Mixed material as well as preparation method and application thereof
By incorporating sodium hydroxide and calcium hydroxide into the shield drying soil, the hydraulic stiffness of the mixed material is stimulated, and the problem of low activity of the mixed material in sulfa aluminate cement is solved, which significantly improves the mechanical properties and hardened slurry. stability.
Patent Information
- Application Number
- CN202411113168.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-14
AI Technical Summary
The low alkalinity of the hardened slurry of sulfaaluminate cement leads to low activity of the mixed material incorporated, which in turn reduces the strength of the sulfaaluminate cement.
Sodium hydroxide is added to the dried shield dry soil for calcination activation, and calcium hydroxide is added during the grinding process. By synergistically stimulating the potential hydraulicity of the mixture, it improves its activity and reduces the activation temperature.
It significantly improves the activity and mechanical properties of the mixed material, improves the low alkalinity environment of sulfur aluminate cement, extends the hydration reaction time, and improves the long-term stability and strength of the hardened slurry.
Smart Images

Figure BDA0004992874040000051
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of building materials, and in particular to a mixed material, a preparation method thereof and an application thereof. Background Art
[0002] Admixtures refer to artificial or natural mineral materials that are added to the mill together with clinker and gypsum when grinding cement to improve cement properties, adjust cement grade, and increase cement production.
[0003] In the related art, when preparing sulphoaluminate cement, limestone, alumina and gypsum with appropriate ingredients are usually used as raw materials, and clinker composed of anhydrous calcium sulphoaluminate and dicalcium silicate as the main minerals is prepared by low-temperature calcination, and then mixed materials are added and ground together. However, sulphoaluminate cement has the characteristic of low alkalinity of hardened paste, which leads to low activity of the mixed materials added, resulting in the defect of reduced strength of sulphoaluminate cement. Summary of the invention
[0004] The purpose of the present application is to provide an admixture, a preparation method and application thereof, which can stimulate the potential hydraulic properties of the admixture to improve the activity of the admixture when preparing sulphoaluminate cement.
[0005] The present application provides a method for preparing a mixed material, comprising:
[0006] Sodium hydroxide is added to the dry shield-dried soil, water is added after the sodium hydroxide is added, mixed and ground, and then dried after the mixed and ground to obtain a powdered raw material;
[0007] The powdered raw material is calcined at 500-680°C, and then rapidly cooled after calcination to obtain clinker;
[0008] Calcium hydroxide is added to the clinker and the mixture is mixed and ground to obtain a mixed material.
[0009] Preferably, the mass fraction of sodium hydroxide is 0.3-3.0wt%.
[0010] Preferably, the powdered raw material is calcined for 30-120 minutes.
[0011] Preferably, the mass fraction of calcium hydroxide is 0.1-3.0wt%.
[0012] Preferably, the rapid cooling is air cooling or water cooling. When the rapid cooling is water cooling, drying is performed after the rapid cooling is completed.
[0013] Preferably, the mass of the added water is 45-55% of the mass of the shield-dried soil after being mixed with sodium hydroxide.
[0014] The present application also provides a mixed material prepared by the mixed material preparation method as described above.
[0015] The embodiments of the present application also provide the use of the admixture as described above in the preparation of sulphoaluminate cement.
[0016] Beneficial effects of this application:
[0017] (1) Provide a method for preparing a mixed material by shield drying soil, wherein an appropriate amount of sodium hydroxide is mixed into the shield drying soil for calcination activation, and an appropriate amount of calcium hydroxide is added during the grinding process, wherein the sodium hydroxide and calcium hydroxide synergistically stimulate the potential water hardness of the mixed material. Mixing sodium hydroxide into the shield drying soil for calcination activation can deeply optimize the shield drying soil structure and effectively improve the activity of the shield drying soil mixed material, and sodium hydroxide has a better fluxing effect and can reduce the activation temperature of the shield drying soil. Adding calcium hydroxide during the grinding process can synergistically modify the shield drying soil prepared by calcination and synergistically improve the low alkaline environment of the slurry. The calcium hydroxide with low solubility and slow rate will stably and long-term stimulate the potential water hardness of the alkali-modified shield drying soil, meet the requirements of the modified shield drying soil for secondary hydration reaction, continuously generate hydration products, continuously improve the slurry structure, and significantly improve the mechanical properties.
[0018] (2) The mixed material prepared by the embodiment of the present application is used to prepare sulphoaluminate cement. Taking full account of the low alkalinity of the hardened slurry of sulphoaluminate cement, a relatively large amount of sodium hydroxide is used to calcine and modify the shield drying soil. This can not only deeply optimize the shield drying soil structure and effectively improve the activity of the shield mixed material, but also improve the low alkalinity environment of the sulphoaluminate hardened slurry. In addition, a relatively large amount of sodium hydroxide has a better fluxing effect and can reduce the activation temperature of the shield drying soil. DETAILED DESCRIPTION
[0019] The present application will be further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0020] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein are only for the purpose of describing the embodiments of this application and are not intended to limit this application.
[0021] The present application provides a method for preparing a mixed material, comprising:
[0022] Sodium hydroxide is added to the dry shield-dried soil, water is added after the sodium hydroxide is added, mixed and ground, and then dried after the mixed and ground to obtain a powdered raw material;
[0023] The powdered raw material is calcined at 500-680°C, and then rapidly cooled after calcination to obtain clinker;
[0024] Calcium hydroxide is added to the clinker and the mixture is mixed and ground to obtain a mixed material.
[0025] Preferably, the mass fraction of sodium hydroxide is 0.3-3.0wt%.
[0026] Preferably, the powdered raw material is calcined for 30-120 minutes.
[0027] Preferably, the mass fraction of calcium hydroxide is 0.1-3.0wt%.
[0028] Preferably, the rapid cooling is air cooling or water cooling. When the rapid cooling is water cooling, drying is performed after the rapid cooling is completed.
[0029] Preferably, the mass of the added water is 45-55% of the mass of the shield-dried soil after being mixed with sodium hydroxide.
[0030] The present application is further described below in conjunction with specific embodiments.
[0031] In the following embodiments and comparative examples, the shield drying soil is mixed with 55.4wt% silicon dioxide, 27.8wt% aluminum oxide, 6.3wt% ferrosoferric oxide, 3.2wt% potassium oxide, 2.1wt% magnesium oxide, 1.3wt% titanium dioxide, 2.0wt% calcium oxide, 1.3wt% sodium oxide and 0.6wt% impurities.
[0032] Example 1
[0033] According to the mass fraction of sodium hydroxide added to the raw material of 0.3wt%, 997.0g of shield drying soil, 3.0g of sodium hydroxide and 450.0g of water were weighed, mixed and ground, and the dried powdered raw material was calcined at 680°C for 40 minutes and then water-cooled and dried to obtain clinker. According to the mass fraction of calcium hydroxide of 3.0wt%, 970.0g of clinker and 30.0g of calcium hydroxide were weighed and ground together to obtain a high-activity mixed material. The activity index of the mixed material was tested with reference to GB / T12957-2005 standard. The results are shown in Table 1, and the activity index is qualified (>65%).
[0034] Example 2
[0035] According to the mass fraction of sodium hydroxide added to the raw material of 3.0wt%, 970.0g of shield drying soil, 30.0g of sodium hydroxide and 550.0g of water were weighed, mixed and ground, and the dried powdered raw material was calcined at 500°C for 120 minutes and then water-cooled and dried to obtain clinker. According to the mass fraction of calcium hydroxide of 2.0wt%, 980.0g of clinker and 20.0g of calcium hydroxide were weighed and ground together to obtain a high-activity mixed material. The activity index of the mixed material was tested with reference to GB / T12957-2005 standard. The results are shown in Table 1, and the activity index is qualified (>65%).
[0036] Example 3
[0037] According to the mass fraction of sodium hydroxide added to the raw material of 1.0wt%, 990.0g of shield drying soil, 10.0g of sodium hydroxide and 500.0g of water were weighed, mixed and ground, and the dried powdered raw material was calcined at 650°C for 30 minutes and then water-cooled and dried to obtain clinker. According to the mass fraction of calcium hydroxide of 0.1wt%, 999.0g of clinker and 1.0g of calcium hydroxide were weighed and ground together to obtain a high-activity mixed material. The activity index of the mixed material was tested with reference to GB / T12957-2005 standard. The results are shown in Table 1, and the activity index is qualified (>65%).
[0038] Example 4
[0039] According to the mass fraction of sodium hydroxide added to the raw material of 2.0wt%, 980.0g of shield drying soil, 20.0g of sodium hydroxide and 500.0g of water were weighed, mixed and ground, and the dried powdered raw material was calcined at 650°C for 100 minutes and then air-cooled to obtain clinker. According to the mass fraction of calcium hydroxide of 2.0wt%, 980.0g of clinker and 20.0g of calcium hydroxide were weighed and ground together to obtain a high-activity mixed material. The activity index of the mixed material was tested with reference to GB / T12957-2005 standard. The results are shown in Table 1, and the activity index is qualified (>65%).
[0040] Comparative Example 1
[0041] According to the mass fraction of sodium hydroxide added to the raw material of 2.0wt%, 980.0g of shield drying soil, 20.0g of sodium hydroxide and 500.0g of water were weighed, mixed and ground, and the dried powdered raw material was calcined at 650°C for 100 minutes and then water-cooled and dried to obtain clinker. According to the mass fraction of calcium hydroxide of 0.01wt%, 999.9g of clinker was weighed and ground with 0.1g of calcium hydroxide to obtain a mixed material. The activity index of the mixed material was tested with reference to GB / T12957-2005 standard. The results are shown in Table 1, and the activity index is unqualified (<65%).
[0042] Comparative Example 2
[0043] According to the mass fraction of sodium hydroxide added to the raw material of 2.0wt%, 980.0g of shield drying soil, 20.0g of sodium hydroxide and 500.0g of water were weighed, mixed and ground, and the dried powdered raw material was calcined at 650°C for 100 minutes and then water-cooled and dried to obtain clinker. According to the mass fraction of calcium hydroxide of 5.0wt%, 950.0g of clinker and 50.0g of calcium hydroxide were weighed and ground together to obtain a mixed material. The activity index of the mixed material was tested with reference to GB / T12957-2005 standard. The results are shown in Table 1, and the activity index is unqualified (<65%).
[0044] Comparative Example 3
[0045] According to the mass fraction of sodium hydroxide added to the raw material of 0.02wt%, 999.8g of shield drying soil, 0.2g of sodium hydroxide and 450.0g of water were weighed, mixed and ground, and the dried powdered raw material was calcined at 650°C for 100 minutes and then water-cooled and dried to obtain clinker. According to the mass fraction of calcium hydroxide of 2.0wt%, 980.0g of clinker and 20.0g of calcium hydroxide were weighed and ground together to obtain a mixed material. The activity index of the mixed material was tested with reference to GB / T12957-2005 standard. The results are shown in Table 1, and the activity index is unqualified (<65%).
[0046] Comparative Example 4
[0047] According to the mass fraction of sodium hydroxide added to the raw material of 5.0wt%, 950.0g of shield drying soil, 50.0g of sodium hydroxide and 550.0g of water were weighed, mixed and ground, and the dried powdered raw material was calcined at 650°C for 100 minutes and then water-cooled and dried to obtain clinker. According to the mass fraction of calcium hydroxide of 2.0wt%, 980.0g of clinker and 20.0g of calcium hydroxide were weighed and ground together to obtain a mixed material. The activity index of the mixed material was tested with reference to GB / T12957-2005 standard. The results are shown in Table 1, and the activity index is unqualified (<65%).
[0048] Comparative Example 5
[0049] According to the mass fraction of sodium hydroxide added to the raw material of 2.0wt%, 980.0g of shield drying soil, 20.0g of sodium hydroxide and 500.0g of water were weighed, mixed and ground, and the dried powdered raw material was calcined at 400°C for 120 minutes and then water-cooled and dried to obtain clinker. According to the mass fraction of calcium hydroxide of 2.0wt%, 980.0g of clinker and 20.0g of calcium hydroxide were weighed and ground together to obtain a mixed material. The activity index of the mixed material was tested with reference to GB / T12957-2005 standard. The results are shown in Table 1, and the activity index is unqualified (<65%).
[0050] Comparative Example 6
[0051] According to the mass fraction of sodium hydroxide added to the raw material of 2.0wt%, 980.0g of shield drying soil, 20.0g of sodium hydroxide and 500.0g of water were weighed, mixed and ground, and the dried powdered raw material was calcined at 650°C for 10 minutes and then water-cooled and dried to obtain clinker. According to the mass fraction of calcium hydroxide of 2.0wt%, 980.0g of clinker and 20.0g of calcium hydroxide were weighed and ground together to obtain a mixed material. The activity index of the mixed material was tested with reference to GB / T12957-2005 standard. The results are shown in Table 1, and the activity index is unqualified (<65%).
[0052] Comparative Example 7
[0053] According to the mass fraction of sodium hydroxide added to the raw material of 2.0wt%, 980.0g of shield drying soil, 20.0g of sodium hydroxide and 500.0g of water were weighed, mixed and ground, and the dried powdered raw material was calcined at 800℃ for 30 minutes and then water-cooled and dried to obtain clinker. According to the mass fraction of calcium hydroxide of 2.0wt%, 980.0g of clinker and 20.0g of calcium hydroxide were weighed and ground together to obtain an active mixed material. The activity index of the mixed material was tested with reference to GB / T12957-2005 standard. The results are shown in Table 1, and the activity index is qualified (>65%).
[0054] Comparative Example 8
[0055] According to the mass fraction of sodium hydroxide added to the raw material of 2.0wt%, 980.0g of shield drying soil, 20.0g of sodium hydroxide and 500.0g of water were weighed, mixed and ground, and the dried powdered raw material was calcined at 680°C for 240 minutes and then water-cooled and dried to obtain clinker. According to the mass fraction of calcium hydroxide of 2.0wt%, 980.0g of clinker and 20.0g of calcium hydroxide were weighed and ground together to obtain an active mixed material. The activity index of the mixed material was tested with reference to GB / T12957-2005 standard. The results are shown in Table 1, and the activity index is qualified (>65%).
[0056] Table 1
[0057]
[0058]
[0059] As shown in Table 1, adding slightly more alkali during the calcination process can optimize the shield drying soil structure and reduce the calcination temperature or time of the shield drying soil, thereby saving production costs. At the same time, matching a small amount of calcium hydroxide as an activator can effectively promote the secondary hydration reaction of the shield drying soil and continuously improve the mechanical properties of the hardened slurry. For example, in Example 4, the activity index of the hardened slurry at 28d is as high as 87.3%.
[0060] Furthermore, by controlling the preparation process parameters (alkali dosage / calcium hydroxide dosage / calcination system, etc.), a better shield drying soil mixture for sulphoaluminate cement can be prepared to match and meet the actual application requirements. It can be seen from Comparative Examples 1 and 2 that too low or too high calcium hydroxide dosage during the hydration process will result in an unqualified activity index, because too low calcium hydroxide dosage will not effectively stimulate the potential water hardness of the alkali-modified shield drying soil; too high dosage will cause the slurry fluidity to deteriorate significantly and form a large number of holes. It can be seen from Comparative Examples 3 and 4 that too low or too high alkali dosage during the calcination process will result in an unqualified shield drying soil activity index, because a small amount of alkali cannot make the activated shield drying soil match the low alkaline environment of the sulphoaluminate cement slurry; excessive alkali will form residues to accelerate the hydration of calcium sulphoaluminate minerals and increase the defects of the hardened slurry. It can be seen from Comparative Examples 5 and 6 that too low calcination temperature or too short time will result in an unqualified activity index, because the alkali-modified shield drying soil reaction cannot effectively occur at this time. It can be seen from Comparative Examples 7 and 8 that a substantial increase in calcination temperature or time will result in a decrease in the activity index, because the initially formed active substances will gradually transform into inactive substances such as nepheline.
[0061] The exemplary embodiments of the present disclosure are specifically shown and described above. It should be understood that the present disclosure is not limited to the configuration or implementation method described herein; on the contrary, the present disclosure is intended to cover various modifications and equivalent configurations contained within the spirit and scope of the appended claims.
Claims
1. A method for preparing a mixed material, It is characterized in that include: Sodium hydroxide is added to the dry shield-dried soil, water is added after the sodium hydroxide is added, mixed and ground, and then dried after the mixed and ground to obtain a powdered raw material; The powdered raw material is calcined at 500-680° C., and then rapidly cooled after calcination to obtain clinker; Calcium hydroxide is added to the clinker and mixed and ground to obtain a mixed material.
2. The method for preparing the mixed material according to claim 1, It is characterized in that The mass fraction of the sodium hydroxide is 0.3-3.0wt%.
3. The method for preparing the mixed material according to claim 1, It is characterized in that The powdered raw material is calcined for 30-120 minutes.
4. The method for preparing the mixed material according to claim 1, It is characterized in that The mass fraction of the calcium hydroxide is 0.1-3.0wt%.
5. The method for preparing the mixed material according to claim 1, It is characterized in that The rapid cooling is air cooling or water cooling. When the rapid cooling is water cooling, drying is performed after the rapid cooling is completed.
6. The method for preparing the mixed material according to claim 1, It is characterized in that The mass of the water added is 45-55% of the mass of the shield dried soil after being mixed with the sodium hydroxide.
7. A mixed material prepared by the method for preparing a mixed material according to any one of claims 1 to 6.
8. Use of the admixture as claimed in claim 7 in the preparation of sulphoaluminate cement.
Citation Information
Patent Citations
Method for preparing clinker-free cement by using weathered tuff
CN103755173A
Regenerated powder solidified shield muck mixed material as well as preparation method and application thereof
CN113979682A
Method for quickly preparing high-activity mixed material at low temperature by utilizing shield dried soil, high-activity mixed material prepared by method and application of high-activity mixed material
CN116102281A