Method for preparing cement binding material from acetic acid and carbonic acid composite modified steel slag fine aggregate

The fine aggregate of steel slag is activated through acetic acid carbonic acid composite excitation technology, and modified steel slag cement-based gelling materials are prepared, which solves the problems of steel slag treatment and environmental pollution, improves the mechanical strength of the material, and achieves the goals of resource circulation and environmental protection.

CN118930089APending Publication Date: 2024-11-12SHANXI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411042738.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Steel slag is generated in large quantities and is difficult to deal with during steelmaking, resulting in environmental pollution and waste of resources, and its mineral gelling activity is not fully utilized, affecting the performance of cement-based gelling materials.

Method used

The fine aggregate of steel slag is activated by acetic acid carbonic acid composite excitation technology. By adding the fine aggregate of steel slag to the acetic acid solution and passing it into carbon dioxide gas for composite excitation, then dehydrating and drying and grinding, acetic acid carbonic acid modified steel slag cement-based glue is prepared. Coagulated material.

Benefits of technology

It effectively eliminates free calcium oxide in steel slag, promotes the active blending of cement-based cementitious materials, improves the mechanical strength of the materials, and realizes permanent carbon sequestration, solving resource circulation and environmental protection problems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930089A_ABST
    Figure CN118930089A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of cement gelling materials, particularly relates to a method for preparing a cement gelling material from acetic acid and carbonic acid composite modified steel slag fine aggregate, and aims to provide a method for preparing the cement gelling material, which is low in cost, low in resource consumption, green, environment-friendly and simple in process. The preparation method comprises the following steps: mixing steel slag fine aggregate with acetic acid with a certain concentration, capturing carbon dioxide in a pressurized environment by a wet process for carbonation, synchronously exciting the gelatinization activity of the steel slag, and then grinding, so that the activity of the steel slag is fully improved, and the steel slag-based cementing material is prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of cementitious materials, and in particular relates to a method for preparing cementitious materials by using acetic acid and carbonic acid composite modified steel slag fine aggregate. Background Art

[0002] Steel slag is an alkaline industrial solid waste discharged during the steelmaking process, and its emission accounts for about 15%-20% of crude steel production. At present, about 70% of steel slag is in storage and landfill. The accumulated steel slag not only occupies a large amount of land resources, but also increases the environmental load. Steel slag is rich in active calcium oxide f-CaO, dicalcium silicate, tricalcium silicate and other minerals, which are similar to the components of cement clinker, but the difficult-to-grind components in steel slag cannot be fully activated, making it difficult for some silicate minerals to exert their potential cementing activity. A large number of studies have shown that the calcium carbonate generated in the composite modification of steel slag is beneficial to improve the mechanical strength of steel slag-based cementitious materials. Due to the good thermodynamic stability of carbonates, the carbonation process of alkaline minerals can play an important role in permanent carbon fixation.

[0003] In view of the large amount of steel slag produced by the current steel industry and the environmental protection target requirements, it is of great practical significance to develop a method for preparing cement-based cementitious materials by using acetic acid and carbonic acid composite modified steel slag fine aggregate to promote the realization of resource recycling in the cement industry. Summary of the invention

[0004] In order to solve the problems existing in the background technology, the present invention provides a method for preparing cementitious materials by using acetic acid and carbonic acid composite modified steel slag fine aggregate with low cost, low resource consumption, green environmental protection and simple process.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] The present invention provides a method for preparing cementitious materials by using acetic acid and carbonic acid composite modified steel slag fine aggregate, comprising the following steps:

[0007] Step 1, adding steel slag fine aggregate into an absorption liquid and placing the mixture into a reaction container, wherein the absorption liquid is an acetic acid solution;

[0008] Step 2, introducing carbon dioxide gas into the reaction container to perform composite excitation activation on the steel slag fine aggregate to obtain activated steel slag fine aggregate;

[0009] Step 3: The activated steel slag fine aggregate is removed from the reaction container, and after dehydration, drying and grinding, the cementitious material is obtained.

[0010] Furthermore, the particle size of the steel slag fine aggregate in step 1 is <4.75 mm.

[0011] Furthermore, in step 1, the liquid-to-solid ratio of the absorption liquid to the steel slag fine aggregate is 0.3-0.6:1, and the concentration of the acetic acid solution is 1wt.%-4wt.%.

[0012] Furthermore, in step 2, the purity of the carbon dioxide gas is 95% to 99.9%, and the partial pressure of the carbon dioxide in the reaction container is 0.2 MPa to 0.6 MPa.

[0013] Furthermore, in step 2, the temperature of the composite excitation activation is 150° C. to 220° C., and the time is 2 h to 6 h.

[0014] Furthermore, in step 3, the powder is ground to a particle size less than 0.075 mm.

[0015] The invention also provides a cementitious material prepared by the method.

[0016] Compared with the prior art, the present invention has the following advantages:

[0017] The preparation method of the present invention uses acetic acid and carbonic acid to compositely stimulate the activity of steel slag, modifies the steel slag fine aggregate in a relatively short time and prepares acetic acid and carbonic acid modified steel slag cement-based cementitious material, eliminates free calcium oxide in the steel slag, and plays a role in permanent carbon fixation, and can be used as an active admixture of cement-based cementitious material. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is a scanning electron microscope image of steel slag before it is compositely modified with acetic acid and carbonic acid.

[0019] Figure 2 This is a scanning electron microscope image of steel slag after composite modification by acetic acid and carbonic acid.

[0020] Figure 3 This is the XRD diagram of steel slag before and after composite modification of acetic acid and carbonic acid. DETAILED DESCRIPTION

[0021] In order to characterize the technical effect of the present invention, the acetic acid and carbonic acid composite modified steel slag fine aggregate is used to prepare cement-based cementitious material in the embodiment, and the cement is used to replace cement for slurry test. The mix ratio is 20-40% of the modified steel slag cement-based cementitious material, and the water-binder ratio is 0.35. The mechanical properties are tested, and the free calcium oxide test is carried out according to the cement stability test method.

[0022] In all embodiments of the present invention, the steel slag is screened, and the steel slag selected is steel slag fine aggregate with a particle size of <4.75 mm, and the chemical composition is shown in Table 1:

[0023] Table 1 Chemical composition of steel slag (wt.%)

[0024]

[0025] Example 1

[0026] The method of preparing cementitious materials by using acetic acid and carbonic acid composite modified steel slag fine aggregate in this embodiment includes the following steps:

[0027] Step 1, adding steel slag fine aggregate and absorption liquid into a carbonization reactor, wherein the liquid-to-solid ratio of the absorption liquid to the steel slag fine aggregate is 0.4, and the absorption liquid is a 1wt.% acetic acid aqueous solution;

[0028] Step 2, introducing carbon dioxide gas into the carbonization reactor of step 1 to perform composite excitation activation on the steel slag fine aggregate, the purity of the carbon dioxide gas is 99.9%, the carbon dioxide partial pressure is 0.4 MPa, the reaction temperature is 180±10° C., the reaction time is 4 h, and the activated steel slag fine aggregate is obtained;

[0029] Step 3: The activated steel slag fine aggregate is removed from the carbonization reactor, dehydrated and dried, and ground into a steel slag-based cementitious material with a particle size of less than 0.075 mm.

[0030] According to the water-cement ratio of 0.35, the dosage of steel slag-based cement binder is 20%. It is mixed with cement and added into the cement mortar mixer. Stir at low speed for 2 minutes and at high speed for 2 minutes to obtain cement slurry. Put the cement slurry into the mold and vibrate it evenly on the vibration table for 1 minute to form it. Cover the cement slurry with plastic film and demould it after curing in indoor environment for 24 hours.

[0031] Comparative Example 1

[0032] The difference between this comparative example and Example 1 is that there is no composite modification of acetic acid and carbonic acid, and the fine aggregate of steel slag without any treatment is ground to a steel slag-based cementitious material with a particle size of less than 0.075 mm.

[0033] The compressive strength test was carried out on the samples of Example 1 and Comparative Example 1 according to GB / T17671-1999 "Test method for strength of cement mortar (ISO method)", and the test results are shown in Table 2.

[0034] Table 2 Compressive strength test results of Example 1 and Comparative Example 1

[0035]

[0036] It can be seen from Table 2 that compared with Comparative Example 1, the compressive strength of Example 1 is significantly improved, with the 1d and 3d strengths increased by 21.46% and 33.64%, respectively, and the 7d and 28d strengths increased by 24.82% and 16.32%, respectively.

[0037] Figure 1 , 2By comparison, it can be seen that after the composite modification of acetic acid and carbonic acid, blocky calcite appears in the steel slag, which can provide nucleation sites for the hydration of silicate and promote the hydration reaction of cement. Figure 3 It can be seen that CaCO3 crystal phase appeared in the mineral composition of steel slag after composite modification with acetic acid and carbonic acid, which proves that composite modification with acetic acid and carbonic acid can promote the hydration and carbonation reaction of steel slag and generate calcium carbonate.

[0038] Example 2

[0039] The method of preparing cementitious materials by using acetic acid and carbonic acid composite modified steel slag fine aggregate in this embodiment includes the following steps:

[0040] Step 1, adding steel slag fine aggregate and absorption liquid into a carbonization reactor, wherein the liquid-to-solid ratio of the absorption liquid to the steel slag fine aggregate is 0.4, and the absorption liquid is a 1wt.% acetic acid aqueous solution;

[0041] Step 2, introducing carbon dioxide gas into the carbonization reactor of step 1 to perform composite excitation activation on the steel slag fine aggregate, the purity of the carbon dioxide gas is 99.9%, the carbon dioxide partial pressure is 0.4 MPa, the reaction temperature is 180±10° C., the reaction time is 4 h, and the activated steel slag fine aggregate is obtained;

[0042] Step 3, removing the activated steel slag fine aggregate from the carbonization reactor, dehydrating and drying, and grinding to a steel slag-based cementitious material with a particle size of less than 0.075 mm;

[0043] According to the water-cement ratio of 0.35, the dosage of steel slag-based cementitious material is 40%, which is mixed with cement and added into the cement mortar mixer. Stir at low speed for 2 minutes and at high speed for 2 minutes to obtain cement slurry. Put the cement slurry into the mold and vibrate it evenly on the vibration table for 1 minute to form it. Cover the cement slurry with plastic film and demold it after curing in indoor environment for 24 hours.

[0044] Comparative Example 2

[0045] The difference between this comparative example and Example 2 is that there is no acetic acid and carbonic acid composite modification, and the steel slag fine aggregate without any treatment is ground to a steel slag-based cementitious material with a particle size of less than 0.075 mm.

[0046] The compressive strength test was performed on the samples of Example 2 and Comparative Example 2 according to GB / T17671-1999 "Test method for strength of cement mortar (ISO method)", and the test results are shown in Table 3.

[0047] Table 3 Compressive strength test results of Example 2 and Comparative Example 2

[0048]

[0049] It can be seen from Table 3 that compared with Comparative Example 2, the strength of Example 2 is significantly improved, with the 1d and 3d strengths increased by 49.50% and 244%, respectively, and the 7d and 28d strengths increased by 19.21% and 19.11%, respectively.

[0050] Example 3

[0051] The method of preparing cementitious materials by using acetic acid and carbonic acid composite modified steel slag fine aggregate in this embodiment includes the following steps:

[0052] Step 1, adding steel slag fine aggregate and absorption liquid into a carbonization reactor, wherein the liquid-to-solid ratio of the absorption liquid to the steel slag fine aggregate is 0.4, and the absorption liquid is a 2wt.% acetic acid aqueous solution;

[0053] Step 2, introducing carbon dioxide gas into the carbonization reactor of step 1 to perform composite excitation activation on the steel slag fine aggregate, the purity of the carbon dioxide gas is 99.9%, the carbon dioxide partial pressure is 0.4 MPa, the reaction temperature is 180±10° C., the reaction time is 3 h, and the activated steel slag fine aggregate is obtained;

[0054] Step 3, removing the activated steel slag fine aggregate from the carbonization reactor, dehydrating and drying, and grinding to a steel slag-based cementitious material with a particle size of less than 0.075 mm;

[0055] According to the water-cement ratio of 0.35, the dosage of steel slag-based cementitious material is 20%, which is mixed with cement and added into the cement mortar mixer. Stir at low speed for 2 minutes and at high speed for 2 minutes to obtain cement slurry. Put the cement slurry into the mold and vibrate it evenly on the vibration table for 1 minute to form it. Cover the cement slurry with plastic film and demould it after curing it in indoor environment for 24 hours.

[0056] Comparative Example 3

[0057] The difference between this comparative example and Example 3 is that there is no acetic acid modification and water is used as the absorption liquid.

[0058] The compressive strength test was carried out on the samples of Example 3 and Comparative Example 3 according to GB / T17671-1999 “Test method for strength of cement mortar (ISO method)”. The test results are shown in Table 4.

[0059] Table 4 Compressive strength test results of Example 3 and Comparative Example 3

[0060]

[0061] It can be seen from Table 4 that compared with Comparative Example 3, the strength of Example 3 is significantly improved, with the 1d and 3d strengths being increased by 42.98% and 27.83% respectively, and the 7d and 28d strengths being increased by 18.93% and 19.25% respectively.

[0062] Example 4

[0063] The method of preparing cementitious materials by using acetic acid and carbonic acid composite modified steel slag fine aggregate in this embodiment includes the following steps:

[0064] Step 1, adding steel slag fine aggregate and absorption liquid into a carbonization reactor, wherein the liquid-to-solid ratio of the absorption liquid to the steel slag fine aggregate is 0.4, and the absorption liquid is a 2wt.% acetic acid aqueous solution;

[0065] Step 2, introducing carbon dioxide gas into the carbonization reactor of step 1 to perform composite excitation activation on the steel slag fine aggregate, the purity of the carbon dioxide gas is 99.9%, the carbon dioxide partial pressure is 0.4 MPa, the reaction temperature is 180±10° C., the reaction time is 3 h, and the activated steel slag fine aggregate is obtained;

[0066] Step 3, removing the activated steel slag fine aggregate from the carbonization reactor, dehydrating and drying, and grinding to a steel slag-based cementitious material with a particle size of less than 0.075 mm;

[0067] According to the water-cement ratio of 0.35, the dosage of steel slag-based cementitious material is 40%, which is mixed with cement and added into the cement mortar mixer. Stir at low speed for 2 minutes and at high speed for 2 minutes to obtain cement slurry. Put the cement slurry into the mold and vibrate it evenly on the vibration table for 1 minute to form it. Cover the cement slurry with plastic film and demold it after curing in indoor environment for 24 hours.

[0068] Comparative Example 4

[0069] The difference between this comparative example and Example 4 is that there is no acetic acid modification and water is used as the absorption liquid.

[0070] The compressive strength test was carried out on the samples of Example 4 and Comparative Example 4 according to GB / T17671-1999 “Test method for strength of cement mortar (ISO method)”. The test results are shown in Table 5.

[0071] Table 5 Compressive strength test results of Example 4 and Comparative Example 4

[0072]

[0073]

[0074] It can be seen from Table 5 that compared with Comparative Example 4, the strength of Example 4 is significantly improved, with the 1d and 3d strengths increased by 21.05% and 45.92%, respectively, and the 7d and 28d strengths increased by 20.46% and 9.09%, respectively.

[0075] Example 5

[0076] The method of preparing cementitious materials by using acetic acid and carbonic acid composite modified steel slag fine aggregate in this embodiment includes the following steps:

[0077] Step 1, adding steel slag fine aggregate and absorption liquid into a carbonization reactor, wherein the liquid-to-solid ratio of the absorption liquid to the steel slag fine aggregate is 0.6, and the absorption liquid is a 4wt.% acetic acid aqueous solution;

[0078] Step 2, introducing carbon dioxide gas into the carbonization reactor of step 1 to perform composite excitation activation on the steel slag fine aggregate, the purity of the carbon dioxide gas is 99.9%, the carbon dioxide partial pressure is 0.6 MPa, the reaction temperature is 220±10° C., the reaction time is 2 h, and the activated steel slag fine aggregate is obtained;

[0079] Step 3, removing the activated steel slag fine aggregate from the carbonization reactor, dehydrating and drying, and grinding to a steel slag-based cementitious material with a particle size of less than 0.075 mm;

[0080] According to the water-cement ratio of 0.35, the dosage of steel slag-based cementitious material is 30%, which is mixed with cement and added into the cement mortar mixer. Stir at low speed for 2 minutes and at high speed for 2 minutes to obtain cement slurry. Put the cement slurry into the mold and vibrate it evenly on the vibration table for 1 minute to form it. Cover the cement slurry with plastic film and demould it after curing it in indoor environment for 24 hours.

[0081] Comparative Example 5

[0082] The difference between this comparative example and Example 5 is that there is no acetic acid and carbonic acid composite modification, and the steel slag fine aggregate without any treatment is ground to a steel slag-based cementitious material with a particle size of less than 0.075 mm.

[0083] The compressive strength test was carried out on the samples of Example 5 and Comparative Example 5 according to GB / T17671-1999 "Test method for strength of cement mortar (ISO method)", and the test results are shown in Table 6.

[0084] Table 6 Compressive strength test results of Example 5 and Comparative Example 5

[0085]

[0086] It can be seen from Table 6 that compared with Comparative Example 5, the strength of Example 5 is significantly improved, with the 1d and 3d strengths increased by 141.16% and 96.27%, respectively, and the 7d and 28d strengths increased by 30.24% and 21.10%, respectively.

[0087] Example 6

[0088] The method of preparing cementitious materials by using acetic acid and carbonic acid composite modified steel slag fine aggregate in this embodiment includes the following steps:

[0089] Step 1, adding steel slag fine aggregate and absorption liquid into a carbonization reactor, wherein the liquid-to-solid ratio of the absorption liquid to the steel slag fine aggregate is 0.3, and the absorption liquid is a 3wt.% acetic acid aqueous solution;

[0090] Step 2, introducing carbon dioxide gas into the carbonization reactor of step 1 to perform composite excitation activation on the steel slag fine aggregate, the purity of the carbon dioxide gas is 95%, the carbon dioxide partial pressure is 0.2MPa, the reaction temperature is 150±10°C, the reaction time is 6h, and the activated steel slag fine aggregate is obtained;

[0091] Step 3, removing the activated steel slag fine aggregate from the carbonization reactor, dehydrating and drying, and grinding to a steel slag-based cementitious material with a particle size of less than 0.075 mm;

[0092] According to the water-cement ratio of 0.35, the dosage of steel slag-based cementitious material is 30%, which is mixed with cement and added into the cement mortar mixer. Stir at low speed for 2 minutes and at high speed for 2 minutes to obtain cement slurry. Put the cement slurry into the mold and vibrate it evenly on the vibration table for 1 minute to form it. Cover the cement slurry with plastic film and demould it after curing it in indoor environment for 24 hours.

[0093] Comparative Example 6

[0094] The difference between this comparative example and Example 6 is that there is no acetic acid modification and water is used as the absorption liquid.

[0095] The compressive strength test was carried out on the samples of Example 6 and Comparative Example 6 according to GB / T17671-1999 “Test method for strength of cement mortar (ISO method)”. The test results are shown in Table 7.

[0096] Table 7 Compressive strength test results of Example 6 and Comparative Example 6

[0097]

[0098] It can be seen from Table 7 that compared with Comparative Example 5, the strength of Example 5 is significantly improved, with the 1d and 3d strengths increased by 41.74% and 53.17%, respectively, and the 7d and 28d strengths increased by 12.54% and 8.07%, respectively.

[0099] Example 7

[0100] This example uses the cement stability test method to test free calcium oxide, and the test results of the example are as follows:

[0101] Table 8 Free calcium oxide results of the examples

[0102]

[0103] In addition, it should be understood that although this specification is described according to the implementation modes, not every implementation mode includes only one independent technical solution, and this description of the specification is only for the sake of clarity.

[0104] Those skilled in the art should regard the specification as a whole. The technical solutions in the various embodiments may also be appropriately combined to form other implementation methods that can be understood by those skilled in the art.

Claims

1. A method for preparing cementitious materials by using acetic acid and carbonic acid composite modified steel slag fine aggregate, characterized in that: The steps include: Step 1, adding steel slag fine aggregate into an absorption liquid and placing the mixture into a reaction container, wherein the absorption liquid is an acetic acid solution; Step 2, introducing carbon dioxide gas into the reaction container to perform composite excitation activation on the steel slag fine aggregate to obtain activated steel slag fine aggregate; Step 3: The activated steel slag fine aggregate is removed from the reaction container, and after dehydration, drying and grinding, the cementitious material is obtained.

2. The method for preparing cementitious materials from steel slag fine aggregate modified by acetic acid and carbonic acid according to claim 1, characterized in that: The particle size of the steel slag fine aggregate in step 1 is less than 4.75 mm.

3. The method for preparing cementitious materials from steel slag fine aggregate modified by acetic acid and carbonic acid according to claim 1, characterized in that: In the step 1, the liquid-to-solid ratio of the absorption liquid to the steel slag fine aggregate is 0.3-0.6:1, and the concentration of the acetic acid solution is 1wt.%-4wt.%.

4. The method for preparing cementitious materials from steel slag fine aggregate modified by acetic acid and carbonic acid according to claim 1, characterized in that: The purity of the carbon dioxide gas in step 2 is 95% to 99.9%, and the partial pressure of the carbon dioxide in the reaction container is 0.2 MPa to 0.6 MPa.

5. The method for preparing cementitious materials from steel slag fine aggregate modified by acetic acid and carbonic acid according to claim 1, characterized in that: The temperature of the composite excitation activation in step 2 is 150° C. to 220° C., and the time is 2 h to 6 h.

6. The method for preparing cementitious materials from steel slag fine aggregate modified by acetic acid and carbonic acid according to claim 1, characterized in that: In step 3, the powder is ground to a particle size less than 0.075 mm.

7. The cementitious material prepared by the method according to any one of claims 1 to 6.