High-permeability and high-strength nano silica sol-based composite grouting material and preparation method thereof
Through the composite of nano-silicon sol and aluminate cement, a composite grouting material with high permeability and high strength is formed, which solves the problem of multi-scale crack enclosed reinforcement of amule rock mass in the prior art, and achieves efficient amule rock mass solidification Knot and anti-seepage effect.
Patent Information
- Application Number
- CN202411129383.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-16
AI Technical Summary
The existing cement-based grouting materials are difficult to meet the closed reinforcement of multi-scale cracks in agrylic rocks, and the nanosilicon sol is used alone with low strength, making it difficult to achieve effective consolidation of agrylic rocks.
Using a nano-silicon sol-based composite grouting material with a mass ratio of 4:5, mixed by composition A (water-containing, aluminate cement and modification admixture) and composition B (nano-silicon sol and coagulant). A composite grouting material with high permeability and high strength is formed to ensure that the interface between the slurry and mudstone is dense, free of voids and excellent adhesion.
The insufficiency is higher than that of conventional cement slurry, the compressive strength reaches ≥10MPa, and the shallow large cracks and seal deep micro cracks at the same time. The material stability is excellent, and it is suitable for grouting and anti-seepage reinforcement of deep muddy rock bodies. .
Smart Images

Figure CN118930199A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of grouting materials, and in particular relates to a high-permeability and high-strength nano-silica sol-based composite grouting material and a preparation method thereof. Technical Background
[0002] Mudstone is widely present in deep underground projects in my country. Due to the presence of a large amount of clay minerals, its engineering characteristics of swelling, softening and disintegration in water can easily lead to long-term large deformation and instability of mudstone surrounding rocks, which seriously affects the safety and stability of underground engineering structures. The physical and mechanical properties of mudstone surrounding rocks can be improved by effectively blocking the dominant seepage channels of surrounding rock fissures by grouting. A large number of studies and practices have shown that deep mudstone presents the characteristics of multi-scale fracture distribution-micro-crack development, and its grouting modification effect is closely related to the injectability of slurry. The particle size of conventional cement-based grouting materials is at the micron level, and the injectability of slurry is poor, which makes it difficult to meet the requirements of micro-crack closure and consolidation. The more developed the micropores of mudstone are, the higher the surface free energy is, and the stronger the adsorption of water is, which makes the cement grouting reinforced rock mass gradually soften and disintegrate, and the strength is weakened. Therefore, the key to grouting reinforcement of multi-scale fractured mudstone is the consolidation of micropores, and the sealing and reinforcement of matrix micropores is the most fundamental problem that cannot be avoided in controlling large deformation of mudstone soft rock.
[0003] Nano-slurry, nano-micro composite slurry, etc. have significant technical advantages and application prospects in the field of grouting prevention and control of mudstone. For example, ultrafine cement has higher injectability in fine cracks than ordinary cement, but it has high fineness, large specific surface area, and is easy to agglomerate. It is necessary to increase the water-cement ratio to reduce the viscosity of the slurry. For example, nano-silica sol has outstanding characteristics such as nano-particle size, low viscosity, and high permeability. It has been promoted and applied to groundwater protection, nuclear waste storage and other fields internationally, but the strength of this slurry is relatively low (<0.5MPa). Grouting with a single material has its disadvantages, so a development trend of grouting materials is composite, using the superposition effect of the performance of multiple components to overcome the performance defects of a single material. At the same time, due to the large number of millimeter-micrometer-nanometer cracks distributed in mudstone, it is difficult to achieve the closure and reinforcement of multi-scale pores and cracks in mudstone using a single-scale slurry. Therefore, a nano-micro-level high-injection and high-strength composite slurry is currently needed to gradient fill and consolidate the multi-scale pores and cracks in mudstone. Summary of the invention
[0004] In view of the shortcomings of the prior art, the present invention provides a high-permeability and high-strength nano-silica sol-based composite grouting material and a preparation method thereof, which has simple steps, is easy to use, does not crack on the slurry surface, and has a dense microstructure with no voids and excellent adhesion at the interface between the slurry and the mudstone.
[0005] In order to achieve the above technical objectives, the present invention provides a high-permeability and high-strength nano-silica sol-based composite grouting material, characterized in that: it is composed of a mixture of a composition A and a composition B in a mass ratio of 4:5, wherein:
[0006] Composition A comprises 35-38% by weight of water, 61-64% by weight of aluminate cement, and 1% by weight of a modifying admixture;
[0007] The composition B comprises 96-99% by mass of nano silica sol and 1-4% by mass of a coagulant.
[0008] Furthermore, the aluminate cement needs to satisfy the following requirements: the mass percentage of Al2O3 is 51-54%, the mass percentage of CaO is 35-37%, the mass percentage of SiO2 is 4-6%, and the specific surface area is ≥400m2 / kg.
[0009] Furthermore, the weight component ratio of the modified admixture is: 75-85 parts of magnesium oxide, 5-10 parts of calcium oxide, and 10-15 parts of sodium silicate; wherein the mass purity of magnesium oxide is not less than 98%, the mass purity of calcium oxide is not less than 98%, and the mass purity of Na2O in sodium silicate is not less than 28.2%.
[0010] Furthermore, the nano silica sol is alkaline industrial silica sol, wherein the concentration of nano silicon dioxide is 10-30%, and the average particle size does not exceed 20 nm.
[0011] Furthermore, the coagulant is a NaCl solution with a mass concentration of 8-10%.
[0012] A method for preparing a high-permeability and high-strength nano-silica sol-based composite grouting material comprises the following steps:
[0013] (1) mixing the water in composition A with aluminate cement and modified admixture, with the stirring time being not less than 3 min and the stirring speed being not less than 500 rpm;
[0014] (2) adding the coagulant in composition B into the nano-silica sol, while adding the coagulant, maintaining continuous stirring, and the stirring time after the addition is not less than 3 minutes, and the stirring rate is not less than 500 revolutions per minute;
[0015] (3) The prepared composition A and composition B are mixed in a mass ratio of 4:5 and stirred for 3-5 min to obtain a nano-silica sol-based composite grouting material.
[0016] Further, composition A is slowly added into composition B, the adding time is not less than 1 min, and the mixing temperature is 15-35°C.
[0017] Beneficial effects: The nano-silica sol-based composite grouting material of the present invention, through the composite of nano-silica sol and special aluminate cement, forms a composite grouting material with nano-micrometer two-level particle size distribution characteristics, with an injectable crack width as low as 50nm and a 3-day compressive strength ≥10MPa. It gives full play to the beneficial characteristics of ultra-high injectability of nano-silica sol and high strength of cement slurry. The injectability is improved by more than 100 times compared with conventional cement slurry, and can simultaneously achieve the dual effects of reinforcing shallow large cracks and sealing deep micro cracks.
[0018] The silica sol-based composite grouting material disclosed in the present invention greatly improves the stability of the slurry and the stone body through the three-level compounding of magnesium oxide, calcium oxide and sodium silicate, realizes that the slurry surface does not crack, the stone rate of the stone body is ≥97.5%, the volume shrinkage rate is ≤0.5%, the long-term volume stability is excellent, the microstructure of the slurry and mudstone interface is dense, free of voids, and has excellent adhesion, and is particularly suitable for grouting anti-seepage reinforcement support engineering of deep muddy fractured rock mass. The material can be adjusted according to the grouting time requirements of different projects by adjusting the proportion of accelerator addition, and the gel time of the material can be controlled within 0.1 to 1.5 hours.
[0019] The preparation method of the silica sol-based composite grouting material of the present invention is simple and easy, has low requirements on production equipment and personnel, has a short production cycle, and all production raw materials are pollution-free, non-toxic, and environmentally friendly, and can be comparable to ultrafine cement. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a surface property diagram of the nano-silica sol-based composite grouting material slurry in an embodiment of the present invention;
[0021] Figure 2 This is a nanometer-scale particle size distribution diagram of the nano-silica sol-based composite grouting material in an embodiment of the present invention;
[0022] Figure 3 is a micron-scale particle size distribution diagram of the nano-silica sol-based composite grouting material in an embodiment of the present invention;
[0023] Figure 4 This is a microstructure diagram of the consolidated body of the nano-silica sol-based composite grouting material in an embodiment of the present invention;
[0024] Figure 5 The microstructure diagram of the interface bonding between the stone body and the mudstone of the patented material of the present invention; (a) is a 2000-fold magnification diagram, (b) is a 5000-fold magnification diagram, and (c) is an 8000-fold magnification diagram;
[0025] Figure 6 This is a diagram of stone body shrinkage and cracking of the nano-silica sol-based composite grouting material in an embodiment of the present invention. DETAILED DESCRIPTION
[0026] An embodiment of the present invention is further described below in conjunction with the accompanying drawings:
[0027] Example 1
[0028] A high-strength nano-silica sol-based composite grouting material is prepared by mixing a composition A and a composition B, wherein the composition A comprises 280 g of water, 512 g of aluminate cement, 6.8 g of magnesium oxide, 0.4 g of calcium oxide, and 0.8 g of sodium silicate; and the composition B comprises 990 g of nano-silica sol and 10 g of NaCl solution.
[0029] The mass percentage of Al2O3 in aluminate cement is 51-54%, the mass percentage of CaO is 35-37%, the mass percentage of SiO2 is 4-6%, and the specific surface area is ≥400m2 / kg. The mass purity of magnesium oxide is not less than 98%, the mass purity of calcium oxide is not less than 98%, and the mass purity of Na2O in sodium silicate is not less than 28.2%. Nano-silica sol is alkaline industrial silica sol, with a silicon dioxide concentration of 30% and an average particle size of 10nm. The mass concentration of NaCl solution is 10%.
[0030] The method for preparing the above material comprises the following steps:
[0031] (1) Mix the water in composition A with aluminate cement and modified admixture, and stir for 3 minutes at a stirring rate of 500 rpm.
[0032] (2) Add the coagulant in composition B into the nano-silica sol, stirring continuously while adding the coagulant. After adding, the stirring time is 3 minutes and the stirring rate is 500 rpm.
[0033] (3) Slowly adding the prepared composition A into the composition B for 1 min, at a mixing temperature of 20° C., and stirring for 3 min to obtain a nano-silica sol-based composite grouting material.
[0034] Example 2
[0035] A high-strength nano-silica sol-based composite grouting material is prepared by mixing a composition A and a composition B, wherein the composition A comprises 296 g of water, 496 g of aluminate cement, 6.4 g of magnesium oxide, 0.56 g of calcium oxide, and 1.04 g of sodium silicate; and the composition B comprises 980 g of nano-silica sol and 20 g of NaCl solution.
[0036] The mass percentage of Al2O3 in aluminate cement is 51-54%, the mass percentage of CaO is 35-37%, the mass percentage of SiO2 is 4-6%, and the specific surface area is ≥400m2 / kg. The mass purity of magnesium oxide is not less than 98%, the mass purity of calcium oxide is not less than 98%, and the mass purity of Na2O in sodium silicate is not less than 28.2%. Nano-silica sol is alkaline industrial silica sol, with a silicon dioxide concentration of 30% and an average particle size of 10nm. The mass concentration of NaCl solution is 10%.
[0037] The method for preparing the above material comprises the following steps:
[0038] (1) Mix the water in composition A with aluminate cement and modified admixture, and stir for 3 minutes at a stirring rate of 500 rpm.
[0039] (2) Add the coagulant in composition B into the nano-silica sol, stirring continuously while adding the coagulant. After adding, the stirring time is 3 minutes and the stirring rate is 500 rpm.
[0040] (3) Slowly adding the prepared composition A into the composition B for 1 min, at a mixing temperature of 20° C., and stirring for 3 min to obtain a nano-silica sol-based composite grouting material.
[0041] Example 3
[0042] A high-strength nano-silica sol-based composite grouting material is prepared by mixing a composition A and a composition B, wherein the composition A comprises 280 g of water, 512 g of aluminate cement, 6 g of magnesium oxide, 0.8 g of calcium oxide, and 1.2 g of sodium silicate; and the composition B comprises 970 g of nano-silica sol and 30 g of NaCl solution.
[0043] The mass percentage of Al2O3 in aluminate cement is 51-54%, the mass percentage of CaO is 35-37%, the mass percentage of SiO2 is 4-6%, and the specific surface area is ≥400m2 / kg. The mass purity of magnesium oxide is not less than 98%, the mass purity of calcium oxide is not less than 98%, and the mass purity of Na2O in sodium silicate is not less than 28.2%. Nano-silica sol is alkaline industrial silica sol, with a silicon dioxide concentration of 30% and an average particle size of 10nm. The mass concentration of NaCl solution is 10%.
[0044] The method for preparing the above material comprises the following steps:
[0045] (1) Mix the water in composition A with aluminate cement and modified admixture, and stir for 3 minutes at a stirring rate of 500 rpm.
[0046] (2) Add the coagulant in composition B into the nano-silica sol, stirring continuously while adding the coagulant. After adding, the stirring time is 3 minutes and the stirring rate is 500 rpm.
[0047] (3) Slowly adding the prepared composition A into the composition B for 1 min, at a mixing temperature of 20° C., and stirring for 3 min to obtain a nano-silica sol-based composite grouting material.
[0048] Comparative Example 1
[0049] The same as Example 1, except that aluminate cement is replaced by silicate cement, and the composition contains 29.7 g of water and 49.5 g of silicate cement.
[0050] Comparative Example 2
[0051] The same as Example 1, except that aluminate cement is replaced by sulphoaluminate cement, and the composition contains 29.7 g of water and 49.5 g of sulphoaluminate cement.
[0052] Comparative Example 3
[0053] The same as Example 1, except that aluminate cement is replaced by silicate cement, and the composition contains 280 g of water and 512 g of silicate cement.
[0054] Comparative Example 4
[0055] The same as Example 1, except that aluminate cement is replaced by sulphoaluminate cement, and the composition contains 280 g of water and 512 g of sulphoaluminate cement.
[0056] Comparative Example 5
[0057] Same as Example 1, except that magnesium oxide is not added.
[0058] Comparative Example 6
[0059] Same as Example 1, except that no calcium oxide is added.
[0060] Comparative Example 7
[0061] Same as Example 1, except that no sodium silicate is added.
[0062] After testing, the nano-silica sol-based composite grouting materials prepared in Examples 1 to 3 have uniform slurry properties and do not shrink or crack. Figure 1 ; The slurry has strong permeability, viscosity, and solidity, such as Figure 2 and Figure 3As shown in the figure, the slurry has a nanometer-micrometer two-level particle size distribution, and the minimum injectable fracture width is as low as 50nm, which is more than 100 times higher than that of cement slurry; the 3-day compressive strength is ≥10MPa, which is more than 100 times higher than that of nano-silica sol stone body, and the microstructure is dense and uniform. Figure 4 The microstructure of the bonding surface in contact with mudstone is dense and void-free. Figure 5 As shown, Figure 5 (a) is a 2000-fold magnification, (b) is a 5000-fold magnification, and (c) is an 8000-fold magnification. The interface adhesion and sealing effect are excellent, which can meet the needs of grouting anti-seepage reinforcement of muddy roadways / tunnels.
[0063] The performance comparison of the nano-silica sol-based composite grouting materials prepared in Comparative Examples 1 to 3 and Example 1 is shown in Table 1.
[0064] Table 1 Performance comparison of nano-silica sol-based composite grouting materials
[0065] Case Gel time / min Compressive strength / MPa Example 1 126 12.7 Comparative Example 1 4.2 0.8 Comparative Example 2 5.5 1.1 Comparative Example 3 ≤0.5 — Comparative Example 4 ≤0.5 —
[0066] According to Table 1, when aluminate cement is replaced by equal weights of silicate cement and sulphoaluminate cement, the composite slurry solidifies instantly, the gel time is ≤0.5min, and the strength cannot be measured. When the addition amount of silicate cement and sulphoaluminate cement becomes 3% of the addition amount of nano-silica sol, the composite slurry has a construction time, and the measured strength is less than one-tenth of that in the embodiment, indicating that with the addition of silicate cement and sulphoaluminate cement, the construction time and compressive strength of the slurry are far from meeting the engineering needs.
[0067] The nano-silica sol-based composite grouting materials prepared in Examples 4 to 6 cannot meet the three-level compounding requirements of the modified admixtures, and the surface of the stone body is generally unevenly deformed, resulting in cracks, such as Figure 6 As shown in the figure, problems such as overall volume shrinkage will cause the rock anti-seepage structure to fail after grouting, and cannot meet the needs of grouting anti-seepage reinforcement of roadways / tunnels.
[0068] The description of the above embodiments is only applicable to help understand the principles of the embodiments of the present invention; at the same time, for those skilled in the art, according to the embodiments of the present invention, there will be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as limiting the present invention.
Claims
1. A high-permeability and high-strength nano-silica sol-based composite grouting material, characterized by: The composition A and the composition B are mixed in a mass ratio of 4:5, wherein: Composition A comprises 35-38% by weight of water, 61-64% by weight of aluminate cement, and 1% by weight of a modifying admixture; The composition B comprises 96-99% by mass of nano silica sol and 1-4% by mass of a coagulant.
2. The high-permeability and high-strength nano-silica sol-based composite grouting material according to claim 1, characterized in that: The aluminate cement needs to satisfy the following requirements: the mass percentage of Al2O3 is 51-54%, the mass percentage of CaO is 35-37%, the mass percentage of SiO2 is 4-6%, and the specific surface area is ≥400m2 / kg.
3. The high-permeability and high-strength nano-silica sol-based composite grouting material according to claim 1, characterized in that: The weight component ratio of the modified admixture is: 75-85 parts of magnesium oxide, 5-10 parts of calcium oxide, and 10-15 parts of sodium silicate; wherein the mass purity of magnesium oxide is not less than 98%, the mass purity of calcium oxide is not less than 98%, and the mass purity of Na2O in sodium silicate is not less than 28.2%.
4. The high-permeability and high-strength nano-silica sol-based composite grouting material according to claim 1, characterized in that: The nano silica sol is alkaline industrial silica sol, in which the concentration of nano silicon dioxide is 10-30% and the average particle size does not exceed 20nm.
5. The high-permeability and high-strength nano-silica sol-based composite grouting material according to claim 1, characterized in that: The coagulant is a NaCl solution with a mass concentration of 8-10%.
6. A method for preparing the high-permeability and high-strength nano-silica sol-based composite grouting material according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) mixing the water in composition A with aluminate cement and modified admixture, with the stirring time being not less than 3 min and the stirring speed being not less than 500 rpm; (2) adding the coagulant in composition B into the nano-silica sol, while adding the coagulant, maintaining continuous stirring, and the stirring time after the addition is not less than 3 minutes, and the stirring rate is not less than 500 revolutions per minute; (3) The prepared composition A and composition B are mixed in a mass ratio of 4:5 and stirred for 3-5 min to obtain a nano-silica sol-based composite grouting material.
7. The high-permeability and high-strength nano-silica sol-based composite grouting material according to claim 1, characterized in that: Slowly add composition A into composition B, the adding time is not less than 1 min, and the mixing temperature is 15-35°C.
Citation Information
Patent Citations
Silica sol slow infiltration reinforcing method of argillaceous soft rock
CN105201528A
Argillaceous soft rock roadway partition multi-granularity grouting reinforcement method
CN107083977A
Low-temperature polymer-fly ash composite synchronous grouting slurry and preparation method thereof
CN116874247A
Early-strength calcium silicate hydrate seed crystal reinforced epoxy composite cement grouting material and preparation method thereof
CN116874255A
Chemical grout composition with enhanced durability and its applications
KR102591539B1