode material are improved, and the cycle stability of the lithium-rich manganese-based positive electrode material is improved; at the same time, a porous aluminum hydroxide coating layer is formed on the surface of the transition layer, and the thickness is uniform and controllable. On the one hand, it reduces the direct contact between the transition metal and the electrolyte, and plays a role in reducing surface side reactions and stabilizing the structure; on the other hand, the aluminum coating forms a large number of porous structures on the surface, which not only increases the specific surface area of the precursor, but also facilitates the subsequent mixed lithium sintering. At the same time, the positive electrode material inherits the porous structure of the precursor surface, which accelerates the deintercalation of lithium ions during the charge and discharge process and improves the rate performance of the lithium-rich manganese-based positive electrode material. The gradient setting of manganese in the core and transition layer of the precursor material and the aluminum hydroxide surface coating work together to make the lithium-rich manganese-based positive electrode material prepared from the lithium-rich manganese-based positive electrode precursor have good rate performance and cycle stability.
[0068] (2) The preparation method provided by the present invention realizes a gradient reduction distribution of manganese from the inside to the outside through a step-by-step co-precipitation reaction, and during the second co-precipitation reaction, the first manganese-based mixed salt solution and the second mixed salt solution are simultaneously mixed, which can realize a natural transition of the manganese content in the inner core and the transition layer, and there is no obvious interface distribution between the inner core and the transition layer, and the inner core and the transition layer are tightly combined to achieve a natural connection; at the same time, through the third co-precipitation reaction, a porous aluminum hydroxide coating layer with uniform and controllable thickness is directly obtained, so that the lithium-rich manganese-based positive electrode material prepared from the lithium-rich manganese-based positive electrode precursor has good rate performance and cycle stability; and the preparation method is simple and easy to control, without the need to add a complex preparation process, and is suitable for large-scale production. DETAILED DESCRIPTION
[0069] The technical scheme of the present invention is further illustrated by specific examples below. Those skilled in the art should understand that the examples are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0070] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in this application are intended to cover non-exclusive inclusions.
[0071] In the description of this application, technical terms such as "first" and "second" are only used to distinguish different objects and cannot be understood as indicating or implying relative importance or implicitly indicating the quantity, specific order or primary and secondary relationship of the indicated technical features.
[0072] Example 1
[0073] The present embodiment provides a lithium-rich manganese-based positive electrode precursor material, which includes a manganese-based precursor material core, a manganese-based precursor material transition layer and a porous aluminum hydroxide coating layer from the inside to the outside; the molar ratio of manganese in the manganese-based precursor material transition layer decreases gradually from the surface of the core to the outside;
[0074] Wherein, the molar ratio of manganese in the first nickel-cobalt-manganese hydroxide precursor material is greater than the molar ratio of manganese in the second nickel-cobalt-manganese hydroxide precursor material;
[0075] The preparation method of the lithium-rich manganese-based positive electrode precursor material is as follows:
[0076] A first nickel-cobalt-manganese mixed sulfate solution A with a nickel-cobalt-manganese molar ratio of 0.20:0.10:0.70 and a second nickel-cobalt-manganese mixed sulfate solution B with a nickel-cobalt-manganese molar ratio of 0.50:0.10:0.40 are respectively prepared, and the mass concentrations of both are 100 g / L, and an aluminum sulfate solution with a mass concentration of 30 g / L is prepared, and a 33% sodium hydroxide solution is prepared as a precipitant solution and 20 g / L ammonia water is prepared as a complexing agent solution;
[0077] Pure water and sodium hydroxide solution were added into the reaction kettle as reaction bottom liquid, nitrogen was introduced, and the initial pH value of the bottom liquid was controlled to be 11.8;
[0078] (1) adding solution A (a first nickel-cobalt-manganese mixed salt solution), a sodium hydroxide solution and an ammonia solution into a reactor simultaneously and in parallel by a metering pump, controlling the feed flow rate of solution A to be 1.2 L / h, setting the stirring speed of the reactor to be 600 rpm, controlling the reaction temperature to be 58° C., and controlling the pH to be between 10.0 and 11.5 to perform a one-step coprecipitation reaction (a first coprecipitation reaction), stopping the feeding when the median particle size of the particles reaches 6.5 μm, and obtaining a first nickel-cobalt-manganese hydroxide precursor material core (D501 is 6.5 μm);
[0079] (2) Changing the flow rate of the mixed salt solution A to V1=1.2-0.08t, starting to introduce the mixed salt solution B, setting the flow rate to V2=0.08t, and after the two are evenly mixed, adding the mixed salt solution to the reactor simultaneously with the sodium hydroxide solution and the ammonia solution, controlling the pH between 10.0-11.5 to carry out a two-step coprecipitation reaction (second coprecipitation reaction), and stopping the feeding after the reaction is carried out for 15h (T=15h, t increases continuously from 0h to 15h), and obtaining a lithium-rich manganese precursor (intermediate particles, the intermediate particles are the first nickel-cobalt-manganese hydroxide precursor material core and the second nickel-cobalt-manganese hydroxide precursor material transition layer coated on the core) with a particle size of 9μm (D502-D501=2.5μm) and a concentration gradient distribution;
[0080] (3) adding aluminum sulfate solution, sodium hydroxide solution and ammonia water with a mass concentration of 30 g / L into the reactor simultaneously and in parallel, controlling the pH between 8.0 and 10.0 to carry out a three-step coprecipitation reaction (third coprecipitation reaction), and stopping the feeding when the median particle size of the particles reaches 10 μm (D503-D502=1 μm);
[0081] (4) After the reaction, the slurry is transferred to a suction filtration bottle, and washed three times with alkali solution and pure water respectively; then the solid material obtained by suction filtration and washing is transferred to an oven and dried at 100° C. to finally obtain the lithium-rich manganese-based positive electrode precursor material.
[0082] Example 2
[0083] The present embodiment provides a lithium-rich manganese-based positive electrode precursor material, which includes a manganese-based precursor material core, a manganese-based precursor material transition layer and a porous aluminum hydroxide coating layer from the inside to the outside; the molar ratio of manganese in the manganese-based precursor material transition layer decreases gradually from the surface of the core to the outside;
[0084] Wherein, the molar ratio of manganese in the first nickel-cobalt-manganese hydroxide precursor material is greater than the molar ratio of manganese in the second nickel-cobalt-manganese hydroxide precursor material;
[0085] The preparation method of the lithium-rich manganese-based positive electrode precursor material is as follows:
[0086] A first nickel-cobalt-manganese mixed sulfate solution A having a nickel-cobalt-manganese molar ratio of 0.25:0.10:0.65 and a second nickel-cobalt-manganese mixed sulfate solution B having a nickel-cobalt-manganese molar ratio of 0.55:0.10:0.35 are respectively prepared, and the mass concentrations of both are 90 g / L, a sodium aluminate solution having a mass concentration of 25 g / L is prepared, and a 33% sodium hydroxide solution is prepared as a precipitant solution and 15 g / L ammonia water is prepared as a complexing agent solution;
[0087] Pure water and sodium hydroxide solution were added into the reaction kettle as reaction bottom liquid, nitrogen was introduced, and the initial pH value of the bottom liquid was controlled to be 12.0;
[0088] (1) adding solution A (a first nickel-cobalt-manganese mixed salt solution), a sodium hydroxide solution and an ammonia solution into a reactor simultaneously and in parallel by a metering pump, controlling the feed flow rate of solution A to be 1.0 L / h, setting the stirring speed of the reactor to be 400 rpm, controlling the reaction temperature to be 50° C., and controlling the pH to be between 9.5 and 11 to perform a one-step coprecipitation reaction (a first coprecipitation reaction), stopping the feeding when the median particle size of the particles reaches 7 μm, and obtaining a first nickel-cobalt-manganese hydroxide precursor material core (D501 is 7 μm);
[0089] (2) Changing the flow rate of the mixed salt solution A to V1=1-0.05t, starting to introduce the mixed salt solution B, setting the flow rate to V2=0.05t, and after the two are evenly mixed, adding the mixed salt solution to the reactor simultaneously with the sodium hydroxide solution and the ammonia solution, controlling the pH between 9.5-11.0 to carry out a two-step coprecipitation reaction (second coprecipitation reaction), and stopping the feeding after the reaction is carried out for 20h (T=20h, t gradually increases from 0h to 20h), and obtaining a lithium-rich manganese precursor (intermediate particles, the intermediate particles are the first nickel-cobalt-manganese hydroxide precursor material core and the second nickel-cobalt-manganese hydroxide precursor material transition layer coated on the core) with a particle size of 10μm (D502-D501=3μm) and a concentration gradient distribution;
[0090] (3) adding a sodium aluminate solution, a sodium hydroxide solution and an ammonia solution with a mass concentration of 25 g / L into the reactor simultaneously and in parallel, controlling the pH between 8.0 and 10.0 to carry out a three-step coprecipitation reaction (the third coprecipitation reaction), and stopping the feeding when the median particle size of the particles reaches 10.1 μm (D503-D502=0.1 μm);
[0091] (4) After the reaction, the slurry is transferred to a suction filtration bottle, and washed three times with alkali solution and pure water respectively; then the solid material obtained by suction filtration and washing is transferred to an oven and dried at 100° C. to finally obtain the lithium-rich manganese-based positive electrode precursor material.
[0092] Example 3
[0093] The present embodiment provides a lithium-rich manganese-based positive electrode precursor material, which includes a manganese-based precursor material core, a manganese-based precursor material transition layer and a porous aluminum hydroxide coating layer from the inside to the outside; the molar ratio of manganese in the manganese-based precursor material transition layer decreases gradually from the surface of the core to the outside;
[0094] Wherein, the molar ratio of manganese in the first nickel-cobalt-manganese hydroxide precursor material is greater than the molar ratio of manganese in the second nickel-cobalt-manganese hydroxide precursor material;
[0095] The preparation method of the lithium-rich manganese-based positive electrode precursor material is as follows:
[0096] A first nickel-cobalt-manganese mixed sulfate solution A having a nickel-cobalt-manganese molar ratio of 0.20:0.10:0.70 and a second nickel-cobalt-manganese mixed sulfate solution B having a nickel-cobalt-manganese molar ratio of 0.50:0.10:0.40 are respectively prepared, and the mass concentrations of both are 95 g / L, and an aluminum sulfate solution having a mass concentration of 26 g / L is prepared, and a 35% sodium hydroxide solution is prepared as a precipitant solution and a 10 g / L ammonium oxalate solution is prepared as a complexing agent solution;
[0097] Pure water and sodium hydroxide solution were added into the reaction kettle as reaction bottom liquid, nitrogen was introduced, and the initial pH value of the bottom liquid was controlled to be 12.5;
[0098] (1) adding solution A (a first nickel-cobalt-manganese mixed salt solution), a sodium hydroxide solution and an ammonia solution into a reactor simultaneously and in parallel by a metering pump, controlling the feed flow rate of solution A to be 1.2 L / h, setting the stirring speed of the reactor to be 600 rpm, controlling the reaction temperature to be 58° C., and controlling the pH to be between 10.5 and 11.5 to perform a one-step coprecipitation reaction (a first coprecipitation reaction), stopping the feeding when the median particle size of the particles reaches 6.5 μm, and obtaining a first nickel-cobalt-manganese hydroxide precursor material core (D501 is 6.5 μm);
[0099] (2) changing the flow rate of the mixed salt solution A to V1=1.2-0.08t, starting to introduce the mixed salt solution B, setting the flow rate to V2=0.08t, and after the two are evenly mixed, adding the mixed salt solution B into the reactor simultaneously with the sodium hydroxide solution and the ammonia solution, controlling the pH between 10.5-11.5 to carry out a two-step coprecipitation reaction (second coprecipitation reaction), and stopping the feeding after the reaction is carried out for 15h (t=15h, t gradually increases from 0h to 15h), and obtaining a lithium-rich manganese precursor (intermediate particles, the intermediate particles are the first nickel-cobalt-manganese hydroxide precursor material core and the second nickel-cobalt-manganese hydroxide precursor material transition layer coated on the core) with a particle size of 7.5μm (D502-D501=1μm) and a concentration gradient distribution;
[0100] (3) adding aluminum sulfate solution, sodium hydroxide solution and ammonium oxalate solution with a mass concentration of 26 g / L into the reactor simultaneously and in parallel, controlling the pH between 8.0 and 10.0 to carry out a three-step coprecipitation reaction (third coprecipitation reaction), and stopping the feeding when the median particle size of the particles reaches 9.5 μm (D503-D502=2 μm);
[0101] (4) After the reaction, the slurry is transferred to a suction filtration bottle, and washed three times with alkali solution and pure water respectively; then the solid material obtained by suction filtration and washing is transferred to an oven and dried at 100° C. to finally obtain the lithium-rich manganese-based positive electrode precursor material.
[0102] Example 4
[0103] The difference between this embodiment and embodiment 1 is that in step (2) of this embodiment, the D502 of the intermediate particles is 11.5 μm (D502-D501=5 μm), and the preparation parameters are adjusted as follows: the flow rate of the mixed salt solution A is set to V1=1.2-0.048t, and the flow rate of the mixed salt solution B is set to V2=0.048t. After mixing evenly, a second coprecipitation reaction is carried out. After a total of 25 hours (T=25 hours, t gradually increases from 0 hours to 25 hours), the feeding is stopped to obtain intermediate particles with a particle size of 11.5 μm (D502-D501=5 μm).
[0104] The rest of the preparation methods and parameters were the same as those in Example 1.
[0105] Example 5
[0106] The difference between this embodiment and embodiment 1 is that in step (2) of this embodiment, the D502 of the intermediate particles is 7 μm (D502-D501=0.5 μm), and the preparation parameters are adjusted as follows: the flow rate of the mixed salt solution A is set to V1=1.2-0.2t, and the flow rate of the mixed salt solution B is set to V2=0.2t. After uniform mixing, a second coprecipitation reaction is carried out. After a total of 6 hours (T=6 hours, t gradually increases from 0 hours to 6 hours), the feeding is stopped to obtain intermediate particles with a particle size of 7 μm (D502-D501=0.5 μm).
[0107] The rest of the preparation methods and parameters were the same as those in Example 1.
[0108] Example 6
[0109] The difference between this embodiment and embodiment 1 is that in step (2) of this embodiment, the D502 of the intermediate particles is 12.5 μm (D502-D501=6 μm), and the preparation parameters are adjusted as follows: the flow rate of the mixed salt solution A is set to V1=1.2-0.04t, and the flow rate of the mixed salt solution B is set to V2=0.04t. After mixing evenly, a second coprecipitation reaction is carried out. After a total of 30 hours (T=25 hours, t gradually increases from 0 hours to 6 hours), the feeding is stopped to obtain intermediate particles with a particle size of 12.5 μm (D502-D501=6 μm).
[0110] The rest of the preparation methods and parameters were the same as those in Example 1.
[0111] Example 7
[0112] The difference between this embodiment and embodiment 1 is that in step (3) of this embodiment, the feeding is stopped when the particle size reaches 12 μm (D503-D502=3 μm).
[0113] The rest of the preparation methods and parameters were the same as those in Example 1.
[0114] Comparative Example 1
[0115] The difference between this comparative example and Example 1 is that the lithium-rich manganese-based positive electrode precursor material provided in this comparative example is a pure first nickel-cobalt-manganese hydroxide core;
[0116] In the preparation method, steps (2) and (3) are not performed.
[0117] The rest of the preparation methods and parameters were the same as those in Example 1.
[0118] Comparative Example 2
[0119] The difference between this comparative example and Example 1 is that the lithium-rich manganese-based positive electrode precursor material provided in this comparative example does not contain a porous aluminum hydroxide coating layer;
[0120] In the preparation method, step (3) is not performed.
[0121] The rest of the preparation methods and parameters were the same as those in Example 1.
[0122] Comparative Example 3
[0123] The difference between this comparative example and Example 1 is that the lithium-rich manganese-based positive electrode precursor material provided in this comparative example does not contain a second nickel-cobalt-manganese hydroxide transition layer;
[0124] In the preparation method, step (2) is not performed, and step (3) is modified to D503-D501=1 μm before stopping the feeding.
[0125] The rest of the preparation methods and parameters were the same as those in Example 1.
[0126] Comparative Example 4
[0127] The difference between this comparative example and Example 1 is that in step (2) of this comparative example, solution A is directly replaced by solution B, that is, during the second coprecipitation reaction, the nickel-cobalt-manganese mixed salt solution is pure second nickel-cobalt-manganese mixed salt solution B.
[0128] The rest of the preparation methods and parameters were the same as those in Example 1.
[0129] [Preparation of lithium-rich manganese-based cathode materials, battery preparation and performance testing]
[0130] Preparation of lithium-rich manganese-based positive electrode material: The lithium-rich manganese-based positive electrode precursor obtained in the above Examples 1-7 and Comparative Examples 1-4 was uniformly mixed with lithium carbonate at a molar ratio of 1:1.5, and sintered at 900° C. in an air atmosphere for 15 hours to obtain the corresponding lithium-rich manganese-based positive electrode material;
[0131] Battery preparation: The lithium-rich manganese-based positive electrode materials, conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) prepared in Examples 1-7 and Comparative Examples 1-4 were weighed in a mass ratio of 8:1:1 and dissolved in N-methylpyrrolidone (NMP) and mixed evenly; then, the slurry was applied on aluminum foil with an applicator and dried in a vacuum drying oven at 80°C for 8h; finally, the aluminum foil was punched into 1.13 cm 2 The positive electrode is obtained by a circular shape;
[0132] The obtained electrode sheet was used as the positive electrode, the lithium metal sheet was used as the counter electrode, and a porous polypropylene membrane (Celgard2400) was used as a separator to separate the positive electrode and the counter electrode. The composition of the electrolyte was: a mixture of 1M LiPF6 and EC, DMC and EMC (EC:DMC:EMC volume ratio = 1:1:1); CR2032 button batteries were assembled in an argon glove box.
[0133] The batteries provided in Examples 1-7 and Comparative Examples 1-4 were subjected to performance tests under the following test conditions:
[0134] Specific surface area (BET) test: The lithium-rich manganese-based positive electrode precursor materials provided in Examples 1-7 and Comparative Examples 1-4 are placed in a U-shaped sample tube, and a mixed gas containing a certain proportion of adsorbate flows through the sample. The adsorption amount of the adsorbate molecule (N2) of the tested sample is determined according to the change in gas concentration before and after adsorption, thereby obtaining the corresponding specific surface area value;
[0135] Specific capacity and cycle performance: The battery was charged and discharged at room temperature (25°C) and 2.5-4.5V at a charge and discharge rate of 0.1C to obtain the initial discharge specific capacity and the capacity retention rate after 100 cycles; the test results are shown in Table 1.
[0136] Rate performance: The rate performance of the battery was tested at different rates of 0.1C, 0.2C, 0.5C, 1C, and 5C. The test results are shown in Table 2.
[0137] Table 1
[0138]
[0139] Table 2
[0140]
[0141]
[0142] From Table 1 and Table 2, we can get:
[0143] From the data results of Examples 1-4, it can be seen that the present invention sets the manganese gradient in the core and the transition layer, and the core and the transition layer are naturally connected, which cooperates with the coating of the porous lithium hydroxide coating layer, so that the lithium-rich manganese-based positive electrode material prepared from the lithium-rich manganese-based positive electrode precursor has good rate performance and cycle stability.
[0144] From the data results of Example 1 and Examples 5 and 6, it can be seen that the difference between D502-D501 is too small, that is, the gradient distribution of manganese is not obvious, which is not conducive to stabilizing the internal structure and improving the cycle performance. However, if the difference is too large, that is, the transition layer is too thick, the overall manganese content will be low, resulting in a low initial discharge capacity.
[0145] From the data results of Example 1 and Example 7, it can be seen that the difference between D503-D502 is too large, that is, the thickness of the aluminum hydroxide coating is too thick, and it is difficult to further improve the cycle stability and rate performance. In addition, the excessively thick aluminum hydroxide coating leads to a high overall aluminum content, resulting in poor electrochemical performance.
[0146] It can be seen from the data results of Example 1 and Comparative Examples 1-3 that the gradient distribution of manganese and the specific aluminum hydroxide coating layer in the present invention must work together to effectively improve the rate performance and cycle stability.
[0147] From the data results of Example 1 and Comparative Example 4, it can be seen that in the second coprecipitation reaction process of the present invention, if only the second nickel-cobalt-manganese mixed salt solution is added, it will be detrimental to the natural connection between the inner core and the transition layer, and obvious interface stratification problems will occur, thereby affecting the overall cyclic stability performance of the material.
[0148] In summary, the present invention realizes a gradient reduction distribution of manganese from the inside to the outside through a step-by-step co-precipitation reaction, and in the second co-precipitation reaction process, the first manganese-based mixed salt solution and the second mixed salt solution are simultaneously mixed, which can realize a natural transition of the manganese content in the inner core and the transition layer, and there is no obvious interface distribution between the inner core and the transition layer, realizing a seamless transition and a natural connection; at the same time, through the third co-precipitation reaction, a porous aluminum hydroxide coating layer with uniform and controllable thickness is directly obtained, so that the lithium-rich manganese positive electrode material prepared from the lithium-rich manganese-based positive electrode precursor has good rate performance and cycle stability; and the preparation method is simple and easy to control, without the need to add a complex preparation process, and is suitable for large-scale production.
[0149] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A lithium-rich manganese-based positive electrode precursor material, characterized in that: The lithium-rich manganese-based positive electrode precursor material includes a manganese-based precursor material core, a manganese-based precursor material transition layer and a porous aluminum hydroxide coating layer from the inside to the outside; the molar ratio of manganese in the manganese-based precursor material transition layer decreases gradually from the surface of the core to the outside.
2. The lithium-rich manganese-based positive electrode precursor material according to claim 1, characterized in that: The manganese-based precursor material core includes a first manganese-based hydroxide, and the manganese-based precursor material transition layer includes a second manganese-based hydroxide; Preferably, the first manganese-based hydroxide and the second manganese-based hydroxide each independently include a transition metal element in addition to the manganese element; Preferably, the transition metal element includes nickel and / or cobalt.
3. A method for preparing a lithium-rich manganese-based positive electrode precursor material as claimed in claim 1 or 2, characterized in that: The preparation method comprises the following steps: Adding a first manganese-based mixed salt solution, a precipitant solution and a complexing agent solution in parallel to perform a first coprecipitation reaction to obtain a manganese-based precursor material core; After obtaining the core of the manganese-based precursor material, a second manganese-based mixed salt solution is additionally added to the raw material added in parallel, and a second coprecipitation reaction is performed to obtain intermediate particles; After obtaining the intermediate particles, stop adding the first manganese-based mixed salt solution and the second manganese-based mixed salt solution, and replace with adding aluminum salt solution to perform a third coprecipitation reaction to obtain the lithium-rich manganese-based positive electrode precursor material.
4. The preparation method according to claim 3, characterized in that: The concentrations of the first manganese-based mixed salt solution and the second manganese-based mixed salt solution are independently 85 to 115 g / L; Preferably, in the first manganese-based mixed salt solution, the molar amount of manganese accounts for ≥ 60%; Preferably, in the second manganese-based mixed salt solution, the molar amount of manganese accounts for 25% to 55%; Preferably, the precipitant solution comprises sodium hydroxide solution and / or potassium hydroxide solution; Preferably, the complexing agent solution comprises any one or a combination of at least two of ammonia water, citric acid, sodium oxalate or EDTA; Preferably, the mass fraction of the precipitant solution is 30-35%; Preferably, the concentration of the complexing agent solution is 5 to 40 g / L.
5. The preparation method according to claim 3 or 4, characterized in that: During the second coprecipitation reaction, the feeding rate of the first nickel-cobalt-manganese mixed salt solution is V1=VV*t / T, where V is the feeding rate of the first nickel-cobalt-manganese mixed salt solution during the first coprecipitation reaction, t is the actual reaction time of the second coprecipitation reaction, and T is the theoretical reaction time of the second coprecipitation reaction; Preferably, during the second coprecipitation reaction, the feed rate of the second nickel-cobalt-manganese mixed salt solution is V2=V*t / T, where V is the feed rate of the first nickel-cobalt-manganese mixed salt solution during the first coprecipitation reaction, t is the actual reaction time of the second coprecipitation reaction, and T is the theoretical reaction time of the second coprecipitation reaction; Preferably, the reaction temperature of the first coprecipitation reaction and the second coprecipitation reaction is independently 50 to 60° C.; Preferably, the pH values of the first coprecipitation reaction and the second coprecipitation reaction are independently 9 to 12; Preferably, the theoretical reaction time of the second coprecipitation reaction is 10 to 40 hours.
6. The preparation method according to any one of claims 3 to 5, characterized in that: The D501 of the core of the manganese-based precursor material is 5 to 12 μm; Preferably, D502 of the intermediate particles and D501 of the core of the manganese-based precursor material satisfy: D502-D501=1-5 μm.
7. The preparation method according to any one of claims 3 to 6, characterized in that: The concentration of the aluminum salt solution is 20 to 50 g / L; Preferably, the pH value of the third coprecipitation reaction is 8 to 10; Preferably, the D503 of the manganese-based precursor material and the D502 of the intermediate particles satisfy: D503-D502=0.1-2 μm; Preferably, after the third coprecipitation reaction is completed, solid-liquid separation, washing and drying are performed.
8. The preparation method according to any one of claims 3 to 7, characterized in that: The preparation method comprises the following steps: Adding in parallel a first manganese-based mixed salt solution having a molar amount of manganese of ≥60%, a precipitant solution and a complexing agent solution to perform a first coprecipitation reaction to obtain a manganese-based precursor material core having a D501 of 5 to 12 μm; After obtaining the manganese-based precursor material core, a second manganese-based mixed salt solution having a molar amount of manganese of 25% to 55% is additionally added to the raw material added in parallel, and a second coprecipitation reaction is performed to obtain intermediate particles, wherein D502 of the intermediate particles and D501 of the manganese-based precursor material core satisfy: D502-D501=1 to 5 μm; After obtaining the intermediate particles, stop adding the first manganese-based mixed salt solution and the second manganese-based mixed salt solution, replace with adding the aluminum salt solution, and perform a third coprecipitation reaction to obtain the manganese-based positive electrode precursor material, wherein the D503 of the manganese-based precursor material and the D502 of the intermediate particles satisfy: D503-D502=0.1-2 μm; Among them, during the second co-precipitation reaction process, the feeding rate of the first nickel-cobalt-manganese mixed salt solution V1 = V-Vt / T, and the feeding rate of the second nickel-cobalt-manganese mixed salt solution V2 = Vt / T, V is the feeding rate of the first nickel-cobalt-manganese mixed salt solution during the first co-precipitation reaction, t is the actual reaction time of the second co-precipitation reaction, and T is the theoretical reaction time of the second co-precipitation reaction.
9. A lithium-rich manganese-based positive electrode material, characterized in that: The lithium-rich manganese-based positive electrode material is obtained by mixing and sintering the lithium-rich manganese-based positive electrode precursor material as described in claim 1 or 2 or the lithium-rich manganese-based positive electrode precursor material prepared by the preparation method according to any one of claims 3 to 8 with a lithium source.
10. A lithium ion battery, characterized in that: The lithium-ion battery comprises the lithium-rich manganese-based positive electrode material as claimed in claim 9.
Citation Information
Cited By
Manganese rock salt coated full-concentration gradient positive electrode material and preparation method and application thereof
CN121063596A